A lithium-rich manganese-based cathode material modified with ammonium formate, its preparation method and application

The preparation method of lithium-rich manganese-based cathode material modified with ammonium formate solves the problems of complex process, high energy consumption and material damage in the existing technology. It realizes simplified process and environmentally friendly material modification, improves the rate performance and long cycle performance of the material, and is suitable for large-scale industrial production.

CN123120693APending Publication Date: 2026-11-17XIAN TECH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611361404.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for constructing spinel phases on the surface of lithium-rich manganese-based cathode materials suffer from problems such as complex processes, high energy consumption, irreversible damage to the material's bulk structure, difficulty in precise control, and poor universality. Furthermore, there is a lack of mild, universal, and efficient modification strategies for constructing spinel phases at room temperature.

Method used

A method for preparing lithium-rich manganese-based cathode materials modified with ammonium formate is proposed. This method involves spray drying and heat treatment of a mixed solution of lithium-rich manganese-based precursor and ammonium formate to prepare lithium-rich manganese oxide cathode materials with increased cell parameters. During the pyrolysis process, ammonium formate generates a weakly reducing atmosphere, which induces Ni element transformation and surface topology transformation into a uniform spinel phase interface layer with a thickness of about 3 nm, thereby improving Li+ diffusion kinetics and suppressing interfacial side reactions.

Benefits of technology

It achieves simplified process and environmentally friendly material modification, improves the rate performance and long-cycle performance of materials, and requires no additional equipment, making it suitable for large-scale industrial production. The modification process does not introduce impurities and meets the requirements of green chemistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120693A_ABST
    Figure CN123120693A_ABST
Patent Text Reader

Abstract

This invention discloses an ammonium formate-modified lithium-rich manganese-based cathode material, its preparation method, and its applications. The cathode material is prepared by spray drying and heat treatment of a mixed solution containing a lithium-rich manganese-based precursor and ammonium formate; the mass fraction of ammonium formate added to the mixed solution is 0.1%–0.7%. This invention introduces ammonium formate during the spray pyrolysis stage. The weakly reducing atmosphere and alkaline environment generated by its decomposition synergistically regulate the structure and surface chemistry of the material, effectively reducing the charge transfer impedance at the electrode / electrolyte interface and promoting lithium-ion desolvation and transport at the interface. The bulk spinel domains, through their three-dimensional ion diffusion channels, significantly reduce the bulk lithium-ion migration barrier, thereby achieving full-scale kinetic optimization from the surface to the bulk phase. The method is simple to operate and has a significant modification effect, providing a feasible strategy for the rational design of high-performance lithium-rich manganese-based cathode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, specifically to an ammonium formate-modified lithium-rich manganese-based cathode material, its preparation method, and its application. Background Technology

[0002] As the most mainstream electrochemical energy storage device, the improvement of the energy density of lithium-ion batteries highly depends on breakthroughs in the performance of cathode materials. Among various cathode material systems, lithium-rich manganese-based cathode materials stand out due to their extremely high theoretical specific capacity (>250 mAh·g). -1 With its high operating voltage exceeding 4.5V, lithium-rich manganese-based materials are hailed as ideal candidates for next-generation high-energy-density lithium-ion battery cathode materials. Compared to traditional LiCoO2 and ternary materials (such as NCM811), lithium-rich manganese-based materials have the following significant advantages. First, they possess higher energy density and longer cycle life, meeting the demands of long-range electric vehicles. Second, due to the extensive use of inexpensive Mn, the content of precious metals Ni / Co is relatively low, significantly reducing raw material costs. Furthermore, Mn's toxicity is far lower than Co's, aligning with the development direction of green chemistry. However, several key technological bottlenecks still need to be overcome before the commercial application of lithium-rich manganese-based cathode materials. First, the irreversible activation of the Li2MnO3 component during the first charge process triggers lattice oxygen release, leading to significant initial irreversible capacity loss and reduced initial coulombic efficiency. Second, the material's intrinsic low electronic conductivity and the low Li... + The sluggish diffusion kinetics severely limit its poor rate performance. Furthermore, severe side reactions occur between residual lithium on the surface and the electrolyte at high voltages. These problems all stem from insufficient material structural stability and poor interfacial compatibility, leading to continuous capacity and voltage decay. These bottlenecks exacerbate each other, severely restricting the practical application and commercialization of lithium-rich manganese oxide cathode materials.

[0003] To address the aforementioned issues, researchers have developed various modification strategies. Patent CN107215900A discloses a method for constructing a surface spinel structure by post-treating lithium-rich manganese-based materials with weak acids such as carbonic acid and acetic acid, combined with heat treatment at 300–600℃. However, this method requires secondary sintering for 2–10 hours, significantly extending the production cycle and increasing energy consumption. Furthermore, the inorganic acid treatment may damage the material's surface structure. Patent CN122136266A proposes adding aminosulfonic acid to a spray pyrolysis precursor salt solution, followed by high-temperature treatment at 1000℃ for 20 minutes, to form an in-situ amorphous protective layer and a composite structure with alternating spinel and disordered phases on the material surface. After 500 cycles at 1C, the capacity retention rate reaches 90.58%. While this method is effective, it does not confirm the formation of a surface spinel phase. Moreover, aminosulfonic acid, as a strong inorganic acid, relies on structural recombination at high temperatures for its modification mechanism, and the method itself lacks universality. Patent CN122291391A describes a wet chemical treatment of the finished lithium-rich manganese-based material using an acidic buffer solution with pH 3–6. After heat treatment in an inert atmosphere at 250–500℃, a spinel phase interface layer with a thickness of 5–50 nm is formed, achieving a capacity retention of 96.4% after 200 cycles at 1C. This method also relies on subsequent heat treatment to induce lattice reconstruction, and the complex composition of the acidic buffer solution increases the difficulty of process control. CN121641914A utilizes reducing organic acids such as tartaric acid and citric acid to modify the lithium-rich manganese-based material at room temperature, eliminating the heat treatment step, and using Li… + / H + Exchange forms Li4Mn5O on the surface 12 The spinel phase yielded an ultra-high specific capacity of 333.98 mAh / g at 0.1C, with a first-cycle coulombic efficiency of 98.76%. This method utilizes the reducing groups of organic acids to simultaneously introduce oxygen defects, but the types of reducing organic acids used are limited, and it is essentially still an acid etching process, which carries the risk of transition metal dissolution. The thickness and uniformity of the spinel layer are highly sensitive to acid concentration and processing time.

[0004] In summary, existing technologies have made some progress in constructing spinel phases on the surface of lithium-rich manganese-based cathode materials, but still have the following shortcomings: (1) Most methods rely on high-temperature heat treatment, which is complex and energy-intensive; (2) There is a risk of transition metal ion dissolution during acid treatment, which causes irreversible damage to the material's bulk structure; (3) Precise control of the thickness and structure of the surface spinel layer still faces challenges; (4) There is a lack of a mild, universal modification strategy that can efficiently construct spinel phases at room temperature. Summary of the Invention

[0005] To overcome the shortcomings of existing technologies, such as complex processes, high energy consumption, irreversible damage to the material's structure, difficulty in precise control, and poor universality, this invention provides an ammonium formate-modified lithium-rich manganese-based cathode material, its preparation method, and its application. The aim is to construct a surface spinel phase without introducing new impurities, thus successfully improving the rate performance and long-cycle performance of the lithium-rich manganese-based cathode material.

[0006] To achieve the purpose of this invention, the technical solution provided by this invention is: an ammonium formate-modified lithium-rich manganese-based cathode material, wherein the cathode material is prepared by spray drying and heat treatment of a mixed solution containing a lithium-rich manganese-based precursor raw material and ammonium formate; the mass fraction of ammonium formate added to the mixed solution is 0.1%-0.7%.

[0007] Furthermore, the ammonium formate-modified lithium-rich manganese-based cathode material has cell parameters a > 2.850629 Å, c > 14.237699 Å, and cell volume V > 100.196 Å. 3 .

[0008] The preparation method of the above-mentioned ammonium formate-modified lithium-rich manganese oxide cathode material includes the following steps: (1) Preparation of precursor solution The mixture of lithium acetate dihydrate, nickel acetate tetrahydrate, cobalt acetate tetrahydrate, manganese acetate tetrahydrate, citric acid monohydrate, and ammonium formate was added to deionized water and stirred to obtain the final product. (2) Preparation of precursor materials The precursor solution obtained in step (1) was spray-dried to obtain the product; (3) Preparation of cathode materials The precursor material obtained in step (2) is heat-treated to obtain the product.

[0009] The beneficial effects of this invention are: the preparation process is simple, environmentally friendly, and the preparation conditions are mild, which is conducive to large-scale industrial production and application.

[0010] Furthermore, in step (1), the stoichiometric ratio of lithium acetate dihydrate, nickel acetate tetrahydrate, cobalt acetate tetrahydrate, and manganese acetate tetrahydrate is 1.2:0.13:0.13:0.54, and an additional 3% by mass of lithium acetate dihydrate is added to compensate for lithium loss during the heat treatment process.

[0011] Furthermore, in step (1), the total concentration of metal acetate in the precursor solution is 0.1-0.2 mol / L, and the concentration of citric acid monohydrate is 0.2-0.5 mol / L.

[0012] Furthermore, in step (1), the stirring speed is 300-1000 rpm, the time is 0.5-2 h, and the temperature is 20-30℃.

[0013] Furthermore, in step (2), the inlet temperature of the spray dryer is 200-250 ℃, the outlet temperature is 80-120 ℃, and the feed rate is 0.5-2 L / h.

[0014] Furthermore, the heat treatment conditions in step (3) are as follows: in an air atmosphere, the temperature is increased to 900-1100 ℃ at a heating rate of 1-5 ℃ / min, and held for 10-30 min.

[0015] The above-mentioned ammonium formate-modified lithium-rich manganese oxide cathode material is used in the preparation of lithium-ion batteries.

[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) In this invention, the weakly reducing atmosphere (containing CO and H2) generated by the decomposition of ammonium formate can induce a significant transformation of Ni from a high oxidation state to a low oxidation state, through Ni 3+ / Ni 2+ The moderate adjustment of the valence state increased the Ni-O bond length, promoted lattice expansion, and was beneficial to improving the Li... + Diffusion kinetics. Furthermore, ammonium formate successfully induced a topological transformation of the surface layer into a uniform spinel phase interface layer approximately 3 nm thick. This spinel phase provides three-dimensional lithium-ion diffusion channels, which are continuously connected with the two-dimensional channels of the internal layered structure. This effectively suppresses interfacial side reactions while enhancing lithium-ion transport, thereby improving the rate performance of the material.

[0017] (2) In this invention, the weak alkaline or reducing atmosphere of ammonium formate can effectively remove the alkaline lithium compounds (mainly Li2CO3 and LiOH) remaining on the surface of the material, eliminate the hidden danger of catalytic decomposition of electrolyte and release of CO2 gas under high pressure, reduce the generation of gas byproducts from the source, effectively suppress the continuous side reaction between the electrode and the electrolyte in high voltage cycling, significantly slow down the growth of interfacial impedance, and significantly improve the long-term cycling stability and capacity retention of the modified material.

[0018] (3) The ammonium formate used in this invention is a common and inexpensive chemical raw material, and its modification process is completed in situ during the spray pyrolysis step, without the need for additional pretreatment, posttreatment or atmosphere control equipment. The entire process is simple, highly compatible with existing spray pyrolysis production lines, easy to achieve large-scale continuous production, and has good industrial application prospects.

[0019] (4) Ammonium formate completely decomposes into gas during pyrolysis, without introducing any impurity elements (such as C, N, etc.) into the material, thus avoiding side reactions or the formation of electrochemically inert phases caused by residues. Furthermore, the decomposition products of ammonium formate are mainly NH3, CO2, and H2O, without introducing heavy metals or toxic and harmful substances. Compared to methods using hazardous gases such as ammonia for atmosphere treatment, the raw materials used in this invention are solid at room temperature, easy to store and transport, have high operational safety, and simple exhaust gas treatment, meeting the requirements of green chemistry. Attached Figure Description

[0020] Figure 1 Here are SEM images of lithium-rich manganese-based cathode materials, where... Figure 1 (a) is a comparative SEM image. Figure 1 (b) is the SEM image of Example 1. Figure 1 (c) is a SEM image of Example 2. Figure 1 (d) is the SEM image of Example 3. Figure 1 (e) is the SEM image of Example 4; Figure 2 The images show the XRD patterns of the lithium-rich manganese-based cathode materials prepared in Examples 1-4 and the comparative examples of this invention; wherein, Figure 2 (a) XRD patterns of Examples 1-4 and the comparative examples. Figure 2 (bd) is Figure 2 (a) Enlarged view, Figure 2 (e) is a comparative XRD refinement image. Figure 2 (f) is the refined XRD pattern of Example 3; Figure 3 The figures shown are Raman diagrams of the lithium-rich manganese-based cathode materials prepared in Examples 1-4 and the comparative examples of this invention. Figure 3 (a) Raman diagrams for Examples 1-4 and the comparative example. Figure 3 (b) is a comparative Raman peak plot. Figure 3 (c) is the Raman peak diagram of Example 3; Figure 4 This is a TEM image of the lithium-rich manganese-based cathode material prepared in Example 3 of the present invention; Figure 5 XPSO1s diagrams of lithium-rich manganese-based cathode materials prepared in Example 3 and the comparative example of the present invention; Figure 6 XPSNi2p diagrams of lithium-rich manganese-based cathode materials prepared in Example 3 and the comparative example of this invention; Figure 7 XPS Mn3s images of lithium-rich manganese-based cathode materials prepared in Example 3 and the comparative example of the present invention; Figure 8The images show the initial charge-discharge cycles of the batteries assembled in Examples 1-4 and the comparative examples of this invention at a current density of 0.1C (20 mA / g). Figure 8 (a) shows the first-lap performance curves for comparison. Figure 8 (b) shows the first-cycle performance curve of Example 1. Figure 8 (c) shows the first-cycle performance curve of Example 2. Figure 8 (d) shows the first-cycle performance curve of Example 3. Figure 8 (e) is the first-cycle performance curve of Example 4; Figure 9 The capacity cycling performance of the batteries assembled in Examples 1-4 and the comparative examples of this invention is shown in the graphs at a current density of 1C (200mA / g). Figure 10 The energy density cycling performance of the batteries assembled in Examples 1-4 and the comparative examples of this invention is shown in the figure at a current density of 1C (200mA / g). Figure 11 The rate performance diagrams are for the batteries assembled in Examples 1-4 and the comparative examples of the present invention. Figure 12 The diagram shows the capacity cycling performance of the batteries assembled in Example 3 and the comparative example of this invention at a current density of 5C (1000mA / g). Detailed Implementation

[0021] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] This invention provides an ammonium formate-modified lithium-rich manganese-based cathode material. The cathode material is prepared by spray drying and heat treatment of a mixed solution containing a lithium-rich manganese-based precursor and ammonium formate. The mass fraction of ammonium formate added to the mixed solution is 0.1%-0.7%. The lithium-rich manganese-based precursor in the mixed solution includes a lithium source, a nickel source, a cobalt source, and a manganese source; the stoichiometric ratio of the lithium source, nickel source, cobalt source, and manganese source is 1.2:0.13:0.13:0.54. The ammonium formate-modified lithium-rich manganese-based cathode material has cell parameters a > 2.850629 Å, c > 14.237699 Å, and cell volume V > 100.196 Å. 3 .

[0023] This invention also provides a method for preparing the ammonium formate-modified lithium-rich manganese-based cathode material, specifically including the following steps: Step (1): Mix lithium source, nickel source, cobalt source, manganese source, complexing agent and ammonium formate and add to water, stir to obtain precursor solution; Step (2): Spray dry the precursor solution obtained in step (1) to obtain the precursor material; Step (3): Heat-treat the precursor material obtained in step (2) to obtain the ammonium formate-modified lithium-rich manganese-based cathode material.

[0024] Further, in step (1), the lithium source is lithium acetate dihydrate, the nickel source is nickel acetate tetrahydrate, the cobalt source is cobalt acetate tetrahydrate, the manganese source is manganese acetate tetrahydrate, and an additional 3% by mass of lithium acetate dihydrate is added to compensate for lithium loss during the heat treatment process; the complexing agent is citric acid monohydrate.

[0025] Further, in step (1), the total concentration of metal acetate is 0.1-0.2 mol / L, and the concentration of citric acid monohydrate is 0.2-0.5 mol / L; the stirring speed is 300-1000 rpm, the stirring time is 0.5-2 h, and the temperature is 20-30℃.

[0026] Furthermore, in step (2), the inlet temperature of the spray dryer is set to 200-250℃, the outlet temperature is set to 80-120℃, and the feed rate is set to 0.5-2L / h.

[0027] Furthermore, the heat treatment conditions in step (3) are as follows: in an air atmosphere, the temperature is raised to 900-1100℃ at a heating rate of 1-5℃ / min and held for 10-30min.

[0028] Example 1: A method for preparing an ammonium formate-modified lithium-rich manganese-based cathode material, specifically including the following steps: (1) Preparation of precursor solution Weigh 18.915g lithium acetate dihydrate, 4.852g nickel acetate tetrahydrate, 4.857g cobalt acetate tetrahydrate and 19.852g manganese acetate tetrahydrate, dissolve them in 1L deionized water, add 63.042g citric acid monohydrate, add 9.5mg ammonium formate, and add an additional 3% by mass of lithium acetate dihydrate to compensate for lithium loss during heat treatment; mechanically stir at 500rpm for 1h at room temperature to obtain the precursor solution.

[0029] (2) Preparation of precursor materials The precursor solution obtained in step (1) is sent to a spray dryer using a peristaltic pump. The inlet temperature of the spray dryer is set to 230°C, the outlet temperature is set to 100°C, and the feed rate is set to 1L / h. The precursor material is obtained by spray drying under high temperature and high pressure.

[0030] (3) Preparation of cathode materials The precursor material obtained in step (2) is placed in an alumina crucible with a length of 120 mm, a width of 120 mm, and a height of 50 mm. The alumina crucible is placed in a box furnace and heated at a rate of 3 °C / min in air atmosphere. It is then heat-treated at 1000 °C for 20 min to obtain a lithium-rich manganese-based cathode material, named 0.1Af-LRMO.

[0031] Example 2: A method for preparing an ammonium formate-modified lithium-rich manganese-based cathode material, specifically including the following steps: The preparation method is the same as in Example 1, except that when preparing the precursor solution, 18.915 g of lithium acetate dihydrate, 4.852 g of nickel acetate tetrahydrate, 4.857 g of cobalt acetate tetrahydrate, and 19.852 g of manganese acetate tetrahydrate were weighed, dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate and 28.5 mg of ammonium formate were added. An additional 3% (w / w) of lithium acetate dihydrate was added to compensate for lithium loss during heat treatment. The mixture was mechanically stirred at 500 rpm for 1 h at room temperature to obtain the precursor solution. The remaining steps were the same as in Example 1. The resulting cathode material was named 0.3Af-LRMO.

[0032] Example 3: A method for preparing an ammonium formate-modified lithium-rich manganese-based cathode material, specifically including the following steps: The preparation method is the same as in Example 1, except that when preparing the precursor solution, 18.915 g of lithium acetate dihydrate, 4.852 g of nickel acetate tetrahydrate, 4.857 g of cobalt acetate tetrahydrate, and 19.852 g of manganese acetate tetrahydrate were weighed, dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate and 47.5 mg of ammonium formate were added. An additional 3% (w / w) of lithium acetate dihydrate was added to compensate for lithium loss during heat treatment. The mixture was mechanically stirred at 500 rpm for 1 h at room temperature to obtain the precursor solution. The remaining steps were the same as in Example 1. The resulting cathode material was named 0.5Af-LRMO.

[0033] Example 4: A method for preparing an ammonium formate-modified lithium-rich manganese-based cathode material, specifically including the following steps: The preparation method is the same as in Example 1, except that when preparing the precursor solution, 18.915 g of lithium acetate dihydrate, 4.852 g of nickel acetate tetrahydrate, 4.857 g of cobalt acetate tetrahydrate, and 19.852 g of manganese acetate tetrahydrate were weighed, dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate and 66.5 mg of ammonium formate were added. An additional 3% (w / w) of lithium acetate dihydrate was added to compensate for lithium loss during heat treatment. The mixture was mechanically stirred at 500 rpm for 1 h at room temperature to obtain the precursor solution. The remaining steps were the same as in Example 1. The resulting cathode material was named 0.7Af-LRMO.

[0034] Comparative example: A method for preparing a lithium-rich manganese-based cathode material, specifically including the following steps: The preparation method is the same as in Example 1, except that when preparing the precursor solution, 18.915 g of lithium acetate dihydrate, 4.852 g of nickel acetate tetrahydrate, 4.857 g of cobalt acetate tetrahydrate, and 19.852 g of manganese acetate tetrahydrate were weighed, dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate was added. An additional 3% (w / w) of lithium acetate dihydrate was added to compensate for lithium loss during heat treatment. The solution was mechanically stirred at 500 rpm for 1 h at room temperature to obtain the precursor solution. The remaining steps were the same as in Example 1. The resulting cathode material was named LRMO.

[0035] I. SEM testing of lithium-rich manganese-based cathode materials prepared in Examples 1-4 and comparative examples of the present invention SEM tests were performed on the lithium-rich manganese-based cathode materials prepared in Examples 1-4 and the comparative examples to observe the morphology and size of the lithium-rich manganese-based cathode materials.

[0036] Experimental results are as follows Figure 1 As shown in the figure, the lithium-rich manganese-based cathode material prepared in the embodiments of the present invention exhibits [performance / advantages]. Figure 1 (a)-(e) are all spherical particles with a particle size of about 400 nm.

[0037] II. XRD Testing of Lithium-Rich Manganese-Based Cathode Materials Prepared in Examples 1-4 and Comparative Examples of the Present Invention The lithium-rich manganese-based cathode materials prepared in Examples 1-4 and the comparative examples were subjected to XRD tests to determine the average structure of the lithium-rich manganese-based cathode materials.

[0038] Experimental results are as follows Figure 2 As shown in (a), it can be seen that compared with the original lithium-rich manganese in the comparative example, the diffraction peak of the ammonium formate-modified lithium-rich manganese shifts to the left, indicating that the lattice constant is larger.

[0039] The XRD results of Example 3 and the comparative example were further refined, and the refined results are shown in Table 1. The original cell parameters a, c, and V of the lithium-rich manganese in the comparative example were 2.850629 Å, 14.237699 Å, and 100.196 Å, respectively. 3 The values ​​are lower than those of the ammonium formate-modified lithium-rich manganese sample 0.5Af-LRMO, which are 2.851533 Å, 14.239450 Å, and 100.272 Å. 3 The increase in cell parameters broadens the Li... + The migration channels are beneficial for improving the dynamic properties of materials.

[0040] Table 1

[0041] III. Raman Testing of Lithium-Rich Manganese-Based Cathode Materials Prepared in Examples 1-4 and Comparative Examples of the Present Invention Raman spectroscopy was performed on the lithium-rich manganese-based cathode materials prepared in Examples 1-4 and the comparative examples to investigate the evolution of their local crystal structures.

[0042] Experimental results are as follows Figure 3 As shown in (a), it can be seen that compared with the original lithium-rich manganese in the comparative example, the peaks of the spinel phase of the ammonium formate-modified lithium-rich manganese are significantly enhanced, and its three-dimensional lithium-ion diffusion channels are conducive to Li... + Diffusion, thereby improving the rate performance of the material.

[0043] IV. TEM Testing of the Lithium-Rich Manganese-Based Cathode Material Prepared in Example 3 of this Invention The lithium-rich manganese-based cathode material prepared in Example 3 was subjected to TEM testing to characterize its local crystal structure in order to clarify its atomic-scale phase composition and lattice arrangement characteristics.

[0044] Experimental results are as follows Figure 4 As shown. HRTEM and corresponding FFT analyses indicate that the bulk phase of the ammonium formate-modified lithium-rich manganese sample has a layered structure with a corresponding (003) interplanar spacing of 0.487 nm. Further high-resolution TEM characterization revealed a spinel-like phase thin layer of approximately 3 nm thickness on the sample surface, while nanoscale spinel-like domain regions were also dispersed within the bulk phase. The surface spinel-like layer can serve as a fast ion conduction layer, reducing the charge transfer impedance at the electrode / electrolyte interface; while the dispersed spinel domains within the bulk phase can act as high-speed channels for lithium ion migration. The synergy of these two factors is beneficial for improving rate performance.

[0045] V. XPS Testing of Lithium-Rich Manganese-Based Cathode Materials Prepared in Example 3 and Comparative Examples of the Invention XPS tests were performed on the lithium-rich manganese-based cathode materials prepared in Example 3 and the comparative example to test the valence states of each element in the lithium-rich manganese-based cathode materials.

[0046] Experimental results are as follows Figures 5-7 As shown, compared to the original lithium-rich manganese in the comparative example, ammonium formate modification induced a significant shift of Ni from a high valence state to a low valence state, while the Mn valence state and oxygen vacancy concentration remained essentially stable. This avoids the collapse of the layered structure caused by the drastic reduction of Mn, and also facilitates the transformation of Ni... 3+ / Ni 2+ The valence state adjustment moderately increased the Ni-O bond length, thereby synergistically promoting lattice expansion (consistent with XRD results), which is beneficial for improving Li + Diffusion kinetics.

[0047] VI. Electrochemical performance testing of the batteries assembled in Examples 1-4 and the comparative examples of the present invention (1) Preparation of positive electrode sheet The lithium-rich manganese-based cathode materials and SuperP prepared in Examples 1-4 and the comparative example were weighed at a mass ratio of 8:1 and placed in a ball mill jar. Tungsten carbide grinding beads were added, and the mass ratio of balls to materials in the ball mill jar was 100:1. Alcohol was added as a dispersant. After ball milling for 6 hours, the mixture was dried in a drying oven to obtain mixture A. Weigh 285 mg of mixture A and 1250 mg of CMC solution with a mass concentration of 1.2%, stir at room temperature for 2 h, sonicate for 2 h, stir again for 2 h, coat with a 0.1 μm scraper onto aluminum foil, place in a vacuum drying oven at 110 °C for 20 h, cut into electrodes with a diameter of 10 mm, and then transfer the cut electrodes to a vacuum oven at 115 °C for 10 h for later use.

[0048] (2) Assemble CR2025 stainless steel button batteries Using lithium metal sheets as the negative electrode, 200 μL of LBC-3045I(G) commercial electrolyte was added. The CR2025 stainless steel button cell was assembled in a glove box filled with argon gas and with a moisture content of less than 0.01 ppm. Its charge and discharge performance was tested after standing at 45°C for 40 hours.

[0049] Electrochemical performance testing of CR2025 stainless steel button cells: The cycle performance of the batteries prepared in Examples 1-4 and the comparative examples was tested using a constant current charge-discharge method. The test temperature was 25°C, and the voltage window was 2.0-4.8V. The test current densities were 0.1C, 1C, 2C, 3C, 5C, and 10C, where 1C = 200mA / g.

[0050] Figure 8 The first charge-discharge curves of the batteries assembled with lithium-rich manganese materials in Examples 1-4 and the comparative example are shown in Table 2. The corresponding discharge specific capacity and initial coulombic efficiency (ICE) are summarized in Table 2. The discharge specific capacity of the original lithium-rich manganese material in the comparative example is 243.63 mAh g.-1 The discharge specific capacity and ICE of the lithium-rich manganese alloys in Examples 1-3 showed a continuous upward trend with increasing ammonium formate addition, with Example 3 reaching the optimal value of 287.77 mAh g⁻¹. -1 And 82.59%. However, when the ammonium formate content was further increased to Example 4, the discharge specific capacity and ICE showed a significant decrease, indicating that excessive ammonium formate treatment would lead to a decline in the electrochemical performance of lithium-rich manganese.

[0051] Table 2

[0052] Figure 9 Table 2 shows the cycling performance curves of the batteries assembled with lithium-rich manganese materials in Examples 1-4 and the comparative example at a 1C rate. The corresponding discharge specific capacity and capacity retention after 600 cycles are summarized in Table 2. After 600 cycles, the original discharge specific capacity of the lithium-rich manganese material in the comparative example decreased to 157.89 mAh·g. -1 The capacity retention rate was 93.38%; while Example 3 still output 227.98 mAhg. -1 The discharge specific capacity is as high as 110.97%. The comparison shows that the lithium-rich manganese sample modified with ammonium formate exhibits significantly superior structural stability and capacity retention during long-term cycling.

[0053] Figure 10 The graph shows the energy density cycling performance of batteries assembled with lithium-rich manganese materials in Examples 1-4 and the comparative example at 1C rate. After 800 cycles, the energy density retention rate of the original lithium-rich manganese material in the comparative example was 73.22%, and the energy density retention rate of Example 3 was 78.7%. This result indicates that ammonium formate modification not only effectively delays capacity decay but also maintains a higher energy output level during long-term cycling.

[0054] Figure 11 This diagram shows the rate performance of batteries assembled with lithium-rich manganese materials in Examples 1-4 and the comparative example of this invention. The specific capacity of the original lithium-rich manganese material in the comparative example is only 96.61 mAh·g at a 10C rate. -1 Example 3, however, still exhibited a high capacity of 132.33 mAh g at the same high magnification. -1 The discharge specific capacity fully demonstrates the effect of ammonium formate modification on Li at high rates. + Significant improvement in diffusion kinetics. More importantly, the discharge specific capacity of Example 3 can be restored to 286.97 mAh g⁻¹ when the current density recovers from 10C to 0.1C. -1 It is close to its initial capacity of 287.77 mAh g. -1 This confirms that the material can maintain good structural integrity and capacity reversibility even after being subjected to a large current impact.

[0055] Figure 12 This diagram shows the capacity cycling performance of batteries assembled with lithium-rich manganese materials in Example 3 and the comparative example of this invention at a 5C rate. The average discharge specific capacity of the comparative example after approximately 800 cycles is 110 mAhg. -1 Example 3 shows that it can maintain nearly 150 mAh g after 800 cycles at a high rate of 5C. -1 The high capacity is improved by nearly 40%. The comparison shows that the lithium-rich manganese sample optimized with ammonium formate exhibits significantly superior structural stability during high-rate cycling.

[0056] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. An ammonium formate-modified lithium-rich manganese-based cathode material, characterized in that, The cathode material is prepared by spray drying and heat treatment of a mixed solution containing lithium-rich manganese-based precursor raw material and ammonium formate; the mass fraction of ammonium formate added to the mixed solution is 0.1%-0.7%.

2. The ammonium formate-modified lithium-rich manganese-based cathode material according to claim 1, characterized in that, The ammonium formate-modified lithium-rich manganese-based cathode material has the following cell parameters: a > 2.850629 Å, c > 14.237699 Å, and cell volume V > 100.196 Å. 3 .

3. A method for preparing ammonium formate-modified lithium-rich manganese-based cathode material as described in any one of claims 1-2, characterized in that, Includes the following steps: Step (1): Mix lithium source, nickel source, cobalt source, manganese source, complexing agent and ammonium formate and add to water, stir to obtain precursor solution; Step (2): Spray dry the precursor solution obtained in step (1) to obtain the precursor material; Step (3): Heat-treat the precursor material obtained in step (2) to obtain the ammonium formate-modified lithium-rich manganese-based cathode material.

4. The method for preparing ammonium formate-modified lithium-rich manganese-based cathode material according to claim 3, characterized in that, In step (1), the lithium source is lithium acetate dihydrate, the nickel source is nickel acetate tetrahydrate, the cobalt source is cobalt acetate tetrahydrate, the manganese source is manganese acetate tetrahydrate, and an additional 3% by mass of lithium acetate dihydrate is added to compensate for lithium loss during the heat treatment process; the complexing agent is citric acid monohydrate.

5. The method for preparing ammonium formate-modified lithium-rich manganese-based cathode material according to claim 3, characterized in that, In step (1), the total concentration of metal acetate is 0.1-0.2 mol / L, and the concentration of citric acid monohydrate is 0.2-0.5 mol / L; the stirring speed is 300-1000 rpm, the stirring time is 0.5-2 h, and the temperature is 20-30℃.

6. The method for preparing ammonium formate-modified lithium-rich manganese-based cathode material according to claim 3, characterized in that, In step (2), the inlet temperature of the spray dryer is set to 200-250℃, the outlet temperature is set to 80-120℃, and the feed rate is set to 0.5-2L / h.

7. The method for preparing ammonium formate-modified lithium-rich manganese-based cathode material according to claim 3, characterized in that, The heat treatment conditions in step (3) are as follows: in an air atmosphere, the temperature is raised to 900-1100℃ at a heating rate of 1-5℃ / min and held for 10-30min.

8. The application of an ammonium formate-modified lithium-rich manganese-based cathode material as described in any one of claims 1-2, or an ammonium formate-modified lithium-rich manganese-based cathode material prepared by the preparation method described in any one of claims 3-7, in the preparation of a lithium-ion battery cathode.

Citation Information

Patent Citations

  • Method for constructing spinel structure on surface layer of lithium-rich manganese-based positive electrode material

    CN107215900A

  • Lithium-rich manganese-based positive electrode material, preparation method, positive electrode plate and lithium ion battery

    CN121641914A

  • Method for constructing lithium-manganese-rich positive electrode material with amorphous protective layer and local spinel-disordered phase periodic alternating composite structure

    CN122136266A

  • Lithium-rich manganese-based positive electrode material, in-situ interface modification method thereof and lithium ion battery

    CN122291391A