Battery
By introducing specific additives into the battery to form a cross-linked polymer SEI film and a synergistically regulated CEI film, the membrane aging problem of energy storage batteries under high temperature, high SOC static conditions and intermittent pulse charging conditions is solved, thereby improving the battery's cycle stability and capacity retention.
Patent Information
- Application Number
- CN202611613514.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot effectively solve the problems of SEI film aging and CEI film uneven distribution in energy storage batteries under high temperature, high SOC static conditions and intermittent pulse charging conditions, which leads to battery performance degradation.
By introducing carbonate additives and alkyl fluorosulfonyl compounds into the battery to form a cross-linked polymer SEI film, and by using sulfate additives and the carbon coating layer of the positive electrode active material to synergistically regulate the CEI film, a CEI film with a scattered distribution of single-crystal Li3N and organic sulfate components is generated, thereby improving the flexibility and ion conductivity of the film structure.
It effectively suppresses the growth of DCR in the battery during high-temperature cycling, improves the capacity retention rate in the later stages of battery cycling, and maintains the battery's efficient operation under combined operating conditions.
Smart Images

Figure CN123120890A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of new energy battery technology, specifically involving batteries. Background Technology
[0002] In practical scenarios such as standby independent energy storage on the grid side, standby in thermal power-coordinated frequency regulation energy storage units, and idle new energy distribution and storage awaiting dispatch, LFP batteries used for energy storage are in a high SOC and high-temperature static state for extended periods, relying solely on intermittent pulse charging to compensate for self-discharge. This constitutes a specific operating scenario for energy storage batteries. Carbon-coated lithium iron phosphate, a commonly used positive electrode active material in energy storage batteries, exhibits localized potential spikes on the surface of secondary lithium iron phosphate particles during pulse charging under these conditions. The prolonged high-temperature, high-SOC static state continuously ages the SEI film on the negative electrode side, and repeated pulse perturbations and intermittent pulse charging also pose challenges to the film. The degradation mechanism under this combined operating condition is highly complex and remains unclear. Existing improvement technologies addressing the continuous interfacial film rupture and repair problem under high-temperature cycling conditions cannot solve the specific problems under these conditions.
[0003] Specifically, existing high-temperature improved electrolyte technologies employ a combination of single negative electrode and single positive electrode optimization additives. However, even with this combined approach, issues such as poor SEI thermal stability, swelling and porosity, disordered CEI thickness, and stress unevenness persist, failing to address the specific operating conditions. Crucially, existing technologies lack an analysis of the degradation mechanism for this particular condition and do not offer targeted solutions. They rely solely on the combined use of single functional additives, failing to provide a holistic and synergistic solution for both the battery system and the additives under these conditions. Summary of the Invention
[0004] To address this issue, this invention proposes a battery that, through a combination of battery system and additive design, offers solutions to the degradation mechanisms at the positive and negative electrode interfaces, addressing the problems inherent in energy storage batteries under the conditions of "long-term high SOC open circuit + intermittent pulse potential disturbance." Specifically, to address the issue of continuous aging and dissolution of the SEI film on the negative electrode side under long-term high-temperature, high-SOC static conditions, a cross-linked polymer organic SEI film component with N-centers is formed by introducing carbonate additives and alkyl fluorosulfonyl compounds, which plays a role in resisting thermal chemical aging and guiding the instantaneous lithium flux during pulses. Furthermore, to address the problem of uneven CEI film distribution and structural instability caused by uneven charge distribution in the carbon coating layer of lithium iron phosphate secondary particles under intermittent pulse charging conditions on the positive electrode side, a sulfate additive and alkyl fluorosulfonyl compounds are introduced to synergistically regulate oxygen defects on the carbon coating layer of the positive electrode active material, generating a CEI film characterized by scattered single-crystal Li3N and organic sulfate (ROSO2Li), maintaining the high flexibility of the film structure and mitigating the local lattice strain problem caused by instantaneous potential jumps during pulses.
[0005] In a first aspect, this application provides a battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode comprises a positive electrode active material layer, the positive electrode active material layer comprises a positive electrode active material, the positive electrode active material comprises lithium iron phosphate, the surface of the lithium iron phosphate is coated with a carbon material, and the electrolyte comprises additive I, additive II, and additive III. The specific structure of additive I is shown in Formula I: Formula I, In Formula I, R1 and R2 each independently represent a straight-chain or branched alkyl group having 1 to 3 carbon atoms; Additive II is vinylene carbonate; Additive III is vinyl sulfate; Based on the total mass of the electrolyte, the mass percentage of additive I is a%, 0.5≤a≤5; Based on the total mass of the electrolyte, the mass percentage of additive II is b%, 0.5≤b≤5; Based on the total mass of the electrolyte, the mass percentage of additive III is c%, where 0.1 ≤ c ≤ 5.
[0006] In this battery, additives I, II, and III in the electrolyte work synergistically to effectively improve the long-term cycle stability of the electrolyte under high-temperature conditions. Furthermore, the electrolyte is well-matched with lithium iron phosphate materials, thereby suppressing the DCR growth of the battery during high-temperature cycling and improving the capacity retention rate in the later stages of battery cycling.
[0007] In some implementations, the battery satisfies at least one of the following conditions: 1≤a≤4; 1≤b≤4; 0.5≤c≤3.
[0008] In some embodiments, the additive I comprises at least one of the following compounds: Compound 1 Compound 2 Compound 3 Compound 4 Compound 5.
[0009] In some implementations, based on the mass of the positive electrode active material, the mass percentage of carbon material is m%, 0.1 ≤ m ≤ 5, and the battery satisfies: -15.93 ≤ ≤55.75.
[0010] In some implementations, the mass percentage of carbon material is m%, 0.1 ≤ m ≤ 3, based on the mass of the positive electrode active material.
[0011] In some implementations, the battery satisfies: -8.63 ≤ ≤18.
[0012] In some embodiments, the electrolyte further includes a lithium salt and an organic solvent, and satisfies at least one of the following (I) to (II): (I) The lithium salt includes at least one of LiPF6, LiAsF6, LiBF4, LiB(C2O4)2, LiBF2C2O4, LiN(SO2F)2, LiN(SO2CF3)2, LiPO2F2, LiPF2(C2O4)2, and LiPF4C2O4; (II) The organic solvent includes at least one of carbonate solvents and carboxylic acid ester solvents.
[0013] In some embodiments, the lithium salt is LiPF6 and LiN(SO2F)2, and the molar ratio of LiPF6 to LiN(SO2F)2 is 1-2:1.
[0014] In some embodiments, the electrolyte further includes an organic solvent that satisfies at least one of the following conditions (III) to (IV): (III) The carbonate solvent includes at least one of ethylene carbonate, propylene carbonate, butene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, or methyl propyl carbonate.
[0015] (IV) The carboxylic acid ester solvent includes at least one of methyl formate, methyl acetate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate or ethyl butyrate.
[0016] This application constructs a multi-component synergistic battery formulation system consisting of "carbon-coated LFP + additive I (formula I compound) + additive II (VC) + additive III (DTD)". On the negative electrode side, it constructs an organic SEI containing an N-center crosslinked polymer with controllable crosslinking density at a controlled rate. On the positive electrode side, it synergistically induces the generation of a highly flexible CEI containing anisotropic Li3N ion channels and organic sulfate (ROSO2Li) components, achieving homogeneous and efficient ion conduction and good anti-erosion-potential perturbation characteristics, and specifically solves the interface problem under this composite working condition. Detailed Implementation
[0017] The embodiments of the present invention are described in detail below. These embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0018] This application is based on the inventor's discoveries and understanding of the following facts and problems: The inventors discovered that in practical applications, LFP batteries used for energy storage operate under conditions of long-term high SOC and high temperature static storage, relying solely on intermittent pulse charging to compensate for self-discharge. Under this combined condition, the interfacial film undergoes only unidirectional chemical aging during the static storage period, resulting in continuous deterioration of its mechanical properties. The instantaneous potential jump and lithium flux impact of pulse charging directly affect this aged film layer, easily leading to cracking, requiring timely repair with additives. To address the problem of continuous thermochemical aging and accelerated dissolution of the SEI film on the negative electrode side under this condition, they proposed using compounds of formula I (alkyl fluorosulfonyl compounds), vinylene carbonate (VC), and vinyl sulfate (DTD) as additives. The synergistic effect of these additives aims to specifically solve the aforementioned problems under this condition. The specific mechanism is as follows: On the negative electrode side, the alkyl fluorosulfonyl compound is preferentially and slowly reduced over VC. The alkyl-N• radicals generated by the breaking of its N-S bond catalyze the ring-opening polymerization of VC, while simultaneously limiting the polymerization rhythm with its own reduction rate, forming a flexible organic SEI with controllable crosslinking density, making the film "tough but not cracked" under pulse impact; at the same time, the short-chain symmetrical alkyl side chains in the alkyl fluorosulfonyl compound strengthen the N center to Li through hyperconjugation. +The coordination guidance ensures ion conduction under instantaneous lithium flux, playing a role in resisting thermal chemical aging and guiding pulsed instantaneous lithium flux. On the positive electrode side, under intermittent pulsed charging conditions, the aging film layer suffers from uneven CEI film distribution and structural instability caused by the uneven charge distribution of the carbon coating layer of lithium iron phosphate secondary particles. Research has found that DTD can induce decomposition at oxygen defects in the carbon coating layer of the positive electrode active material under the electronegative attraction of nitrogen-containing free radicals generated by the decomposition of alkyl fluorosulfonyl compounds, forming an inorganic-organic composite CEI film with scattered distribution of single-crystal Li3N and organic sulfate (ROSO2Li). This specific interface can maintain the high flexibility of the film structure and solve the local lattice strain caused by the instantaneous potential jump brought about by the pulse.
[0019] Furthermore, during the design and verification of a specific cross-linked organic polymer interface film on the negative electrode side, the inventors unexpectedly discovered that only through the synergistic reaction of alkyl fluorosulfonyl compounds and halogen-free carbonate additives can an SEI with cross-linked organic polymers as the main component be formed. This has an important impact on the stability of the cross-linked polymer backbone and can withstand the continuous test of thermochemical aging under this operating condition.
[0020] Therefore, based on the research into the degradation mechanism under the above-mentioned combined operating conditions and the design of solutions, the inventors determined a targeted battery formulation that combines the above-mentioned additive combination with the carbon coating structure of the positive electrode of lithium iron phosphate battery cell to synergistically solve the problem of this combined operating condition.
[0021] In view of the above, in a first aspect, this application provides a battery. In some embodiments, the battery includes a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode includes a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material, the positive electrode active material includes lithium iron phosphate material, the surface of the lithium iron phosphate is coated with a carbon material, and the electrolyte includes additive I, additive II, and additive III; The specific structure of additive I is shown in Formula I: Formula I, In Formula I, R1 and R2 each independently represent a straight-chain or branched alkyl group having 1 to 3 carbon atoms; Additive II is vinylene carbonate; Additive III is vinyl sulfate; Based on the total mass of the electrolyte, the mass percentage of additive I is a%, 0.5≤a≤5; Based on the total mass of the electrolyte, the mass percentage of additive II is b%, 0.5≤b≤5; Based on the total mass of the electrolyte, the mass percentage of additive III is c%, where 0.1 ≤ c ≤ 5.
[0022] In batteries using lithium iron phosphate (LFP) materials with carbon coating structures as the positive electrode active material, the carbon coating layer can buffer the impact of instantaneous potential disturbances during pulse charging on the lattice / interface of LFP secondary particles. During each pulse charging, local potential spikes appear on the surface of the LFP secondary particles. Under repeated pulse disturbances, unstable interfacial byproducts are easily generated on the surface of bare LFP secondary particles. A continuous and dense carbon coating layer can homogenize the local potential distribution on the particle surface, suppress the continuous accumulation of non-selective interfacial side reactions on the positive electrode particle surface under pulse potential disturbances, and reduce electrolyte decomposition on the positive electrode particle surface. However, simple carbon coating cannot improve the two-phase static lithium distribution relaxation of LFP to cope with the instantaneous potential jumps and local lattice strain problems caused by the instantaneous lithium ion extraction induced by pulse charging.
[0023] Additive I possesses a higher HUMO energy level, allowing it to preferentially undergo slow reduction decomposition at the negative electrode compared to Additive II. Because the N-center of Additive I is connected to an alkyl side chain, the electron cloud density at the N-center varies with the length and spatial torsion characteristics of the alkyl side chain. Under high temperature and high SOC conditions, at the negative electrode interface, Additive I and Additive II undergo reduction decomposition sequentially. Due to the influence of the alkyl side chain, the N / S bond of Additive I breaks, generating an alkyl-N• radical, while Additive II gains electrons to generate a highly reactive radical anion, VC•. - Under the catalysis of alkyl-N• radicals, further ring-opening polymerization was carried out to generate an organic SEI film component with a polymer backbone having N atoms as crosslinking centers. This crosslinking polymerization process was limited by the reductive decomposition of additive I, thus further inhibiting the ring-opening polymerization rate of additive II and effectively suppressing the growth of high interfacial impedance under high temperature and high SOC. In addition, the inventors found that alkyl groups were used in the compound shown in additive I, instead of alkenyl, alkynyl, or benzene ring non-alkyl groups. This was mainly because the above non-alkyl groups would lead to enhanced overall molecular activity, resulting in their rapid consumption during battery charging and discharging. Furthermore, the symmetry and carbon chain length of the alkyl side chain of additive I also have a significant impact on the crosslinking density of the polymer backbone. Short and symmetrical alkyl side chains have a hyperconjugation effect on the nitrogen lone pair electrons on the N atom, which can effectively enhance the crosslinking density between the N center and Li. + Its coordination ability allows it to more effectively guide Li through electron cloud polarization. + Jump. This characteristic significantly improves the transport efficiency of the SEI film at the negative electrode interface under high temperature and high SOC conditions in response to the instantaneous lithium flux brought about by pulse charging.
[0024] On the positive electrode side, because the N center on additive I contains lone pairs of electrons and has a certain electronegativity, it is easy to be directionally adsorbed to the positive electrode side. After losing electrons and undergoing oxidative decomposition, it preferentially forms nitrogen-containing free radicals. At the same time, it can bind to the sulfate groups in additive III through electronegativity attraction. It can be directionally adsorbed and decomposed with the oxygen defect sites on the carbon layer of lithium iron phosphate secondary particles with a continuous and dense carbon coating and a homogeneous potential distribution. At the oxygen defect sites, the nitrogen-containing free radicals and sulfate groups undergo oxidative decomposition, further generating single-crystal Li3N composed of alternating stacks of Li2N layers and pure Li layers along the c-axis. This layered structure leads to strong anisotropy in lithium ion transport, and lithium ions can pass through the interface film with low potential barrier. This type of CEI film, composed mainly of inorganic compounds such as Li3N and organic compounds such as organic sulfates (ROSO2Li), exhibits high ion conduction efficiency and chemical stability. Most importantly, these scattered Li3N inorganic components and organic sulfates (ROSO2Li) can help lithium ions to rapidly desorb and maintain high flexibility, improving the two-phase static lithium distribution relaxation of lithium iron phosphate to cope with the instantaneous potential jump caused by pulse charging and the local lattice strain problem caused by the instantaneous desorption of lithium ions.
[0025] In summary, by combining additives I, II, and III in this battery system, the challenges faced by operating under a combined usage mode characterized by long-term resting phase-calendar aging as the main process and pulse charging as the auxiliary process can be effectively addressed. This process suppresses capacity loss of the battery under "long-term high SOC open circuit + intermittent pulse potential disturbance". In addition, it can effectively improve DCR growth during the cycle aging process under high temperature conditions and maintain efficient reversible lithium capacity.
[0026] It is understandable that the content of additives I, II and III in the electrolyte also affects their synergistic effect. The amount of additives I, II and III added in a matching manner has a significant regular effect on the capacity maintenance, self-discharge and even high-temperature cycle aging performance of the battery system under the combined use mode of long-term static stage-calendar aging as the main mode and pulse charging as the auxiliary mode.
[0027] In some implementations, 0.5 ≤ a ≤ 5, preferably 1 ≤ a ≤ 4. As a specific example, a can be 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, or any two of them.
[0028] In some implementations, 0.5 ≤ b ≤ 5, and preferably, 1 ≤ b ≤ 4. As a specific example, b can be 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, or any two of them.
[0029] In some implementations, 0.1 ≤ c ≤ 5, preferably 0.5 ≤ c ≤ 3. As a specific example, c can be 0.1, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, or any two of them.
[0030] When the mass percentage (a%) of additive I is less than 0.5%, the amount of additive I added is too small, and it is impossible to form an organic SEI film component with N atoms as the crosslinking center, thus failing to enhance the interaction between the N centers and Li. + Coordination ability, guiding Li + The effect of skipping and slowing down the consumption rate of additive II is not obvious. The interfacial film dominated by the decomposition of additive II will still decompose into a thin and porous deteriorated form under high temperature and high SOC conditions, making it difficult to maintain a high reversible capacity. When the mass percentage (a%) of additive I is greater than 5%, the excessive addition of additive I may cause a significant increase in the viscosity of the electrolyte phase, reduce the ion transport rate at the electrode interface, and make it difficult to synergistically generate organic SEI film components with the target crosslinking density and N-atom-centered polymer backbone with additive II. The interfacial impedance surges, deteriorating ion transport and interfacial film stability.
[0031] When the mass percentage b% of additive II is less than 0.5%, the amount of additive II added is too small, and its effect on alleviating the changes in mechanical stress on the electrode surface caused by the self-discharge behavior due to electron tunneling and protecting the integrity of the electrode active material is limited. When the mass percentage b% of additive II is greater than 5%, the amount of additive II added is too large, the impedance increases significantly, and the consumption of additive II will be accelerated under high temperature and long-term aging conditions.
[0032] When the mass percentage (c%) of additive III is less than 0.1%, the amount of additive III added is too small, and the effect of forming a highly thermochemically stable and dense interface film containing beneficial components such as LiSO3, LiSO4 and organic sulfates (ROSO2Li) is limited. This directly results in limited improvement in ion transport efficiency and limited effect in suppressing damage from high-temperature static aging and the instantaneous potential jump impact caused by pulse charging. When the mass percentage (c%) of additive III is greater than 5%, the amount of additive III added is too large, and it is difficult to control the thickness growth of the interface film, which leads to an increase in the ion transport path. Lithium ions cannot be rapidly extracted and maintain high flexibility, causing local lattice strain problems. It is difficult to maintain the reversible capacity of the battery under the combined use mode of long-term static stage-calendar aging as the main mode and pulse charging as the auxiliary mode.
[0033] In some embodiments, the additive I comprises at least one of the following compounds: Compound 1 (CAS: 354-44-9) Compound 2 (CAS: 1458771-72-6), Compound 3 (CAS: 2826747-29-7), Compound 4 (CAS: 382-97-8) Compound 5 (CAS: 3136357-24-6).
[0034] In some embodiments, the electrolyte further includes a lithium salt and an organic solvent, and satisfies at least one of the following (I) to (II): (I) The lithium salt includes at least one of LiPF6, LiAsF6, LiBF4, LiB(C2O4)2, LiBF2C2O4, LiN(SO2F)2, LiN(SO2CF3)2, LiPO2F2, LiPF2(C2O4)2, and LiPF4C2O4; (II) The organic solvent includes at least one of carbonate solvents and carboxylic acid ester solvents.
[0035] Specifically, the defined lithium salt has high ionic conductivity, ensuring rapid migration of lithium ions in the electrolyte, which helps to form a good SEI film and can also effectively passivate the positive electrode current collector. At the same time, the lithium salt has high oxidation stability, which can induce the formation of a stable CEI film on the positive electrode surface. This film has excellent oxidation stability and can effectively inhibit the oxidative decomposition of the electrolyte on the surface of the positive electrode active material.
[0036] In some embodiments, the lithium salt is LiPF6 and LiN(SO2F)2 (LIFSI). Preferably, the molar amounts of LiPF6 and LiN(SO2F)2 are n(LiPF6) and n(LiFSI), respectively, where the ratio of n(LiPF6):n(LiFSI) is 1-2:1. Within this ratio range, LiFSI can improve the ionic conductivity and high-temperature stability of the electrolyte, participate in the construction of the electrode interface film, and increase the Young's modulus of the interface film. The decomposition of lithium salt produces an interface film containing S and F components, which improves the interface ion transport efficiency and the cycle stability of the battery. When n(LiPF6):n(LiFSI) < 1, the proportion of LiFSI is too high, which will reduce the oxidation resistance of the electrolyte; excessive lithium salt decomposes, continuously consumes the electrolyte and triggers a large number of side reactions, depletes active lithium, is not conducive to the reversible insertion and extraction of lithium, and causes the battery capacity to continuously decay.
[0037] When n(LiPF6):n(LiFSI) > 2, the amount of LiFSI added is insufficient, and the improvement effect on the system is limited; the thermochemical stability of the interface film deteriorates, continuously inducing side reactions and causing battery performance degradation.
[0038] In some embodiments, the electrolyte further includes an organic solvent that satisfies at least one of the following conditions (III) to (IV): (III) The carbonate solvent includes at least one of ethylene carbonate, propylene carbonate, butene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, or methyl propyl carbonate.
[0039] (IV) The carboxylic acid ester solvent includes at least one of methyl formate, methyl acetate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate or ethyl butyrate.
[0040] In some embodiments, the positive electrode may include a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector. The positive electrode active material layer may include a positive electrode active material, a positive electrode binder, and a positive electrode conductive agent, wherein the positive electrode active material includes lithium iron phosphate material. It is understood that lithium iron phosphate material should be interpreted broadly, including both unmodified intrinsic lithium iron phosphate and doped and / or coated modified lithium iron phosphate. In some embodiments, the positive electrode active material includes carbon-coated lithium iron phosphate, or lithium iron phosphate with a carbon coating layer on its surface. As an example, the lithium iron phosphate material is carbon-coated secondary lithium iron phosphate particles, including secondary lithium iron phosphate particles and a carbon coating layer covering the surface of the secondary lithium iron phosphate particles.
[0041] In some embodiments, we further introduce the mass percentage of carbon coating as an important factor affecting the stability of the interfacial film under specific operating conditions. Specifically, the mass percentage m% of carbon material in the positive electrode active material can affect the number of oxygen defect sites on the positive electrode surface and the efficiency of ion transport, with a more pronounced effect at high temperatures. The number of oxygen defect sites directly affects the film quality of the interfacial film, while the ion transport efficiency of the interfacial film is also affected by the thickness of the carbon coating. Under high-temperature static and pulse charging conditions, the thermochemical stability of the interfacial film and its ion transport efficiency are key factors in whether the battery can maintain high reversible capacity.
[0042] Controlling the value of 0.1≤m≤5 is beneficial for forming a uniform carbon coating layer with appropriate thickness. This ensures a homogeneous potential distribution on the particle surface, suppresses the continuous accumulation of non-selective interfacial side reactions on the cathode particle surface under pulsed potential disturbance, and reduces the decomposition of electrolyte on the cathode particle surface. At the same time, due to the homogeneous production of the interfacial film, the cathode material particles are less prone to microcrack propagation and structural collapse, resulting in lower internal resistance and helping to maintain the macroscopic structural integrity of the cathode material particles under pulsed charging.
[0043] Based on the mass of the positive electrode active material, the mass percentage of the carbon material is m%, 0.1≤m≤5, preferably 0.1≤m≤3. As a specific example, m can be 0.1, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, or any two of them.
[0044] We found that the amounts of Formula I compound, VC, and DTD, and the mass percentage of carbon material, do not act independently, but rather have a mutually restrictive matching relationship.
[0045] Based on the above reasons, the relationship between the four factors mentioned above is introduced, and the battery satisfies: -15.93≤ ≤55.75, preferred -8.63≤ ≤18. It can organically combine the amount of electrolyte additives and the content of carbon coating, which is more conducive to solving this working condition.
[0046] As a specific example Specifically, it can be -15.93, -15, -10, -8.63, -5, 0, 5, 10, 15, 18, 20, 25, 30, 35, 40, 45, 50, 55, 55.75, or any two of them.
[0047] When the carbon coating percentage (m) is less than 0.1, it is difficult to form a sufficient number of suitable oxygen defect sites, making it impossible to effectively control the construction of the interface film and form a scattered distributed CEI film with compounds such as Li3N, LiSO3, LiSO4, and organic sulfates (ROSO2Li) as the main components. If the carbon coating layer is too thin, the electronic conductivity is insufficient, resulting in uneven charging within the electrode and increased polarization at the positive electrode interface. This makes it difficult to buffer the volumetric strain caused by the instantaneous extraction of lithium ions under pulse charging conditions and to suppress further oxidation and decomposition of the electrolyte. When the m value is greater than 5, the carbon coating layer is too thick, significantly lengthening the lithium ion transport path and reducing the ion transport efficiency at the positive electrode interface. Lithium ions cannot rapidly extract and maintain high flexibility, leading to local lattice strain problems. This makes it difficult to maintain the reversible capacity of the battery under a combined operating mode characterized by long-term static storage-calendar aging and supplemented by pulse charging.
[0048] The above formula In this context, the relation can be broken down into: and -m 2 The superposition of two composite terms, the physical meaning of each composite term and their coupling relationship are as follows: in The term represents the synergistic effect of additives I, II, and III: Under long-term high-temperature static conditions, the content of additive I directly affects the stability of the film formed at the negative electrode interface of additive II. By controlling the content of additives I and II, an organic SEI film component with a polymer skeleton centered on N atoms and a target crosslinking density can be generated. Furthermore, the effect of additive I content on the formation of the target crosslinking density film component exhibits a non-linear (exponential growth) characteristic. On the positive electrode side, the content of additives I and III jointly influences the crystal orientation and content of Li3N and organic sulfates (ROSO2Li) generated by the oxidative decomposition of nitrogen-containing free radicals and sulfate groups at the oxygen defect sites of the carbon layer on lithium iron phosphate secondary particles, thus jointly determining the ion conductivity, Young's modulus, and chemical stability of the CEI film. Therefore, a... 2 +c represents the nonlinear regulatory effect of additive I on the consumption rate of additive II, and the key effects of additive I and additive III on the construction of the positive electrode interface film. b represents the necessity of the content of additive II in this system and its influence on the quality of the interface film under high temperature and high SOC. It needs to be clarified that the construction of the electrode interface film uses the content of additive II as the matrix part. The denominator b corresponds to the effective content of additive II necessary for constructing an organic SEI film with a polymer backbone containing N crosslinking centers. As a base parameter of the whole synergistic effect, it measures how much positive and negative electrode synergistic modification benefit can be leveraged with the same SEI film-forming substrate, or in other words, the synergistic modification effect that each unit of effective film-forming substrate (effective content of additive II) can bear / achieve. Additive II is a necessary matrix component for forming the target organic SEI backbone. Only when additive II provides an effective film-forming matrix can the content of additive II be increased. 2 +c characterizes two types of modification contributions: a 2 c reflects the nonlinear regulatory effect of additive I on the film formation process of additive II matrix, and c reflects the synergistic effect of additive I and additive III on the CEI construction on the positive electrode side. When the effective content b of additive II is higher than the minimum film formation threshold, b determines the basic volume of the SEI polymer matrix and its intrinsic properties against high temperature and high SOC conditions. The essence of this study is to normalize the comprehensive synergistic modification intensity of additives I and III in the regulation of crosslinking in the negative electrode and the construction of CEI in the positive electrode, using the intrinsic interfacial quality of additive II as a benchmark.
[0049] when When the concentration of additive III is too low, additive I is insufficient to delay the consumption of additive II. Additive II continues to decompose under long-term high-temperature static conditions and repeated pulsed current conditions. The resulting interfacial film will still decompose into a thin and porous deteriorated form under high temperature and high SOC conditions, making it difficult to maintain a high reversible capacity. In addition, if the amount of additive III is too low, the effect of forming a highly thermochemically stable and dense interfacial film containing beneficial components such as LiSO3, LiSO4, and organic sulfates (ROSO2Li) is limited. This is directly reflected in the limited improvement of ion transport efficiency and the limited effect of suppressing high-temperature static aging damage and the instantaneous potential jump impact caused by pulsed current.
[0050] when When the concentration of additives is too high, it means that the content of additives I and III is too high relative to additive II. This results in an excess of functional regulating components and an insufficient amount of film substrate components. Excessive additive I increases the viscosity of the electrolyte phase, reduces the interfacial ion transport rate, and impairs its ability to synergistically construct the target N crosslinked polymer SEI framework with a small amount of additive II. This makes it difficult for the SEI to buffer the uneven mechanical stress under high-temperature static storage and repeated pulse charging. Excessive additive III causes uncontrolled growth of the cathode CEI thickness, increases the ion transport path, reduces interfacial flexibility, and induces local lattice strain, making it difficult to maintain the reversible capacity under the combined operating conditions of calendar aging as the main factor and pulse charging as the auxiliary factor. The coupling of these two factors will further increase the polarization of the full cell, causing the SEI / CEI, which lacks a sufficient amount of additive II substrate, to bear greater stress.
[0051] m 2 The term represents the nonlinear trade-off between electron conduction and ion transport in the carbon coating layer: the square of the term is used as the minuend to characterize the nonlinear impact of the carbon coating layer on battery performance. The carbon coating layer directly affects the number of oxygen defect sites and the efficiency of ion transport on the surface of the positive electrode, with the impact being more pronounced at high temperatures. The number of oxygen defect sites directly affects the film quality of the interfacial film, while the ion transport efficiency of the interfacial film is also affected by the thickness of the carbon coating layer. The carbon coating layer can provide efficient electron conduction, construct oxygen defect sites, and assist in the regulation of the interfacial film; however, an excessively thick carbon coating layer will significantly lengthen the lithium-ion transport path and reduce the interfacial ion transport efficiency, and this trade-off increases nonlinearly with thickness. 2 The term is incorporated into the formula as a negative contribution to quantify the balance between the electronic conduction gain and ion transport loss of the carbon coating layer.
[0052] This study quantifies and matches the synergistic relationship between the amounts of additives I, II, and III and their respective quantities in relation to the overall quantity of the additives and the quality of the electrode interface film. This ensures that additives I, II, and III work synergistically to protect the electrode while clarifying the relationship between the quantities of each component and their impact on the quality of the electrode interface film; then, subtracting m... 2This paper incorporates the nonlinear effects of carbon coating modification on the positive electrode side into the same evaluation system, ultimately forming a composite formula for electrolyte-positive electrode. By limiting the composite characteristic value within the range defined in this application, a globally optimal balance of four parameters can be achieved: Additive I effectively delays the consumption of Additive II, participates in the construction of organic SEI film components with N-atom crosslinking centers in the polymer skeleton, reduces the growth of interfacial impedance while improving the transmission efficiency of instantaneous lithium flux brought by pulse charging, and achieves excellent resistance of the interfacial film under high temperature and high SOC; Additive III, under the electronegative attraction of Additive I, acts directionally on the carbon layer oxygen defect sites on the lithium iron phosphate secondary particles with homogeneous potential distribution for directional adsorption and decomposition. At the oxygen defect sites, oxidation decomposition generates single-crystal Li3N with strong anisotropy for lithium ion transport, reducing the barrier for lithium ions to pass through the interfacial film. The CEI film, composed mainly of inorganic compounds such as Li3N and organic compounds such as organic sulfates (ROSO2Li), forms a scattered distribution. This facilitates rapid lithium ion extraction and maintains high flexibility, improving the two-phase static lithium distribution relaxation of lithium iron phosphate to cope with the instantaneous potential jump caused by pulse charging and the local lattice strain caused by the instantaneous extraction of lithium ions. The carbon coating layer provides a large number of oxygen defect sites, ensuring the scattered distribution of Li3N and organic sulfates (ROSO2Li), guaranteeing electron conduction without excessively hindering ion transport, improving the charge-mass binding ratio at the electrode interface, and mitigating the side reactions and self-discharge phenomena caused by the high charge state at the interface. At the same time, it helps lithium ions to extract rapidly and maintain high flexibility, improving the two-phase static lithium distribution relaxation of lithium iron phosphate to cope with the instantaneous potential jump caused by pulse charging and the local lattice strain caused by the instantaneous extraction of lithium ions.
[0053] This application does not impose any particular restrictions on the preparation method of the positive electrode active material, as long as it can achieve the purpose of this invention. It can be commercially available or prepared using conventional methods. For example, the positive electrode active material in this application can be prepared by the following method: Lithium hydroxide (LiOH·H2O), ammonium dihydrogen phosphate (NH4H2PO4), and ferrous acetate (Fe(CH3COO)2) are accurately weighed in a molar ratio of 1:1:1 according to the stoichiometric ratio of the target product LiFePO4 as the main raw materials for the lithium iron phosphate precursor. This application does not impose any particular restrictions on the types of lithium, phosphorus, and iron sources. Considering the volatilization loss during high-temperature calcination, the lithium source can be in excess by 3-5%; glucose (C6H2PO4) is selected. 12O6) is used as the carbon source. The carbon content and target carbon coating amount of glucose can be controlled by accurately calculating and weighing the required mass of glucose according to the mass ratio of lithium iron phosphate precursor and glucose of 1:(0.05~0.5), dissolving it in deionized water to prepare a clear solution. The weighed main raw materials (lithium source, phosphorus source, iron source) are placed in a high-speed shear dispersion reactor. An appropriate amount of deionized water is added, and under the protection of an inert atmosphere (such as nitrogen or argon), high-speed shear stirring is carried out in the range of room temperature to 60°C to form a uniform suspension / solution mixture system. Subsequently, under continuous stirring, the above carbon source solution is slowly added dropwise to the above mixture system to ensure uniform dispersion of the carbon source. The above uniformly mixed slurry is immediately spray-dried. During spray drying, the inlet temperature is controlled at 200-250°C and the outlet temperature is controlled at 100-120°C to obtain microspherical dried precursor powder. This process rapidly transforms the liquid mixture into a uniform solid mixture and initially forms an amorphous carbon network framework. The precursor powder obtained from spray drying is placed in a tube furnace and pre-sintered at 350-450°C at a heating rate of 2-5°C / min under an inert atmosphere (such as high-purity argon) for 3-6 hours. After natural cooling, the pre-sintered intermediate product is ground to break up any possible soft agglomerates. The ground powder is then placed back in the tube furnace and subjected to high-temperature crystallization calcination under a flowing inert atmosphere (argon or a nitrogen-argon mixture). The calcination procedure is as follows: heating to 650-750°C at 3-5°C / min and holding at this temperature for 8-15 hours. During this high-temperature stage, the lithium iron phosphate (LFP) crystal structure is fully formed and grown, while the residual glucose carbon source is pyrolyzed in the inert atmosphere, forming a uniform, continuous, and highly conductive amorphous carbon layer that coats the surface of the secondary lithium iron phosphate particles. After high-temperature calcination, the furnace is cooled to room temperature in an inert atmosphere. The cooled sintered block is taken out and mechanically ground and sieved (e.g., through a 400-mesh sieve) to obtain lithium iron phosphate cathode active material powders with different carbon coating contents.
[0054] According to embodiments of this application, the positive electrode conductive agent may include one or more of conductive carbon black (SP), carbon nanotubes (CNT), graphene, and conductive graphite; the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and cellulose-based polymers.
[0055] According to embodiments of this application, the positive current collector can be a metal current collector or a composite current collector. Metal current collectors include at least one of aluminum foil current collectors and carbon-coated aluminum foil current collectors; composite current collectors may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. Composite current collectors can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0056] According to embodiments of this application, the negative electrode sheet may include a negative electrode current collector and a negative electrode material layer disposed on at least one side of the negative electrode current collector. The negative electrode material layer may include a negative electrode active material, a negative electrode binder, and a negative electrode conductive agent.
[0057] According to embodiments of this application, the negative electrode active material includes at least one of graphite, hard carbon, soft carbon, carbon fiber, mesophase carbon microspheres, silicon-based materials, tin-based materials, and lithium titanate. Specifically, the negative electrode active material includes graphite. Therefore, it exhibits high capacity and good stability.
[0058] According to embodiments of this application, the negative electrode binder includes at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), cellulose-based polymers, styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, and carboxymethyl chitosan. The above-mentioned binders exhibit good adhesion, ensuring strong bonding of materials within the negative electrode material layer while also providing strong adhesion between the negative electrode material layer and the negative electrode current collector, thus improving the structural stability of the negative electrode sheet.
[0059] According to embodiments of this application, the negative electrode conductive agent includes at least one selected from superconducting carbon, conductive carbon black (SP), conductive graphite, acetylene black, carbon black, Ketjen black, carbon nanotubes (CNTs), graphene, and carbon nanofibers. The aforementioned conductive agents exhibit superior conductivity, which is beneficial for improving the conductivity of the negative electrode sheet, thereby enhancing the overall electrochemical performance of the battery.
[0060] According to embodiments of this application, the negative electrode current collector can be a metal current collector or a composite current collector. Metal current collectors include at least one of copper foil current collectors and carbon-coated copper foil current collectors; composite current collectors may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. Composite current collectors can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0061] According to embodiments of this application, the diaphragm includes polyethylene diaphragm, polypropylene diaphragm, polyethylene / polypropylene composite diaphragm, etc.
[0062] The embodiments of this application are described in detail below.
[0063] Example: The embodiments and comparative examples provided below illustrate the implementation of this application in more detail. Various tests and evaluations were conducted according to the methods described below. Furthermore, unless otherwise specified, "parts" and "%" are quality standards.
[0064] Test methods and equipment: 1. 55℃ pulse power compensation test: At 25℃, the battery was charged at a constant current of 0.2C for 285 minutes, with a charging cutoff voltage of 3.45V, to 95% SOC. It was then discharged at a constant current of 0.2C to 2.0V, and the discharge capacity was recorded as C1. After resting for 3 hours, it was charged again at a constant current of 0.2C for 285 minutes, with a charging cutoff voltage of 3.45V, to 95% SOC. It was then placed in a 55℃ constant temperature chamber and left to rest in an open circuit for 15 days. After resting, it was charged at 0.04C and 3.65V at 55℃ for 2 hours, stopping charging once the voltage was reached. The cutoff current was ≤0.005C, and the battery was placed back into a 55℃ resting chamber. This 15-day resting + pulse charging cycle was repeated four times. The battery was then removed and discharged at a constant current of 0.2C to 2.0V at 25℃, and the discharge capacity was recorded as C2. The capacity retention rate was calculated. The comparative battery was tested under the same conditions.
[0065] 55℃-95% SOC battery pulse charging test capacity retention rate (%) = C2 / C1×100%; The capacity retention rate at 0.2C constant current discharge at 25 ℃ was used to evaluate the damage resistance and interface stability of 95% SOC lithium-ion batteries at 55 ℃. The higher the capacity retention rate, the better the performance of the lithium-ion battery under long-term high SOC open circuit and intermittent pulse potential disturbance conditions.
[0066] 2. Cyclic performance test at 45℃: The lithium-ion battery was placed in a 45 ℃ constant temperature chamber and left to stand for 2 hours to allow it to reach a constant temperature. It was then charged at a constant current of 1.0C until the voltage reached 3.8V, followed by constant voltage charging at 3.8V until the cutoff current reached 0.05C. Finally, it was discharged at a constant current of 1.0C until the voltage reached 2.0V. The initial discharge capacity was recorded as C3. This constituted one charge-discharge cycle. This process was repeated 500 times, and the discharge capacity after the 500th cycle was recorded as C4.
[0067] 45℃ capacity retention rate (%) = C4 / C3 × 100%; The capacity retention rate at 45 °C is used to evaluate the cycle performance of lithium-ion batteries at 45 °C. A higher capacity retention rate indicates better cycle performance of the lithium-ion battery at 45 °C.
[0068] 3. 45℃ Cyclic DCR Change Rate Test: Before cycling at 45°C, the battery was subjected to a complete 0.5C charge-discharge cycle to obtain the reference capacity C01. After 1000 cycles at 45°C, the battery was subjected to a complete 0.5C charge-discharge cycle to obtain the reference capacity C02. The battery was then charged at a constant current of 0.5C to 50% SOC and allowed to rest for 2 hours to allow the voltage to stabilize. Internal resistance testing was performed using the pulse method: Before cycling at 45°C, the battery was discharged at a constant current of 1C (the specific current value was determined based on C01) for 10 seconds, and the load voltage V1 and current I1 were recorded before the discharge ended; then it was allowed to rest for 10 seconds, and the open-circuit voltage V01 was recorded at the end of the rest period. After 1000 cycles at 45°C, the battery was discharged at a constant current of 1C (the specific current value was determined based on C02) for 10 seconds, and the load voltage V2 and current I2 were recorded before the discharge ended; then it was allowed to rest for 10 seconds, and the open-circuit voltage V02 was recorded at the end of the rest period.
[0069] The DC internal resistance (DCR) is calculated using the following formula, in milliohms.
[0070] DCR1=(V01-V1) / I1×1000, DCR2=(V02-V2) / I2×1000; DCR change rate (%) = DCR2 / DCR1 × 100%; The DCR growth of lithium-ion batteries during 45℃ cycling is evaluated by the DCR change rate. The smaller the DCR change rate, the fewer the interfacial side reactions of the lithium-ion battery and the higher the cycle stability.
[0071] 4. High-temperature storage performance test at 60℃ The lithium-ion battery was placed in a 25°C constant temperature chamber and left to stand for 2 hours to allow it to reach a constant temperature. It was then charged at a constant current and constant voltage of 1.0C to 3.8V, with a cutoff current of 0.05C. It was then discharged at a constant current of 1.0C to 2.0V, and this cycle was repeated 5 times. Afterward, it was charged again at a constant current and constant voltage of 1.0C to 3.8V, with a cutoff current of 0.05C. The thickness d1 of the lithium-ion battery was measured at this point. The battery was then placed in a 60°C constant temperature chamber for 30 days. After storage, the lithium-ion battery was left to stand in a 25°C constant temperature chamber for 2 hours. After this period, the thickness d2 of the lithium-ion battery was measured.
[0072] Thickness expansion rate (%) after 30 days of storage at 60℃ = (d2-d1) / d1×100%. The lower the thickness expansion rate, the fewer side reactions the lithium-ion battery has during high-temperature storage, the better the high-temperature storage performance of the lithium-ion battery, and the better the chemical and thermal stability of the electrode interface film.
[0073] Example 1 <Preparation of Electrolyte> In an argon-atmospheric glove box (water content <1 ppm, oxygen content <1 ppm), ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed uniformly at a mass ratio of 3:7 to obtain a basic organic solvent. Lithium salt LiPF6 was then added, followed by additives I, II, and III. After dissolving and mixing uniformly, an electrolyte was obtained. Based on the mass of the electrolyte, the mass percentages of LiPF6, basic organic solvent, additives I, II, and III were 12.5%, 82.5%, 2%, 2%, and 1%, respectively.
[0074] <Preparation of the positive electrode> <Precursor Solution Preparation> Lithium hydroxide (LiOH·H2O), ammonium dihydrogen phosphate (NH4H2PO4), and ferrous acetate (Fe(CH3COO)2) were precisely weighed according to the stoichiometric ratio of the target product LiFePO4, i.e., a molar ratio of 1:1:1, as the main raw materials for lithium iron phosphate precursor.
[0075] Preparation of carbon source solution: Glucose (C6H4O) was selected. 12 Using O6 as a carbon source, glucose was accurately weighed and added to deionized water at a mass ratio of 1:0.1 to lithium iron phosphate precursor and glucose, and stirred evenly to obtain a second mixture.
[0076] The weighed main raw materials (lithium source, phosphorus source, and iron source) were placed in a high-speed shear dispersion reactor. An appropriate amount of deionized water was added, and the mixture was subjected to high-speed shear stirring within a temperature range of room temperature to 60°C under argon protection to form a homogeneous precursor suspension / solution mixture. Subsequently, the carbon source solution was slowly added dropwise to the mixture while continuously stirring to ensure uniform dispersion of the carbon source.
[0077] <Spray Drying and Pre-sintering> The uniformly mixed slurry was immediately spray-dried. The inlet temperature was controlled at 200℃ and the outlet temperature at 100℃, resulting in microspherical dried precursor powder. This process rapidly transforms the liquid mixture into a homogeneous solid mixture and initially forms an amorphous carbon network framework. The spray-dried precursor powder was placed in a tube furnace and pre-sintered at 400℃ under high-purity argon protection at a heating rate of 3℃ / min for 5 hours.
[0078] High-Temperature Crystallization Calcination and Carbon Coating After the pre-sintered intermediate product is allowed to cool naturally, it is then ground to break up any possible soft agglomerates. The ground powder is then placed back into a tube furnace and subjected to high-temperature crystallization calcination under a flowing inert atmosphere. The calcination procedure is as follows: the temperature is increased to 700°C at a rate of 5°C / min, and held at this temperature for 10 hours.
[0079] After high-temperature calcination, the sintered block is cooled to room temperature in an inert atmosphere. The cooled sintered block is then removed, mechanically ground, and passed through a 400-mesh sieve to obtain the final carbon-coated lithium iron phosphate (LFP) cathode active material powder. Based on the total mass of carbon-coated lithium iron phosphate, the mass percentage of carbon material is 2%.
[0080] <Preparation of the positive electrode> The prepared positive electrode active material lithium iron phosphate (LFP), conductive agent superconducting carbon black (Super P), carbon nanotubes (CNT), and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 94.5:3:0.5:2. N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly under vacuum to obtain a positive electrode slurry with a solid content of 55 wt%. The positive electrode slurry was uniformly coated on one surface of a 16 μm thick positive electrode current collector aluminum foil. After drying at 85 ℃, a positive electrode sheet with a single-sided coating of positive electrode active material layer with a coating thickness of 37 μm was obtained. The above steps were repeated on the other surface of the positive electrode current collector aluminum foil to obtain a positive electrode sheet with a double-sided coating of positive electrode active material layer. After drying at 85 ℃, the sheet was rolled, trimmed, cut, and slit. After slitting, the sheet was dried at 85 ℃ under vacuum for 5 hours. The tabs were then welded to obtain a positive electrode sheet with a specification of 70 mm × 54 mm. The areal density of the positive electrode active material is 15 mg / cm³.2 .
[0081] <Preparation of Negative Electrode Sheets> A negative electrode active material (graphite), a conductive agent (superconducting carbon black, Super P), a binder (styrene-butadiene rubber, SBR), and a thickener (sodium carboxymethyl cellulose, CMC) were mixed in a mass ratio of 95:1.5:2:1.5. Deionized water was added, and the mixture was stirred evenly under vacuum to obtain a negative electrode slurry with a solid content of 49 wt%. The negative electrode slurry was uniformly coated onto one surface of a 9 μm thick copper foil current collector. After drying at 85 ℃, a negative electrode sheet with a single-sided coating of negative electrode active material layer with a coating thickness of 48.5 μm was obtained. The above steps were repeated on the other surface of the copper foil current collector to obtain a negative electrode sheet with a double-sided coating of negative electrode active material layer. After drying at 85 ℃, the sheet was rolled, trimmed, cut, and slit. After slitting, the sheet was dried at 85 ℃ under vacuum for 5 hours, and tabs were welded to obtain a negative electrode sheet with a specification of 74 mm × 58 mm. The areal density of the negative electrode active material was 7 mg / cm³. 2 .
[0082] <Preparation of the diaphragm> A 12 µm thick polyethylene (PE) ceramic diaphragm (provided by Shenzhen Xingyuan Material Technology Co., Ltd., model PE ceramic 10+2) is used.
[0083] <Preparation of Lithium-ion Batteries> The prepared positive electrode, separator, and negative electrode are stacked sequentially, with the separator positioned between the positive and negative electrodes to act as a separator. The stacked battery is then assembled, with the positive tab connected to the positive electrode and the negative tab connected to the negative electrode, forming the electrode assembly. The electrode assembly is placed in an aluminum foil packaging bag, with the positive and negative tabs extended from the inside to the outside of the bag. It is then vacuum-dried at 85 °C for 48 hours, and injected with the prepared electrolyte at an injection rate of 4.5 g / Ah. After vacuum sealing, formation, aging, and capacity testing, a lithium-ion battery is obtained. The formation upper limit voltage is 3.55 V, the formation temperature is 45 °C, and the formation resting time is 2 hours. The aging temperature is 45 °C, and the aging resting time is 24 hours. Capacity testing involves charging to 3.8 V at 0.1C, resting for 5 minutes, and then discharging to 2.0 V at 0.1C, repeating this process three times.
[0084] Examples 2-36 Except for adjusting the relevant preparation parameters according to Table 1, everything else is the same as in Example 1.
[0085] The target carbon coating amount can be controlled by adding glucose with different carbon contents. The required mass of glucose can be accurately calculated and weighed according to different mass ratios of lithium iron phosphate precursor and glucose. Lithium iron phosphate positive electrode active material powders with different carbon coating contents can be prepared according to the process of Example 1. When the mass percentage of additive I, additive II, and additive III changes, the mass percentage of the basic organic solvent changes accordingly, while the mass percentage of lithium salt remains unchanged. The sum of the mass percentages of additive I, additive II, additive III, basic organic solvent, and lithium salt is 100%.
[0086] Examples 37 to 40 Except for keeping the amount of lithium salt constant as shown in Table 2 in the <Preparation of Electrolyte>, adjusting the type and molar ratio of lithium salt, changing the mass percentage of the basic organic solvent accordingly, and keeping the percentage of other components in the electrolyte constant, everything else is the same as in Example 17.
[0087] Comparative Examples 1 to 7 Except for adjusting the type and mass percentage of additive I (a%), additive II (b%), and additive III (c%) according to Table 1 in <Electrolyte Preparation>, the mass percentage of the basic organic solvent is changed accordingly, while the percentage of other components in the electrolyte remains unchanged; and / or, lithium iron phosphate cathode active materials with different carbon coating contents as shown in Table 1 are selected; the rest is the same as in Example 1.
[0088] Comparative Example 8 Except that additive I is not added in the <Preparation of Electrolyte>, the mass percentage of the basic organic solvent is changed accordingly, and the percentage of other components in the electrolyte remains unchanged, everything else is the same as in Example 1.
[0089] Comparative Example 9 Except that additive II is not added in the <Preparation of Electrolyte>, the mass percentage of the basic organic solvent is changed accordingly, and the percentage of other components in the electrolyte remains unchanged, the rest is the same as in Example 1.
[0090] Comparative Example 10 Except that additive III was not added in the <Preparation of Electrolyte>, the mass percentage of the basic organic solvent was changed accordingly, and the percentage of other components in the electrolyte remained unchanged, everything else was the same as in Example 1.
[0091] Comparative Example 11 Except for the absence of carbon material in the <precursor solution preparation>, the preparation steps were the same as in Example 1. The preparation steps for Comparative Example 11 were as follows: <Precursor Solution Preparation> According to the stoichiometric ratio of the target product LiFePO4, lithium hydroxide (LiOH·H2O), ammonium dihydrogen phosphate (NH4H2PO4), and ferrous acetate (Fe(CH3COO)2) were accurately weighed as the main raw materials for lithium iron phosphate precursor.
[0092] The weighed main raw materials (lithium source, phosphorus source, and iron source) were placed in a high-speed shear dispersion reactor. An appropriate amount of deionized water was added, and the mixture was subjected to high-speed shear stirring in the range of room temperature to 60°C under argon protection to form a homogeneous precursor suspension / solution mixture.
[0093] <Spray Drying and Pre-sintering> The uniformly mixed slurry was immediately spray-dried. The inlet temperature was controlled at 200℃ and the outlet temperature at 100℃, resulting in microspherical dried precursor powder. This process rapidly transforms the liquid mixture into a homogeneous solid mixture. The spray-dried precursor powder was placed in a tube furnace and pre-sintered at 400℃ under high-purity argon protection at a heating rate of 3℃ / min for 5 hours.
[0094] High-temperature crystallization and calcination After the pre-sintered intermediate product is allowed to cool naturally, it is then ground to break up any possible soft agglomerates. The ground powder is then placed back into a tube furnace and subjected to high-temperature crystallization calcination under a flowing inert atmosphere. The calcination procedure is as follows: the temperature is increased to 700°C at a rate of 5°C / min, and held at this temperature for 10 hours.
[0095] After high-temperature calcination, the material was cooled to room temperature in an inert atmosphere. The cooled sintered block was then removed, mechanically ground, and passed through a 400-mesh sieve to obtain the final lithium iron phosphate cathode active material powder. The remaining preparation processes and steps were the same as in Example 1.
[0096] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Table 1 and Table 2.
[0097] Table 1
[0098] Note: In Table 1, " / " indicates that the corresponding preparation parameters or substances do not exist.
[0099] Table 2
[0100] As shown in Table 1, the batteries prepared in Examples 1-32 of this application exhibit high capacity retention rates after 4 cycles of pulse charging at 55°C and after 1000 cycles at 45°C, demonstrating good cycle stability. Furthermore, they show low DCR changes after 1000 cycles at 45°C and low thickness expansion rates after 60 days of storage at 60°C, indicating good overall performance. In contrast, the batteries in Comparative Examples 8-11 show poor overall performance. Their capacity retention rates after 4 cycles of pulse charging at 55°C and after 1000 cycles at 45°C are significantly lower than those of the examples in this application, while their DCR changes after 1000 cycles at 45°C and thickness expansion rates after 60 days of storage at 60°C are significantly higher. Comparative Examples 8-10 did not introduce a single electrolyte additive; Comparative Example 11 did not introduce a carbon coating layer. Therefore, Comparative Examples 8-10 failed to achieve electrochemical performance comparable to the examples in this application. This shows that the simultaneous introduction of additives I, II, III and a carbon coating layer into the electrolyte can significantly improve the capacity retention rate in the later stages of battery cycling and significantly suppress the DCR growth of the battery during high-temperature cycling.
[0101] Comparing Examples 1, 6-7, 18-19 with Comparative Examples 1 and 2, it can be seen that when the mass percentage (a%) of additive I in the electrolyte is controlled within the range of 0.5-5%, it is beneficial to obtain a secondary battery with good cycle stability. Furthermore, the performance is even better when a% is in the range of 1-4%. For example, Examples 1 and 6-7 achieved a capacity retention rate of 84.11%-88.95% after 4 cycles of pulse charging at 55℃, and a capacity retention rate of 86.50%-90.84% after 1000 cycles at 45℃. The DCR change rate after 1000 cycles at 45℃ and the thickness expansion rate after 60 days of storage at 60℃ were 15.08%-18.93% and 2.34%-5.10%, respectively, significantly better than Comparative Examples 1 and 2. This indicates that the secondary battery has better capacity retention in the later stages of battery cycling and significantly suppresses the DCR growth during high-temperature cycling.
[0102] Comparing Examples 1, 8-9, 20-21 with Comparative Examples 3-4 reveals that controlling the mass percentage b% of additive II in the electrolyte within the range of 0.5%-5% is beneficial for obtaining a secondary battery with good cycle stability. Furthermore, performance is even better when a% is in the range of 1%-4%. For example, Examples 1 and 8-9 achieved a capacity retention rate of 86.66%-88.95% after 4 cycles of pulse charging at 55°C, and a capacity retention rate of 88.58%-90.84% after 1000 cycles at 45°C. The DCR change rate after 1000 cycles at 45°C and the thickness expansion rate after 60 days of storage at 60°C were 15.08%-18.56% and 2.34%-5.03%, respectively, significantly better than Comparative Examples 3-4. This indicates that the secondary battery exhibits better capacity retention in the later stages of battery cycling and significantly suppresses DCR growth during high-temperature cycling.
[0103] A comparison of Examples 1, 10-11, and 22-23 with Comparative Examples 5-6 shows that when the mass percentage (c%) of additive III in the electrolyte is controlled within the range of 0.1%-5%, it is beneficial to obtain a secondary battery with good cycle stability. Furthermore, the performance is even better when a% is in the range of 0.5%-3%. For example, Examples 1 and 10-11 achieved a capacity retention rate of 88.02%-88.95% after 4 cycles of pulse charging at 55°C, and a capacity retention rate of 89.92%-90.84% after 1000 cycles at 45°C. The DCR change rate after 1000 cycles at 45°C and the thickness expansion rate after 60 days of storage at 60°C were 15.08%-18.32% and 2.34%-4.99%, respectively, significantly better than Comparative Examples 5-6. This indicates that the secondary battery has better capacity retention in the later stages of battery cycling and significantly suppresses the DCR growth during high-temperature cycling.
[0104] A comparison of Examples 1, 14-15, 26-27 with Examples 34-35 shows that when the mass percentage (m%) of carbon material is controlled within the range of 0.1%-5.0%, it is beneficial to obtain a secondary battery with good cycle stability. Furthermore, Examples 1 and 14-15 achieved a capacity retention rate of 80.25%-88.95% after four cycles of pulse charging at 55°C, and a capacity retention rate of 81.87%-90.84% after 1000 cycles at 45°C. The DCR change rate after 1000 cycles at 45°C and the thickness expansion rate after 60 days of storage at 60°C were 15.08%-21.78% and 2.34%-8.26%, respectively, significantly better than Examples 34-35. This indicates that the secondary battery has better capacity retention in the later stages of battery cycling and significantly suppresses the DCR growth during high-temperature cycling.
[0105] Comparing Examples 1 and 6-30 with Examples 35-36 and Comparative Example 7, it can be seen that when... Maintaining the temperature within the range of -15.93 to 55.75°C is beneficial for obtaining secondary batteries with good rate performance and cycle stability. Furthermore, when... The performance is even better when the temperature is in the range of -8.63 to 18. For example, in Examples 1 and 6-26, the capacity retention rate after 4 cycles of pulse charging at 55°C is 79.71%-88.95%, and the capacity retention rate after 1000 cycles at 45°C is 81.20%-90.84%. The DCR change rate after 1000 cycles at 45°C and the thickness expansion rate after 60 days of storage at 60°C are 15.08%-21.88% and 2.34%-8.30%, respectively, which are significantly better than Examples 35-36 and Comparative Example 7. This shows that the secondary battery has better rate performance and cycle stability, and can effectively reduce metal ion dissolution.
[0106] Comparing Example 1 with Examples 2-5 reveals that in this electrolyte / battery system, both the alkyl chain length and symmetry on the nitrogen atom significantly affect the crosslinking density of the polymer backbone. Furthermore, the presence of asymmetric alkyl chain structures influences the overall electron cloud distribution of the molecule. The carbon chain exhibits spatial torsion; asymmetric carbon chains lead to varying degrees of weakening of the N-S bond energy, resulting in reduced chemical stability. Symmetrical structures offer greater stability. The nitrogen lone pair electrons on the nitrogen atom have a hyperconjugating effect, effectively enhancing the interaction between the nitrogen center and the Li atom. + Its coordination ability allows it to more effectively guide Li through electron cloud polarization. + Furthermore, longer chain lengths result in longer organic alkyl chain segments in the membrane composition. These longer organic alkyl chain segments can reduce the rate of lithium ion passage through the interfacial membrane to some extent, thereby reducing the efficiency of lithium insertion / extraction and exhibiting a slight increase in impedance and capacity decay.
[0107] As shown in Table 2, the preferred ratio of LiPF6 to LiFSI (LiN(SO2F)2) molar amounts is 1 ≤ n(LiPF6):n(LiFSI) ≤ 2. Within this range, an appropriate amount of LiFSI can improve the ionic conductivity and high-temperature stability of the electrolyte. It can also participate in the construction of the interfacial film, increase the Young's modulus of the interfacial film, decompose to generate interfacial film components containing S and F, further improve ion transport efficiency, and enhance the cycle stability of the battery. When n(LiPF6):n(LiFSI) < 1, excessive LiFSI reduces the oxidation resistance of the electrolyte, and the decomposition of lithium salt further consumes the electrolyte. More side reactions consume active lithium, which is not conducive to the occurrence of continuous reversible lithium intercalation and deintercalation processes, and the capacity continuously decays. When n(LiPF6):n(LiFSI) > 2, a small amount of LiFSI has a limited effect on improving the system, reduces the oxidation potential of the electrolyte, and the generated interfacial film has thermochemical instability, leading to the continuous occurrence of side reactions and deteriorating performance.
[0108] In this specification, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0109] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A battery, characterized in that, It includes a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode includes a positive electrode active material layer, which includes a positive electrode active material, namely lithium iron phosphate, and the surface of the lithium iron phosphate is coated with a carbon material. The electrolyte contains additive I, additive II and additive III; The specific structure of additive I is shown in Formula I: Equation I, In Formula I, R1 and R2 each independently represent a straight-chain or branched alkyl group having 1 to 3 carbon atoms; Additive II is vinylene carbonate; Additive III is vinyl sulfate; Based on the total mass of the electrolyte, the mass percentage of additive I is a%, 0.5≤a≤5; Based on the total mass of the electrolyte, the mass percentage of additive II is b%, 0.5≤b≤5; Based on the total mass of the electrolyte, the mass percentage of additive III is c%, where 0.1 ≤ c ≤ 5.
2. The battery according to claim 1, characterized in that, At least one of the following conditions must be met: 1≤a≤4; 1≤b≤4; 0.5≤c≤3。 3. The battery according to claim 1, characterized in that, The additive I includes at least one of the following compounds: Compound 1 Compound 2 Compound 3 Compound 4 Compound 5.
4. The battery according to claim 1, characterized in that, Based on the mass of the positive electrode active material, the mass percentage of the carbon material is m%, and 0.1 ≤ m ≤ 5; the battery satisfies: -15.93 ≤ ≤55.
75.
5. The battery according to claim 4, characterized in that, Based on the mass of the positive electrode active material, the mass percentage of the carbon material is m%, 1≤m≤3.
6. The battery according to claim 4, characterized in that, The battery satisfies: -8.63≤ ≤18.
7. The battery according to claim 1, characterized in that, The electrolyte further includes a lithium salt and an organic solvent, and satisfies at least one of the following (I) to (II): (I) The lithium salt includes at least one of LiPF6, LiAsF6, LiBF4, LiB(C2O4)2, LiBF2C2O4, LiN(SO2F)2, LiN(SO2CF3)2, LiPO2F2, LiPF2(C2O4)2, and LiPF4C2O4; (II) The organic solvent includes at least one of carbonate solvents and carboxylic acid ester solvents.
8. The battery according to claim 7, characterized in that, The lithium salt is LiPF6 and LiN(SO2F)2, and the molar ratio of LiPF6 to LiN(SO2F)2 is 1-2:
1.
9. The battery according to claim 7, characterized in that, The organic solvent satisfies at least one of the following conditions (III) to (IV): (III) The carbonate solvent includes at least one of ethylene carbonate, propylene carbonate, butene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, or methyl propyl carbonate. (IV) The carboxylic acid ester solvent includes at least one of methyl formate, methyl acetate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate or ethyl butyrate.