A lithium metal battery electrolyte, its preparation method and its application
By utilizing the dipole-dipole interaction of flexible solvent and diluent, anions are preferentially decomposed in lithium metal batteries to form a gradient SEI film with a high proportion of inorganic components. This solves the problems of lithium dendrite growth and dead lithium accumulation, and improves the cycle life and coulombic efficiency of lithium metal batteries.
Patent Information
- Application Number
- CN202611479213.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Lithium metal anodes suffer from problems such as uncontrollable lithium dendrite growth and dead lithium accumulation during charge-discharge cycles, resulting in short battery cycle life and low coulombic efficiency.
An electrolyte design containing a flexible solvent, a diluent, and a lithium salt is adopted. Through the interaction between the third polar group of the diluent and the dipole-dipole interaction of the flexible solvent, the flexible solvent is stabilized in a low polarity spatial conformation. This promotes the entry of anions into the first solvation layer of lithium ions and their preferential decomposition on the negative electrode surface, forming a gradient SEI film with a high proportion of inorganic components. This enhances mechanical strength and guides the uniform deposition of lithium ions.
It inhibits lithium dendrite growth, reduces interface impedance, improves coulombic efficiency and extends cycle life, while also expanding the design space for electrolyte composition.
Smart Images

Figure CN123120888A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochemical energy storage technology, and in particular to a lithium metal battery electrolyte, its preparation method, and its application. Background Technology
[0002] Lithium metal boasts a theoretical specific capacity of up to 3860 mAh / g and an electrochemical potential of -3.040 V (relative to the standard hydrogen electrode), making it the anode material with the lowest known potential. These two characteristics, when matched with a high-voltage cathode, suggest that batteries could achieve energy densities of 450–600 Wh / kg. However, lithium metal anodes suffer from uncontrollable lithium dendrite growth and continuous accumulation of dead lithium during charge-discharge cycles. These issues lead to shorter cycle life and lower coulombic efficiency, thus limiting the practical application of lithium metal anodes. To address these problems, researchers have proposed various improvement strategies. Among these, electrolyte engineering control is widely considered one of the most promising engineering approaches due to its lack of need to change electrode materials and battery structure and its good compatibility with existing production lines.
[0003] In conventional electrolytes, the first solvation layer of lithium ions is mainly occupied by solvent molecules. During charging and discharging, when a solid electrolyte interface film forms on the negative electrode surface, solvent molecules are usually the first to decompose. Solvent decomposition products have several drawbacks: firstly, the transport of lithium ions within them is not uniform, easily inducing lithium dendrite growth and the accumulation of dead lithium; secondly, they have low mechanical strength, making them prone to breakage during volume changes caused by lithium deposition and extraction; and thirdly, they have low electron insulation, making it difficult to prevent continuous electrolyte penetration and reaction with lithium, leading to repeated rupture, repair, and thickening of the interface film during long battery cycles, resulting in a continuous increase in interfacial impedance, a decrease in coulombic efficiency, and insufficient cycle life. The localized high-concentration electrolyte strategy was developed to address this problem. This strategy introduces a diluent to encourage anions to enter the first solvation layer of lithium ions, causing the anions to decompose before the solvent on the negative electrode surface, forming an interface film mainly composed of inorganic components such as lithium fluoride. This type of inorganic interface film has high mechanical strength and can guide uniform lithium deposition to slow down dendrite growth. However, in this strategy, the diluent mainly plays the role of diluting the main solvent, and its ability to promote the participation of anions in solvation is limited. Therefore, the above-mentioned interface regulation effect is also relatively limited. Summary of the Invention
[0004] The purpose of this invention is to provide a lithium metal battery electrolyte, its preparation method, and its application, in order to solve the problems mentioned in the background art.
[0005] The technical solution adopted in this invention is: a lithium metal battery electrolyte, wherein the electrolyte contains at least: lithium salt;
[0006] A flexible solvent comprising a first polar group, a second polar group, and a flexible segment connecting the two, the flexible solvent having multiple spatial conformations based on the internal rotation of the flexible segment;
[0007] A diluent containing a third polar group;
[0008] Furthermore, based on the dipole-dipole interactions between the first polar group, the second polar group, and the third polar group, the flexible solvent is in a spatial conformation in which the dipole vectors of the first polar group and the second polar group are antiparallel.
[0009] Preferably, the dipole moment of the third polar group is greater than or equal to 3.0D.
[0010] Preferably, the diluent includes at least one selected from sulfolane, sulfolane, dimethyl sulfone, propylene carbonate, ethylene carbonate, and γ-butyrolactone.
[0011] Preferably, the flexible segment comprises —(CH2) n — where n is an integer greater than or equal to 2.
[0012] Preferably, the flexible solvent includes at least one selected from adiponitrile, glutaronitrile, octanoic acid, 1,2-bis(methanesulfonyl)ethane, 1,3-bis(methanesulfonyl)propane and 1,2-bis(acetyl)ethane.
[0013] Preferably, the molar ratio of the flexible solvent to the diluent is 1:(0.5~8).
[0014] Preferably, the electrolyte contains a basic organic solvent, which includes at least one selected from 1,2-dimethoxyethane, 1,3-dioxolane, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether. The volume ratio of the basic organic solvent to the total volume of the flexible solvent and the diluent is 1:(0.4~0.8). The lithium salt includes at least one selected from lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide. The concentration of the lithium salt in the basic organic solvent is 0.8 mol / L to 4 mol / L.
[0015] Preferably, the electrolyte includes an interfacial film-forming functional aid, which includes at least one of fluoroethylene carbonate, lithium difluorooxalate borate, and tris(trimethylsilyl)phosphate; the mass of the interfacial film-forming functional aid accounts for 0.5% to 5% of the mass of the electrolyte.
[0016] The technical solution of the present invention also includes: a method for preparing the above-mentioned lithium metal battery electrolyte, which includes the steps of: dissolving lithium salt in a basic organic solvent under an inert atmosphere, and then adding a flexible solvent and a diluent in sequence, and mixing them evenly to obtain a lithium metal battery electrolyte.
[0017] The technical solution of the present invention also includes: the application of the above-mentioned lithium metal battery electrolyte in lithium metal batteries.
[0018] The beneficial effects of this invention are as follows: through the dipole-dipole interaction between the third polar group of the diluent and the first or second polar group of the flexible solvent, the flexible solvent is stabilized in a low polarity spatial conformation in a statistically average sense, reducing its coordination ability for lithium ions, promoting the entry of anions into the first solvation layer of lithium ions and preferential decomposition on the negative electrode surface, forming a gradient SEI film with a high proportion of inorganic components near the negative electrode and a high proportion of organic components near the electrolyte, thereby improving the mechanical strength of the interface, guiding the uniform deposition of lithium ions, inhibiting lithium dendrite growth and dead lithium accumulation, reducing interface impedance, improving coulombic efficiency and extending cycle life, and at the same time broadening the design space of electrolyte composition. Attached Figure Description
[0019] Figure 1 This is a comparison chart of the cycle capacity retention rates of the secondary soft-pack lithium metal batteries prepared in Example 1 and Comparative Example 1 of the present invention.
[0020] Figure 2 This is a comparison of the electrochemical impedance spectroscopy of the lithium metal secondary soft-pack batteries prepared in Example 1 and Comparative Example 1 after 100 cycles. Detailed Implementation
[0021] To better illustrate the objectives, complete technical approach, and advantages of this invention, the following detailed description will be provided in conjunction with specific embodiments. However, the embodiments described below are only a part of the embodiments of this invention and do not include all embodiments. Other embodiments that can be obtained by those skilled in the art without creative effort based on the embodiments of this invention are all within the protection scope of this invention.
[0022] In the embodiments described below, unless otherwise specified, the conventional methods used are all technical means recognized or commonly used by those skilled in the art, and the instruments, reagents, consumables, etc. used in the embodiments of the present invention can be obtained through legitimate commercial channels.
[0023] This invention provides a lithium metal battery electrolyte containing at least a lithium salt, a flexible solvent, and a diluent. The flexible solvent contains a first polar group, a second polar group, and a flexible segment connecting the two. This flexible segment has internal rotational freedom, allowing the flexible solvent to have multiple spatial conformations in the electrolyte under the combined influence of thermal motion and lithium-ion coordination, and it tends to transform into a strongly polar conformation with high coordination with lithium ions. The diluent contains a third polar group, which, when spatially adjacent to the first or second polar group,... This method, through dipole-dipole interactions, increases the proportion of flexible solvents in a spatial conformation where the dipole vectors of the first and second polar groups are antiparallel. This allows the flexible solvent to remain statistically stable in this spatial conformation, thereby reducing its molecular polarity and coordination ability with lithium ions. This promotes the entry of anions into the first solvation layer of lithium ions and lowers the desolvation energy barrier, resulting in anion decomposition at the negative electrode surface before the solvent during SEI film formation. This creates a gradient SEI film with a high proportion of inorganic components near the negative electrode and a high proportion of organic components near the electrolyte. In this gradient SEI film, the higher proportion of inorganic components near the negative electrode provides higher mechanical strength and guides uniform lithium ion deposition, thus mitigating dendrite growth. The higher proportion of organic components near the electrolyte provides better compatibility with the electrolyte, which helps maintain interface stability during cycling. Based on this, the interfacial impedance of the battery is reduced, coulombic efficiency is improved, and cycle life is extended.
[0024] Based on the above technical approach, the design space for electrolyte components is significantly broadened. Existing strategies for inducing conformational changes in flexible solvents mostly rely on hydrogen bonding, but the bond energy of hydrogen bonds is typically only 2–8 kJ / mol, thus limiting their conformational stability. Furthermore, hydrogen bond formation has specific requirements for donor-acceptor pairing, limiting currently available flexible solvents to cyclic ether compounds with specific compositions. In contrast, the dipole-dipole interaction employed in this approach does not depend on specific donor-acceptor pairings; it can participate as long as the molecule contains a strongly polar group, and its strength is proportional to the square of the dipole moment, allowing for flexible control by selecting functional groups of different polarities. Therefore, this approach not only offers better conformational stability but also provides a wider range of selectable flexible solvents.
[0025] In the construction of the aforementioned locally high-concentration electrolyte system, the lithium salt first needs to form a sufficiently solvated structure with the flexible solvent, placing the lithium ions in a solvated environment dominated by the flexible solvent. Subsequently, the dipole-dipole interactions of the diluent reduce the molecular polarity of the flexible solvent, promoting the entry of anions into the first solvation layer of lithium ions. This process of first solvation and then reducing polarity requires the flexible solvent to undergo a spatial conformational change in the electrolyte; therefore, the flexible segment preferably contains —(CH2).n — and n is an integer greater than or equal to 2. An integer n greater than or equal to 2 means that the flexible segment is composed of at least two methylene groups, and the segment length is sufficient to provide the necessary internal rotational freedom, allowing the flexible solvent to effectively switch between strongly polar conformations and low-polarity spatial conformations.
[0026] In addition, the flexible solvent also needs to possess a first polar group and a second polar group capable of effectively coordinating with lithium ions, thus requiring a certain dipole moment for both. If the dipole moments of the first and second polar groups are too small, their coordination ability is insufficient, making it difficult to form a sufficiently solvated structure with lithium ions, and also difficult to form a sufficiently strong dipole-dipole interaction with the third polar group. Therefore, the first and second polar groups can be selected from conventional strongly polar groups, such as cyano, sulfone, and carbonyl groups. Thus, the flexible solvent in this case is preferably adiponitrile, glutaronitrile, octanoic acid, 1,2-bis(methanesulfonyl)ethane, 1,3-bis(methanesulfonyl)propane, or 1,2-bis(acetyl)ethane.
[0027] Based on the selection of the aforementioned flexible solvent, in order to ensure that, upon addition of the diluent, the flexible solvent remains stably in a low-polarity spatial conformation in a statistically average sense through the dipole-dipole interaction between the third polar group and the first or second polar group, the diluent should contain at least one third polar group, and the dipole moment of the third polar group should be greater than or equal to 3.0D. It is understood that the term "third polar group" is a general term for the strongly polar groups in the diluent, not a specific functional group. That is, when the diluent contains multiple third polar groups, these third polar groups can be the same functional group or different functional groups.
[0028] Furthermore, the diluent should have a weak coordination ability for lithium ions to avoid competing with anions for positions in the first solvation layer of lithium ions. Based on the above considerations, the diluents used in this application are preferably sulfolane, sulfolane, dimethyl sulfone, propylene carbonate, ethylene carbonate, or γ-butyrolactone. Under the action of these diluents, the first and second polar groups of the flexible solvent tend to adopt a low-polarity spatial conformation with antiparallel dipole vectors. At this time, the flexible solvent changes from a coordinating solvent to a nearly inert low-polarity medium, and its donor ability is greatly weakened. It is difficult for the two polar end groups to simultaneously form chelate coordination with the same lithium ion. The diluent itself also has a weak coordination ability for lithium ions. Therefore, the solvation structure of lithium ions in the electrolyte changes from being mainly SSIP to being mainly an anion-participated solvation structure consisting of contact ion pairs (CIP) and aggregates (AGG).
[0029] After determining the specific selection of the flexible solvent and diluent, their ratio also needs to be controlled. An improper ratio may lead to insufficient stability of the low-polarity spatial conformation of the flexible solvent, or excessive dilution of the lithium salt, resulting in a decrease in the ionic conductivity of the electrolyte liquid phase. Based on research and verification, the molar ratio of the flexible solvent to the diluent is preferably controlled at 1:(0.5~8), more preferably 1:(1~8). When the aforementioned molar ratio is lower than 1:0.5, the amount of diluent is insufficient, making it difficult to stabilize the flexible solvent in a statistically average sense through dipole-dipole interactions; when the aforementioned molar ratio is higher than 1:8, the amount of diluent is excessive, which will reduce the effective concentration of the lithium salt and the bulk ionic conductivity, thereby affecting the overall ion transport capacity of the electrolyte and the rate performance of the battery.
[0030] Further research revealed that introducing basic organic solvents into the aforementioned electrolyte system can further improve the dissolution and dissociation behavior of lithium salts. Lithium salts have relatively limited solubility and dissociation in flexible solvents, while basic organic solvents such as 1,2-dimethoxyethane, 1,3-dioxolane, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether have moderate dielectric constants, exhibit good dissolution ability for lithium salts, and possess small molecular size and low viscosity, which is beneficial for lithium ion migration. Therefore, in some preferred embodiments, the electrolyte also contains the aforementioned basic organic solvents to maintain a suitable effective lithium ion concentration and ion mobility, thereby further ensuring good rate performance and low-temperature performance of the battery.
[0031] Research and verification have shown that the concentration of lithium salts in basic organic solvents can be controlled between 0.8 mol / L and 4 mol / L. If the lithium salt concentration is too low, the number of lithium ions in the electrolyte that can participate in the electrochemical reaction is insufficient, making it difficult to support the battery's capacity. If the lithium salt concentration is too high, the electrolyte viscosity increases, ion migration is hindered, and the lithium salt may not completely dissolve and dissociate. Therefore, this concentration range can ensure sufficient lithium ion concentration while also considering the electrolyte's ionic conductivity.
[0032] Furthermore, the volume ratio of the base organic solvent to the total volume of the flexible solvent and diluent can be controlled within 1:(0.4~0.8). If this ratio is too low, the amount of base organic solvent is insufficient, resulting in limited improvement in the dissolution and dissociation of lithium salts; if this ratio is too high, the overall proportion of the flexible solvent and diluent in the electrolyte is low, reducing the number of flexible solvent molecules available to participate in lithium-ion coordination and be regulated by dipole-dipole interactions, thus decreasing the degree to which anions enter the first solvation layer of lithium ions. Therefore, the above volume ratio range is beneficial for maintaining the regulatory effect of dipole-dipole interactions on the solvation structure while improving lithium salt dissolution and dissociation.
[0033] In practice, lithium salts conventionally used in the field can be used, as long as they can be fully dissolved and dissociated in a basic organic solvent. Taking into account the solubility, degree of dissociation, and compatibility with other components of the electrolyte, lithium bis(fluorosulfonyl)imide or lithium bis(trifluoromethanesulfonyl)imide can be selected as lithium salts.
[0034] In addition, interfacial film-forming functional aids can be added to the electrolyte to further improve the film-forming behavior on the negative electrode surface. Interfacial film-forming functional aids can be selected from fluoroethylene carbonate, lithium difluorooxalate borate, or tris(trimethylsilyl)phosphate, and their mass is preferably controlled at 0.5% to 5% of the total electrolyte mass.
[0035] This invention also provides a method for preparing the above-mentioned lithium metal battery electrolyte. The method includes: under an inert atmosphere, first dissolving a lithium salt in a basic organic solvent, stirring until the lithium salt is completely dissolved, allowing it to fully dissociate and form a homogeneous lithium salt solution; then sequentially adding a flexible solvent and a diluent, continuing stirring until all components are uniformly mixed, thus obtaining the lithium metal battery electrolyte. This preparation process is carried out under an inert atmosphere, which avoids interference from moisture and oxygen in the air on the lithium salt and electrolyte components. The sequential addition of the flexible solvent and diluent facilitates the gradual dispersion and mixing of the components, thereby ensuring the uniformity and stability of the electrolyte composition and performance.
[0036] This invention also provides the application of the above-mentioned lithium metal battery electrolyte in lithium metal batteries. This electrolyte can be used in lithium metal batteries, and is particularly suitable for secondary battery systems with lithium metal as the negative electrode, specifically including lithium-lithium symmetrical coin cells, lithium metal secondary soft-pack batteries, etc. During battery charging and discharging, the electrolyte, through the dipole-dipole interaction between the third polar group of the diluent and the first or second polar group of the flexible solvent, allows the flexible solvent to remain in a statistically average low-polarity spatial conformation, promoting the participation of anions in lithium-ion solvation and preferentially decomposing to form a gradient SEI film rich in inorganic components on the negative electrode surface. This improves the interfacial stability of the lithium metal negative electrode, inhibits lithium dendrite growth and dead lithium accumulation, and extends the battery's cycle life.
[0037] The following are specific embodiments and comparative examples of the present invention.
[0038] Example 1
[0039] (1) Preparation of lithium metal battery electrolyte
[0040] In a glove box filled with high-purity argon gas and with water and oxygen content both below 0.5 ppm, lithium difluorosulfonamide was dissolved in 1,2-dimethoxyethane to prepare a lithium salt solution with a concentration of 2 mol / L.
[0041] Adiponitrile and sulfolane were added sequentially to a lithium salt solution at a volume ratio of 5:2:3 for 1,2-dimethoxyethane, adiponitrile, and sulfolane. The mixture was stirred at 500 rpm for 45 minutes on a magnetic stirrer until homogeneous, thus obtaining a lithium metal battery electrolyte.
[0042] (2) Preparation of positive electrode sheet
[0043] High-nickel ternary cathode material NCM811, conductive carbon black, conductive carbon nanotubes, and binder PVDF were taken in a mass ratio of 97:1:0.5:1.5 and uniformly dispersed in NMP, with a PVDF to NMP mass ratio of 5:100, to prepare the cathode slurry. The cathode slurry was uniformly coated onto an aluminum foil current collector, and after drying, rolling, slitting, and die-cutting, the cathode sheet was obtained.
[0044] (3) Assemble a soft-pack battery
[0045] After cutting the 0.04mm thick lithium strip into appropriate sizes, a hydraulic press is used to press the copper tabs onto the lithium sheet at a fixed position to obtain the metallic lithium negative electrode sheet.
[0046] The lithium metal secondary battery electrode assembly is prepared by repeatedly stacking ceramic-coated composite separator, lithium metal negative electrode sheet, ceramic-coated composite separator, and positive electrode sheet in sequence. Then, the lithium metal battery electrolyte is injected, and after packaging, formation, and degassing processes, a lithium metal secondary soft-pack battery is produced.
[0047] Comparative Example 1
[0048] (1) Preparation of electrolyte
[0049] In a glove box filled with high-purity argon gas and with water and oxygen content both below 0.5 ppm, lithium difluorosulfonamide was dissolved in 1,2-dimethoxyethane to prepare an electrolyte with a lithium salt concentration of 2 mol / L.
[0050] (2) Preparation of positive electrode sheet
[0051] High-nickel ternary cathode material NCM811, conductive carbon black, conductive carbon nanotubes, and binder PVDF were taken in a mass ratio of 97:1:0.5:1.5 and uniformly dispersed in NMP, with a PVDF to NMP mass ratio of 5:100, to prepare the cathode slurry. The cathode slurry was uniformly coated onto an aluminum foil current collector, and after drying, rolling, slitting, and die-cutting, the cathode sheet was obtained.
[0052] (3) Assemble a soft-pack battery
[0053] After cutting the 0.04mm thick lithium strip into appropriate sizes, a hydraulic press is used to press the copper tabs onto the lithium sheet at a fixed position to obtain the metallic lithium negative electrode sheet.
[0054] The lithium metal secondary battery electrode assembly is prepared by repeatedly stacking ceramic-coated composite separator, lithium metal negative electrode sheet, ceramic-coated composite separator, and positive electrode sheet in sequence. Then, the electrolyte is injected, and after encapsulation, formation, and degassing processes, a lithium metal secondary soft-pack battery is produced.
[0055] Performance testing:
[0056] The lithium metal secondary pouch cells prepared in Example 1 and Comparative Example 1 were subjected to charge-discharge cycle performance tests. The charge rate was 0.2C, the discharge rate was 0.5C, the charge cut-off voltage was 4.35V, and the discharge cut-off voltage was 3.0V. After 100 charge-discharge cycles of the pouch cells from Example 1 and Comparative Example 1 under the above conditions, electrochemical impedance spectroscopy (EIS) tests were performed on the corresponding cells. The test conditions were: voltage amplitude 5 mV, and test frequency range 0.01 Hz to 10000 Hz. The test results are shown in the appendix. Figure 1 and attached Figure 2 .
[0057] analyze Figure 1 It can be seen that the cycle stability of the pouch cell prepared in Example 1 is significantly better than that of Comparative Example 1. Under the same charge and discharge regime, the former exhibits slower capacity decay. Specifically, the capacity retention rate of the pouch cell prepared in Comparative Example 1 drops to 88% after 100 cycles, and further decreases to 80% by the 113th cycle, reaching the end of its cycle life. In contrast, the capacity retention rate of the pouch cell prepared in Example 1 remains as high as 99% after 100 cycles, and is maintained at 98% after 150 cycles. Even after 240 cycles, the capacity retention rate is still 87%, far exceeding the 80% failure threshold. Using 80% capacity retention rate as the cycle life benchmark, the cycle life of Example 1 is more than 112% higher than that of Comparative Example 1.
[0058] analyze Figure 2 It can be seen that the interfacial impedance of the pouch cell prepared in Example 1 is significantly lower than that of Comparative Example 1, and its increase with cycling is more gradual. Specifically, by the 100th cycle, the total interfacial impedance of Comparative Example 1 had increased sharply to 80.65 mΩ, while that of Example 1 had only increased moderately to 45.52 mΩ. The impedance at the same number of cycles was only 56.44% of that of Comparative Example 1. The interfacial impedance of the pouch cell prepared in Comparative Example 1 underwent irreversible rapid degradation in the later stages of cycling, while the interfacial impedance of the pouch cell prepared in Example 1 remained far lower than that of Comparative Example 1.
[0059] The above results show that the lithium metal battery electrolyte prepared in Example 1 is superior to that in Comparative Example 1 in terms of cycle stability and interfacial impedance, and can effectively suppress capacity decay and interfacial impedance growth. The reason for this is that the dipole moment of the -C≡N groups at both ends of adiponitrile is approximately 3.9D, while the dipole moment of the -S=O group of sulfolane is approximately 4.8D. Under the dipole-dipole interaction of the -S=O group of sulfolane, the -C≡N groups at both ends of adiponitrile are anchored to an antiparallel dipole vector orientation, reducing the net dipole moment of the adiponitrile molecule from approximately 56D in the high-polarity conformation to approximately 0.5~1.5D. As a result, the adiponitrile molecule is statistically stable in a low-polarity spatial conformation, thus weakening its coordination ability for lithium ions. Anions are more likely to participate in solvation and preferentially decompose on the negative electrode surface to form a gradient SEI film with a high proportion of inorganic components near the negative electrode and a high proportion of organic components near the electrolyte.
[0060] It should be understood that the specific embodiments described above are merely illustrative or explanatory of the principles of the invention and do not constitute a limitation thereof. Therefore, any modifications, equivalent substitutions, improvements, etc., made without departing from the spirit and scope of the invention should be included within the protection scope of the invention. Furthermore, the appended claims are intended to cover all variations and modifications falling within the scope and boundaries of the claims, or equivalent forms of such scope and boundaries.
Claims
1. A lithium metal battery electrolyte, characterized in that, The electrolyte contains at least: Lithium salts; A flexible solvent comprising a first polar group, a second polar group, and a flexible segment connecting the two, the flexible solvent having multiple spatial conformations based on the internal rotation of the flexible segment; A diluent containing a third polar group; Furthermore, based on the dipole-dipole interactions between the first polar group, the second polar group, and the third polar group, the flexible solvent is in a spatial conformation in which the dipole vectors of the first polar group and the second polar group are antiparallel.
2. The lithium metal battery electrolyte according to claim 1, characterized in that, The dipole moment of the third polar group is greater than or equal to 3.0D.
3. The lithium metal battery electrolyte according to claim 2, characterized in that, The diluent includes at least one of sulfolane, sulfolane, dimethyl sulfone, propylene carbonate, ethylene carbonate, and γ-butyrolactone.
4. The lithium metal battery electrolyte according to any one of claims 1-3, characterized in that, The flexible segment includes —(CH2) n — where n is an integer greater than or equal to 2.
5. The lithium metal battery electrolyte according to claim 4, characterized in that, The flexible solvent includes at least one selected from adiponitrile, glutaronitrile, octanoic acid, 1,2-bis(methanesulfonyl)ethane, 1,3-bis(methanesulfonyl)propane and 1,2-bis(acetyl)ethane.
6. The lithium metal battery electrolyte according to any one of claims 1-3 and 5, characterized in that, The molar ratio of the flexible solvent to the diluent is 1:(0.5~8).
7. The lithium metal battery electrolyte according to claim 6, characterized in that, The electrolyte contains a basic organic solvent, which includes at least one of 1,2-dimethoxyethane, 1,3-dioxolane, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether. The volume ratio of the basic organic solvent to the total volume of the flexible solvent and the diluent is 1:(0.4~0.8). The lithium salt includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide. The concentration of the lithium salt in the basic organic solvent is 0.8 mol / L to 4 mol / L.
8. The lithium metal battery electrolyte according to any one of claims 1-3, 5, and 7, characterized in that, The electrolyte includes an interfacial film-forming functional aid, which includes at least one of fluoroethylene carbonate, lithium difluorooxalate borate, and tris(trimethylsilyl)phosphate; the mass of the interfacial film-forming functional aid accounts for 0.5% to 5% of the mass of the electrolyte.
9. The method for preparing the lithium metal battery electrolyte according to any one of claims 1-8, characterized in that, The steps include: dissolving lithium salt in a basic organic solvent under an inert atmosphere, then adding a flexible solvent and a diluent in sequence, and mixing thoroughly to obtain a lithium metal battery electrolyte.
10. The application of the lithium metal battery electrolyte according to any one of claims 1-8 in lithium metal batteries.