An in-situ polymer-modified dry metal fluoride cathode, its preparation method and application

By employing an in-situ polymer-modified dry preparation method, the problems of ion transport and interfacial contact in dry metal fluoride cathodes under high loading conditions were solved, thereby improving the battery capacity and stability and achieving highly efficient electrochemical performance.

CN123120652APending Publication Date: 2026-11-17ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611334498.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing dry-process metal fluoride cathodes suffer from problems such as compressed ion transport channels, insufficient electrolyte supply, uncontrolled conversion product space, and dynamic interface impedance accumulation under high loading conditions. It is difficult to simultaneously solve the problems of internal ion transport, conversion product space constraint, and dynamic interface contact.

Method used

A dry preparation method using in-situ polymer modification is employed. This method involves mixing a metal fluoride positive electrode active material with a conductive agent, then fibrillating it with a PTFE binder. A precursor solution of cyclic ether monomers, lithium source electrolyte, and initiator is introduced to form a polymer network. The mixture is then blended and hot-pressed to create a continuous Li+ transport environment and buffer volume changes.

Benefits of technology

It significantly improves the capacity utilization of active materials, enhances electrolyte wetting and ion transport within the electrode, reduces transport resistance, maintains the contact state between the positive electrode active material and the conductive network, and improves the energy conversion efficiency and cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120652A_ABST
    Figure CN123120652A_ABST
Patent Text Reader

Abstract

This invention relates to the field of secondary battery technology, and particularly to an in-situ polymer-modified dry-process metal fluoride cathode, its preparation method, and its applications. The preparation method disclosed in this invention involves mixing metal fluoride, a conductive agent, and PTFE in a dry powder state, followed by fibrillation of the PTFE. Subsequently, a pre-polymerized precursor solution composed of cyclic ether monomers, a lithium source electrolyte, and an initiator is introduced to avoid interference from prematurely introduced cyclic ether monomers in the liquid phase on the fibrillation film formation process of the PTFE. After blending and hot pressing, a polyether-type polymer network is in-situ distributed between the metal fluoride, the conductive agent, and the PTFE fibers. The polyether segments in this polymer network can provide continuous Li... + Improve the transport environment, enhance electrolyte wetting and ion transport within the high-area-load dry electrode, and reduce transport resistance in the thickness direction and volume changes during the concentration polarization buffer metal fluoride conversion reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of secondary battery technology, and in particular to an in-situ polymer-modified dry metal fluoride cathode, its preparation method, and its application. Background Technology

[0002] The improvement of energy density in lithium-ion batteries depends on the development of high-capacity cathode materials. Metal fluorides (such as FeF3 and CuF2), through their multi-electron conversion reaction mechanisms, can provide theoretical specific capacities far exceeding those of traditional intercalated cathodes (FeF3 approximately 712 mAh / g, CuF2 approximately 528 mAh / g) and higher operating potentials, making them a crucial research direction for high-energy-density lithium battery cathode materials. However, the low intrinsic electronic / ionic conductivity of metal fluoride cathode materials severely restricts their electrochemical performance. During charge and discharge, metal fluorides undergo reversible phase remodeling reactions between metal fluorides, elemental metals, and lithium fluoride (LiF), accompanied by significant phase reconstruction and volume changes. This multiphase coexistence and dynamic evolution easily leads to a continuous increase in interfacial impedance and intensified electrochemical polarization within the electrode, thereby reducing energy conversion efficiency and cycle stability. For the CuF2 system, there is also the issue of Cu... 2+ / Cu + The migration of other copper-containing intermediates in the electrolyte further disrupts the spatial reversibility of the reaction and exacerbates capacity decay.

[0003] To improve the actual energy density of metal fluoride cathodes, it is necessary to simultaneously increase the proportion and areal loading of active materials in the electrode. However, traditional wet coating processes use organic solvents for slurry preparation. During the drying process of thick electrodes, binders and conductive agents are prone to migration and agglomeration, leading to uneven distribution of binders and conductive agents, electrode cracking, and pore structure collapse, making it difficult to meet the requirements for high-capacity electrodes. Dry electrode technology achieves powder bonding through the fibrillated network of polytetrafluoroethylene (PTFE), which can significantly reduce or even eliminate the use of organic solvents. It also facilitates the construction of high-capacity thick electrodes and has become an important technical route for achieving high areal capacity output in metal fluoride cathodes.

[0004] However, existing dry-process metal fluoride electrodes still face the following challenges:

[0005] Firstly, after high-load electrodes are densified by roll forming, the internal ion transport channels are easily compressed. Since the PTFE matrix itself has low ionic conductivity, the external liquid electrolyte mainly relies on passive wetting after assembly to enter the electrode interior. When the surface load and electrode thickness increase, the electrolyte supply to the deep active material region becomes insufficient, and Li... +Problems such as extended transport paths and uneven reaction front distribution become prominent, leading to decreased utilization of active materials and increased polarization. Although wetting can be improved by increasing the amount of electrolyte, this will reduce the actual energy density of the cell and exacerbate interfacial side reactions.

[0006] Secondly, the conversion reaction of metal fluorides involves drastic volume reconstruction and phase separation. The metal / LiF nanophase generated by discharge is prone to spatial separation in subsequent cycles, leading to the detachment of the electronic conductivity network, ion transport phase, and active reaction interface, severely limiting the reversibility of the reversible reaction. Existing solutions that rely solely on PTFE mechanical bonding or increasing the amount of external electrolyte cannot simultaneously solve the three core problems of ion transport within thick electrodes, spatial constraint of conversion products, and dynamic interfacial contact.

[0007] Therefore, how to maintain the high loading capacity advantage of dry electrodes while constructing a stable internal ion / electron transport network and achieving spatial confinement of conversion products is a technical challenge that needs to be solved for metal fluoride cathode materials to achieve practical application. Summary of the Invention

[0008] To address the problems existing in the prior art, this invention provides a method for preparing in-situ polymer-modified dry metal fluoride cathodes, aiming to solve three interconnected bottleneck problems of insufficient ion conductor phase, spatial runaway of conversion products, and accumulation of dynamic interface impedance under high loading conditions in metal fluoride cathodes.

[0009] This invention discloses a method for preparing an in-situ polymer-modified dry metal fluoride cathode, comprising the following steps: The metal fluoride positive electrode active material is mixed evenly with a conductive agent, and then mixed evenly with a polytetrafluoroethylene (PTFE) binder. The PTFE binder is then fully fibrillated to obtain the positive electrode powder. The cyclic ether monomer, lithium source electrolyte and initiator are mixed evenly and prepolymerized to obtain a precursor solution; The precursor solution and the positive electrode powder are mixed evenly, so that the precursor solution is adsorbed on the surface of the positive electrode active material and in the gaps between the polytetrafluoroethylene binder fibers to obtain the mixed powder. The mixed powder is spread and hot-pressed to obtain a metal fluoride positive electrode film; the metal fluoride positive electrode film is thermally bonded to the surface of the current collector, and then post-processed to obtain the positive electrode.

[0010] Furthermore, the metal fluoride positive electrode active material is selected from at least one of FeF3, CuF2, FeF2, CoF2, NiF2, and MnF2.

[0011] Furthermore, the conductive agent includes at least one of Ketjen black (KB), carbon black (CB), graphene, carbon nanotubes (CNTs), and carbon nanofibers.

[0012] Furthermore, the mass ratio of the metal fluoride positive electrode active material, the conductive agent, and the polytetrafluoroethylene binder in the positive electrode powder is 85-94:3-8:1-7.

[0013] Furthermore, the cyclic ether monomer is selected from at least one of 1,3-dioxolane (DOL), 1,1,1-trifluoro-2,3-epoxypropane, 1,3-dioxane, and 1,4-dioxane.

[0014] Furthermore, the lithium source electrolyte is selected from at least one of LiTFSI, LiFSI, LiPF6, LiBF4, LiClO4, and LiDFOB; the molar concentration of the lithium source electrolyte in the precursor solution is 0.1-1 mol / L.

[0015] Furthermore, the precursor solution in the mixed powder accounts for 3-8 wt% of the mass of the positive electrode powder; the initiator is selected from Lewis acid and protic acid; the added mass of the initiator is 0.05-0.5 wt% of the mass of the cyclic ether monomer.

[0016] Furthermore, the hot pressing is a roll forming process; the roll forming pressure is 15-25 MPa; the post-processing includes thinning to the target compaction density, cutting, and vacuum drying.

[0017] The present invention also discloses an in-situ polymer-modified dry metal fluoride cathode, which is prepared by the preparation method described above.

[0018] The present invention also discloses a lithium-ion battery, comprising the dry-process metal fluoride positive electrode described above.

[0019] In summary, the advantages and beneficial effects of the present invention are as follows: The dry-process metal fluoride cathode preparation method provided by this invention completes the mixing of metal fluoride, conductive agent, and PTFE in a dry powder state, followed by PTFE fibrillation. Subsequently, a prepolymerized precursor solution composed of cyclic ether monomers, lithium source electrolyte, and initiator is introduced to avoid interference from prematurely introduced cyclic ether monomers in the liquid phase on the PTFE fibrillation film formation process. After blending and hot pressing, a polyether polymer network is distributed in situ between the metal fluoride, conductive agent, and PTFE fibers. The polyether segments in this polymer network can provide continuous Li... +The transport environment is improved, enhancing electrolyte wetting and ion transport within the high areal load dry electrode, and reducing transport resistance and concentration polarization in the thickness direction. Simultaneously, the flexible polymer network and PTFE fiber network form a composite support structure that buffers volume changes during the metal fluoride conversion reaction and maintains the contact state between the positive electrode active material particles, the conductive network, and the ion transport network. Attached Figure Description

[0020] Figure 1 The graph shows the discharge capacity test results of the batteries assembled in Examples 1-3 of this invention. Figure 2 The graph shows the discharge capacity test results of the batteries assembled in Examples 4-6 of this invention. Figure 3 The graph shows the discharge capacity test results of the battery assembled in Comparative Example 1 of this invention. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments and corresponding drawings. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0022] The embodiments of the present invention are described in detail below. The following examples are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0023] Example 1 Step 1: Preparation of positive electrode powder Anhydrous FeF3 was used as the positive electrode active material. The positive electrode active material and Ketjenblack were added to a high-speed mixer and pre-mixed for 20-30 minutes at a paddle speed of 20-30 m / s to ensure uniform distribution of the conductive agent Ketjenblack on the surface of the positive electrode active material particles. Then, PTFE binder was added and dispersed at high speed to fully fibrillate the PTFE and construct a three-dimensional fiber bonding network, which encapsulates the FeF3 positive electrode active material and the conductive agent Ketjenblack particles, resulting in positive electrode powder. The mass ratio of FeF3 positive electrode active material, Ketjenblack, and PTFE binder in the positive electrode powder was 91.6:6.2:2.2.

[0024] Step 2: Prepare the precursor solution 1,3-Dioxolane (DOL) and 1,1,1-trifluoro-2,3-epoxypropane were used as cyclic ether monomers, with a volume ratio of DOL to 1,1,1-trifluoro-2,3-epoxypropane of 4:1; lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was used as the lithium source electrolyte. In an argon-atmospheric glove box, a 0.1 mol / L LiTFSI solution was prepared using the cyclic ether monomers as solvents. Then, 0.1 wt% aluminum trifluoromethanesulfonate (Al(OTF)3) initiator (relative to the mass of the cyclic ether monomers) was added, and the mixture was stirred for 3-5 min to obtain a homogeneous and transparent solution. The prepared solution was sealed and placed in a 60°C environment for prepolymerization for 5 min to obtain the precursor solution.

[0025] Step 3: Blending the precursor solution with the positive electrode powder Add a precursor solution of 3 wt% of the positive electrode powder to the positive electrode powder. Under low-speed stirring, the precursor solution is uniformly adsorbed on the surface of the metal fluoride particles and in the gaps between the PTFE fibers to obtain a mixed powder that is in the form of thin sheets and can be further dry-coated.

[0026] Step 4: Preparation of self-supporting electrode film by hot roller thinning The mixed powder is evenly spread and rolled into shape using a differential speed roller press at 80°C. The roller gap and roller pressure are adjusted according to the target surface load, with the roller pressure being 15-25 MPa, to prepare a self-supporting dry metal fluoride positive electrode film.

[0027] A metal fluoride positive electrode film was hot-pressed onto the surface of a carbon-coated aluminum foil current collector at 100°C, and thinned to the target compaction density of 1.2-2.0 g / cm³. 3 The electrode was then punched into a circular sheet with a diameter of 10 mm. The electrode was placed in a vacuum oven and vacuum dried overnight at 80°C to remove residual unreacted monomers and trace amounts of moisture, thus obtaining an in-situ polymer-modified dry metal fluoride positive electrode sheet.

[0028] Example 2 The only difference between this embodiment and Embodiment 1 is that the precursor solution in step 3 accounts for 5 wt% of the positive electrode powder.

[0029] Example 3 The only difference between this embodiment and Embodiment 1 is that the precursor solution in step 3 accounts for 8 wt% of the positive electrode powder.

[0030] Example 4 The only difference between this embodiment and Embodiment 1 is that anhydrous CuF2 is used as the positive electrode active material in step 1.

[0031] Example 5 The difference between this embodiment and Embodiment 1 is that anhydrous CuF2 is used as the positive electrode active material in step 1 and the precursor solution accounts for 5 wt% of the positive electrode powder in step 3.

[0032] Example 6 The difference between this embodiment and Embodiment 1 is that anhydrous CuF2 is used as the positive electrode active material in step 1 and the precursor solution accounts for 8 wt% of the positive electrode powder in step 3.

[0033] Comparative Example 1 The only difference between this comparative example and Example 1 is that the precursor solution is not added to the positive electrode powder in step 3.

[0034] Button battery assembly The battery was assembled in a glove box where the water and oxygen content were both below 0.1 ppm. The negative electrode was made of lithium metal, the separator was made of glass fiber or other separators suitable for lithium metal batteries, and the electrolyte was a lithium salt electrolyte matched with the metal fluoride positive electrode, which was a solution of 1 M LiTFSI dissolved in DME (1,2-dimethoxyethane):DOL (1,3-dioxolane) = 1:1 Vol. After the positive electrode, negative electrode, separator and electrolyte prepared in the examples and comparative examples were assembled, they were allowed to stand to allow the electrolyte to fully impregnate them before the battery performance was tested.

[0035] Performance testing The discharge capacity of the assembled battery at 0.1C was tested at 25℃, and the test results are as follows: Figures 1-3 As shown in Table 1, the discharge specific capacity of Comparative Example 1 without the addition of precursor solution was 565.8 mAh g. -1 Examples 1-3 used FeF3 as the positive electrode active material, and added 3 wt%, 5 wt%, and 8 wt% precursor solutions, respectively, achieving discharge specific capacities of 742.1, 775.9, and 787.7 mAh·g, respectively. -1 Compared to Comparative Example 1, the increases were 176.3, 210.1, and 221.9 mAh·g, respectively. -1 The increases were approximately 31.2%, 37.1%, and 39.2%, respectively. This indicates that introducing the precursor solution into the dry FeF3 cathode can significantly improve the capacity utilization of the active material.

[0036] Further comparison of Examples 1-3 reveals that the discharge specific capacity generally increases as the amount of precursor solution added increases from 3 wt% to 8 wt%. Specifically, when the amount increases from 3 wt% to 5 wt%, the capacity increases from 742.1 mAh·g. -1 Increased to 775.9 mAh·g -1 After further increasing to 8 wt%, the capacity reached 787.7 mAh·g.- ¹. This indicates that increasing the content of the precursor solution is beneficial to improving ion transport and interfacial reactions on the surface of FeF3 particles and inside the electrode. However, when the addition amount reaches more than 5 wt%, the capacity improvement gradually decreases, indicating that its improvement effect tends to saturate.

[0037] Examples 4-6 used CuF2 as the positive electrode active material, with precursor solution addition amounts of 3 wt%, 5 wt%, and 8 wt%, respectively, corresponding to discharge specific capacities of 503.9 mAh·g. -1 501.8 mAh·g -1 and 520.1 mAh·g -1 The overall capacity change was small with different addition amounts, with the highest discharge specific capacity of 520.1 mAh·g obtained at 8 wt%. -1 This indicates that the in-situ polymerization modification method can also be applied to CuF2 dry cathode.

[0038] The above results indicate that the precursor solution has good compatibility with the dry electrode system, and can significantly promote the release of active material capacity, especially in the FeF3 cathode.

[0039] Table 1 Test Results

[0040] Finally, it should be noted that any modification or equivalent substitution of some or all of the technical features made based on the technical solutions of this invention and the embodiments thereof, without departing from the corresponding technical solutions of this invention, shall fall within the patent scope of this invention and the embodiments thereof.

Claims

1. A method for preparing an in-situ polymer-modified dry metal fluoride cathode, characterized in that, include: The metal fluoride positive electrode active material is mixed evenly with a conductive agent, and then mixed evenly with a polytetrafluoroethylene binder. The polytetrafluoroethylene binder is fully fibrillated to obtain positive electrode powder. The cyclic ether monomer, lithium source electrolyte and initiator are mixed evenly and prepolymerized to obtain a precursor solution; The precursor solution and the positive electrode powder are mixed evenly, so that the precursor solution is adsorbed on the surface of the positive electrode active material and in the gaps between the polytetrafluoroethylene binder fibers to obtain the mixed powder. The mixed powder is spread and hot-pressed to obtain a metal fluoride positive electrode film; the metal fluoride positive electrode film is thermally bonded to the surface of the current collector, and then post-processed to obtain the positive electrode.

2. The preparation method according to claim 1, characterized in that, The metal fluoride positive electrode active material is selected from at least one of FeF3, CuF2, FeF2, CoF2, NiF2, and MnF2.

3. The preparation method according to claim 1, characterized in that, The conductive agent includes at least one of Ketjen black, carbon black, graphene, carbon nanotubes, and carbon nanofibers.

4. The preparation method according to claim 1, characterized in that, The mass ratio of the metal fluoride positive electrode active material, the conductive agent, and the polytetrafluoroethylene binder in the positive electrode powder is 85-94:3-8:1-7.

5. The preparation method according to claim 1, characterized in that, The cyclic ether monomers are selected from at least one of 1,3-dioxolane, 1,1,1-trifluoro-2,3-epoxypropane, 1,3-dioxane, and 1,4-dioxane.

6. The preparation method according to claim 1, characterized in that, The lithium source electrolyte is selected from at least one of LiTFSI, LiFSI, LiPF6, LiBF4, LiClO4, and LiDFOB; the molar concentration of the lithium source electrolyte in the precursor solution is 0.1-1 mol / L.

7. The preparation method according to claim 1, characterized in that, The precursor solution in the mixed powder accounts for 3-8 wt% of the mass of the positive electrode powder; the initiator is selected from Lewis acid and protic acid; the added mass of the initiator is 0.05-0.5 wt% of the mass of the cyclic ether monomer.

8. The preparation method according to claim 1, characterized in that, The hot pressing is a roll forming process; the roll forming pressure is 15-25 MPa; the post-processing includes thinning to the target compaction density, cutting, and vacuum drying.

9. An in-situ polymer-modified dry-process metal fluoride cathode, characterized in that, It is prepared by the preparation method according to any one of claims 1-8.

10. A lithium-ion battery, characterized in that, Includes the dry metal fluoride cathode as described in claim 9.