Lithium-ion battery electrolyte containing additives that scavenge reactive oxygen species and free radicals

By using polymethylpiperidine organic compound additives in lithium batteries, reactive oxygen species and free radicals are eliminated, and an excellent interfacial film is generated. This solves the problems of electrolyte decomposition and cathode material degradation in lithium batteries under high voltage, improves battery performance, and enables the regeneration of waste electrolyte. It is suitable for the treatment of both new and old electrolytes.

CN123120872APending Publication Date: 2026-11-17KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611474744.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium batteries suffer from electrolyte decomposition and electrode material degradation due to reactive oxygen species and free radicals at high voltages. Current solutions cannot suppress the generation of reactive oxygen species and free radicals at the source, and the preparation process is complicated and costly, making it difficult to meet the needs of large-scale industrial applications.

Method used

Using polymethylpiperidine organic compounds as additives can dynamically capture and remove reactive oxygen species and free radicals in the cathode material and electrolyte, generating a thin and dense solid electrolyte interface film, improving the diffusion kinetics of the interface layer, and can be used for the regeneration treatment of waste electrolyte.

Benefits of technology

It significantly improves battery capacity, coulombic efficiency, and long-cycle stability, reduces interfacial impedance, and enables the recycling of waste electrolyte, possessing low cost and broad technological application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120872A_ABST
    Figure CN123120872A_ABST
Patent Text Reader

Abstract

This invention discloses a lithium-ion battery electrolyte containing functional additives for scavenging reactive oxygen species and free radicals. The additives effectively remove reactive oxygen species released from ultra-high nickel ternary layered cathode oxide materials under high voltage, as well as free radicals generated by electrolyte decomposition. Simultaneously, the products of the reaction between these additives and reactive oxygen species and free radicals facilitate the formation of a positive and negative electrode-electrolyte interface phase with excellent diffusion kinetics and high mechanical strength, promoting lithium-ion diffusion and further protecting the positive and negative electrodes. The raw materials for this electrolyte additive are widely available and inexpensive. Lithium-ion batteries using electrolytes containing this additive or treated waste electrolytes exhibit excellent cycle stability and efficiency, demonstrating potential for large-scale commercial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrochemical energy storage technology, specifically relating to an electrolyte additive with active oxygen and free radical scavenging functions, a lithium battery electrolyte containing the additive, an electrochemical device based on interface functional group management, and its preparation method. Background Technology

[0002] Currently, commercially available lithium-ion battery electrolyte systems primarily utilize carbonates, ethers, sulfones, and sulfite compounds as solvents, supplemented by difluorophosphates such as lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, and lithium difluorooxalate borate. However, when these electrolytes are used in lithium-ion battery systems employing high-voltage layered oxides as cathode materials, significant degradation and violent side reactions with the cathode and anode materials occur at operating voltages exceeding 4.3 V. The reason for this is that at high voltages, reactive oxygen species (such as O2) escape from the crystal lattice of the layered oxide cathode material. 2⁻ The electrolyte decomposes and generates a large number of free radicals (such as ·CH3, ·OCH3, ·OCOOCH3, H2C=CHO·). These highly reactive oxygen species and free radicals continuously attack the positive and negative electrode-electrolyte interface phases, the crystal structure of the electrode material, and the electrolyte components, leading to severe electrolyte decomposition and electrode material structural degradation.

[0003] Specifically, reactive oxygen species (ROS) are mainly generated during the irreversible phase transition of layered oxide cathode materials from a rhombohedral phase to a disordered spinel or rock salt phase; while free radicals originate from the electrochemical oxidation of the electrolyte solvent and lithium salt. Free radicals attack the cathode material, exacerbating the irreversible phase transition and further promoting the escape of ROS from the crystal lattice. The escaped ROS then oxidize the electrolyte, generating more free radicals, forming a vicious chain reaction that ultimately leads to the massive decomposition of the electrolyte and the collapse of the cathode material structure. This process can cause a series of problems, including increased interfacial impedance, a heightened risk of thermal runaway, and a sharp decline in battery cycle life.

[0004] To address these challenges, existing research primarily focuses on modifying cathode materials, using methods such as atomic layer deposition, molecular layer deposition, elemental doping, and surface coating. These strategies mainly emphasize constructing physical barriers to physically isolate the escape of reactive oxygen species and the attack of free radicals, but they cannot effectively suppress the generation of reactive oxygen species and free radicals at their source, nor can they reduce their content within the system. Furthermore, the aforementioned methods involve cumbersome and costly fabrication processes, and some methods even sacrifice the energy density and rate performance of the battery, making it difficult to meet the demands of large-scale industrial applications. Summary of the Invention

[0005] To address the problems of electrolyte decomposition and electrode material degradation caused by reactive oxygen species and free radicals in existing high-voltage lithium-ion battery systems, this invention provides a lithium-ion battery electrolyte containing additives that scavenge reactive oxygen species and free radicals, and its applications. The additives used in this invention have the following core functions: First, they can dynamically capture and remove reactive oxygen species and free radicals generated by the cathode material and electrolyte during battery cycling; second, after reacting with reactive oxygen species and free radicals, these additives can generate thin, dense solid electrolyte interphase (SEI) and cathode electrolyte interphase (CEI) films with high ionic conductivity, thereby inhibiting further electrolyte decomposition and improving the diffusion kinetics of lithium ions at the interface layer; third, by directly adding these additives to waste electrolyte, reactive oxygen species and free radicals can be eliminated simultaneously, resulting in a one-step regeneration of a directly usable electrolyte.

[0006] Through the aforementioned functions, this type of additive can effectively alleviate electrolyte decomposition and cathode material structural degradation during cycling, significantly improving battery capacity, coulombic efficiency, and long-cycle stability. Simultaneously, as a treatment additive for waste electrolyte, it enables one-step recycling of waste electrolyte, solving the problem of large-scale waste electrolyte storage and treatment, and significantly improving treatment efficiency.

[0007] The specific technical solution of the present invention is as follows:

[0008] A lithium battery electrolyte containing additives that scavenge reactive oxygen species and free radicals includes an electrolyte and an additive that converts reactive oxygen species into components capable of forming high-performance interfacial films; the additive is an organic compound containing a polymethylpiperidine structure, and the concentration of the additive in the lithium battery electrolyte is 0.1–3.0 wt%.

[0009] The polymethylpiperidine organic compounds are 4-dimethylamino-2,2,6,6-tetramethylpiperidine, N,N'-bis-(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide, 1,2,3,4-butanetetracarboxylic acid tetra(1,2,2,6,6-pentamethyl-4-piperidinyl) ester, 1-(methyl)-8-(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, or 1,2,3,4-butanetetracarboxylic acid-1,2,3-tris(2,2,6,6-tetramethyl-4-piperidinyl)-4-tridecane ester;

[0010] The additive can react with reactive oxygen species and free radicals to generate beneficial components of a solid electrolyte interface film on the negative electrode surface and beneficial components of a positive electrode electrolyte interface film on the positive electrode surface.

[0011] The electrolyte is obtained by preparation or by dismantling and recycling waste batteries; the prepared electrolyte includes organic solvents, linear carboxylic acid ester compounds, lithium salts and film-forming additives.

[0012] This invention employs polymethylpiperidine organic compounds as electrolyte additives. Their mechanism of action is as follows: First, the unique electron cloud distribution of the piperidine ring endows it with a certain electron affinity, enabling it to attract highly reactive oxygen species through active sites and undergo binding reactions. Second, the nitrogen atom in the piperidine ring contains lone pairs of electrons, which can share electron pairs with reactive oxygen species and hydrocarbon radicals, lowering their high-energy states and converting them into relatively stable multitwin oxygen and nitrogen-containing compounds, achieving a scavenging effect. This alleviates side reactions between the electrolyte and the cathode material, significantly improving battery cycle stability. Third, the nitrogen-containing compounds generated after the additive reacts with reactive oxygen species and radicals adhere to the positive and negative electrode interfaces, significantly improving interface properties, increasing lithium deposition efficiency, and reducing lithium nucleation overpotential. This type of additive is inexpensive, uses readily available raw materials, and has a simple electrolyte preparation process. It can be used as an additive for newly prepared electrolytes as well as a treatment agent for waste electrolytes, showing broad technological application prospects.

[0013] The lithium battery electrolyte can be obtained through conventional preparation or by dismantling and recycling used batteries. Specifically, it can be prepared using carbonate, ether, sulfone, or sulfite solvents with lithium salts.

[0014] Preferably, the thickness of the solid electrolyte interface film is 3-15 nm; the thickness of the positive electrode electrolyte interface film is 2-6 nm.

[0015] Preferably, the thickness of the solid electrolyte interface film is 3.77-12.29 nm; the thickness of the positive electrode electrolyte interface film is 1.92-5.63 nm.

[0016] Preferably, the organic solvent includes one or more of carbonates, ethers, sulfones, and sulfite solvents.

[0017] Preferably, the carbonate solvent is a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 1:1:1; the ether solvent is a mixture of ethylene glycol dimethyl ether (DME) and 1,1,2,2-tetrafluoro-3-(1,1,2,2-tetrafluoroethoxy)propane (HFE) in a volume ratio of 1:1; the sulfone solvent is a mixture of sulfolane sulfonate (TMS) and sulfolane sulfone (BS) in a volume ratio of 1:1; and the sulfite solvent is a mixture of dimethyl sulfite (DMS) and ethylene sulfite (ES) in a volume ratio of 1:1.

[0018] Preferably, the lithium salt is one or more selected from lithium hexafluorophosphate, lithium bis(trifluoromethyl)sulfonylimide, lithium difluorooxalate borate, and lithium oxalate. The total concentration of the lithium salt in the solvent is 1 mol / L.

[0019] The prepared electrolyte may also contain film-forming additives, which may be selected from one or more of fluoroethylene carbonate, ethylene sulfate, and propylene sulfate.

[0020] The waste electrolyte can be obtained by dismantling discarded button batteries, pouch batteries, or cylindrical batteries that have reached the end of their service life.

[0021] Preferably, the film-forming additive includes one or more of fluoroethylene carbonate, ethylene sulfate, and propylene sulfate.

[0022] The preparation method of the lithium battery electrolyte containing functional additives for scavenging reactive oxygen species and free radicals is carried out in an environment where the water content and oxygen content are both below 0.1 ppm. The method includes the following steps: mixing the solvent and stirring evenly, adding lithium salt, film-forming additives, and polymethylpiperidine organic compound additives and stirring until the solution is clear and transparent to obtain the lithium battery electrolyte containing functional additives for scavenging reactive oxygen species and free radicals.

[0023] Specifically, the following steps are included:

[0024] S1: Solvent premixing: Mix the organic solvent and linear carboxylic acid ester compound, stir to obtain a mixed solvent, cool to 10-20℃ and keep warm for later use;

[0025] S2: Lithium salt preparation and dissolution: The lithium salt is added to the reactor in multiple portions while stirring. Sulfur-containing substances are added (these substances react with linear carboxylic acid ester compounds to improve cycle performance) while stirring. Polymethylpiperidine compounds are added in multiple portions: first, 70% of the total polymethylpiperidine additive is added and stirred rapidly for 30 minutes; after standing for 15 minutes, the remaining 30% is added. The multiple additions of lithium salt to the reactor refer to adding 60%-70% of the total lithium salt weight first. The sulfur-containing substances are selected from one or more of the following: 1,3-propanesulfonyl lactone (PS), methylene disulfonate (MMDS), vinyl sulfate (DTD), 1,3-propenesulfonate lactone (PST), 1,4-butanesulfonyl lactone, ethyl methanesulfonate, butyl methanesulfonate, vinyl sulfite (ES), and 1,3-dithiaane.

[0026] The process of adding lithium salt to the reactor in multiple stages is as follows: 60%-70% of the total lithium salt feed is injected into the reactor through a closed pipe under a nitrogen atmosphere using a vacuum conveying system, so that the powder is instantly entrained and dispersed by the high-speed rotating solvent, with the temperature rise rate controlled to be less than 3℃ / min; 20%-35% of the total lithium salt feed is added at a rate of 200-400g / min, and stirring is carried out continuously for 30-60 minutes, with the temperature controlled to be below 30℃ and the temperature rise rate below 2℃ / min; 5%-10% of the total lithium salt feed is pulsed and circulated, with each feeding time being 10 seconds and the amount being 20g, while stirring to control the solution temperature at 25-30℃, then pausing the feeding for 20 seconds, and repeating until the solution is completely clear and transparent, thus completing the feeding process.

[0027] S3: Addition and maturation of bis(fluorosulfonyl)imide lithium salt: Add the remaining lithium salt to the system and stir continuously for 4-8 hours to obtain a lithium battery electrolyte containing functional additives that scavenge reactive oxygen species and free radicals.

[0028] In the above method, step S2, the specific operation of adding the polymethylpiperidine compound in multiple batches is as follows: first add 70% of the total amount of polymethylpiperidine dilution, stir rapidly for 30 minutes; after standing for 15 minutes, add the remaining 30%.

[0029] A lithium battery includes a lithium battery electrolyte containing additives for scavenging reactive oxygen species and free radicals, as well as a positive electrode, a negative electrode, and a separator. A high-voltage, ultra-high nickel ternary layered oxide is used as the positive electrode material. The positive electrode material is a high-voltage, ultra-high nickel ternary layered oxide material with a nickel content of ≥95%, specifically selected from LiNi. 0.95 Co 0.025 Mn 0.025 O2, LiNi 0.96 Co 0.03 Mn 0.01 O2 or LiNi 0.98 Co 0.01 Mn 0.01 O2. The positive electrode material is an aluminum foil current collector loaded with active material, and the loading of active material is 8.0 to 8.5 mg / cm².

[0030] Preferably, the method for preparing the aluminum foil current collector loaded with active material is as follows: any of the above-mentioned positive electrode active materials, conductive carbon Super P and binder PVDF are mixed and ground in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) and coated onto the aluminum foil current collector, dried in a vacuum oven at 120°C for 8 hours, and then cut into round sheets with a diameter of 15 mm by a punching machine to obtain the positive electrode sheet.

[0031] The negative electrode material can be a copper foil current collector loaded with artificial graphite, or a lithium metal sheet directly. The preparation method of the copper foil current collector loaded with artificial graphite is as follows: artificial graphite, conductive carbon Super P, binder sodium carboxymethyl cellulose (CMC), and thickener styrene-butadiene rubber (SBR) are mixed and ground in a mass ratio of 95.8:1.0:1.4:1.8, dissolved in NMP, and then coated onto the copper foil current collector. The mixture is then dried in a vacuum oven at 60°C for 8 hours, and cut into 16 mm diameter discs using a die-cutting machine to obtain the negative electrode sheet. Lithium metal sheets can be directly cut and used as the negative electrode.

[0032] The diaphragm is preferably made of polypropylene material Celgard-2500.

[0033] This invention provides the application of the lithium battery electrolyte containing the above-mentioned additives for scavenging reactive oxygen species and free radicals.

[0034] One application method is as follows: a polymethylpiperidine organic compound is added as an electrolyte additive to the prepared basic electrolyte, and then the electrolyte containing the additive is dropped onto both sides of the diaphragm so that it can fully contact and wet the positive and negative electrode plates.

[0035] Another application method is to use polymethylpiperidine organic compounds as treatment additives, add them directly to the waste electrolyte, stir evenly to obtain regenerated electrolyte, and then drop this regenerated electrolyte onto both sides of the diaphragm so that it can fully contact and wet the positive and negative electrode plates.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] The lithium battery electrolyte provided by this invention uses polymethylpiperidine organic compounds with active oxygen and free radical scavenging functions as additives, which significantly improves the cycle performance of lithium batteries using high-voltage, ultra-high nickel ternary layered oxides as positive electrode materials, extends the battery's cycle life, increases lithium deposition efficiency, and reduces lithium deposition overpotential. Simultaneously, these additives can also be used as treatment agents for waste electrolytes, generating reusable lithium battery electrolytes in one step.

[0038] The lithium battery provided by this invention has an electrolyte additive that can effectively remove active oxygen released from the positive electrode material under high voltage and free radicals generated by electrolyte decomposition. Furthermore, the products of the reaction between the additive and active oxygen and free radicals help form a positive and negative electrode-electrolyte interface phase with excellent diffusion kinetics and high mechanical strength, which can both promote lithium-ion diffusion and further protect the positive and negative electrode materials.

[0039] The electrolyte additive used in this invention is made from readily available and inexpensive raw materials. Electrolytes using this additive, as well as lithium batteries assembled from waste electrolytes treated with this additive, exhibit excellent cycle stability and low interfacial impedance, demonstrating broad prospects for large-scale commercial application. Attached Figure Description

[0040] Figure 1 This is a comparison chart of the positive electrode half-cell cycle performance using a carbonate electrolyte with added 4-dimethylamino-2,2,6,6-tetramethylpiperidine (Examples 1-1 to 1-2) and a blank carbonate electrolyte (Comparative Example 1). Figure 2 The graph shows the cycling performance of the positive electrode half-cell using an ether electrolyte containing 1,2,3,4-butanetetracarboxylic acid-1,2,3-tris(2,2,6,6-tetramethyl-4-piperidinyl)-4-tetane ester (Example 3). Figure 3 This is a comparison chart of the cycling performance of the positive electrode half-cell using a sulfite electrolyte with added 1,2,3,4-butanediol tetracarboxylate tetra(1,2,2,6,6-pentamethyl-4-piperidinyl) ester (Example 5) and a sulfite electrolyte with added 1-(methyl)-8-(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate (Example 6). Figure 4 This is a comparison chart of the cycling performance of the positive electrode half-cell using waste electrolyte with added N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide (Example 7) and untreated waste electrolyte (Comparative Example 6).

[0041] Figure 5 Transmission electron microscopy (TEM) images of the SEI layer and CEI layer of the graphite anode using an ether electrolyte containing N,N'-bis-(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine (Example 2) and an ether electrolyte containing 1,2,3,4-butanetetracarboxylic acid-1,2,3-tris(2,2,6,6-tetramethyl-4-piperidinyl)-4-tetrazol ester (Example 3).

[0042] Figure 6 Transmission electron microscopy (TEM) images of the graphite anode SEI layer and cathode CEI layer using a carbonate electrolyte with 4-dimethylamino-2,2,6,6-tetramethylpiperidinamide (Examples 1-2) and a sulfite electrolyte with N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamine (Example 4).

[0043] Figure 7 These are transmission electron micrographs of the SEI layer of the graphite anode and the CEI layer of the graphite cathode using blank carbonate electrolyte (Comparative Example 1) and blank ether electrolyte (Comparative Example 2).

[0044] Figure 8 This is a comparison chart of the lithium deposition / stripping efficiency of lithium copper half-cells in the first 20 cycles using carbonate electrolyte with added 4-dimethylamino-2,2,6,6-tetramethylpiperidine (Examples 1-1 to 1-2) and blank carbonate electrolyte (Comparative Example 1). Figure 9 This is a comparison chart of the lithium deposition / stripping efficiency of a lithium copper half-cell using an ether electrolyte containing 1,2,3,4-butanetetracarboxylic acid-1,2,3-tris(2,2,6,6-tetramethyl-4-piperidinyl)-4-tetane ester (Example 3) and a sulfite electrolyte containing 1-(methyl)-8-(1,2,2,6,6-pentamethyl-4-piperidin) sebacic acid ester (Example 6) for the first 20 cycles. Figure 10 This is a comparison chart of the lithium deposition / stripping efficiency of lithium copper half-cells in the first 20 cycles using waste electrolyte with added N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide (Example 7) and untreated waste electrolyte (Comparative Example 6). Figure 11 This is a comparison chart of the first-cycle lithium deposition overpotential of a lithium-copper battery using a carbonate electrolyte with added 4-dimethylamino-2,2,6,6-tetramethylpiperidine (Examples 1-1 to 1-2) and a blank carbonate electrolyte (Comparative Example 1). Figure 12 This is a comparison of the first-cycle lithium deposition overpotential of lithium-copper batteries using an ether electrolyte containing 1,2,3,4-butanetetracarboxylic acid-1,2,3-tris(2,2,6,6-tetramethyl-4-piperidinyl)-4-tetrazolium ester (Example 3), a sulfite electrolyte containing 1,2,3,4-butanetetracarboxylic acid tetra(1,2,2,6,6-pentamethyl-4-piperidinyl) ester (Example 5), and a sulfite electrolyte containing 1-(methyl)-8-(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate (Example 6). Figure 13 This is a comparison chart of the first-cycle lithium deposition overpotential of a lithium copper half-cell using waste electrolyte with added N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide (Example 7) and untreated waste electrolyte (Comparative Example 6). Figure 14 The graph shows the voltage changes during the deposition / stripping process of a lithium-lithium symmetric battery using a carbonate electrolyte with added 4-dimethylamino-2,2,6,6-tetramethylpiperidine (Examples 1-1 to 1-2) and a blank carbonate electrolyte (Comparative Example 1). Figure 15 The graph shows the voltage changes during the deposition / stripping process of a lithium-lithium symmetric battery using a sulfone electrolyte with added N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide (Example 4) and a sulfone electrolyte without added reactive oxygen species scavenging additives (Comparative Example 4). Figure 16This is a voltage change graph of the deposition / stripping process of a lithium-lithium symmetric battery using an ether electrolyte containing 1,2,3,4-butanetetracarboxylic acid-1,2,3-tris(2,2,6,6-tetramethyl-4-piperidinyl)-4-tetrazolium ester (Example 3) and a sulfite electrolyte containing 1,2,3,4-butanetetracarboxylic acid tetra(1,2,2,6,6-pentamethyl-4-piperidinyl) ester (Example 5). Figure 17 This is a voltage change graph of the lithium-lithium symmetric battery deposition / stripping process using waste electrolyte with added N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide (Example 7) and untreated waste electrolyte (Comparative Example 6). Figure 18 This is a voltage variation graph of the intermittent lithium deposition process in a lithium-copper battery using a carbonate electrolyte with added 4-dimethylamino-2,2,6,6-tetramethylpiperidine (Examples 1-1 to 1-2) and a blank carbonate electrolyte (Comparative Example 1). Figure 19 This is a voltage variation diagram of the intermittent lithium deposition process in a lithium-copper battery using an ether electrolyte with added N,N'-bis-(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine (Example 2) and an ether electrolyte without added reactive oxygen free radical scavenging additives (Comparative Example 2). Figure 20 This is a voltage variation diagram of the intermittent lithium deposition process in a lithium-copper battery using waste electrolyte with added N,N'-bis-(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine (Example 8) and untreated waste electrolyte (Comparative Example 6). Detailed Implementation

[0045] Within the scope of this invention, those skilled in the art can make various modifications and variations to its specific embodiments. The specification and embodiments of this invention are merely illustrative and should not be construed as limiting the scope of protection.

[0046] The polymethylpiperidine organic compounds, lithium salts, solvents, battery casings, separators, high-voltage ultra-high nickel ternary layered oxide cathode materials, lithium metal sheets, and waste electrolytes involved in the embodiments of this invention were all purchased from the market. This invention does not impose any particular restrictions on the specific models of the battery casings, lithium sheets, or separators.

[0047] Example 1

[0048] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, 1.0 mol / L LiPF6 was added to a mixed solvent of EC, EMC, and DEC (volume ratio EC:EMC:DEC = 1:1:1). Three mixed solvents were prepared in total. 0.1 wt%, 0.3 wt%, and 0.5 wt% of 4-dimethylamino-2,2,6,6-tetramethylpiperidine were added to each mixture. After thorough mixing, lithium battery electrolytes containing 0.1 wt%, 0.3 wt%, and 0.5 wt% additives were obtained, and these were respectively designated as Example 1-1, Example 1-2, and Example 1-3.

[0049] Battery assembly: (1) Positive half-cell: The positive electrode half-cell is coated with LiNi 0.98 Co 0.01 Mn 0.01 O2 positive electrode material was cut into 15 mm diameter discs with a loading of 8.5–10 mg / cm². The electrolyte prepared in Example 1 was used in a volume of 60 μL. The separator was a Celgard-2500 with a diameter of 18 mm. The negative electrode was a 15 mm diameter lithium metal sheet. The battery casing was a CR2025 stainless steel shell. The positive half-cell was assembled in an argon-filled glove box for testing long-cycle performance and impedance. (2) Lithium-copper half-cell: Fresh copper foil was cut into 16 mm diameter discs as working electrodes. The electrolyte prepared in Example 1 was used in a volume of 60 μL. The separator was a Celgard-2500 with a diameter of 18 mm. The negative electrode was a 15 mm diameter lithium metal sheet. The casing was a CR2025 type. The lithium-copper half-cell was assembled for testing the nucleation overpotential of lithium, deposition / stripping efficiency, and the degree of reaction between the electrolyte and lithium metal. (3) Lithium-lithium symmetric battery: A lithium sheet with a diameter of 15 mm is used as both the working electrode and the counter electrode. The electrolyte prepared in Example 1 is used in a quantity of 60 μL. The separator is a Celgard-2500 with a diameter of 18 mm. The casing is a CR2025 type. The lithium-lithium symmetric battery is assembled to test the nucleation overpotential of lithium.

[0050] Electrochemical performance testing:

[0051] Positive half-cell: After standing at 25°C for 8 hours, it is activated at a rate of 0.1 C for 3 cycles, and then charged and discharged at a rate of 1 C in the voltage range of 2.8 to 4.3 V.

[0052] Lithium-copper half-cell (continuous testing): After standing at 25°C for 8 hours, continuous lithium stripping / deposition tests were conducted at a current density of 0.5 mA / cm² and a deposition amount of 0.5 mAh / cm².

[0053] Lithium-copper half-cell (intermittent deposition): After standing at 25°C for 8 hours, lithium is deposited in a single pass at a current density of 10 µA / cm², followed by standing until the cell voltage is ≥0.05 V, and then deposition continues, repeating the cycle.

[0054] Lithium-lithium symmetric cells: After standing at 25°C for 8 hours, continuous deposition / stripping tests were conducted at current densities of 0.5 mA / cm²-1 mAh / cm² and deposition amounts.

[0055] Example 2

[0056] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, DME and HFE were mixed at a volume ratio of 1:1. 1.0 mol / L LiTFSI was added, followed by 5.0 wt% fluoroethylene carbonate as a film-forming additive. Finally, 0.3 wt% N,N'-bis-(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine was added. After mixing thoroughly, a lithium battery electrolyte containing 0.3 wt% additive was obtained.

[0057] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is LiNi. 0.96 Co 0.03 Mn 0.01 O2.

[0058] Example 3

[0059] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, DME and HFE were mixed at a volume ratio of 1:1, 1.0 mol / L LiDFOB was added, followed by 0.4 wt% of 1,2,3,4-butanetetracarboxylic acid-1,2,3-tris(2,2,6,6-tetramethyl-4-piperidinyl)-4-tridecane ester. After mixing thoroughly, a lithium battery electrolyte containing 0.4 wt% additives was obtained.

[0060] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is LiNi. 0.96 Co 0.03 Mn 0.01 O2.

[0061] Example 4

[0062] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, TMS and BS were mixed at a volume ratio of 1:1. 0.5 mol / L LiPF6 and 0.5 mol / L LiTFSI were added, followed by 5.0 wt% vinyl sulfate as a film-forming additive. Finally, 0.2 wt% N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide was added and mixed thoroughly to obtain the electrolyte containing the additive.

[0063] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is LiNi. 0.98 Co 0.01 Mn 0.01 O2.

[0064] Example 5

[0065] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, DMS and ES were mixed at a volume ratio of 1:1. LiFSI and LiTFSI were added, with the concentration of both lithium salts in the solvent being 0.5 mol / L. Finally, 0.3 wt% of tetra(1,2,2,6,6-pentamethyl-4-piperidinyl) 1,2,3,4-butanetetracarboxylic acid tetra(1,2,2,6,6-pentamethyl-4-piperidinyl) ester was added, and the mixture was stirred until clear and transparent to obtain an electrolyte containing additives.

[0066] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is LiNi. 0.95 Co 0.025 Mn 0.025 O2.

[0067] Example 6

[0068] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, DMS and ES were mixed at a volume ratio of 1:1. LiFSI and LiTFSI were added, with the concentration of both lithium salts in the solvent being 0.5 mol / L. Finally, 0.5 wt% of 1-(methyl)-8-(1,2,2,6,6-pentamethyl-4-piperidine) sebacate was added and stirred until clear and transparent to obtain an electrolyte containing additives.

[0069] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is LiNi. 0.95 Co 0.025 Mn 0.025 O2.

[0070] Example 7

[0071] Electrolyte preparation: 3.0 wt% of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide was directly added to the electrolyte of the waste lithium battery and stirred until clear and transparent to obtain the regenerated electrolyte.

[0072] Battery assembly and electrochemical testing: Same as Example 1. The positive electrode material used in the positive half-cell is LiNi. 0.98 Co 0.01 Mn 0.01 O2.

[0073] Example 8

[0074] Electrolyte preparation: 2.0 wt% of N,N'-bis-(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine was directly added to the electrolyte of the waste lithium battery and stirred until clear and transparent to obtain the regenerated electrolyte.

[0075] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is LiNi. 0.98 Co 0.01 Mn 0.01 O2.

[0076] Comparative Example 1

[0077] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, 1.0 mol / L LiPF6 was added to a mixed solvent of EC, EMC and DEC (volume ratio 1:1:1) and stirred until clear and transparent to obtain an electrolyte without additives.

[0078] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is the same as in Example 1.

[0079] Comparative Example 2

[0080] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, DME and HFE were mixed at a volume ratio of 1:1, 1.0 mol / L LiTFSI was added, and then 5.0 wt% fluoroethylene carbonate was added. The mixture was stirred and mixed evenly to obtain an electrolyte without additives.

[0081] Battery assembly and electrochemical testing: Same as in Example 2. The positive electrode material used in the positive half-cell is the same as in Example 2.

[0082] Comparative Example 3

[0083] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, DME and HFE were mixed at a volume ratio of 1:1, and 1.0 mol / L LiDFOB was added. The mixture was stirred until clear and transparent to obtain an electrolyte without additives.

[0084] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is the same as in Example 3.

[0085] Comparative Example 4

[0086] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm, H2O < 0.1 ppm, TMS and BS were mixed at a volume ratio of 1:1. 0.5 mol / L LiPF6 and 0.5 mol / L LiTFSI were added, followed by 5.0 wt% vinyl sulfate. The mixture was stirred until clear and transparent to obtain an electrolyte without additives.

[0087] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is the same as in Example 4.

[0088] Comparative Example 5

[0089] Electrolyte preparation: In a glove box filled with high-purity argon and containing O2 < 0.1 ppm and H2O < 0.1 ppm, DMS and ES were mixed at a volume ratio of 1:1. LiFSI and LiTFSI were added, with the concentration of both lithium salts being 0.5 mol / L. The mixture was stirred until clear and transparent to obtain an electrolyte without additives.

[0090] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is the same as in Example 5.

[0091] Comparative Example 6

[0092] Electrolyte preparation: Directly use untreated waste electrolyte.

[0093] Battery assembly and electrochemical testing: Same as in Example 1. The positive electrode material used in the positive half-cell is the same as in Example 7.

[0094] Data aggregation and analysis

[0095] The specific electrolyte formulation data for each embodiment and comparative example are summarized in Table 1, and the electrochemical performance data are summarized in Table 2.

[0096] Table 1

[0097]

[0098] Table 2

[0099]

[0100] From Table 2 and Figure 1 It can be seen that 4-dimethylamino-2,2,6,6-tetramethylpiperidine was added in Examples 1-1, 1-2, and 1-3, with the best effect observed at an addition amount of 0.3 wt%, achieving an initial specific capacity of 228.80 mAh / g for the positive electrode half-cell and a capacity retention rate of 73.34% after 300 cycles. In contrast, the initial specific capacity and capacity retention rate of Examples 1-1, 1-3, and Comparative Example 1 were inferior to those of Example 1-2. This indicates that 4-dimethylamino-2,2,6,6-tetramethylpiperidine has a significant reactive oxygen species scavenging effect, and there is an optimal range for its addition amount.

[0101] Figure 2 and Figure 3 The results show that polymethylpiperidine organic compounds, as reactive oxygen free radical scavenging additives, also exhibit excellent effects in ether electrolytes (Example 3) and sulfite electrolytes (Examples 5 and 6), maintaining a high capacity retention rate after 300 cycles, indicating that this type of additive has universality in different solvent systems.

[0102] In addition, polymethylpiperidine compounds also have the function of treating waste electrolytes. For example... Figure 4 As shown, after adding 3.0 wt% N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide, the positive electrode half-cell of Example 7 exhibited significantly better cycling performance compared to Comparative Example 6.

[0103] To demonstrate the impact of additives on the thickness of the formed SEI and CEI layers, a full cell was disassembled and cycled 50 times with the corresponding electrolyte, and transmission electron microscopy (TEM) images of the positive and negative electrode materials were taken. When the SEI layer thickness is 3-13 nm, the SEI on the negative electrode side is sufficient to passivate the reduction reaction and inhibit dendrite growth; if it is too thin, it will not be able to effectively isolate the negative electrode material from the electrolyte. When the CEI layer thickness is 2-6 nm, the interface layer is thin and dense, rich in nitrides, which can efficiently conduct lithium ions while blocking the attack of reactive oxygen species / free radicals; if it is too thick, it will hinder the transport of lithium ions.

[0104] like Figure 5 , Figure 6As shown, the average thickness of the SEI layer in Examples 2 and 3 is 12.29 nm and 8.63 nm, respectively, which can effectively passivate the negative electrode layer; the average thickness of the CEI layer is 1.92 nm and 2.63 nm, respectively, both exhibiting thin and dense characteristics, and the corresponding positive electrode half-cell cycle data are optimal. The average thickness of the SEI layer in Examples 1-2 and 4 is 4.55 nm and 3.77 nm, respectively, slightly thinner than that in Examples 2 and 3; the average thickness of the CEI layer is 4.05 nm and 5.63 nm, respectively, slightly thicker than that in Examples 2 and 3. Therefore, the cycle retention rate of the positive electrode half-cells in these two examples is slightly inferior to that in Examples 3 and 4.

[0105] like Figure 7 As shown, the average thickness of the SEI layer in Comparative Example 1 and Comparative Example 2 is 3.46 nm and 2.50 nm, respectively. The SEI layer and CEI layer formed in the electrolyte without the addition of piperidine additives cannot effectively passivate the negative electrode material and alleviate the decomposition of the electrolyte, and their corresponding half-cell cycle data are the worst.

[0106] To characterize the extent of side reactions between lithium metal and the electrolyte, lithium-copper batteries were further assembled to test the lithium deposition / stripping efficiency and deposition overpotential. Higher average efficiency and lower overpotential indicate less severe side reactions between lithium metal and the electrolyte. This reflects that the additives, on the one hand, scavenge free radicals in the electrolyte, mitigating side reactions with lithium metal, and on the other hand, form a nitrogen-containing inorganic interface layer, lowering the energy barrier for lithium ion nucleation / deposition.

[0107] like Figure 8 , Figure 9 As shown, the average deposition / stripping efficiencies of Examples 1-2, 3, and 6 were 91.95%, 93.71%, and 93.47%, respectively, while that of Comparative Example 1 was only 62.07%, demonstrating the significant effect of polymethylpiperidine additives in alleviating side reactions. Figure 10 Further evidence shows that this type of additive has a similar effect in waste electrolytes.

[0108] like Figure 11 , Figure 12 , Figure 13 As shown, the lithium deposition overpotential in Examples 1-2 was 50.08 mV, while that in Comparative Example 1 was 66.21 mV, indicating that the nitrogen-containing interface layer significantly improved the diffusion rate of lithium ions. The ether-based and sulfite-based electrolytes with this additive exhibited lower nucleation overpotentials. Comparative Example 6, containing a waste electrolyte, had the highest nucleation overpotential of 238.71 mV, attributed to the presence of a large amount of solvent / lithium salt decomposition debris and active oxygen. However, the addition of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide reduced the lithium nucleation overpotential to 53.98 mV.

[0109] The deposition / stripping voltage curves of lithium-ion symmetric batteries can also reflect the compatibility between the electrolyte and lithium metal. (See Table 2 and...) Figure 14 , Figure 15 , Figure 16 , Figure 17 It can be seen that: the lithium-lithium symmetric batteries of Examples 1-2 failed due to short circuit after 492 hours of cycling, while Comparative Example 1 short-circuited after only 191 hours; the symmetric battery of Example 4 had a significantly longer cycle time than Comparative Example 4; the symmetric batteries of Examples 3 and 5 both had cycle times exceeding 1000 hours; the battery with the added additive waste electrolyte (Example 7) had a cycle time of up to 409 hours, while the untreated waste electrolyte (Comparative Example 6) had an initial voltage higher than that of Example 7 and short-circuited in less than 150 hours of cycling. All of the above data indicate that the addition of polymethylpiperidine organic compounds significantly improves the compatibility of the electrolyte with lithium metal.

[0110] Intermittent lithium deposition experiments can more directly reflect the degree of side reactions between lithium metal and the electrolyte. The principle involves depositing small amounts of lithium onto a copper foil multiple times. After the electrolyte reacts with the lithium metal, the battery voltage increases. Once a certain value is reached, deposition continues, and this process is repeated. Therefore, within the same time frame, fewer cycles indicate a less severe reaction between the lithium metal and the electrolyte.

[0111] like Figure 18 , Figure 19 , Figure 20 As shown, compared with Comparative Example 1, Comparative Example 2 and Comparative Example 2, and Comparative Example 8 and Comparative Example 6, the batteries using electrolytes with added reactive oxygen species scavenging additives all exhibited fewer lithium deposition cycles and lower overpotentials. Based on this, it can be concluded that the polymethylpiperidine organic compounds react with the free radicals generated from electrolyte decomposition to produce nitrogen-containing compounds, which not only alleviates the side reactions between the electrolyte and lithium metal but also forms a high-performance interface layer.

[0112] In summary, this invention achieves the following significant advantages by adding polymethylpiperidine organic compounds with reactive oxygen species scavenging functions to the lithium battery electrolyte:

[0113] (1) The polymethylpiperidine organic compounds used in this invention have the function of scavenging reactive oxygen free radicals. The electron cloud arrangement of the piperidine ring endows it with certain electron affinity characteristics, which can attract highly reactive reactive oxygen through active sites and undergo binding reactions. At the same time, the lone pair electrons of the nitrogen atom in the piperidine ring can form an electron pair sharing mechanism with reactive oxygen and hydrocarbon free radicals, reduce their high energy state, and transform them into relatively stable multi-trace oxygen and nitrogen-containing compounds, thereby achieving the scavenging effect, effectively suppressing the side reactions of the electrolyte and cathode materials, and significantly enhancing the cycle stability of the battery.

[0114] (2) The nitrogen-containing compounds generated by the reaction of the additive with active oxygen and free radicals are uniformly attached to the positive and negative electrode interfaces to form a stable interface film, which significantly improves the uniformity of the electrode interface and the ion conduction ability, effectively enhances the density and uniformity of lithium deposition, inhibits dendrite growth, and reduces the overpotential of lithium nucleation, thereby further enhancing the cycle stability and safety of the battery.

Claims

1. A lithium battery electrolyte containing additives that scavenge reactive oxygen species and free radicals, characterized in that, The electrolyte includes an additive that converts reactive oxygen free radicals into components capable of forming high-performance interfacial films; the additive is an organic compound containing a polymethylpiperidine structure, and the concentration of the additive in the lithium battery electrolyte is 0.1–3.0 wt%. The polymethylpiperidine organic compounds are 4-dimethylamino-2,2,6,6-tetramethylpiperidine, N,N'-bis-(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-phenylenediamide, 1,2,3,4-butanetetracarboxylic acid tetra(1,2,2,6,6-pentamethyl-4-piperidinyl) ester, 1-(methyl)-8-(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, or 1,2,3,4-butanetetracarboxylic acid-1,2,3-tris(2,2,6,6-tetramethyl-4-piperidinyl)-4-tridecane ester; The additive can react with reactive oxygen species and free radicals to generate beneficial components of a solid electrolyte interface film on the negative electrode surface and beneficial components of a positive electrode electrolyte interface film on the positive electrode surface. The electrolyte is obtained by preparation or by dismantling and recycling waste batteries; the prepared electrolyte includes organic solvents, linear carboxylic acid ester compounds, lithium salts and film-forming additives.

2. The lithium battery electrolyte containing additives for scavenging reactive oxygen species and free radicals according to claim 1, characterized in that, The thickness of the solid electrolyte interface film is 3-15 nm; the thickness of the positive electrode electrolyte interface film is 2-6 nm.

3. The lithium battery electrolyte containing additives for scavenging reactive oxygen species and free radicals according to claim 1, characterized in that, The thickness of the solid electrolyte interface film is 3.77-12.29 nm; the thickness of the positive electrode electrolyte interface film is 1.92-5.63 nm.

4. The lithium battery electrolyte containing additives for scavenging reactive oxygen species and free radicals according to claim 1, characterized in that, The organic solvent includes one or more of the following: carbonates, ethers, sulfones, and sulfite solvents.

5. The lithium battery electrolyte containing additives for scavenging reactive oxygen species and free radicals according to claim 4, characterized in that, The carbonate solvent is a mixture of ethylene carbonate, methyl ethyl carbonate, and diethyl carbonate in a volume ratio of 1:1:1; the ether solvent is a mixture of ethylene glycol dimethyl ether and 1,1,2,2-tetrafluoro-3-(1,1,2,2-tetrafluoroethoxy)propane in a volume ratio of 1:1; the sulfone solvent is a mixture of sulfolane and sulfolane in a volume ratio of 1:1; and the sulfite solvent is a mixture of dimethyl sulfite and ethylene sulfite in a volume ratio of 1:

1.

6. The lithium battery electrolyte containing additives for scavenging reactive oxygen species and free radicals according to claim 4, characterized in that, The lithium salt is one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethyl)sulfonylimide, and lithium difluorooxalate borate.

7. The lithium battery electrolyte containing additives for scavenging reactive oxygen species and free radicals according to claim 4, characterized in that, The film-forming additive includes one or more of fluoroethylene carbonate, ethylene sulfate, and propylene sulfate.

8. The method for preparing a lithium battery electrolyte containing functional additives for scavenging reactive oxygen species and free radicals according to any one of claims 1 to 7, characterized in that, The preparation process is carried out in an environment where the water content and oxygen content are both below 0.1 ppm, and includes the following steps: after mixing the solvent and stirring evenly, lithium salt, film-forming additive, and polymethylpiperidine organic compound additive are added and stirring is continued until the solution is clear and transparent, thus obtaining a lithium battery electrolyte containing additives that scavenge reactive oxygen species and free radicals.

9. The method for preparing the lithium battery electrolyte containing functional additives for scavenging reactive oxygen species and free radicals according to claim 8, characterized in that, Includes the following steps: S1: Solvent premixing: Mix the organic solvent and linear carboxylic acid ester compound, stir to obtain a mixed solvent, cool to 10-20℃ and keep warm for later use; S2: Preparation and dissolution of lithium salt: The lithium salt is added to the reactor in multiple portions while stirring. Sulfur-containing substances are added while stirring continuously. Polymethylpiperidine compounds are added in multiple portions: first, 70% of the total weight of the polymethylpiperidine additive is added, and the mixture is stirred rapidly for 30 minutes; after standing for 15 minutes, the remaining 30% is added. The multiple additions of lithium salt to the reactor refer to adding 60%-70% of the total weight of lithium salt first. The sulfur-containing substances are selected from one or more of the following: 1,3-propanesulfonyl lactone (PS), methylene disulfonate (MMDS), vinyl sulfate (DTD), 1,3-propenesulfonate lactone (PST), 1,4-butanesulfonyl lactone, ethyl methanesulfonate, butyl methanesulfonate, vinyl sulfite (ES), and 1,3-dithiaane. The process of adding lithium salt to the reactor in multiple stages is as follows: 60%-70% of the total lithium salt feed is injected into the reactor through a closed pipe under a nitrogen atmosphere using a vacuum conveying system, so that the powder is instantly entrained and dispersed by the high-speed rotating solvent, with the temperature rise rate controlled to be less than 3℃ / min; 20%-35% of the total lithium salt feed is added at a rate of 200-400g / min, and stirring is carried out continuously for 30-60 minutes, with the temperature controlled to be below 30℃ and the temperature rise rate below 2℃ / min; 5%-10% of the total lithium salt feed is pulsed and circulated, with each feeding time being 10 seconds and the amount being 20g, while stirring to control the solution temperature at 25-30℃, then pausing the feeding for 20 seconds, and repeating until the solution is completely clear and transparent, thus completing the feeding process. S3: Addition and maturation of bis(fluorosulfonyl)imide lithium salt: Add the remaining lithium salt to the system and stir continuously for 4-8 hours to obtain a lithium battery electrolyte containing functional additives that scavenge reactive oxygen species and free radicals.

10. A lithium battery, characterized in that, The lithium battery electrolyte containing functional additives for scavenging reactive oxygen species and free radicals, as described in any one of claims 1 to 7, as well as a positive electrode, a negative electrode, and a separator.