A supercapacitor
By using cyclic electrolyte salts and acetonitrile solvents in supercapacitors and introducing Fe elements into the aluminum current collector, the problems of interfacial bonding force and electrolyte adsorption-desorption resistance were solved, thus realizing a supercapacitor with low impedance and long life.
Patent Information
- Application Number
- CN202611570452.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing supercapacitors have limited interfacial bonding between the aluminum foil current collector and the activated carbon electrode layer, which easily leads to contact degradation. Furthermore, there is resistance to the adsorption and desorption of anions and cations in the electrolyte, resulting in increased impedance and shortened service life, especially under high temperature or high voltage conditions.
An electrolyte salt with a cyclic structure and acetonitrile solvent are used, and trace amounts of Fe are introduced into the aluminum current collector to form Al-Fe intermetallic compounds or Fe oxide nanoparticles. The concentration of the electrolyte salt and the thickness of the aluminum current collector are optimized to improve the interfacial bonding force and ion transport efficiency, and reduce the interfacial resistance.
Low impedance growth and long lifespan of supercapacitors were achieved by optimizing the electrolyte salt concentration and the Fe content in the aluminum current collector, ensuring the orderly adsorption of electrolyte salt cations, reducing interfacial charge transfer resistance, inhibiting corrosion reactions, and extending service life.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochemical technology, specifically to a supercapacitor that can balance low impedance growth and long lifespan. Background Technology
[0002] Supercapacitors primarily store energy through ion adsorption (electrically double-layer capacitors). They are a novel type of energy storage device that falls between batteries and traditional electrostatic capacitors. Supercapacitors can store hundreds or thousands of times more charge than traditional electrolytic capacitors, can be fully charged and discharged within seconds, have higher power input or output than batteries, and can reach full charge in a shorter time. Due to their high power density, long cycle life, and rapid charge / discharge capabilities, supercapacitors are widely used in new energy vehicles, wind power pitch control systems, and power grid frequency regulation. As supercapacitors are increasingly widely adopted, consumers are placing more stringent demands on them, especially regarding longer lifespan and lower impedance (ESR). Therefore, achieving both low impedance and long lifespan is one of the research directions for supercapacitors.
[0003] Currently, commercially available supercapacitor electrolytes mainly use acetonitrile (ACN) or propylene carbonate (PC) solutions of tetraethylammonium tetrafluoroborate (TEABF4) or spirocyclic quaternary ammonium salt (SBPBF4); acetonitrile solutions of N,N-dimethylpyrrolidone tetrafluoroborate (DMPBF4) are also gradually becoming widely used. However, the above-mentioned existing technologies still have the following technical problems: 1. The interfacial bonding force between the aluminum foil current collector and the activated carbon electrode layer is limited. During long-term use, contact deterioration easily occurs between the electrode layer and the current collector, leading to a gradual increase in interfacial resistance; at the same time, the aluminum foil contains BF4... - There is a risk of electrochemical corrosion in organic electrolytes—although the natural oxide layer (Al2O3) on the surface of aluminum foil has a passivation protection effect, under high voltage (≥3.0V), BF4... - The trace amounts of HF produced during decomposition slowly erode the oxide layer, exposing the aluminum substrate and causing localized pitting corrosion, thus accelerating interface deterioration. Secondly, significant resistance remains in the adsorption and desorption of anions and cations in the electrolyte, especially after a period of use under high temperature or high voltage conditions, leading to some degree of blockage in the activated carbon pores. Therefore, these technical issues limit the lifespan of supercapacitors and hinder the reduction of impedance.
[0004] Therefore, developing a supercapacitor that balances long lifespan and low impedance growth is a technical challenge in this field. Summary of the Invention
[0005] Based on this, the purpose of the present invention is to provide a supercapacitor that balances long lifespan and low impedance growth.
[0006] The present invention adopts the following technical solution: A supercapacitor includes a separator, an electrolyte, and two electrode plates. The separator is located between the two electrode plates, and the electrode plates include an aluminum current collector and an active material layer disposed on at least one surface of the aluminum current collector. The aluminum current collector contains Fe element, and the Fe element content is appm based on the total mass of the aluminum current collector; The electrolyte comprises an electrolyte salt and an organic solvent, wherein the organic solvent comprises acetonitrile, and the content of acetonitrile is 45-100% based on the total mass of the organic solvent being 100%. The electrolyte salt includes the compound shown in structural formula 1: Structural Formula 1 Among them, A - It is tetrafluoroborate, where R1 and R2 are each independently selected from C1 to C3 alkyl groups, and n is 0 or 1; The concentration of the compound represented by structural formula 1 in the electrolyte is c mol / L; The supercapacitor satisfies the following conditions: 0.6≤a / c≤700, 1≤a≤500, 0.7≤c≤2.
[0007] The supercapacitor provided by this invention uses a compound with a cyclic structure as shown in Formula 1 as the electrolyte salt. This compound has a smaller cation radius, higher structural rigidity, and significantly better oxidation stability and resistance to voltage decomposition than the traditional TEABF4 and SPBF4 systems. This effectively reduces capacity decay caused by solute decomposition under high voltage, achieving a longer cycle life. Simultaneously, the smaller cation radius allows it to more fully penetrate the microporous structure of activated carbon, reducing ion adsorption / desorption resistance and thus significantly lowering the equivalent series resistance (ESR) of the supercapacitor. Acetonitrile, as an organic solvent, possesses low viscosity, high dielectric constant, and strong coordination ability. It exhibits excellent solubility and dissociation of the quaternary ammonium salt shown in Formula 1, with a solubility of up to 67%, ensuring rapid ion transport in the electrolyte. Furthermore, it possesses high stability, is not easily oxidized, and is not easily decomposed, providing fundamental physical properties for the long lifespan of the supercapacitor. Specifically, introducing a certain amount of Fe into the aluminum current collector can form trace amounts of Al-Fe intermetallic compounds or Fe-containing oxide nanoparticles on the current collector surface. This increases the micro-roughness and surface energy of the current collector surface, enhances the mechanical bonding and physical adsorption between the active material layer and the current collector, and reduces the interfacial contact resistance. Simultaneously, the Fe-based active sites on the current collector surface can guide the orderly adsorption of electrolyte salt cations, forming a more regularly arranged adsorption layer structure at the current collector interface. This further reduces the interfacial charge transfer impedance and ensures the stability of the interfacial structure during long-term use, preventing a continuous increase in contact impedance and ensuring the continued effectiveness of the electrolyte salt's ion transport advantages. Furthermore, the introduction of trace amounts of Fe can alter the distribution of electrochemical active sites on the current collector surface, reduce localized corrosion current density, and inhibit the formation of the electrolyte salt anion tetrafluoroborate (BF4). - Irreversible decomposition reaction on the surface of the current collector.
[0008] Based on the synergistic effect between the concentration (c mol / L) of the compound shown in structural formula 1 in the electrolyte and the Fe content (appm) in the aluminum current collector, the inventors discovered through extensive research that when both conditions are met (0.6 ≤ a / c ≤ 700, 1 ≤ a ≤ 500, 0.7 ≤ c ≤ 2), the distribution of electrochemical active sites on the current collector surface and the electrolyte salt can reach optimal balance. The Fe-based active sites on the aluminum current collector surface guide the orderly adsorption of electrolyte salt cations, forming a more regularly arranged adsorption layer structure at the current collector interface, further reducing the interfacial charge transfer impedance and the local corrosion current density. This avoids the problems of insufficient distribution of electrochemical active sites, increased local corrosion current density, and increased impedance caused by an excessively small ratio, while also preventing the problems of excessive Fe content caused by an excessively large ratio, which reduces the current collector's elongation and bending life, poses a risk of micro-fractures during long-term use, and degrades its lifespan. This achieves a synergistic improvement in low impedance growth and long lifespan. Preferably, the supercapacitor satisfies 6.5 ≤ a / c ≤ 450.
[0009] Introducing a certain amount of Fe into aluminum current collectors can form trace amounts of Al-Fe intermetallic compounds or Fe-containing oxide nanoparticles on the surface of the current collector. This increases the micro-roughness and surface energy of the aluminum current collector surface, enhances the mechanical bonding and physical adsorption between the active material layer and the aluminum current collector, reduces interfacial contact resistance, and improves the stability of the interfacial structure during long-term use. Simultaneously, the introduction of trace Fe can alter the distribution of electrochemical active sites on the surface of the aluminum current collector, reduce localized corrosion current density, and inhibit BF4 corrosion. - Irreversible decomposition reactions occur on the surface of aluminum current collectors, especially under high operating voltages of 3.0V and above. Fe-containing aluminum current collectors exhibit superior corrosion resistance. Excessive Fe content reduces the elongation and bending life of the aluminum current collector, posing a risk of micro-fractures with prolonged use. Specifically, the Fe content in the aluminum current collector is 1 ppm, 5 ppm, 10 ppm, 30 ppm, 50 ppm, 80 ppm, 100 ppm, 150 ppm, 200 ppm, 250 ppm, 300 ppm, 350 ppm, 400 ppm, 450 ppm, 500 ppm, or any two of these ranges; preferably, the Fe content in the aluminum current collector is 10~400 ppm.
[0010] Specifically, in some embodiments of the present invention, the aluminum current collector is aluminum foil, and the Fe element can be introduced into the aluminum current collector in the following ways: Fe element, iron oxide or iron alloy, etc. are added during the aluminum foil casting process, and the Fe element content in the aluminum current collector is controlled by controlling the amount added.
[0011] Specifically, in some embodiments of the present invention, the concentration of the electrolyte salt is limited to achieve rapid ion migration of cations in the organic solvent and reduce the corrosion of the current collector by the electrolyte. Specifically, the concentration c of the compound represented by structural formula 1 is 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.8 mol / L, 2 mol / L, or any two of these ranges; preferably, the concentration c of the compound represented by structural formula 1 is 0.8 mol / L to 1.6 mol / L.
[0012] Specifically, in some embodiments of the present invention, the active material layer includes carbon material and potassium (K) element. The introduction of K element helps improve the electronic conductivity and ion transport performance of the electrode material, reducing electrode impedance; on the other hand, it can be pre-embedded on the inner surface of the electrode pores, constructing ion transport pre-channels and further reducing the adsorption / desorption resistance of cations. However, excessive content can occupy the pores of active materials such as activated carbon, causing reduction and preventing electrolyte cations from utilizing the activated carbon pores, resulting in capacity decay and performance degradation. Specifically, based on the total mass of the active material layer, the mass content of K element in the active material layer is 1 ppm, 5 ppm, 8 ppm, 10 ppm, 30 ppm, 80 ppm, 100 ppm, 150 ppm, 200 ppm, 250 ppm, 300 ppm, 350 ppm, 400 ppm, 450 ppm, 500 ppm, or any two of these ranges. Preferably, the mass content of K element in the active material layer is 30-400 ppm.
[0013] Specifically, in some embodiments of the present invention, potassium (K) can be added to the active material layer in the following ways: by doping the carbon material during its preparation, or by adding potassium salts such as potassium tetrafluoroborate (KBF4) or potassium acetate (CH3COOK) during the slurry preparation process of the electrode plate. The content of potassium in the active material layer is controlled by adjusting the amount of potassium added.
[0014] Specifically, in some embodiments of the present invention, the thickness of the aluminum current collector is 15~40μm. Controlling the thickness of the aluminum current collector within this range, combined with the corrosion resistance of Fe, achieves a synergistic improvement in low impedance growth and long lifespan performance at the structural level. On the one hand, sufficient thickness can resist the corrosion and erosion of the aluminum current collector by the electrolyte under high temperature and high voltage conditions, preventing rapid spikes in contact impedance caused by corrosion perforation and continuous thickening of the interface oxide layer, thus extending the device's float charge and cycle life. On the other hand, controlling the thickness within a reasonable upper limit can prevent excessively high ohmic impedance of the aluminum current collector itself, maintaining a tight bond between the active material layer and the aluminum current collector for a long time, stabilizing the interface contact impedance, and ensuring the device maintains low impedance characteristics over a long period. If the aluminum current collector thickness is too thin, its corrosion resistance and deformation resistance will be insufficient; if the aluminum current collector thickness is too thick, its ohmic impedance will be too high. Specifically, the thickness of the aluminum current collector is 15μm, 18μm, 20μm, 22μm, 25μm, 28μm, 30μm, 32μm, 35μm, 38μm, 40μm or any two of these ranges.
[0015] Specifically, in some embodiments of the present invention, the thickness of the active material layer on one side of the aluminum current collector is 60~200μm. Controlling the thickness of the active material layer within this range achieves a balance between ion transport efficiency and electrode structural stability, resulting in a device with lower impedance and a longer lifespan. A suitable thickness controls the diffusion path length of ions within the active material layer, ensuring rapid ion adsorption and desorption, reducing the ion transport impedance of the electrode, and imparting a lower impedance to the device. Simultaneously, under high temperature and high pressure environments, structural collapse and active material shedding are less likely to occur, maintaining a stable pore structure for a long time and effectively extending the device's lifespan. If the thickness is too large, the ion diffusion path becomes too long, significantly increasing the ion transport impedance; if the thickness is too small, the active material load per unit area is insufficient, leading to excessively high local current density, which exacerbates interfacial side reactions and current collector corrosion, resulting in a shortened device lifespan. Specifically, the thickness of the active material layer on one side of the aluminum current collector is 60μm, 80μm, 100μm, 120μm, 140μm, 160μm, 180μm, 200μm or any two of these ranges.
[0016] Specifically, in some embodiments of the present invention, the content of acetonitrile is 45%, 50%, 55%, 60%, 65%, 70%, 72%, 75%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96%, 100%, or any two of these, based on the total mass of the organic solvent being 100%.
[0017] The cation of the compound shown in Structural Formula 1 is a quaternary ammonium cation with a five / six-membered pyrrolidine / piperidine ring structure. Its cyclic structure endows the cation with high structural rigidity and a small ionic radius, which is beneficial for rapid ion migration in organic solvents. Specifically, in some embodiments of the present invention, the cation of the compound shown in Structural Formula 1 includes one or more of N,N-dimethylpyrrolidine, N,N-diethylpyrrolidine, N,N-dipropylpyrrolidine, N-methyl-N-ethylpyrrolidine, N-ethyl-N-propylpyrrolidine, N,N-dimethylpiperidine, N,N-diethylpiperidine, N,N-dipropylpiperidine, N-methyl-N-ethylpiperidine, N-methyl-N-propylpiperidine, and N-ethyl-N-propylpiperidine.
[0018] More specifically, in some embodiments of the present invention, the compound represented by structural formula 1 includes one or more of N,N-dimethylpyrrolidineonium tetrafluoroborate, N,N-diethylpyrrolidineonium tetrafluoroborate, N,N-dipropylpyrrolidineonium tetrafluoroborate, N-methyl-N-ethylpyrrolidineonium tetrafluoroborate, N-methyl-N-propylpyrrolidineonium tetrafluoroborate, N-ethyl-N-propylpyrrolidineonium tetrafluoroborate, N,N-dimethylpiperidineonium tetrafluoroborate, N,N-diethylpiperidineonium tetrafluoroborate, N,N-dipropylpiperidineonium tetrafluoroborate, N-methyl-N-ethylpiperidineonium tetrafluoroborate, N-methyl-N-propylpiperidineonium tetrafluoroborate, and N-ethyl-N-propylpiperidineonium tetrafluoroborate. Preferably, the electrolyte salt is selected from one or more of N,N-dimethylpyrrolidineonium tetrafluoroborate, N-methyl-N-ethylpyrrolidineonium tetrafluoroborate, N,N-dimethylpiperidineonium tetrafluoroborate, and N-methyl-N-ethylpiperidineonium tetrafluoroborate.
[0019] In a preferred embodiment of the present invention, the organic solvent is acetonitrile, and the compound represented by structural formula 1 is N,N-dimethylpyrrolidone tetrafluoroborate.
[0020] Specifically, in some embodiments of the present invention, the organic solvent further includes sulfolane, and the mass ratio of acetonitrile to sulfolane is 1 to 13.5. Sulfolane has a high boiling point and excellent electrochemical stability. When used in combination with acetonitrile, it can further improve the high-temperature stability of the electrolyte, broaden the upper limit of the supercapacitor's operating temperature, and maintain good ionic conductivity and low-temperature performance of the electrolyte. However, sulfolane has a low freezing point and high viscosity. If the amount used is too high, it will lead to a decrease in the supercapacitor's capacity, excessive impedance, and poor low-temperature performance; while if the amount used is too low, its advantages cannot be realized. More specifically, the mass ratio of acetonitrile to sulfolane is 1, 1.5, 2.1, 3.5, 4, 5, 6.8, 7.4, 8.3, 9, 10, 10.7, 11.5, 12.6, 13.5, or any two of these values.
[0021] Specifically, in some embodiments of the present invention, the carbon material includes one or more of activated carbon, nano-carbon, graphene, lignin carbon, mesoporous carbon, carbon nanotubes, or porous carbon fibers; the single-sided areal density of the active material layer is 50~110 g / m². 2 Specifically, the areal density of the active material layer on one side is 50 g / m³. 2 60g / m 2 70g / m 2 80g / m 2 90g / m 2 100g / m 2 110g / m 2Or the range between any two of them.
[0022] Specifically, in some embodiments of the present invention, the charging cutoff voltage of the supercapacitor is 2.7V~3.2V.
[0023] In specific implementation, the charging cutoff voltage of the supercapacitor can be 2.7V, 2.75V, 2.8V, 2.85V, 2.9V, 2.95V, 3.0V, 3.05V, 3.1V, 3.15V, 3.2V, or any range between two of these. Within the above voltage range, the electrolyte system of the present invention exhibits excellent electrochemical stability, effectively suppressing solute decomposition and side reactions, and ensuring a long cycle life for the supercapacitor.
[0024] Specifically, in some embodiments of the present invention, the operating temperature range of the supercapacitor is -40℃ to 85℃. More preferably, the operating temperature range of the supercapacitor is -40℃ to 65℃. The supercapacitor system of the present invention exhibits high ionic conductivity and good stability over a wide temperature range, ensuring that the supercapacitor maintains low impedance and high capacitance at low temperatures and a long cycle life at high temperatures.
[0025] The supercapacitor of this application uses the compound shown in structural formula 1 as the electrolyte salt, acetonitrile as the organic solvent, and introduces Fe element into the aluminum current collector. The Fe element content 'a' in the aluminum current collector and the concentration 'c' of the compound shown in structural formula 1 are limited to satisfy 0.6≤a / c≤700, 1≤a≤500, and 0.7≤c≤2. The electrolyte salt with a smaller cation radius can effectively reduce the capacity decay caused by solute decomposition under high voltage and achieve a longer cycle life. Acetonitrile has excellent solubility and dissociation for quaternary ammonium salts, ensuring rapid ion transport in the electrolyte. At the same time, the introduction of Fe element into the aluminum current collector can ensure that the electrochemical active sites on the surface of the aluminum current collector reach the optimal balance with the electrolyte salt. Trace amounts of Al-Fe intermetallic compounds or Fe oxide nanoparticles are formed on the surface of the aluminum current collector, which improves the micro-roughness and surface energy of the aluminum current collector surface, enhances the mechanical interlocking and physical adsorption between the active material layer and the aluminum current collector, reduces the interfacial contact resistance, and improves the stability of the interfacial structure during long-term use. Meanwhile, the introduction of trace amounts of Fe can change the distribution of electrochemical active sites on the surface of the aluminum current collector, reduce the local corrosion current density, inhibit the irreversible decomposition reaction of tetrafluoroborate on the surface of the current collector, and improve corrosion resistance, thereby significantly improving the service life of the supercapacitor of the present invention and significantly reducing the impedance growth rate. Detailed Implementation
[0026] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present invention.
[0027] Example 1 The supercapacitor in this embodiment is fabricated as follows: Assemble a supercapacitor model in a glove box: The cell includes two electrode plates and a fiber cloth separator inserted between them. The electrode plates include an aluminum current collector (aluminum foil containing Fe) and an active material layer disposed on both sides of the aluminum current collector (using activated carbon YP-50 as the active material, with the mass ratio of activated carbon YP-50, conductive agent Super P, and binder PAA being 90:5:5, and the rated capacity (nominal capacity) of the supercapacitor being designed to be 60F). Immerse the cell in the electrolyte and seal it using an aluminum shell and adhesive granules. The aluminum current collector contains 100 ppm Fe and has a thickness of 25 μm. The activated carbon contains potassium (K), and the K content in the active material layer is controlled by adjusting the K content in the activated carbon. In this embodiment, the K content in the active material layer is 250 ppm. The surface density and thickness of the active material layer on one side are controlled by adjusting the coating amount and the calendering pressure. In this embodiment, the thickness of the active material layer on one side is 100 μm, and the surface density on one side is 70 g / m³. 2 .
[0028] An electrolyte with an electrolyte concentration of 1.0 mol / L was prepared using N,N-dimethylpyrrolidone ontium tetrafluoroborate as the electrolyte salt and acetonitrile (ACN) as the organic solvent.
[0029] Examples 2-47 and Comparative Examples 1-8 The differences between Examples 2-47 and Comparative Examples 1-8 and Example 1 lie in the types and contents of the electrolyte salt and organic solvent, the Fe content in the aluminum current collector, the mass content of K in the active material layer, the thickness of the aluminum current collector, and the thickness of the active material layer on one side. All other aspects are the same as in Example 1. Specific differences are shown in Tables 1-5.
[0030] The supercapacitors prepared in each embodiment and comparative example were subjected to the following performance tests: (1) Pre-cycle (10 times): At 25°C, the supercapacitor is charged to the upper limit voltage of 3.0V at a constant current of 10mA / F(I) and left to stand for 15 seconds; then discharged to the voltage of 1.5V at a constant current of 10mA / F(I) and left to stand for 5 seconds. This cycle is repeated 10 times. The following data are recorded: The voltage after constant current charging to the upper limit voltage of 3.0V and resting for 15 seconds during the last cycle is U1; The time required for constant current discharge to reach 1.5V during the last cycle is t0, and the actual cutoff voltage is U2. During the last cycle, the voltage after constant current discharge to 1.5V and resting for 5 seconds is U3.
[0031] Calculate using the following formula: Capacity at 25℃ = I × t0 / (U1 - U2); 25℃ ESR = (U3 - U2) / I.
[0032] (2) ESR test at -40℃: Charge and discharge test was performed in a -40℃ low temperature chamber under the same test conditions as the pre-cycle test, for 10 cycles, and the following data were recorded: During the last cycle, the constant current discharge to the actual cutoff voltage of 1.5V is U4; The voltage after constant current discharge to 1.5V and resting for 5 seconds during the last cycle is U5.
[0033] Calculate using the following formula: -40℃ ESR=(U5-U4) / I .
[0034] (3) 65℃ life test: In a 65℃ high-temperature chamber, the supercapacitor was charged at a constant current of 10mA / F(I) to the upper limit voltage of 3.0V, and then charged at a constant voltage of 3.0V for 1000h; the supercapacitor was then removed and cooled to 25℃, and then a charge-discharge test was performed under the same conditions as the pre-cycle test, 10 cycles were performed, and the following data were recorded: The voltage after constant current charging to the upper limit voltage of 3.0V and resting for 15 seconds during the last cycle is U6; The time required for constant current discharge to reach 1.5V during the last cycle is t, and the actual cutoff voltage is U7. During the last cycle, the voltage is U8 after constant current discharge to 1.5V and resting for 5 seconds.
[0035] Calculate using the following formula: The capacity after 1000 hours of float charging at 65℃ = I×t / (U6-U7); Capacity retention rate (%) after 1000h float charge at 65℃ = Capacity after 1000h float charge at 65℃ / Capacity at 25℃ × 100%; ESR after float charging at 65℃ for 1000h = (U8-U7) / I; The ESR growth rate (%) after 1000h float charge at 65℃ = (ESR after 1000h float charge at 65℃ - ESR at 25℃) / ESR at 25℃ × 100%.
[0036] The test results are shown in Tables 1-5.
[0037] Table 1 shows some parameters of the supercapacitors prepared in Examples 1-16 and Comparative Examples 1-6. The differences between Examples 2-16, Comparative Examples 1-6 and Example 1 are only in the Fe content 'a' in the aluminum current collector, the concentration 'c' of the compound shown in structural formula 1, and the value of the relationship a / c, as shown in Table 1. The test results are shown in Table 1.
[0038] Table 1 In the table, " / " indicates that the item is not included.
[0039] As can be seen from the test results of Examples 1-16 and Comparative Examples 1-6, the supercapacitor provided by the present invention uses the compound with a cyclic structure shown in Formula 1 as the electrolyte salt, acetonitrile as the organic solvent, and the aluminum current collector contains Fe element. When the mass content a of Fe element in the aluminum current collector and the concentration c of the compound shown in Formula 1 are limited to 0.6≤a / c≤700, 1≤a≤500, and 0.7≤c≤2, the distribution of electrochemical sites on the surface of the aluminum current collector and the electrolyte salt can reach the optimal balance, thus achieving a synergistic improvement in low impedance growth and long life of the supercapacitor.
[0040] Meanwhile, when the supercapacitor further satisfies 6.5≤a / c≤450, 10≤a≤400, and 0.8≤c≤1.6, the Fe-based active sites on the current collector surface can guide the orderly adsorption of electrolyte salt cations, forming a more regularly arranged adsorption layer structure at the current collector interface. This further reduces the interfacial charge transfer resistance and ensures the stability of the interfacial structure during long-term use, preventing a continuous increase in contact resistance and ensuring the continued performance of the electrolyte salt's ion transport advantages. This optimizes the supercapacitor's lifespan and reduces impedance growth.
[0041] As can be seen from the test results of Comparative Examples 1-6, when at least one of the following—the mass content of Fe element a in the aluminum current collector, the concentration c of the compound shown in structural formula 1, and the relationship a / c—does not meet the specified range, it will lead to problems such as increased local corrosion current density, increased impedance, or reduced service life of the current collector, ultimately resulting in an increased impedance growth rate and decreased capacity retention performance of the supercapacitor.
[0042] Table 2 shows some parameters of the supercapacitors prepared in Examples 1 and 17-25. The only difference between Examples 17-25 and Example 1 is the mass content of K element in the active material layer, as shown in Table 2. Test results are shown in Table 2.
[0043] Table 2 As can be seen from the test results of Examples 1 and 17-25, when the mass content a of Fe element in the aluminum current collector of the supercapacitor of the present invention and the concentration c of the compound shown in structural formula 1 satisfy 0.6≤a / c≤700, 1≤a≤500, and 0.7≤c≤2, further introducing K element into the active material layer and limiting the content of K element to between 1 and 500 ppm helps to improve the electronic conductivity and ion transport performance of the electrode material and reduce the electrode impedance; at the same time, it can be pre-embedded on the inner surface of the electrode pores to construct ion transport pre-channels, further reducing the adsorption / desorption resistance of cations, thereby improving the low impedance performance and capacity retention of the supercapacitor.
[0044] Table 3 shows some parameters of the supercapacitors prepared in Examples 1 and 26-34. The only difference between Examples 26-34 and Example 1 is the thickness of the aluminum current collector and the thickness of the single-sided active material layer, as shown in Table 3. Test results are shown in Table 3.
[0045] Table 3 As can be seen from the test results of Examples 1 and 26-34, when the mass content a of Fe element in the aluminum current collector of the supercapacitor of the present invention and the concentration c of the compound shown in structural formula 1 satisfy 0.6≤a / c≤700, 1≤a≤500, and 0.7≤c≤2, and further limiting the thickness of the aluminum current collector to 15~40μm and the thickness of the active material layer on one side of the aluminum current collector to 60~200μm, it can resist the corrosion of the aluminum current collector by the electrolyte and avoid the aluminum current collector itself having excessively high ohmic impedance; at the same time, it achieves a balance between ion transport efficiency and electrode structure stability, so that the supercapacitor has lower impedance and better service life.
[0046] Table 4 shows some parameters of the supercapacitors prepared in Examples 35-43. The only difference between Examples 35-43 and Example 1 is the composition of the organic solvent, as shown in Table 4. Test results are shown in Table 4.
[0047] Table 4 In the formula, " / " indicates that the term is not included.
[0048] As can be seen from the test results of Examples 1 and 35-43 in Table 4, when the mass content a of Fe element in the aluminum current collector of the supercapacitor of the present invention and the concentration c of the compound shown in structural formula 1 satisfy 0.6≤a / c≤700, 1≤a≤500, and 0.7≤c≤2, a mixed organic solvent of acetonitrile and sulfolane is used and the mass ratio of acetonitrile to sulfolane is limited to 1~13.5. Sulfolane has a high boiling point and excellent electrochemical stability. When used in combination with acetonitrile, it can further improve the high temperature stability of the electrolyte, broaden the upper limit of the operating temperature of the supercapacitor, and at the same time maintain the good ionic conductivity and low temperature performance of the electrolyte.
[0049] Table 5 shows some parameters of the supercapacitors prepared in Examples 1, 44-47, and Comparative Examples 7-8. The only difference between Examples 44-47, Comparative Examples 7-8 and Example 1 is the type of electrolyte salt, as detailed in Table 5. Test results are shown in Table 5.
[0050] Table 5 As can be seen from the test results of Examples 1 and 44-47, when the mass content 'a' of Fe element in the aluminum current collector of the supercapacitor of the present invention and the concentration 'c' of the compound shown in structural formula 1 satisfy 0.6 ≤ a / c ≤ 700, 1 ≤ a ≤ 500, and 0.7 ≤ c ≤ 2, different cyclic compounds shown in structural formula 1 can all improve the low impedance growth and long lifespan of the supercapacitor. Meanwhile, as can be seen from the test results of Comparative Examples 7-8, compared with other electrolyte salts, the cyclic quaternary ammonium cation structure of the present invention has higher rigidity and smaller ionic radius, which is beneficial for achieving rapid ion migration in organic solvents, resulting in a longer cycle life and reduced ESR of the supercapacitor.
[0051] The present invention has been further described above with reference to specific embodiments. However, it should be understood that the specific description herein should not be construed as limiting the nature and scope of the present invention. Various modifications made to the above embodiments by those skilled in the art after reading this specification are all within the scope of protection of the present invention.
Claims
1. An ultracapacitor, characterized by, It includes a diaphragm, an electrolyte, and two electrode plates. The diaphragm is located between the two electrode plates. The electrode plates include an aluminum current collector and an active material layer disposed on at least one surface of the aluminum current collector. The aluminum current collector contains Fe element, and the Fe element content is a ppm based on the total mass of the aluminum current collector; The electrolyte comprises an electrolyte salt and an organic solvent, wherein the organic solvent comprises acetonitrile, and the content of acetonitrile is 45-100% based on the total mass of the organic solvent being 100%. The electrolyte salt includes the compound shown in structural formula 1: Structural Formula 1 wherein A - is tetrafluoroborate, R1, R2are each independently selected from C1-C3 alkyl, n is 0 or 1 ; The concentration of the compound represented by structural formula 1 in the electrolyte is c mol / L; The supercapacitor satisfies the following conditions: 0.6≤a / c≤700, 1≤a≤500, 0.7≤c≤2.
2. The ultracapacitor of claim 1, wherein, The supercapacitor satisfies at least one of the following conditions: (1) 6.5 ≤ a / c ≤ 450; (2)10≤a≤400; (3)0.8≤c≤1.6。 3. The ultracapacitor of claim 1, wherein, The active material layer includes carbon materials and potassium (K) element, and the mass content of potassium element in the active material layer is 1~500 ppm based on the total mass of the active material layer.
4. The ultracapacitor of claim 1, wherein, The thickness of the aluminum current collector is 15~40μm.
5. The ultracapacitor of claim 1, wherein, The thickness of the active material layer on one side of the aluminum current collector is 60~200μm.
6. The supercapacitor of any one of claims 1-5, wherein, The cation of the compound shown in structural formula 1 includes one or more of N,N-dimethylpyrrolidineonium, N,N-diethylpyrrolidineonium, N,N-dipropylpyrrolidineonium, N-methyl-N-ethylpyrrolidineonium, N-methyl-N-propylpyrrolidineonium, N-ethyl-N-propylpyrrolidineonium, N,N-dimethylpiperidineonium, N,N-diethylpiperidineonium, N,N-dipropylpiperidineonium, N-methyl-N-ethylpiperidineonium, N-methyl-N-propylpiperidineonium, and N-ethyl-N-propylpiperidineonium.
7. The ultracapacitor of claim 6, wherein, The organic solvent is acetonitrile, and the compound represented by structural formula 1 is N,N-dimethylpyrrolidone tetrafluoroborate.
8. The ultracapacitor of claim 6, wherein, The organic solvent also includes sulfolane, and the mass ratio of acetonitrile to sulfolane is 1 to 13.
5.
9. The ultracapacitor of claim 3, wherein, The carbon material includes one or more of activated carbon, nano-carbon, graphene, lignin carbon, mesoporous carbon, carbon nanotubes, or porous carbon fibers.
10. The supercapacitor of any one of claims 1-5, wherein, The single-sided areal density of the active material layer is 50 to 110 g / m 2 ; and / or, The charging cutoff voltage of the supercapacitor is 2.7V~3.2V; And / or, The supercapacitor operates in a temperature range of -40℃ to 85℃.