An electrolyte, its preparation method and application

By employing the synergistic effect of PEG, CMC-Na, and PAM in lead-acid gel batteries, a three-dimensional SiO2 gel framework was constructed, solving the problems of narrow filling process window and easy structural degradation in lead-acid gel batteries, and achieving high battery consistency and long life.

CN123120912APending Publication Date: 2026-11-17JYC BATTERY MFR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611233063.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Lead-acid gel batteries suffer from problems in the filling process, such as difficulty in ensuring the uniformity of gel electrolyte dispersion and a narrow gelation time window, leading to batch-to-batch inconsistencies. Furthermore, the structure of the gel electrolyte is prone to degradation during cycling, resulting in battery capacity decay.

Method used

A rigid three-dimensional gel framework of SiO2 was constructed by using PEG steric hindrance. Combined with flexible long chains of CMC-Na and reversible hydrogen bonding of PAM, the gelation time window was extended and the structural stability was enhanced. The CMC-Na molecular chains, which were pre-swollen, were intercalated into the gaps between SiO2 particles. The reversible hydrogen bonding of PAM provided dynamic repair capabilities, forming bridging structural units.

Benefits of technology

It extends the gelation time window, improves batch consistency of the filling process window, alleviates gel cracking and capacity decay issues, and enhances battery cycle life and low-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention discloses an electrolyte, its preparation method, and its application, belonging to the field of electric vehicle energy storage device manufacturing technology. The electrolyte formulation includes concentrated sulfuric acid, deionized water, fumed silica, polyacrylamide, sodium carboxymethyl cellulose, phosphoric acid, sodium sulfate, boric acid, and polyethylene glycol, arranged in a specific ratio. This invention utilizes the steric hindrance of PEG to construct a three-dimensional SiO2 gel rigid framework, within which pre-swollen flexible long-chain CMC-Na is wound. An acidic environment is used to enhance the reversible hydrogen bond crosslinking of PAM. The resulting gel electrolyte extends the gelation time window from the conventional 15-30 minutes to 45-75 minutes, and improves the thixotropic recovery rate to over 87%. The resulting colloidal electrolyte has a wide filling process window, good structural stability, and excellent low-temperature performance, improving the problems of colloidal cracking and capacity decay, extending battery cycle life and float charge life. Furthermore, the preparation process is simple and cost-controllable, showing good prospects for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electric vehicle energy storage device manufacturing technology, and more particularly to the manufacturing of electrolytes for secondary batteries. Background Technology

[0002] Traditional liquid lead-acid batteries use dilute sulfuric acid as the electrolyte, with lead dioxide and spongy lead as the positive and negative electrodes, respectively, immersed in a flowing sulfuric acid solution. These batteries suffer from problems such as electrolyte stratification, acid leakage during transportation, and acid mist emission during charging, and require regular water replenishment for maintenance. To address these issues, gel batteries were developed—by adding gelling agents such as fumed silica to the sulfuric acid electrolyte, the liquid electrolyte is transformed into a gel state, forming a three-dimensional porous network structure with a silica gel framework, encapsulating the electrolyte. After the gel solidifies, the framework shrinks, creating cracks that provide a channel for oxygen released from the positive electrode during charging to reach the negative electrode, enabling oxygen recombination and battery sealing, thus achieving advantages such as maintenance-free operation, no leakage, and long lifespan. Compared to traditional liquid lead-acid batteries, gel lead-acid batteries have advantages such as no acid stratification, the ability to be placed in any orientation, and low self-discharge; however, they still face the following long-standing technical challenges in practical applications: I. The contradiction between the thixotropic properties of colloidal electrolytes and the filling process. Colloidal electrolytes need to have low viscosity during filling to flow smoothly into the battery casing, while after injection, they need to quickly form a stable three-dimensional network gel structure to prevent leakage. In existing technologies, fumed silica is commonly used as a gelling agent, but its dispersion uniformity is difficult to guarantee, and the gelation time window is too narrow (usually 15-30 minutes), resulting in insufficient filling process window and making batch-to-batch consistency differences easily caused by fluctuations in operating time during production. II. Structural Degradation of Colloidal Electrolytes During Long-Term Cycling. During battery charge-discharge cycles, the three-dimensional gel network structure of colloidal electrolytes undergoes irreversible shrinkage, cracking, and even collapse due to the periodic changes in hydroxide ion concentration and the mechanical disturbance of bubbles. This manifests as colloidal dehydration and shrinkage (i.e., "drying out"), leading to a gradual increase in the contact resistance between the electrolyte and the plates, thereby accelerating battery capacity decay. This problem is particularly prominent under deep-cycle operating conditions (such as solar energy storage). Summary of the Invention

[0003] This invention addresses the aforementioned technical problems of existing lead-acid gel electrolytes by providing an improved gel electrolyte and its preparation method. This invention utilizes the steric hindrance of PEG to construct a three-dimensional rigid SiO2 gel framework, within which pre-swollen flexible long-chain CMC-Na is wound. Furthermore, an acidic environment is used to enhance the reversible hydrogen bond crosslinking of PAM. The resulting gel electrolyte extends the gelation time window from the conventional 15-30 minutes to 45-75 minutes, and improves the thixotropic recovery rate to over 87%. The obtained gel electrolyte exhibits a generous filling process window, good structural stability, and excellent low-temperature performance, improving issues such as gel cracking and capacity decay, and extending battery cycle life and float charge life.

[0004] The specific plan is as follows: An electrolyte comprises, by weight, 33-38 parts concentrated sulfuric acid, 54-60 parts deionized water, 4.5-6.5 parts fumed silica, 0.20-0.40 parts polyacrylamide, 0.30-0.60 parts nano-carboxymethyl cellulose sodium, 0.30-0.50 parts phosphoric acid, 0.80-1.20 parts sodium sulfate, 0.10-0.25 parts boric acid, and 0.4-0.8 parts polyethylene glycol.

[0005] The concentrated sulfuric acid (H2SO4) has the CAS number 7664-93-9, is of analytical grade, has a mass fraction ≥98.0%, and an iron content ≤0.00005%. Deionized water resistivity ≥18.0 MΩ·cm (25℃); The BET specific surface area of ​​fumed silica (SiO2) is 200 ± 25 m². 2 / g, average primary particle size 7–16 nm, loss on ignition ≤2.0%; Polyacrylamide (PAM) CAS number 9003-05-8, non-ionic, molecular weight 80×10 4 ~120×10 4 g / mol, degree of hydrolysis ≤5%; Nano-carboxymethyl cellulose sodium (CMC-Na) has CAS number 9004-32-4, degree of substitution (DS) of 0.85-0.95, and viscosity of 2% aqueous solution (25℃) of 800-1200 mPa·s. Phosphoric acid (H3PO4) was of analytical grade with a mass fraction ≥85.0%. Sodium sulfate (Na2SO4) was of analytical grade, anhydrous, and with a purity ≥99.0%. Boric acid (H3BO3) was tested at analytical grade with a purity ≥99.0%. Polyethylene glycol (PEG), CAS: 25322-68-3, molecular weight 4000-6000.

[0006] Each of the above components has a clearly defined CAS number and structural formula, and all are common commercially available products.

[0007] Further, by weight, it includes 35.5 parts concentrated sulfuric acid, 57 parts deionized water, 5.2 parts fumed silica, 0.28 parts polyacrylamide, 0.45 parts sodium nanocarboxymethyl cellulose, 0.4 parts phosphoric acid, 1.0 part sodium sulfate, 0.17 parts boric acid, and 0.6 parts polyethylene glycol.

[0008] Furthermore, the molecular weight of the polyethylene glycol is 4000-6000.

[0009] The molecular weight range of polyethylene glycol is limited to 4000-6000 to ensure that it can provide sufficiently long molecular chains to form hydrogen bond bridges in colloidal systems, while also having good solubility and dispersion stability.

[0010] A method for preparing an electrolyte includes the following steps: Step 1: Prepare nano-carboxymethyl cellulose sodium pre-swelling solution; Step 2: Prepare a sulfuric acid-phosphoric acid mixed solution; Step 3: Pre-dispersion of fumed silica; Step 4: Add the pre-swollen sodium carboxymethyl cellulose nano solution to the fumed silica pre-dispersion solution for pre-mixing, and then add polyethylene glycol and polyacrylamide; Step 5: Add the sulfuric acid-phosphoric acid mixture to the composite gelling base material from Step 4, so that the dispersed fumed silica associates into a three-dimensional network framework and enhances the reversible hydrogen bond bridging between different components of the gel system.

[0011] Furthermore, step one includes the following sub-steps: Step 11: Heat deionized water in a water bath and add the prescribed amount of sodium carboxymethyl cellulose under stirring conditions; After all the nano-carboxymethyl cellulose sodium was added in step 12, the solution was stirred and dispersed until the nano-carboxymethyl cellulose sodium was completely dissolved and there were no visible particles, resulting in a transparent and uniform nano-carboxymethyl cellulose sodium pre-swelling solution. Step 13: Allow the pre-swollen solution of nano-carboxymethyl cellulose sodium to cool naturally and stand for at least 20 hours before use.

[0012] After pre-swelling, sodium carboxymethyl cellulose (CMC-Na) has fully extended molecular chains, forming a transparent and uniform flexible network framework.

[0013] Furthermore, step two includes the following sub-steps: Step 21: Place deionized water in an ice-water bath and cool it to below 15°C. Add the prescribed amount of concentrated sulfuric acid dropwise, controlling the dropping rate so that the system temperature does not exceed 45°C. After all the concentrated sulfuric acid has been added in step 22, continue stirring and cool to 30℃±2℃; Step 23: Add the prescribed amount of phosphoric acid to reactor B under stirring conditions, and continue stirring until homogeneous to obtain a sulfuric acid-phosphoric acid mixed solution.

[0014] Furthermore, step three includes the following sub-steps: Step 31: Add the prescribed amounts of sodium sulfate, boric acid, and polyethylene glycol to deionized water and stir until completely dissolved; Step 32: Under stirring conditions, slowly add the formulated amount of fumed silica to the solution in sub-step 31. After all the silica has been added, stir and disperse to obtain a fumed silica pre-dispersion slurry. Step 33: Place the pre-dispersed fumed silica slurry in an ultrasonic dispersion device and perform ultrasonic dispersion treatment to break up the agglomerates of fumed silica. During the ultrasonic treatment, control the slurry temperature to not exceed 40°C. In step 34, under stirring conditions, dilute sulfuric acid is slowly added dropwise to the slurry after ultrasonic treatment in step 33 to adjust the pH value of the slurry to 4.5~5.0. During this process, the system temperature is controlled not to exceed 40℃. After the adjustment is completed, stirring is continued to obtain a fumed silica stabilized slurry with pH=4.5~5.0, which is then placed in a constant temperature environment of 30~35℃ for later use.

[0015] Fumed silica is used as the main gelling agent, and its uniform dispersion and deagglomeration are achieved through ultrasonic dispersion and pH adjustment.

[0016] Furthermore, step four includes the following sub-steps: Step 41: Transfer the nano-carboxymethyl cellulose sodium pre-swelling solution from Step 1 to the pre-dispersed slurry of fumed silica from Step 3, and mix them evenly under stirring conditions. Step 42: Evenly sprinkle the formulated amount of polyacrylamide into the mixed solution of sub-step 41, increase the stirring speed, and continue stirring until PAM is completely dissolved to obtain a ternary composite gelling base material containing a preliminary network aggregate of fumed silica, a flexible network of nano-carboxymethyl cellulose sodium, and a reversible hydrogen bond cross-linked network between polyacrylamide, fumed silica, and nano-carboxymethyl cellulose sodium.

[0017] Nano-sized sodium carboxymethyl cellulose is interwoven between silica particles through hydrogen bonds and physical entanglement.

[0018] Furthermore, step five includes the following sub-steps: Step 51: Add the sulfuric acid-phosphoric acid mixed solution from Step 2 to the ternary composite gelling base material from Sub-Step 42 under stirring conditions. After all the solution is added, continue stirring until a uniform colloidal dispersion system is formed. Step 52: Stop stirring and perform vacuum degassing of the prepared colloidal electrolyte to remove air bubbles trapped during stirring. Step 53 discharges the material to obtain the finished colloidal electrolyte.

[0019] Polyethylene glycol inhibits the aggregation of fumed silica and sodium carboxymethyl cellulose through physical barrier effects. Strong acid enhances the reversible hydrogen bond crosslinking between polyacrylamide, fumed silica, and nano-sodium carboxymethyl cellulose, forming a bridging structural unit of "SiO2 particles—PAM / CMC-Na polymer chains—SiO2 particles". This inhibits and delays the rapid chemical bonding of SiO2 particles through hydrogen bonds to form a colloidal network structure in the early stage of acid addition, thus prolonging the gelation time window.

[0020] An application of the electrolyte as described above in a lead-acid gel battery includes the following steps: ① The prepared gel electrolyte is injected into the formed lead-acid gel battery casing through a filling machine. The filling environment temperature is 25℃±3℃. ② After filling, place the battery in a constant temperature room at 25℃±2℃ for 6 hours to allow the colloidal electrolyte to fully gel. ③ After gelation is complete, recharge the battery at 0.05C. 10 Charging with current for 2 hours makes the ion distribution in the electrolyte more uniform; ④ After recharging, the battery is sealed, cleaned, tested, and packaged according to standard procedures.

[0021] Compared with the prior art, the present invention has at least one of the following technical effects: 1) In step three, PEG is pre-adsorbed onto the surface of SiO2 to form a steric hindrance layer, which delays the rapid chemical bonding of SiO2 particles through hydrogen bonds to form a colloidal network structure in the early stage of acid addition (i.e., delays the rapid association of SiO2 particles in the early stage of acid addition); in step four, CMC-Na molecular chains are interspersed between particles to form physical inhibition; in step five, fumed silica (SiO2) nanoparticles are used as rigid nodes, and polyacrylamide (PAM) molecular chains and their complex with sodium carboxymethyl cellulose (CMC-Na) molecular chains are used as flexible bridging units. The three interact through reversible hydrogen bonds to form a bridging structural unit of "SiO2 particles - PAM / CMC-Na polymer chains - SiO2 particles". This changes the gelation process from a single "particle-particle direct association" to a slow guidance of particles to form a network through bridging by polymers, avoiding rapid association of SiO2 particles and significantly extending the gelation time window to 45-75 minutes. This provides a sufficient process window for the infusion operation and effectively improves batch consistency.

[0022] 2) Conventional SiO2 colloidal networks are maintained solely by silanol hydrogen bonds. During charge-discharge cycles, they are susceptible to irreversible shrinkage, cracking, and even collapse due to bubble disturbances and periodic changes in ion concentration, resulting in colloidal "drying" and capacity decay. This invention utilizes pre-swollen CMC-Na molecular chains, fully extended and interwoven into the gaps between SiO2 particles. These chains bind to the SiO2 network through hydrogen bonds and physical entanglement. The flexible long chains buffer local stress concentrations through chain segment movement when the gel network is under stress, effectively inhibiting the initiation and propagation of microcracks. The reversible hydrogen bond crosslinking of PAM provides dynamic repair capabilities to the network; hydrogen bond breaks caused by shearing or stress can be re-established during rest. The steric hindrance layer of PEG maintains the uniform dispersion of SiO2 particles, preventing local structural weakness caused by agglomeration. The synergistic effect of these three elements enables the colloidal system to maintain structural integrity under deep cycling conditions, improving the degree of colloidal cracking from obvious cracks to minor cracks, and extending the high-temperature float charge life from approximately 260 days to 390 days.

[0023] 3) The gel framework of colloidal electrolytes physically inhibits ion migration. At low temperatures, electrolyte viscosity increases, and ionic conductivity further decreases, resulting in generally low low-temperature capacity retention of batteries. This invention utilizes the synergistic effect of the PEG steric hindrance layer and the CMC-Na flexible network to make the gel network more uniform and ordered, reducing the blockage of ion transport channels by SiO2 aggregates. Simultaneously, the reversible cross-linked network of PAM prevents excessive gel shrinkage, preserving more free pathways for ion migration. Example 1 achieved a low-temperature capacity retention of 65.8% at -20℃, a significant improvement compared to the closest prior art (approximately 55%), demonstrating the effectiveness of this invention in improving low-temperature ion conduction.

[0024] 4) This invention uses non-ionic PEG as a steric hindrance stabilizer, avoiding competitive adsorption of ionic dispersants on the electrode surface; CMC-Na is fixed by the SiO2 network after pre-swelling, reducing its direct contact and reduction deposition risk on the negative electrode surface; phosphoric acid forms a Pb3(PO4)2 protective film on the positive electrode grid surface, inhibiting positive electrode corrosion; boric acid is specifically adsorbed on the negative electrode surface to increase the hydrogen evolution overpotential. Each component has a clearly defined function and complements the others, avoiding harmful side reactions. The 100% DOD cycle life is increased from approximately 420 cycles to 625 cycles, demonstrating the effectiveness of this invention in suppressing early capacity loss and extending battery life.

[0025] 5) When the pH of the system drops sharply to 1.2, a large amount of H+... + By protonating the carboxymethyl (-COONa) groups on the CMC-Na molecular chain to -COOH, the electrostatic repulsion between molecular chains disappears, solubility decreases, and free CMC-Na will aggregate and precipitate. However, in this invention, the steric hindrance layer of PEG, on the one hand, physically hinders H... +The direct contact between CMC-Na and SiO2 particles slows down the protonation process, ensuring that an effective amount of CMC-Na long chains are interspersed within the SiO2 particle gaps. On the other hand, even if the PEG molecular chains adsorbed on the particle surface partially desorb, they can still delay the coiling and aggregation of CMC-Na molecular chains in solution through steric repulsion. Furthermore, under strong acid conditions, the ether oxygen atoms of PEG can form hydrogen bonds or ion-dipole interactions with hydrated hydrogen ions, enhancing the electrostatic adsorption force on the negatively charged SiO2 surface and strengthening its electrostatic attraction and binding effect on CMC-Na molecular chains. This "fixes" CMC-Na near the PEG / SiO2 composite interface, preventing it from freely migrating into the liquid phase and aggregating. This synergistic effect of the three aspects allows CMC-Na to maintain an effective dispersion even in a thermodynamically predisposing strong acid environment, thus preventing the disruption of the gel network uniformity and ensuring the long-term structural stability and crack resistance of the colloid.

[0026] 6) This invention first thoroughly mixes CMC-Na with SiO2 particles under neutral conditions. Pre-binding is achieved through hydrogen bonds between the carboxymethyl groups (-COONa) on the CMC-Na molecular chain and the silanol groups (Si-OH) on the SiO2 surface, anchoring CMC-Na to the surface of the SiO2 particles or embedding it within the interstices of their aggregates. Simultaneously, PEG is introduced to pre-form a steric hindrance layer, further enhancing the fixation and protection of CMC-Na. Then, when sulfuric acid is added stepwise to adjust to a strongly acidic environment, the CMC-Na molecular chains, physically fixed by the SiO2 network and sterically inhibited by the PEG layer, cannot freely migrate into the liquid phase to aggregate and precipitate due to spatial constraints. This effectively reduces the aggregation and precipitation defects of free CMC-Na in strong acid caused by carboxyl protonation. This sequential design ensures that the effective amount of CMC-Na remains stable in an extended state in the final colloidal system, giving full play to its flexible network reinforcement and anti-drying shrinkage function. This extends the gelation time from the conventional 15-30 minutes to 45-75 minutes, providing a sufficient infusion process window and significantly improving the stability of the colloidal structure and the high-temperature float life. Detailed Implementation

[0027] In the following description, specific details such as particular system architectures and techniques are set forth for illustrative purposes and not for limitation, in order to provide a thorough understanding of the embodiments of this application. However, those skilled in the art will understand that this application may also be implemented in other embodiments without these specific details. In other instances, detailed descriptions of well-known systems, apparatuses, circuits, and methods have been omitted so as not to obscure the description of this application with unnecessary detail.

[0028] Example 1 An electrolyte comprises, by weight parts: 35.5 parts concentrated sulfuric acid (H2SO4), 57 parts deionized water, 5.2 parts fumed silica (SiO2), 0.28 parts polyacrylamide (PAM), 0.45 parts sodium carboxymethyl cellulose nanoparticles (CMC-Na), 0.4 parts phosphoric acid (H3PO4), 1.0 part sodium sulfate (Na2SO4), 0.17 parts boric acid (H3BO3), and 0.6 parts polyethylene glycol (PEG). Each part comprises 1 kg. The following examples and comparative examples are the same.

[0029] The preparation method of this electrolyte is as follows: Step 1: Preparation of CMC-Na pre-swelling solution.

[0030] Step 11: Take 23% of the formula amount of deionized water (calculated according to the total formula amount), place it in stainless steel mixing tank A, heat it to 75°C in a water bath, and slowly add the formula amount of nano carboxymethyl cellulose sodium (CMC-Na) under stirring conditions (stirring speed 250 rpm) for 4 minutes. Step 12: After all CMC-Na has been added, transfer the mixing vessel A to a high-speed disperser and disperse at 1000 rpm for 25 minutes until CMC-Na is completely dissolved and no visible particles remain, resulting in a transparent and uniform pre-swollen CMC-Na solution. Step 13: Allow the CMC-Na pre-swollen solution to cool naturally to below 38°C, then seal and store for later use.

[0031] Step 2: Preparation of sulfuric acid-phosphoric acid mixed solution.

[0032] Step 21: Take 33% of the formula amount of deionized water (calculated according to the total formula amount) and place it in acid-resistant glass reactor B. Place reactor B in an ice-water bath. When the water temperature inside the reactor drops to 12℃, start adding the formula amount of concentrated sulfuric acid (H2SO4) dropwise. Control the dropping rate so that the system temperature does not exceed 43℃.

[0033] Step 22: After all the concentrated sulfuric acid has been added, continue stirring (125 rpm) and cool to 30°C.

[0034] Step 23: Add the prescribed amount of phosphoric acid (H3PO4) to reactor B under stirring conditions, and continue stirring for 12 minutes until homogeneous to obtain a sulfuric acid-phosphoric acid mixed solution, which is then placed in a constant temperature environment of 30°C for later use.

[0035] Step 3: Pre-dispersion of fumed silica.

[0036] Step 31: Take the remaining deionized water and place it in stainless steel mixing tank C. Add the prescribed amounts of sodium sulfate (Na2SO4), boric acid (H3BO3), and polyethylene glycol (PEG, molecular weight 5000). Stir (180 rpm) until completely dissolved.

[0037] Step 32: Under stirring conditions (350 rpm), slowly add the amount of fumed silica in the formula to the mixing tank C. The addition time is 10 min. After all the silica has been added, increase the speed to 1800 rpm and disperse at high speed for 30 min to obtain the fumed silica pre-dispersion slurry.

[0038] Step 33: Place the mixing vessel C in an ultrasonic dispersion device at a frequency of 40kHz and a power density of 0.5W / cm³. 2 Under certain conditions, ultrasonic treatment was performed for 13 minutes to break down the agglomerates of fumed silica and make the dispersion more uniform. During the ultrasonic treatment, circulating cooling water was used to control the slurry temperature to not exceed 38℃.

[0039] Step 34: Under stirring conditions (400 rpm), slowly add dilute sulfuric acid (10% by mass) dropwise to the mixing tank C to adjust the pH value of the slurry to 4.8 (using a pH meter for online monitoring). During this process, control the system temperature to not exceed 38℃. After adjustment, continue stirring for 8 minutes to obtain a fumed silica stabilized slurry with pH=4.8, and place it in a constant temperature environment at 32℃ for later use.

[0040] Step 4: Premixing of the composite gelling system.

[0041] Step 41: Transfer the CMC-Na pre-swollen solution from mixing tank A in step one to mixing tank C after ultrasonic treatment in step three, and mix for 18 minutes under stirring conditions (600 rpm).

[0042] Step 42: Evenly sprinkle the prescribed amount of polyacrylamide (PAM) into mixing tank C at a rate of 7 g / min, while simultaneously increasing the stirring speed to 700 rpm and continuing to stir for 25 minutes until the PAM is completely dissolved, thus obtaining the composite gelling base. During this process, control the system temperature to not exceed 38℃ (if necessary, a circulating cooling water jacket can be used for cooling) to obtain the composite gelling base.

[0043] Step 5: Final preparation of colloidal electrolyte.

[0044] Step 51: Slowly add the sulfuric acid-phosphoric acid mixed solution from reaction vessel B in step 2 to batching vessel C under stirring (250 rpm) at a rate of 2.5 L / min (for 100 L batches). After all the solution has been added, continue stirring (500 rpm) for 40 min until a uniform colloidal dispersion system is formed.

[0045] Step 52: Stop stirring and degas the prepared colloidal electrolyte using a vacuum degassing device (vacuum degree -0.09MPa) for 13 minutes to remove the air bubbles trapped during stirring.

[0046] Step 53: Discharge the material to obtain the finished colloidal electrolyte.

[0047] The application of the above electrolyte in lead-acid gel batteries includes the following steps: ① The prepared gel electrolyte is injected into the formed lead-acid gel battery casing through a filling machine at an ambient temperature of 25℃. ② After filling, place the battery in a constant temperature room at 25°C for 6 hours to allow the colloidal electrolyte to fully gel. ③ After gelation is complete, recharge the battery (at 0.05C). 10 Charging with current for 2 hours makes the ion distribution in the electrolyte more uniform. ④ After recharging, the battery is sealed, cleaned, tested, and packaged according to standard procedures.

[0048] Example 2 An electrolyte comprises, by mass parts: 33 parts concentrated sulfuric acid (H2SO4), 60 parts deionized water, 4.5 parts fumed silica (SiO2), 0.40 parts polyacrylamide (PAM), 0.30 parts sodium carboxymethyl cellulose nanoparticles (CMC-Na), 0.50 parts phosphoric acid (H3PO4), 0.80 parts sodium sulfate (Na2SO4), 0.25 parts boric acid (H3BO3), and 0.4 parts polyethylene glycol (PEG).

[0049] The preparation method of this electrolyte is as follows: Step 1: Preparation of CMC-Na pre-swelling solution.

[0050] Step 11: Take 25% of the formula amount of deionized water (calculated according to the total formula amount), place it in stainless steel mixing tank A, heat it to 73°C in a water bath, and slowly add the formula amount of nano carboxymethyl cellulose sodium (CMC-Na) under stirring conditions (stirring speed 200 rpm) for 5 minutes.

[0051] After all CMC-Na is added in step 12, transfer the mixing tank A to a high-speed disperser and disperse it at a speed of 800 rpm for 30 minutes until CMC-Na is completely dissolved and there are no visible particles, resulting in a transparent and uniform CMC-Na pre-swollen liquid. Step 13: Allow the CMC-Na pre-swollen solution to cool naturally to below 35°C for later use. During the cooling process, seal the vessel opening with plastic wrap to prevent moisture evaporation.

[0052] Step 2: Preparation of sulfuric acid-phosphoric acid mixed solution.

[0053] Step 21: Take 30% of the formula amount of deionized water (calculated according to the total formula amount) and place it in acid-resistant glass reactor B. Place reactor B in an ice-water bath. When the water temperature inside the reactor drops below 10℃, start adding the formula amount of concentrated sulfuric acid (H2SO4) dropwise. Control the dropping rate so that the system temperature does not exceed 40℃.

[0054] After all the concentrated sulfuric acid has been added in step 22, continue stirring (150 rpm) and cool to 28°C.

[0055] Step 23: Add the prescribed amount of phosphoric acid (H3PO4) to reactor B under stirring conditions, and continue stirring for 10 minutes until homogeneous to obtain a sulfuric acid-phosphoric acid mixed solution, which is then placed in a constant temperature environment of 28°C for later use.

[0056] Step 3: Pre-dispersion of fumed silica.

[0057] Step 31: Take the remaining amount of deionized water (i.e., the total amount of the formula minus the amount of water used in steps one and two) and place it in a stainless steel mixing tank C. Add the amount of sodium sulfate (Na2SO4), boric acid (H3BO3), and polyethylene glycol (PEG, molecular weight 4000) as specified in the formula, and stir (150 rpm) until completely dissolved.

[0058] Step 32: Under stirring conditions (300 rpm), slowly add the amount of fumed silica in the formula to the mixing tank C. The addition time is 12 min. After all the silica has been added, increase the speed to 1500 rpm and disperse at high speed for 35 min to obtain the fumed silica pre-dispersed slurry.

[0059] Step 33: Place the mixing vessel C in an ultrasonic dispersion device at a frequency of 40kHz and a power density of 0.5W / cm³. 2 Under certain conditions, ultrasonic treatment was performed for 15 minutes to break down the agglomerates of fumed silica and make the dispersion more uniform. During the ultrasonic treatment, circulating cooling water was used to control the slurry temperature to not exceed 35℃.

[0060] Step 34: Under stirring conditions (300 rpm), slowly add dilute sulfuric acid (10% by mass) dropwise to the mixing tank C to adjust the pH value of the slurry to 4.5 (using a pH meter for online monitoring). During this process, control the system temperature to not exceed 40℃. After adjustment, continue stirring for 10 minutes to obtain a fumed silica stabilized slurry with pH≈4.5, and place it in a constant temperature environment at 30℃ for later use.

[0061] Step 4: Premixing of the composite gelling system.

[0062] Step 41: Transfer the CMC-Na pre-swollen solution from mixing tank A in step one to mixing tank C after ultrasonic treatment in step three, and mix for 20 minutes under stirring conditions (500 rpm).

[0063] Step 42: Evenly sprinkle the prescribed amount of polyacrylamide (PAM) into mixing tank C at a rate of 5 g / min, while simultaneously increasing the stirring speed to 600 rpm and continuing to stir for 30 minutes until the PAM is completely dissolved to obtain the composite gelling base. During this process, control the system temperature to not exceed 35℃ (if necessary, a circulating cooling water jacket can be used for cooling).

[0064] Step 5: Final preparation of colloidal electrolyte.

[0065] Step 51: Slowly add the sulfuric acid-phosphoric acid mixed solution from reaction vessel B in step 2 to batching vessel C under stirring (200 rpm) at a rate of 2 L / min (for 100 L batches). After all the solution has been added, continue stirring (400 rpm) for 45 min until a uniform colloidal dispersion system is formed.

[0066] Step 52: Stop stirring and degas the prepared colloidal electrolyte using a vacuum degassing device (vacuum degree -0.085MPa) for 15 minutes to remove the air bubbles that were trapped during stirring.

[0067] Step 53: Discharge the material to obtain the finished colloidal electrolyte.

[0068] The application of the above electrolyte in lead-acid gel batteries includes the following steps: ① The prepared gel electrolyte is injected into the formed lead-acid gel battery casing through a filling machine at an ambient temperature of 25℃. ② After filling, place the battery in a constant temperature room at 25°C for 6 hours to allow the colloidal electrolyte to fully gel. ③ After gelation is complete, recharge the battery (at 0.05C). 10 Charging with current for 2 hours makes the ion distribution in the electrolyte more uniform. ④ After recharging, the battery is sealed, cleaned, tested, and packaged according to standard procedures.

[0069] Example 3 An electrolyte comprises, by mass parts: 38 parts sulfuric acid (H2SO4), 54 parts deionized water, 6.5 parts fumed silica (SiO2), 0.20 parts polyacrylamide (PAM), 0.60 parts sodium carboxymethyl cellulose nanoparticles (CMC-Na), 0.30 parts phosphoric acid (H3PO4), 1.20 parts sodium sulfate (Na2SO4), 0.10 parts boric acid (H3BO3), and 0.8 parts polyethylene glycol (PEG).

[0070] The preparation method of this electrolyte is as follows: Step 1: Preparation of CMC-Na pre-swelling solution.

[0071] Step 11: Take 20% of the formula amount of deionized water (calculated according to the total formula amount), place it in stainless steel mixing tank A, heat it to 77°C in a water bath, and slowly add the formula amount of nano carboxymethyl cellulose sodium (CMC-Na) under stirring conditions (stirring speed 300 rpm) for 3 minutes.

[0072] After all CMC-Na is added in step 12, transfer the mixing tank A to a high-speed disperser and disperse it at a speed of 1200 rpm for 20 minutes until CMC-Na is completely dissolved and there are no visible particles, resulting in a transparent and uniform CMC-Na pre-swollen liquid. Step 13: Allow the CMC-Na pre-swollen solution to cool naturally to 40°C for later use. During the cooling process, seal the vessel opening with plastic wrap to prevent moisture evaporation.

[0073] Step 2: Preparation of sulfuric acid-phosphoric acid mixed solution.

[0074] Step 21: Take 35% of the formula amount of deionized water (calculated according to the total formula amount) and place it in acid-resistant glass reactor B. Place reactor B in an ice-water bath. When the water temperature inside the reactor drops below 15℃, start adding the formula amount of concentrated sulfuric acid (H2SO4) dropwise. Control the dropping rate so that the system temperature does not exceed 45℃.

[0075] After all the concentrated sulfuric acid has been added in step 22, continue stirring (100 rpm) and cool to 32°C.

[0076] Step 23: Add the prescribed amount of phosphoric acid (H3PO4) to reactor B under stirring conditions, and continue stirring for 15 minutes until homogeneous to obtain a sulfuric acid-phosphoric acid mixed solution, which is then placed in a constant temperature environment of 32°C for later use.

[0077] Step 3: Pre-dispersion of fumed silica.

[0078] Step 31: Take the remaining amount of deionized water (i.e., the total amount of the formula minus the amount of water used in steps one and two) and place it in a stainless steel mixing tank C. Add the amount of sodium sulfate (Na2SO4), boric acid (H3BO3), and polyethylene glycol (PEG, molecular weight 6000) as specified in the formula, and stir (200 rpm) until completely dissolved.

[0079] Step 32: Under stirring conditions (400 rpm), slowly add the amount of fumed silica in the formula to the mixing tank C for 8 minutes. After all the silica has been added, increase the speed to 2000 rpm and disperse at high speed for 25 minutes to obtain the fumed silica pre-dispersed slurry.

[0080] Step 33: Place the mixing vessel C in an ultrasonic dispersion device at a frequency of 40kHz and a power density of 0.5W / cm³. 2 Under certain conditions, ultrasonic treatment was performed for 10 minutes to break down the agglomerates of fumed silica and make the dispersion more uniform. During the ultrasonic treatment, circulating cooling water was used to control the slurry temperature to not exceed 35℃.

[0081] Step 34: Under stirring conditions (300 rpm), slowly add dilute sulfuric acid (10% by mass) dropwise to the mixing tank C to adjust the pH value of the slurry to 5.0 (using a pH meter for online monitoring). During this process, control the system temperature to not exceed 40℃. After adjustment, continue stirring for 5 minutes to obtain a fumed silica stabilized slurry with pH≈5.0, and place it in a constant temperature environment of 35℃ for later use.

[0082] Step 4: Premixing of the composite gelling system.

[0083] Step 41: Transfer the CMC-Na pre-swollen solution from mixing tank A in step one to mixing tank C after ultrasonic treatment in step three, and mix for 15 minutes under stirring conditions (700 rpm).

[0084] Step 42: Evenly sprinkle the prescribed amount of polyacrylamide (PAM) into the mixing tank C at a sprinkling rate of 8 g / min, while simultaneously increasing the stirring speed to 800 rpm and continuing to stir for 20 minutes until the PAM is completely dissolved to obtain the composite gelling base. During this process, control the system temperature to not exceed 40℃ (if necessary, a circulating cooling water jacket can be used for cooling).

[0085] Step 5: Final preparation of colloidal electrolyte.

[0086] Step 51: Slowly add the sulfuric acid-phosphoric acid mixed solution from reaction vessel B in step 2 to batching vessel C under stirring (300 rpm) at a rate of 3 L / min (for 100 L batches). After all the solution has been added, continue stirring (600 rpm) for 30 min until a uniform colloidal dispersion system is formed.

[0087] Step 52: Stop stirring and degas the prepared colloidal electrolyte using a vacuum degassing device (vacuum degree -0.095MPa) for 10 minutes to remove the air bubbles that were trapped during stirring.

[0088] Step 53: Discharge the material to obtain the finished colloidal electrolyte.

[0089] The application of the above electrolyte in lead-acid gel batteries includes the following steps: ① The prepared gel electrolyte is injected into the formed lead-acid gel battery casing through a filling machine at an ambient temperature of 25℃. ② After filling, place the battery in a constant temperature room at 25°C for 6 hours to allow the colloidal electrolyte to fully gel. ③ After gelation is complete, recharge the battery (at 0.05C). 10 Charging with current for 2 hours makes the ion distribution in the electrolyte more uniform. ④ After recharging, the battery is sealed, cleaned, tested, and packaged according to standard procedures.

[0090] Comparative Example 1 Compared to Example 1, Comparative Example 1 does not add CMC-Na, but remains the same as Example 1. Specifically, the preparation step of the CMC-Na pre-swelling solution is omitted in Comparative Example 1 (i.e., step one is completely deleted), while the remaining steps remain unchanged. In step two, 33% of the prescribed amount of deionized water is placed in reactor B, cooled to 12°C in an ice-water bath, and 98% concentrated sulfuric acid of the prescribed amount is added dropwise, controlling the system temperature to not exceed 43°C. After cooling to 30°C, 85% phosphoric acid of the prescribed amount is added, and the mixture is stirred for 12 minutes until homogeneous, yielding a sulfuric acid-phosphoric acid mixed solution for later use. In step three, 44% of the prescribed amount of deionized water is placed in mixing vessel C, and sodium sulfate, boric acid, and PEG of the prescribed amount are added. After stirring until completely dissolved, fumed silica of the prescribed amount is added within 10 minutes at 350 rpm, and the mixture is then dispersed at 1800 rpm for 30 minutes, ultrasonically treated for 12 minutes, and the pH is adjusted to 4.8 with 10% dilute sulfuric acid to obtain a PEG / SiO2 stabilized slurry for later use. In step four, the slurry obtained in step three is stirred at 700 rpm, and the formulated amount of PAM is added at a rate of 7 g / min. The mixture is stirred continuously for 25 minutes until completely dissolved, resulting in a gelling base material free of CMC-Na. Step five is performed as in step five of Example 1 to obtain the finished colloidal electrolyte.

[0091] Comparative Example 2 Compared to Example 1, Comparative Example 2 does not add PEG, but remains the same as Example 1. Specifically, in step three, the addition of PEG is omitted, as is the pH adjustment step with dilute sulfuric acid to 4.8; the remaining steps remain unchanged. Step one involves preparing the CMC-Na pre-swelling solution according to Step one of Example 1. Step two involves preparing the sulfuric acid-phosphoric acid mixed solution according to Step two of Example 1. In step three, 25.0 kg of the remaining deionized water is placed in mixing vessel C, and the prescribed amounts of sodium sulfate and boric acid (without PEG) are added. After stirring until completely dissolved, the prescribed amount of fumed silica is added within 10 minutes at 350 rpm. The mixture is then dispersed at 1800 rpm for 30 minutes, followed by ultrasonic treatment for 12 minutes. pH adjustment with dilute sulfuric acid is not performed, maintaining the naturally formed pH of boric acid at ≈5~6, resulting in a PEG-free SiO2 slurry for later use. In step four, the CMC-Na pre-swelling solution is transferred to mixing tank C, mixed at 600 rpm for 18 min, and then PAM is added at a rate of 7 g / min. The mixture is then stirred at 700 rpm for 25 min until completely dissolved, yielding a PEG-free gelling base. Step five is performed as in step five of Example 1.

[0092] Comparative Example 3 Compared to Example 1, Comparative Example 3 does not add PAM, but remains the same as Example 1. Specifically, the addition and dissolution of PAM in step four is omitted, while the remaining steps remain unchanged. Step one: Prepare the CMC-Na pre-swelling solution according to step one of Example 1. Step two: Prepare the sulfuric acid-phosphoric acid mixed solution according to step two of Example 1. Step three: Prepare the PEG / SiO2 stabilized slurry (pH=4.8) according to step three of Example 1. In step four, the CMC-Na pre-swelling solution is transferred to mixing tank C, mixed at 600 rpm for 18 min, and then the addition and dissolution of PAM are omitted. The CMC-Na / PEG / SiO2 composite system is directly used as the gelling base in step five. Step five is performed according to step five of Example 1 to obtain a PAM-free finished colloidal electrolyte.

[0093] Comparative Example 4 Compared to Example 1, Comparative Example 4 does not add CMC-Na and PAM, but remains the same as Example 1. Specifically, this comparative example omits the preparation of the CMC-Na pre-swelling solution (i.e., step one is completely removed) and the addition of PAM (the PAM sprinkling and dissolving operations are not performed in step four), while the remaining steps remain unchanged. In step two, 33% of the prescribed amount of deionized water is placed in reactor B, cooled to 12°C in an ice-water bath, and 98% concentrated sulfuric acid of the prescribed amount is added dropwise, controlling the system temperature to not exceed 43°C. After cooling to 30°C, 85% phosphoric acid of the prescribed amount is added, and the mixture is stirred for 12 minutes until homogeneous, yielding a sulfuric acid-phosphoric acid mixed solution for later use. In step three, 44% of the prescribed amount of deionized water is placed in mixing tank C, and the prescribed amounts of sodium sulfate, boric acid, and PEG are added. After stirring until completely dissolved, fumed silica is added within 10 minutes at 350 rpm, and the mixture is then dispersed at 1800 rpm for 30 minutes. The mixture is then ultrasonically treated for 12 minutes, and the pH is adjusted to 4.8 with 10% dilute sulfuric acid to obtain a PEG / SiO2 stabilized slurry for later use. In step four, the PEG / SiO2 stabilized slurry obtained in step three is directly used as the gelling base material in step five, without the addition of CMC-Na and PAM. Step five is performed as in step five of Example 1 to obtain a finished colloidal electrolyte without CMC-Na and PAM.

[0094] Comparative Example 5 Compared to Example 1, Comparative Example 5 does not add CMC-Na, PAM, or PEG, but remains the same as Example 1. Compared to Example 1, this comparative example omits the preparation of the CMC-Na pre-swelling solution (step one is completely removed), the addition of PEG (PEG is not added in step three), and the addition of PAM (PAM sprinkling and dissolving operations are not performed in step four). The pH adjustment step of dilute sulfuric acid to 4.8 is also omitted in step three, while the remaining steps remain unchanged. Step two involves preparing a sulfuric acid-phosphoric acid mixed solution according to step two of Example 1. In step three, 44% of the prescribed amount of deionized water is placed in mixing vessel C, and the prescribed amounts of sodium sulfate and boric acid (without PEG) are added. After stirring until completely dissolved, fumed silica is added within 10 minutes at 350 rpm, and the mixture is then dispersed at 1800 rpm for 30 minutes, followed by ultrasonic treatment for 12 minutes. The pH adjustment with dilute sulfuric acid is not performed, maintaining the naturally formed pH of boric acid at ≈5~6, resulting in a SiO2 slurry without any organic additives for later use. In step four, the SiO2 slurry obtained in step three is directly used as the gelling base material in step five, without adding any organic polymer components. Step five is operated as in step five of Example 1 to obtain a finished colloidal electrolyte that does not contain CMC-Na, PAM, and PEG, i.e., a pure fumed silica gel system.

[0095] Comparative Example 6 Compared to Example 1, Comparative Example 6 omits the preparation of the CMC-Na pre-swelling solution in step one. Instead, 0.45 parts of sodium carboxymethyl cellulose (CMC-Na) are directly added in powder form to mixing tank C (i.e., the PEG / SiO2 stabilized slurry obtained in step three, pH=4.8) in sub-step 41 of step four. 25% of deionized water is added in step 21, and 75% of deionized water is added in step 31. The specific operation is as follows: In sub-step 41 of step four, CMC-Na powder is evenly sprinkled into mixing tank C at a speed of approximately 4 g / min under a stirring speed of 600 rpm, and stirred continuously for 40 min until completely dissolved (based on visual observation of no undissolved particles). The system temperature is controlled to not exceed 38°C. The remaining steps (addition of PAM in steps two, three, and four, and step five) are exactly the same as in Example 1.

[0096] The detailed testing methods for various performance aspects of this invention are as follows: Gelation time: A rheometer method was used. The rheometer cylinder was kept at a constant temperature of 25±0.1℃, and 70 mL of fresh colloidal electrolyte was added along the cylinder wall. The gelation time was initially 800 s. -1 Pre-treatment at a constant shear rate for 1 min ensures consistent initial conditions, then the rate is switched to 0.5–1.0 s. -1 A constant shear rate was used to record the viscosity change over time. A viscosity-time curve was plotted, and the critical time point at which the viscosity suddenly increases is the gelation time. This method is based on the principle that the viscosity of the system increases when gaseous SiO2 forms a three-dimensional gel network.

[0097] Thixotropic recovery of the colloidal electrolyte: Thixotropic recovery was tested using a rotational rheometer. The colloidal electrolyte sample was kept at 25±2℃ and subjected to an application of [temperature value missing] for 10 s. -1 A constant high shear rate was continuously sheared for 5 min to simulate the infusion flow state and disrupt the gel network. After shearing was stopped, the gel was allowed to recover at rest for 30 min, during which the viscosity was measured intermittently in oscillating mode (strain ≤0.1%). Thixotropic recovery rate (%) = viscosity after 30 min recovery / initial viscosity × 100%.

[0098] Low-temperature capacity retention: Refer to the standard methods of GB / T 36280-2018 and GB / T 1833, step 21-2009. The battery was subjected to a 0.1C temperature at 25±2℃. 10 After fully charging, place the container in a -20±1℃ low-temperature chamber for 16~24 hours. Then, at -20℃, use a 0.1C... 10 Discharge the current to the termination voltage and record the low-temperature discharge capacity. Low-temperature capacity retention rate (%) = (-20℃ discharge capacity / 25℃ discharge capacity) × 100%.

[0099] 100% DOD cycle life: Refer to GB / T 36280-2018 standard. The battery operates at 25±2℃ with a 0.1C cycle life. 10 Fully charge with current, then at 0.1C. 10 Discharge the current to the termination voltage (10.5V / 12V per cell) and record the discharge capacity for each discharge. Terminate the test when the discharge capacity is lower than 80% of the rated capacity for three consecutive discharges. The cumulative number of cycles is the 100% DOD cycle life.

[0100] High-temperature float charge life: Refer to DL / T 637-2019 standard. Place the battery in a constant temperature chamber at 40±1℃ and continuously float charge at a constant voltage of 2.35V / cell (410V for 12V batteries in step 1). Perform capacity testing (0.1C) monthly. 10 Discharge to the termination voltage). When the capacity drops to 80% of the initial capacity, the test is terminated. The cumulative number of float charge days is the high-temperature float charge life.

[0101] Capacity retention after 90 days of rest: The battery was subjected to a 0.1C load at 25±2℃. 10 After fully charging, allow to stand in an open circuit for 90 days. After the standing period, inflate at 0.1C. 10 Discharge the current to the termination voltage and record the remaining capacity. Capacity retention rate (%) = (remaining capacity after 90 days / initial capacity) × 100%.

[0102] Colloidal cracking degree: After the cycle life test, the battery was dissected and the colloidal electrolyte block was removed. The crack morphology on the surface of the colloidal block was observed and photographed using a digital microscope (50~200x). The cracks were qualitatively graded according to their number, width and distribution characteristics: slight cracks (a few fine cracks), obvious cracks (multiple visible cracks), moderate cracks (network cracks), severe cracking (dense network cracks), and complete fragmentation (no intact structure).

[0103] Conductivity: Refer to GB / T 2024, step 53-2013, using the AC impedance method. Inject the colloidal electrolyte into a capillary conductivity cell (conductivity constant calibrated with KCl standard solution), maintain the temperature to 25±0.1℃, connect to an electrochemical workstation (e.g., Solartron 1174), and operate at 100 Hz~10 Hz. 6 A 10mV sinusoidal AC signal is applied within the Hz frequency range, and the AC impedance spectrum is measured. The intercept of the semicircle on the real axis from the analytical spectrum is the electrolyte resistance R. e Conductivity κ=K cell / R e .

[0104] Table 1 shows the performance test results for each embodiment and comparative example. Referring to Table 1, the gelation time in Example 1 was extended from the usual range of 25-30 minutes for conventional fumed silica gel systems to 62 minutes, with the gelation time window extended by approximately 107%-148%, providing ample process window for the infusion operation. The low-temperature capacity retention rate (65.8%) is approximately 19.6% higher than the discharge capacity requirement for low-temperature batteries in the communications industry—a discharge capacity of no less than 80%~90% of the rated capacity under low-temperature conditions, and approximately 55% for conventional gel batteries at -20℃. The cycle life (625 cycles) is better than the industry standard requirement of at least 900 cycles for valve-regulated sealed gel batteries used in communications, representing an improvement of approximately 48.8% compared to the typical value of around 420 cycles for conventional gel batteries. The high-temperature float life (390 days) is approximately 50% higher than the design benchmark of at least 10 years for room-temperature float life of communication gel batteries, and approximately 260 days for conventional products under accelerated aging at high temperatures. The thixotropic recovery rate (87%) is approximately 33.8% higher than the recovery rate of approximately 65% ​​for conventional SiO2 gel systems, and the degree of gel cracking has improved from "obvious cracks" to "slight cracks." Furthermore, all performance characteristics are the best among the three embodiments.

[0105] The formulation of Example 2 has the highest PAM content. The addition of PAM makes the three-dimensional network structure more compact, and the gelation time (55 min) is shorter than that of Example 1 but longer than the typical range of 25-30 minutes for conventional fumed silica gel systems. Due to the higher PAM content, the solution resistance and charge transfer resistance are increased, and the low-temperature capacity retention (61.2%), cycle life (582 cycles), and float charge life (372 days) are all lower than those of Example 1, but are still significantly better than the prior art's 55%, 420 cycles, and 260 days.

[0106] The formulation in Example 3 has the highest PEG content. The increased PEG content enhances the steric hindrance protection layer, and the crack resistance (mild cracking) is comparable to that of Example 1. However, due to the lowest PAM content, the gel network density decreases, and the gelation time (50 min) is the shortest among the three examples, but still better than the typical range of 25-30 minutes for conventional fumed silica gel systems.

[0107] Compared to Example 1, the thixotropic recovery rate of Comparative Example 1 decreased from 87% to 68%, a reduction of approximately 21.8%. The degree of colloid cracking after cycling deteriorated from "slight cracks" to "significant cracks." This is presumably related to the reduced structural reconstruction ability and anti-shrinkage ability of the colloid after shear failure due to the lack of CMC-Na's flexible network reinforcement. The high-temperature float life was thus reduced by approximately 11.5% (390 → 345 days), presumably due to the reduction in flexible segments of the gel network caused by the absence of CMC-Na, which cannot effectively buffer the stress caused by bubble disturbance and ion concentration changes during long-term cycling. However, the steric hindrance layer of PEG still played a role, and the low-temperature capacity retention rate (58.2%) and cycle life (540 cycles) were still superior to the prior art, indicating that PEG's acid shock protection is effective, but the absence of CMC-Na caused a significant drop in overall performance.

[0108] Compared to Example 1, the gelation time of Comparative Example 2 was shortened from 62 min to 40 min. This is presumably related to the weakened steric hindrance protection of SiO2 during the acid addition process in step five after the absence of PEG, leading to increased aggregation and sedimentation of CMC-Na due to strong acid impact, which is related to the disappearance of the gelation-retarding effect of PEG. The thixotropic recovery rate decreased from 87% to 72%, a decrease of approximately 17.2%, which is related to the reduced uniform structural units in the gel network that can participate in reversible hydrogen bond reconstruction due to the weakened steric hindrance protection of PEG and the increased aggregation and sedimentation of CMC-Na. The degree of colloid cracking was "moderate cracking," which is related to the increased aggregation of CMC-Na due to the absence of PEG, resulting in an uneven gel network and stress concentration leading to moderate cracking. The high-temperature float life decreased by approximately 41% in one step (390 → 335 days), which is related to the uneven colloid caused by the absence of PEG and accelerated drying at high temperatures. This indicates that the absence of PEG mainly affects long-term structural stability and resistance to drying shrinkage. However, due to the continued role of the flexible network of CMC-Na and the reversible crosslinking of PAM, the low-temperature capacity retention (60.5%) and cycle life (555 cycles) are still superior to existing technologies.

[0109] Compared to Example 1, the gelation time of Comparative Example 3 was drastically shortened to 42 min (a reduction of approximately 32.3%), presumably due to the loss of reversible hydrogen bond crosslinking caused by PAM deficiency, resulting in the direct and rapid association of SiO2 particles and a significant reduction in gelation time. The thixotropic recovery rate decreased to 65% (a reduction of approximately 53% in step 2), presumably due to the inability to establish a reversible hydrogen bond crosslinking network caused by PAM deficiency, leading to ineffective recovery of the structure after shearing. The significant decrease in thixotropic recovery rate and the reduction in high-temperature float life by approximately 16.7% (390 → 325 days) are presumably related to the loss of reversible crosslinking caused by PAM deficiency, the inability to effectively repair the colloidal network, and accelerated drying and cracking failure at high temperatures. Correspondingly, the degree of colloidal cracking worsened from "minor cracks" to "severe crazing." This indicates that PAM, as a reversible hydrogen bond crosslinking agent, is a key component in extending the gelation time window and endowing the colloid with crack resistance. The cycle life (495 cycles) is still improved compared to the prior art (approximately 420 cycles), but the improvement is significantly narrowed (from approximately 48.8% improvement in Example 1 to approximately 17.9% improvement). This is presumably because the battery lacks a reversible repair mechanism during long-term cycling after the PAM is missing.

[0110] Compared to Comparative Example 1, removing PAM from Comparative Example 1 (which already contained PEG and PAM, but lacked CMC-Na) shortened the gelation time from 52 min to 38 min (a decrease of approximately 26.9%). This is presumably related to the fact that PAM, even in the absence of CMC-Na, can still significantly delay gelation through hydrogen bonding with SiO2. The thixotropic recovery rate decreased from 68% to 61% (a decrease of approximately 10.3%), presumably related to the fact that PAM forms reversible hydrogen bonds with SiO2 through its amide groups, contributing additional crosslinking recovery points to the network and improving the thixotropic recovery rate. The high-temperature float charge lifetime decreased from 345 days to 310 days (a decrease of approximately 10.1%), and the degree of colloidal cracking worsened from "obvious cracks" to "severe cracking," presumably related to the fact that PAM still provides partial reversible hydrogen bonding and crack resistance protection even in the absence of CMC-Na. The cycle life decreased from 540 cycles to 480 cycles (a decrease of approximately 11.1%), which is presumably related to the fact that PAM buffers cyclic stress and delays colloidal structure degradation through a reversible hydrogen bond cross-linking network, thereby extending the cycle life.

[0111] Compared to Comparative Example 3, removing CMC-Na from Comparative Example 3 (which already contained PEG and CMC-Na, but no PAM) reduced the gelation time from 42 min to 38 min (a decrease of approximately 9.5%). This is presumably related to the physical inhibition and entanglement of the long CMC-Na chains between SiO2 particles, delaying direct particle association and thus postponing gelation. The thixotropic recovery rate decreased from 65% to 61% (a decrease of approximately 6.2%), presumably related to the flexible entanglement and spatial inhibition of the long CMC-Na chains, providing additional physical crosslinking points for the network and assisting in hydrogen bond reconstruction. The high-temperature float charge lifetime decreased from 325 days to 310 days (a decrease of approximately 4.6%), and the cycle life decreased from 495 cycles to 480 cycles (a decrease of approximately 3.0%), with relatively small degradation. This is presumably related to the fact that CMC-Na mainly provides flexible resistance to shrinkage, but the gel framework and hydrogen bond crosslinking are still maintained by SiO2 and PAM, thus the impact of its absence is limited. The degree of colloidal cracking deteriorated from "moderate cracking" to "severe cracking," which is presumably related to the flexible long chains of CMC-Na interpenetrating between SiO2 particles, buffering local stress and delaying crack initiation through steric hindrance and physical entanglement.

[0112] Referring to Table 1, in Comparative Example 5, compared to Comparative Example 4, further removal of PEG shortened the gelation time from 38 min to 26 min (a decrease of approximately 31.6%). This is presumably related to the disappearance of PEG steric hindrance, allowing SiO2 particles to directly and rapidly associate, thus significantly reducing the gelation time. The thixotropic recovery rate decreased from 61% to 52% (a decrease of approximately 14.8%), presumably related to the PEG steric hindrance assisting particle redispersement, providing physical crosslinking points, and promoting partial reconstruction of the network after shearing. The high-temperature float charge lifetime decreased from 310 days to 250 days (a decrease of approximately 19.4%), and the degree of colloidal cracking worsened from "severe cracking" to "complete fragmentation." This is presumably related to the PEG steric hindrance layer delaying SiO2 aggregation, buffering stress concentration, and effectively inhibiting the propagation of drying shrinkage cracks. Cycle life decreased from 480 cycles to 400 cycles (a decrease of approximately 16.7%), and low-temperature capacity retention decreased from 55.0% to 50.2% (a decrease of approximately 8.7%). This is presumably related to the steric hindrance of PEG maintaining the uniformity and stability of the gel network, reducing local failures, and thus improving cycling and low-temperature performance. Overall, the degradation in gelation time (a decrease of 31.6%) and high-temperature float life (a decrease of 19.4%) was the most significant. This is presumably related to the main role of PEG steric hindrance in delaying gelation and inhibiting drying cracking, further demonstrating the important role of PEG in this invention.

[0113] Compared to Example 1, the gelation time of Comparative Example 6 decreased (62→55 min), presumably due to the weakened physical inhibition effect of CMC-Na caused by decreased dispersion uniformity. This is because complete dissolution of conventional CMC-Na requires 10-20 hours of static swelling treatment, and 30-40 minutes of stirring is insufficient to allow the molecular chains to fully extend to their optimal state. Some CMC-Na may exist in a more coiled conformation, with lower extensibility and flexibility, thus reducing its coating efficiency on SiO2 particles. The decrease in thixotropic recovery rate (87%→74%) is presumably related to the reduced auxiliary effect of the flexible network of CMC-Na on hydrogen bond reconstruction due to insufficient molecular chain extension. The decrease in high-temperature float life and cycle life is also presumably related to the direct correlation between the degree of CMC-Na's anti-drying shrinkage function and the extension state of the molecular chains—pre-swelling allows the CMC-Na molecular chains to be fully hydrated, more effectively interpenetrating in the gaps of the SiO2 network, buffering local stress and inhibiting crack propagation. Compared to Comparative Example 1, the degree of colloid cracking changed from obvious cracks to slight cracks, which is presumably related to the increased structural reconstruction ability and colloid resistance to drying shrinkage after shear failure following the reinforcement effect of the flexible network of some CMC-Na.

[0114] In the above embodiments, the descriptions of each embodiment have different focuses. For parts that are not described in detail or recorded in a certain embodiment, please refer to the relevant descriptions of other embodiments.

[0115] Those skilled in the art will recognize that the units and algorithm steps of the various examples described in conjunction with the embodiments disclosed herein can be implemented in electronic hardware, or a combination of computer software and electronic hardware. Whether these functions are implemented in hardware or software depends on the specific application and design constraints of the technical solution. Those skilled in the art can use different methods to implement the described functions for each specific application, but such implementation should not be considered beyond the scope of this application.

Claims

1. An electrolyte, characterized in that, The composition by weight is as follows: 33-38 parts concentrated sulfuric acid, 54-60 parts deionized water, 4.5-6.5 parts fumed silica, 0.20-0.40 parts polyacrylamide, 0.30-0.60 parts nano-carboxymethyl cellulose sodium, 0.30-0.50 parts phosphoric acid, 0.80-1.20 parts sodium sulfate, 0.10-0.25 parts boric acid, and 0.4-0.8 parts polyethylene glycol.

2. The electrolyte as described in claim 1, characterized in that, The composition by weight includes 35.5 parts concentrated sulfuric acid, 57 parts deionized water, 5.2 parts fumed silica, 0.28 parts polyacrylamide, 0.45 parts nano-carboxymethyl cellulose sodium, 0.4 parts phosphoric acid, 1.0 part sodium sulfate, 0.17 parts boric acid, and 0.6 parts polyethylene glycol.

3. The electrolyte as described in claim 1, characterized in that, The molecular weight of the polyethylene glycol is 4000-6000.

4. A method for preparing an electrolyte, characterized in that, Includes the following steps: Step 1: Prepare nano-carboxymethyl cellulose sodium pre-swelling solution; Step 2: Prepare a sulfuric acid-phosphoric acid mixed solution; Step 3: Pre-dispersion of fumed silica; Step 4: Add the pre-swollen sodium carboxymethyl cellulose nano solution to the fumed silica pre-dispersion solution for pre-mixing, and then add polyethylene glycol and polyacrylamide; Step 5: Add the sulfuric acid-phosphoric acid mixture to the composite gelling base material from Step 4, so that the dispersed fumed silica associates into a three-dimensional network framework and enhances the reversible hydrogen bond bridging between different components of the gel system.

5. The method for preparing an electrolyte as described in claim 4, characterized in that, Step one includes the following sub-steps: Step 11: Heat deionized water in a water bath and add the prescribed amount of sodium carboxymethyl cellulose under stirring conditions; After all the nano-carboxymethyl cellulose sodium was added in step 12, the solution was stirred and dispersed until the nano-carboxymethyl cellulose sodium was completely dissolved and there were no visible particles, resulting in a transparent and uniform nano-carboxymethyl cellulose sodium pre-swelling solution. Step 13: Allow the pre-swollen solution of nano-carboxymethyl cellulose sodium to cool naturally and stand for at least 20 hours before use.

6. The method for preparing an electrolyte as described in claim 4, characterized in that, Step two includes the following sub-steps: Step 21: Place deionized water in an ice-water bath and cool it to below 15°C. Add the prescribed amount of concentrated sulfuric acid dropwise, controlling the dropping rate so that the system temperature does not exceed 45°C. After all the concentrated sulfuric acid has been added in step 22, continue stirring and cool to 30℃±2℃; Step 23: Add the prescribed amount of phosphoric acid to reactor B under stirring conditions, and continue stirring until homogeneous to obtain a sulfuric acid-phosphoric acid mixed solution.

7. The method for preparing an electrolyte as described in claim 4, characterized in that, Step 3 includes the following sub-steps: Step 31: Add the prescribed amounts of sodium sulfate, boric acid, and polyethylene glycol to deionized water and stir until completely dissolved; Step 32: Under stirring conditions, slowly add the formulated amount of fumed silica to the solution in sub-step 31. After all the silica has been added, stir and disperse to obtain a fumed silica pre-dispersion slurry. Step 33: Place the pre-dispersed fumed silica slurry in an ultrasonic dispersion device and perform ultrasonic dispersion treatment to break up the agglomerates of fumed silica. During the ultrasonic treatment, control the slurry temperature to not exceed 40°C. In step 34, under stirring conditions, dilute sulfuric acid is slowly added dropwise to the slurry after ultrasonic treatment in step 33 to adjust the pH value of the slurry to 4.5~5.

0. During this process, the system temperature is controlled not to exceed 40℃. After the adjustment is completed, stirring is continued to obtain a fumed silica stabilized slurry with pH=4.5~5.0, which is then placed in a constant temperature environment of 30~35℃ for later use.

8. The method for preparing an electrolyte as described in claim 4, characterized in that, Step four includes the following sub-steps: Step 41: Transfer the nano-carboxymethyl cellulose sodium pre-swelling solution from Step 1 to the pre-dispersed slurry of fumed silica from Step 3, and mix them evenly under stirring conditions. Step 42: Evenly sprinkle the formulated amount of polyacrylamide into the mixed solution of sub-step 41, increase the stirring speed, and continue stirring until PAM is completely dissolved to obtain a ternary composite gelling base material containing a preliminary network aggregate of fumed silica, a flexible network of nano-carboxymethyl cellulose sodium, and a reversible hydrogen bond cross-linked network between polyacrylamide, fumed silica, and nano-carboxymethyl cellulose sodium.

9. The method for preparing an electrolyte as described in claim 4, characterized in that, Step five includes the following sub-steps: Step 51: Add the sulfuric acid-phosphoric acid mixed solution from Step 2 to the ternary composite gelling base material from Sub-Step 42 under stirring conditions. After all the solution is added, continue stirring until a uniform colloidal dispersion system is formed. Step 52: Stop stirring and perform vacuum degassing of the prepared colloidal electrolyte to remove air bubbles trapped during stirring. Step 53 discharges the material to obtain the finished colloidal electrolyte.

10. The application of the electrolyte as described in any one of claims 1-3 in a lead-acid gel battery, comprising the following steps: ① The prepared gel electrolyte is injected into the formed lead-acid gel battery casing through a filling machine. The filling environment temperature is 25℃±3℃. ② After filling, place the battery in a constant temperature room at 25℃±2℃ for 6 hours to allow the colloidal electrolyte to fully gel. ③ After gelation is complete, recharge the battery at 0.05C. 10 Charging with current for 2 hours makes the ion distribution in the electrolyte more uniform; ④ After recharging, the battery is sealed, cleaned, tested, and packaged according to standard procedures.