An aqueous sodium-ion battery electrolyte, its preparation method and application, and sodium-ion batteries.
By constructing a localized water-repellent layer using sodium acetate, potassium acetate, or ammonium acetate and anionic surfactants in aqueous sodium-ion batteries, the problems of limited electrochemical window and cathode compatibility were solved, enabling the application of efficient and stable electrolytes, reducing costs and improving battery performance.
Patent Information
- Application Number
- CN202611130372.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing aqueous sodium-ion batteries have limited electrochemical windows, and high-concentration acetate electrolytes lead to cathode compatibility issues and poor ion transport. Furthermore, the materials are expensive or toxic.
Sodium acetate and potassium acetate or ammonium acetate are used as the first solute, and anionic surfactants are used as the second solute. A local water-repellent layer is constructed by limiting the total acetate concentration and electrostatic adsorption to inhibit the dissolution of transition metals. This method uses bulk industrial materials.
This invention achieves a wide electrochemical window, high stability, low cost, and environmentally friendly electrolyte, which suppresses the dissolution of transition metals in the positive electrode and improves the long-term stability and ion transport efficiency of the battery.
Smart Images

Figure CN123120918A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion battery technology, and more particularly to an aqueous sodium-ion battery electrolyte, its preparation method and application, and sodium-ion batteries. Background Technology
[0002] Aqueous sodium-ion batteries have attracted significant attention in the field of large-scale energy storage due to their intrinsic safety and the availability and low cost of raw materials. However, this system faces a key bottleneck: the stable electrochemical window of water is approximately 1.23 V, which severely limits the battery's operating voltage and energy density. To overcome this limitation, researchers have proposed a high-concentration electrolyte strategy to significantly reduce free water molecules in the system, thereby effectively suppressing water activity and decomposition reactions. However, sodium salts with high solubility and the ability to act as independent supporting electrolytes, such as sodium perchlorate and sodium trifluoromethanesulfonate, are limited in their widespread use in aqueous sodium batteries due to their high cost or potential hazards.
[0003] Acetates are considered ideal electrolyte candidates due to their low cost and environmental friendliness. However, sodium acetate alone has relatively limited solubility in water, making it impossible to construct an electrochemical window sufficient for adequate ion intercalation / deintercalation reactions in both positive and negative electrode materials. To address this, some studies have proposed using a mixture of multiple acetates to increase the total salt concentration and thus expand the window. However, this high-concentration strategy still has room for improvement. A slightly alkaline chemical environment can pose challenges to the compatibility of the positive and negative electrodes, and high salt concentrations are typically accompanied by high viscosity, which is detrimental to efficient ion transport at the interface. Therefore, there is an urgent need in this field for an electrolyte solution that can be applied to practical applications without sacrificing the low-cost advantage of acetates. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides an aqueous sodium-ion battery electrolyte, its preparation method, and its application, as well as a sodium-ion battery. The aqueous sodium-ion battery electrolyte of this invention comprises: water, a first solute, and a second solute. The first solute includes sodium acetate (used to provide sodium ions as charge carriers) and at least one of potassium acetate or ammonium acetate (both have room temperature solubility > 20 mol / kg, increasing the overall salt concentration). The second solute is an anionic surfactant (specifically inhibiting the dissolution of transition metals at the positive electrode). This invention uses a limited total acetate concentration (20~33 mol / kg) to maintain a sufficiently wide electrochemical window and is in a liquid state, which is beneficial for maintaining high conductivity and long-term battery stability. This invention utilizes the electrostatic adsorption of the anionic surfactant at the positive electrode and constructs a localized water-repellent layer through hydrophobic tail chains to inhibit the dissolution of transition metals induced by water molecules (specifically solving the application problem of high-concentration acetate electrolytes). The materials used in this invention are all bulk industrial products, do not contain toxic or expensive elements, and have economic and environmental advantages.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] In a first aspect, the present invention provides an aqueous sodium-ion battery electrolyte, comprising: water, a first solute, and a second solute;
[0007] The first solute is acetate;
[0008] The acetate includes a first acetate and a second acetate; the first acetate is sodium acetate, and the second acetate includes at least one of potassium acetate or ammonium acetate;
[0009] Based on water as a solvent, the concentration of sodium acetate in the electrolyte is 3~10 mol / kg, the concentration of the second acetate is 10~25 mol / kg, and the concentration of total acetate is 20~33 mol / kg;
[0010] The second solute is an anionic surfactant.
[0011] Preferably, the anionic surfactant has the general formula RX. - M + ;
[0012] Wherein, R is an alkyl group having 8 to 18 carbon atoms;
[0013] The X - Selected from any one of sulfate, sulfonate, or benzenesulfonate;
[0014] The M + It is selected from any one of sodium ions, potassium ions, or ammonium ions.
[0015] Preferably, the concentration of the anionic surfactant in the electrolyte is 0.1 to 3 times its critical micelle concentration in pure water at room temperature.
[0016] Preferably, the anionic surfactant is at least one of sodium dodecyl sulfate, sodium dodecyl sulfonate, and sodium dodecylbenzene sulfonate.
[0017] Preferably, the concentration of sodium acetate in the electrolyte is 5-8 mol / kg;
[0018] The concentration of the second acetate in the electrolyte is 18~20 mol / kg.
[0019] Preferably, the concentration of the anionic surfactant in the electrolyte is 0.5 to 1.5 times its critical micelle concentration in pure water at room temperature.
[0020] Secondly, the present invention also provides a method for preparing the aqueous sodium-ion battery electrolyte, comprising the following steps:
[0021] The first and second solutes are added to water and stirred to obtain an aqueous sodium-ion battery electrolyte.
[0022] Thirdly, the present invention also provides the application of the aqueous sodium-ion battery electrolyte or the aqueous sodium-ion battery electrolyte prepared by the preparation method described above in the preparation of sodium-ion batteries.
[0023] Fourthly, the present invention also provides a sodium-ion battery, comprising the aqueous sodium-ion battery electrolyte described above or the aqueous sodium-ion battery electrolyte prepared by the preparation method described above.
[0024] Preferably, the sodium-ion battery further includes a positive electrode, a negative electrode, and a separator, wherein the positive electrode active material used in the positive electrode includes at least one of Prussian blue analogues and transition metal oxides;
[0025] The active material used in the negative electrode is NASICON-type phosphate.
[0026] The aqueous sodium-ion battery electrolyte, its preparation method, and its application of the present invention have the following advantages over the prior art:
[0027] The aqueous sodium-ion battery electrolyte of the present invention comprises: water, a first solute, and a second solute; the first solute comprises sodium acetate (used to provide sodium ions as charge carriers) and at least one of potassium acetate or ammonium acetate, and the second solute is an anionic surfactant (specifically inhibiting the dissolution of transition metals at the positive electrode); the electrolyte of the present invention uses a limited total acetate concentration (20~33 mol / kg) to maintain a sufficiently wide electrochemical window and is in a liquid state, which is beneficial for maintaining high conductivity and long-term battery stability; the present invention utilizes the electrostatic adsorption of anionic surfactants on the positive electrode and constructs a localized water-repellent layer through hydrophobic tail chains to inhibit the dissolution of transition metals induced by water molecules (specifically solving the application problem of high-concentration acetate electrolytes); the materials used in the present invention are all bulk industrial products, do not contain toxic or expensive elements, and have economic and environmental advantages. Attached Figure Description
[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0029] Figure 1 LSV curves of aqueous sodium-ion battery electrolytes in Examples 1 and Comparative Examples 1-3;
[0030] Figure 2 The cycle performance curves of the aqueous sodium-ion batteries in Comparative Examples 2-3 and Example 1 are shown.
[0031] Figure 3 Charge-discharge curves (cycle 100) of the aqueous sodium-ion batteries in Comparative Example 3 and Example 1.
[0032] Figure 4 The Fe and Mn content in the electrolyte of the aqueous sodium-ion batteries in Comparative Example 3 and Example 1 after 1000 cycles. Detailed Implementation
[0033] The present invention will now be clearly and completely described with reference to specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0034] This invention provides an aqueous sodium-ion battery electrolyte, comprising: water, a first solute, and a second solute;
[0035] The first solute is acetate;
[0036] Acetates include first acetate and second acetate; the first acetate is sodium acetate (used to provide sodium ions as charge carriers), and the second acetate includes at least one of potassium acetate or ammonium acetate (both have a room temperature solubility of >20 mol / kg, increasing the overall salt concentration);
[0037] Using water as a solvent, the concentration of sodium acetate in the electrolyte is 3~10 mol / kg (to maintain sufficient carrier concentration), the concentration of second acetate in the electrolyte is 10~25 mol / kg, and the total acetate concentration in the electrolyte is 20~33 mol / kg; that is, 1 kg of water contains 3~10 mol of sodium acetate, 10~25 mol of second acetate, and 20~33 mol of total acetate.
[0038] The second solute is an anionic surfactant (specifically inhibiting the dissolution of transition metals at the positive electrode).
[0039] The aqueous sodium-ion battery electrolyte of this invention uses a limited total acetate concentration of 20-33 mol / kg (above 20 mol / kg, the expanded electrochemical window is still insufficient to support the application of the positive and negative electrodes; above 33 mol / kg, the electrolyte may deviate from the homogeneous liquid region, resulting in problems such as stratification and solidification). This maintains a sufficiently wide electrochemical window and is in a liquid state, which is beneficial for maintaining high conductivity and long-term battery stability. This invention utilizes the electrostatic adsorption of anionic surfactants on the positive electrode and constructs a localized water-repellent layer through hydrophobic tail chains to inhibit the dissolution of transition metals induced by water molecules (specifically solving the application problems of high-concentration acetate electrolytes). The materials used in this invention are all bulk industrial products, do not contain toxic or expensive elements, and have economic and environmental advantages.
[0040] In some embodiments, the general formula of the anionic surfactant is RX. - M + ;
[0041] R is an alkyl group with 8 to 18 carbon atoms, forming a hydrophobic end (if the carbon chain is short, the hydrophobic effect is insufficient; if the carbon chain is long, the solubility decreases significantly, and it precipitates in high-concentration salt solutions).
[0042] X - It represents a hydrophilic group, selected from any one of sulfate, sulfonate or benzenesulfonate (the group itself has a certain antioxidant property and strong stability).
[0043] M + The cation is selected from any one of sodium, potassium, or ammonium ions (to maintain consistency with the cations in the mixed acetate and not introduce additional cations that would cause interference).
[0044] In some embodiments, the concentration of anionic surfactant in the electrolyte is 0.1 to 3 times its critical micelle concentration (CMC) in pure water at room temperature. Specifically, the amount of anionic surfactant added to the electrolyte is between 0.1 and 3 times its CMC in pure water at room temperature (25°C). If the concentration is less than 0.1 times, the concentration in the electrolyte is too low, making it difficult to form a sufficient adsorption layer to protect the positive electrode, and the improvement effect is not significant. If the concentration is greater than 3 times, in high-salt-concentration systems, salting out may disrupt the homogeneity of the system, causing phase separation and other problems, affecting ion transport. Considering that the CMC changes with ionic strength when surfactants are used in high-concentration electrolytes, the CMC measured in pure water provides a clear reference. Within this concentration range, surfactants mostly exist in the form of molecules or small aggregates, do not significantly change the macroscopic state of the electrolyte, and at the same time play an adsorption role, repelling water molecules from attacking transition metals.
[0045] In some embodiments, the anionic surfactant is at least one of sodium dodecyl sulfate, sodium dodecyl sulfonate, and sodium dodecylbenzene sulfonate.
[0046] In some embodiments, the concentration of sodium acetate in the electrolyte is 5-8 mol / kg;
[0047] The concentration of second acetate in the electrolyte is 18~20 mol / kg.
[0048] In some embodiments, the concentration of anionic surfactant in the electrolyte is 0.5 to 1.5 times its critical micelle concentration in pure water at room temperature.
[0049] Based on the same inventive concept, the present invention also provides a method for preparing the above-mentioned aqueous sodium-ion battery electrolyte, comprising the following steps:
[0050] The first and second solutes are added to water and stirred to obtain an aqueous sodium-ion battery electrolyte.
[0051] Specifically, the first and second solutes are added to water, stirred at 60-80°C for 1-2 hours, and then naturally cooled at room temperature for 12 hours to obtain an aqueous sodium-ion battery electrolyte.
[0052] Based on the same inventive concept, the present invention also provides an application of the above-mentioned aqueous sodium-ion battery electrolyte or the aqueous sodium-ion battery electrolyte prepared by the above-described preparation method in the preparation of sodium-ion batteries.
[0053] Based on the same inventive concept, the present invention also provides a sodium-ion battery, comprising the aqueous sodium-ion battery electrolyte described above or the aqueous sodium-ion battery electrolyte prepared by the preparation method described above.
[0054] In some embodiments, the sodium-ion battery further includes a positive electrode, a negative electrode, and a separator, wherein the positive electrode active material used in the positive electrode includes at least one of Prussian blue analogues and transition metal oxides.
[0055] The active material used in the negative electrode is a NASICON-type phosphate, such as sodium titanium phosphate NaTi2(PO4)3, carbon-coated sodium titanium phosphate, etc.; the separator can be a glass fiber separator, a polypropylene nonwoven separator, etc.
[0056] The following detailed embodiments further illustrate the aqueous sodium-ion battery electrolyte, its preparation method, its application, and sodium-ion batteries of the present invention. This section further explains the content of the present invention in conjunction with specific embodiments, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods, and equipment used in the present invention are conventional reagents, methods, and equipment in the art.
[0057] In the following examples and comparative examples, Prussian blue analogue Na... x The preparation method of MnFe(CN)6 includes the following steps:
[0058] S1. Dissolve 3 mmol MnSO4·H2O and 3 mmol sodium citrate dihydrate Na3C6H5O7·2H2O in 150 mL of deionized water to obtain solution A;
[0059] S2. Dissolve 3 mmol of Na4Fe(CN)6·10H2O in 150 mL of deionized water to obtain solution B;
[0060] S3. Under an argon atmosphere, at 60°C, solution A was added dropwise to solution B at a rate of 0.5 mL / min. After the addition was complete, the mixture was stirred at 60°C for 24 h, then allowed to cool naturally to room temperature (25°C). The mixture was then allowed to stand at room temperature for 3 h, centrifuged, and the resulting precipitate was washed successively with deionized water and anhydrous ethanol. Finally, it was vacuum dried at 80°C for 12 h to obtain the Prussian blue analog Na. x MnFe(CN)6.
[0061] The preparation methods of carbon-coated sodium titanium phosphate materials in the following examples and comparative examples include the following steps:
[0062] Sodium bicarbonate, ammonium dihydrogen phosphate, and anatase titanium dioxide powder were used as raw materials. The sodium, titanium, and phosphorus content was added to a mixture of ethanol and water (volume ratio of ethanol to water was 1:10) in a molar ratio of 1:2:3. The mass ratio of all raw material powders to the ethanol and water mixture was 30:70. Polyvinylpyrrolidone was selected as a dispersant, added at 1 wt.% of the powder. The mixture was ball-milled at high speed (200 rpm) for 2 hours to obtain a uniform slurry. Conductive carbon black (to a mass fraction of 20%) was added to the slurry, and the mixture was further ball-milled at 200 rpm for 2 hours before being poured out. The resulting slurry was spray-dried at an inlet air temperature of 220℃ and an outlet air temperature of 110℃, and the resulting spherical powder precursor was collected. The precursor was placed in a sintering furnace filled with inert gas (argon) and sintered at 750℃ under an argon atmosphere for 10 hours to obtain carbon-coated sodium titanium phosphate material.
[0063] Example 1
[0064] This embodiment provides an aqueous sodium-ion battery electrolyte, which is prepared as follows: 11.48 g of anhydrous sodium acetate, 35.33 g of anhydrous potassium acetate, and 47.3 mg of sodium dodecyl sulfate (fully ground in a mortar) are weighed and placed in a beaker. 20.00 g of deionized water (18 mol / kg potassium acetate + 7 mol / kg sodium acetate + 1 times CMC sodium dodecyl sulfate) is added, and the mixture is placed on a magnetic stirrer, heated to 60°C, and stirred thoroughly for 2 hours until completely dissolved. The mixture is then allowed to cool naturally at room temperature for more than 12 hours to obtain the aqueous sodium-ion battery electrolyte.
[0065] This embodiment also provides an aqueous sodium-ion battery including the aqueous sodium-ion battery electrolyte, positive electrode, negative electrode and separator prepared in Example 1;
[0066] The preparation method of the positive electrode is as follows: The positive electrode active material, Prussian blue analogue Na... x MnFe(CN)6, conductive carbon black (SuperP), and binder (PVDF) were ground uniformly in a mass ratio of 70:15:15. The organic solvent N-methylpyrrolidone was added to the mixture to obtain a positive electrode slurry (solid content controlled at 40%, meaning the sum of the mass fractions of the positive electrode active material, conductive carbon black, and binder in the positive electrode slurry was 40%). The positive electrode slurry was coated onto a titanium mesh and vacuum dried at 80℃ for 12 h to obtain the positive electrode.
[0067] The negative electrode is prepared as follows: carbon-coated sodium titanium phosphate material, conductive carbon black (SuperP), and binder (PVDF) are ground uniformly in a mass ratio of 70:15:15. The organic solvent N-methylpyrrolidone is added to the mixture to obtain a negative electrode slurry (the solid content is controlled at 40%, meaning the sum of the mass fractions of the negative electrode active material, conductive carbon black, and binder in the positive electrode slurry is 40%). The negative electrode slurry is coated onto a titanium mesh and vacuum dried at 80℃ for 12 h to obtain the negative electrode.
[0068] Among them, the coating amount of positive electrode slurry and negative electrode slurry is controlled so that the mass ratio of positive electrode active material to negative electrode active material is 1.2:1;
[0069] The diaphragm is a glass fiber diaphragm;
[0070] The 20 mL aqueous sodium-ion battery electrolyte, positive electrode, negative electrode, and separator prepared in Example 1 were assembled into an aqueous sodium-ion battery.
[0071] Comparative Example 1
[0072] This comparative example provides an aqueous sodium-ion battery electrolyte, which is prepared as follows: 13.12 g of anhydrous sodium acetate and 15.70 g of anhydrous potassium acetate are weighed and placed in a beaker, and 20.00 g of deionized water (8 mol / kg potassium acetate + 8 mol / kg sodium acetate, total concentration 16 mol / kg) is added. The beaker is placed on a magnetic stirrer, heated to 60°C, and stirred thoroughly for 2 hours until completely dissolved. The mixture is then allowed to cool naturally at room temperature for more than 12 hours to obtain the aqueous sodium-ion battery electrolyte.
[0073] This comparative example also provides an aqueous sodium-ion battery, which is the same as Example 1, except that the electrolyte used is the aqueous sodium-ion battery electrolyte prepared in Comparative Example 1.
[0074] Comparative Example 2
[0075] This comparative example provides an aqueous sodium-ion battery electrolyte, which is prepared as follows: 13.12 g of anhydrous sodium acetate and 54.96 g of anhydrous potassium acetate are weighed and placed in a beaker, and 20.00 g of deionized water (28 mol / kg potassium acetate + 8 mol / kg sodium acetate, total concentration 36 mol / kg) is added. The beaker is placed on a magnetic stirrer, heated to 60°C, and stirred thoroughly until completely dissolved. The mixture is then allowed to cool naturally at room temperature for more than 12 hours to obtain the aqueous sodium-ion battery electrolyte.
[0076] This comparative example also provides an aqueous sodium-ion battery, which is the same as Example 1, except that the electrolyte used is the aqueous sodium-ion battery electrolyte prepared in Comparative Example 2.
[0077] Comparative Example 3
[0078] This comparative example provides an aqueous sodium-ion battery electrolyte, which is prepared as follows: 11.48 g of anhydrous sodium acetate and 35.33 g of anhydrous potassium acetate are weighed and placed in a beaker, and 20.00 g of deionized water (18 mol / kg potassium acetate + 7 mol / kg sodium acetate) is added. The mixture is placed on a magnetic stirrer, heated to 60°C, and stirred thoroughly until completely dissolved. The mixture is then allowed to cool naturally at room temperature for more than 12 hours to obtain the aqueous sodium-ion battery electrolyte.
[0079] This comparative example also provides an aqueous sodium-ion battery, which is the same as Example 1, except that the electrolyte used is the aqueous sodium-ion battery electrolyte prepared in Comparative Example 3.
[0080] Performance testing
[0081] Performance testing of aqueous sodium-ion battery electrolyte: The electrochemical window of the electrolyte was determined by linear sweep voltammetry (LSV) using a three-electrode setup. A titanium metal mesh without any other coating was used as the working electrode, and a platinum metal sheet and a saturated calomel electrode (SCE) were used as the counter electrode and reference electrode, respectively, to test the electrochemical window of the electrolyte using the aqueous sodium-ion battery electrolytes from Examples 1 and Comparative Examples 1-3. The scan rate was 0.5 mV / s, and the scan range was -1.2 to 1.5 V.
[0082] Performance testing of aqueous sodium-ion batteries: The charge / discharge range is 0.5~1.5 V, and constant current charge / discharge is performed at room temperature. The rate is set to 0.5C for the first three cycles, and 2C for subsequent cycles. The rate setting and capacity calculation are based on the positive electrode. The content of transition metals (Mn, Fe) in the electrolyte after cycling is tested by inductively coupled plasma (ICP).
[0083] Figure 1 The LSV curves are for the aqueous sodium-ion battery electrolytes in Example 1 and Comparative Examples 1-3.
[0084] from Figure 1 The LSV curves in Example 1 show that the comparative example, with its lower total acetate concentration, has not yet formed a sufficient electrochemical window (large current response at low potentials). Due to the alkalinity of acetate, as the salt concentration increases, the electrochemical window expands while the hydrogen evolution potential shifts significantly negatively, whereas the oxygen evolution potential no longer changes significantly (comparative examples 1-3). This ensures sufficient protection for the negative electrode, while the positive electrode remains vulnerable to water molecule attack at high potentials, facing the problem of transition metal ion dissolution. Compared to comparative example 3 (which differs only in surfactant), the electrolyte in Example 1 shows a positive shift in oxidation initiation potential and a significantly reduced current response at the same high potential, even outperforming comparative example 2 with its higher total acetate concentration. This indicates that the method described in this invention can more efficiently construct a localized hydrophobic layer at the positive electrode interface, further suppressing water-related decomposition reactions.
[0085] Figure 2 The cycling performance curves of the aqueous sodium-ion batteries in Comparative Examples 2-3 and Example 1 are shown.
[0086] from Figure 2 It can be seen that the aqueous sodium-ion battery in Comparative Example 3 exhibits better cycle performance than Comparative Example 2. This indicates that increasing the acetate concentration (electrochemical window) does not equate to improved performance when applied to a specific battery system. On the contrary, increased viscosity and deviation from the stable homogeneous liquid phase hinder ion transport, accelerating cycle degradation. Meanwhile, the sodium-ion battery in Example 1 demonstrates superior long-cycle performance compared to Comparative Example 3, proving the beneficial effects of this invention.
[0087] Figure 3 Charge-discharge curves of the aqueous sodium-ion batteries in Comparative Example 3 and Example 1 (100th cycle, 2C constant current charge-discharge).
[0088] Depend on Figure 3 It can be seen that after adding anionic surfactant in Example 1, the charge-discharge curve of sodium-ion battery remained good, no obvious polarization or side reaction was introduced, and the compatibility was good.
[0089] Figure 4 The Fe and Mn content in the electrolyte of the aqueous sodium-ion batteries in Comparative Example 3 and Example 1 after 1000 cycles.
[0090] Depend on Figure 4 The ICP test results show that after 1000 cycles of the aqueous sodium-ion battery in Comparative Example 3, the Fe content in the electrolyte is approximately 10.2 mg / L and the Mn content is approximately 2.3 mg / L; after 1000 cycles of the aqueous sodium-ion battery in Example 1, the Fe content in the electrolyte is approximately 9.0 mg / L and the Mn content is approximately 1.6 mg / L. After long-term cycling, compared with Example 1, the sodium-ion battery in Comparative Example 3 showed a higher concentration of positive electrode transition metals (Fe, Mn) leaching in the electrolyte. This proves that the present invention can specifically suppress the attack of water molecules on the surface of the positive electrode active material and the subsequent leaching of transition metals. This result is consistent with the trend of cycling performance.
[0091] It is understood that the technical features of the above embodiments can be combined arbitrarily. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0092] The above are merely preferred embodiments of this application, and only specifically describe the technical principles of this application. These descriptions are only for explaining the principles of this application and should not be construed as limiting the scope of protection of this application in any way. Based on this explanation, any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application, as well as other specific embodiments of this application that can be conceived by those skilled in the art without creative effort, should be included within the scope of protection of this application.
Claims
1. An aqueous sodium-ion battery electrolyte, characterized in that, include: Water, first solute, and second solute; The first solute is acetate; The acetate includes a first acetate and a second acetate; the first acetate is sodium acetate, and the second acetate includes at least one of potassium acetate or ammonium acetate; Based on water as a solvent, the concentration of sodium acetate in the electrolyte is 3~10 mol / kg, the concentration of the second acetate is 10~25 mol / kg, and the concentration of total acetate is 20~33 mol / kg; The second solute is an anionic surfactant.
2. The aqueous sodium-ion battery electrolyte as described in claim 1, characterized in that, The anionic surfactant has the general formula RX. - M + ; Wherein, R is an alkyl group having 8 to 18 carbon atoms; The X - Selected from any one of sulfate, sulfonate, or benzenesulfonate; The M + It is selected from any one of sodium ions, potassium ions, or ammonium ions.
3. The aqueous sodium-ion battery electrolyte as described in claim 1, characterized in that, The concentration of the anionic surfactant in the electrolyte is 0.1 to 3 times its critical micelle concentration in pure water at room temperature.
4. The aqueous sodium-ion battery electrolyte as described in claim 2, characterized in that, The anionic surfactant is at least one of sodium dodecyl sulfate, sodium dodecyl sulfonate, and sodium dodecylbenzene sulfonate.
5. The aqueous sodium-ion battery electrolyte as described in claim 1, characterized in that, The concentration of sodium acetate in the electrolyte is 5-8 mol / kg; The concentration of the second acetate in the electrolyte is 18~20 mol / kg.
6. The aqueous sodium-ion battery electrolyte as described in claim 3, characterized in that, The concentration of the anionic surfactant in the electrolyte is 0.5 to 1.5 times its critical micelle concentration in pure water at room temperature.
7. A method for preparing an aqueous sodium-ion battery electrolyte as described in any one of claims 1 to 6, characterized in that, Includes the following steps: The first and second solutes are added to water and stirred to obtain an aqueous sodium-ion battery electrolyte.
8. The application of an aqueous sodium-ion battery electrolyte as described in any one of claims 1 to 6 or an aqueous sodium-ion battery electrolyte prepared by the preparation method described in claim 7 in the preparation of sodium-ion batteries.
9. A sodium-ion battery, characterized in that, Includes the aqueous sodium-ion battery electrolyte as described in any one of claims 1 to 6 or the aqueous sodium-ion battery electrolyte prepared by the preparation method described in claim 7.
10. The sodium-ion battery as described in claim 9, characterized in that, It also includes a positive electrode, a negative electrode, and a separator, wherein the positive electrode active material used in the positive electrode includes at least one of Prussian blue analogues and transition metal oxides; The active material used in the negative electrode is NASICON-type phosphate.