A composite electrolyte for Prussian blue and its analogues as cathode materials, its preparation method, and the battery thereof.
By using a composite electrolyte in Prussian blue analogue batteries, material defects are repaired in situ and a protective interface is formed, solving the structural instability problem of Prussian blue analogue cathode materials and achieving long cycle life and high performance of the batteries.
Patent Information
- Application Number
- CN202611148565.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-30
- Publication Date
- 2026-11-17
AI Technical Summary
Under current technology, the crystal structure of Prussian blue analog cathode materials is unstable, resulting in short cycle life and poor cycle stability due to phase transition and metal ion dissolution during cycling.
A composite electrolyte is used, containing zinc salts, metal ions, buffer synergists, structural reinforcing agents, and cycle stabilizers. By adding multiple functional components to the electrolyte, material defects are repaired in situ, a protective interface is formed, and the stability of the crystal structure is enhanced.
It significantly improves the cycle stability of Prussian blue analog cathode materials and the long-term performance of batteries, reduces the capacity decay rate, and enhances the rate performance and discharge capacity of batteries.
Smart Images

Figure CN123120919A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aqueous zinc-ion batteries, specifically to a composite electrolyte for Prussian blue and similar battery cathode materials, a preparation method thereof, and a battery thereof. Background Technology
[0002] Currently, the most studied cathode materials for zinc-ion batteries are manganese-based materials, vanadium-based materials, Prussian blue, and their analogues. The large-pore, open-framework structure of Prussian blue and its analogues allows for ion insertion and extraction while maintaining structural stability, giving them the potential to serve as hosts for various charge carrier ions. However, Prussian blue analogues obtained through co-precipitation methods in existing technologies suffer from insufficient structural stability due to the unavoidable vacancies in the crystal structure during rapid crystallization, affecting long cycle life. Furthermore, during cycling, phase transitions leading to lattice distortion and the dissolution of metal ions further contribute to poor cycle stability, hindering widespread application.
[0003] Therefore, it is necessary to improve the stability of the crystal structure of Prussian blue analogues to enhance their long-cycle performance in aqueous zinc-ion battery systems. Summary of the Invention
[0004] In view of this, the purpose of the present invention is to provide a composite electrolyte, preparation method and battery for Prussian blue and its analogue battery cathode materials, to solve the technical problems of crystal structure collapse and insufficient cycle stability in aqueous zinc-ion battery Prussian blue analogue cathode systems.
[0005] The present invention discloses a composite electrolyte for aqueous zinc-ion batteries. The raw materials of the composite electrolyte include zinc salt, metal ions, buffer synergist, structural reinforcing agent, and cycle stabilizer; wherein the buffer synergist is one or a mixture of two or more of ethylene glycol, glycerol, sorbitol, betaine, and ammonium acetate.
[0006] Furthermore, the structural reinforcing agent is one or a mixture of two or more of borates, phosphates, and silicates;
[0007] Furthermore, the cycle stabilizer is one or a mixture of two or more of the following: sulfonated betaine, xylitol, trace amounts of lithium nitrate, and sodium adipic acid salt;
[0008] Furthermore, the zinc salt is one or a mixture of two or more of zinc sulfate, zinc chloride, and zinc trifluoromethanesulfonate;
[0009] Furthermore, the metal ion is at least one selected from Mn²⁺, Ni²⁺, Co²⁺, Cu²⁺, and Fe²⁺;
[0010] Furthermore, the metal ions are a combination of Mn²⁺-Ni²⁺, Mn²⁺-Co²⁺, and Ni²⁺-Co²⁺, wherein in Mn²⁺-Ni²⁺, Mn²⁺:Ni²⁺ = 1:2; in Mn²⁺-Co²⁺, Mn²⁺:Co²⁺ = 1:1; and in Ni²⁺-Co²⁺, i²⁺: -Co²⁺ = 2:1.
[0011] Furthermore, the concentration of zinc salt is 2–4 mol / L, the concentration of metal ions is 0.05–2 mol / L, the concentration of buffer synergist is 0.05–0.2 mol / L, the concentration of structural reinforcing agent is 0.01–0.05 mol / L, and the concentration of cycle stabilizer is 0.01–0.05 mol / L.
[0012] This invention also discloses a method for preparing a composite electrolyte for aqueous zinc-ion batteries, comprising the following steps:
[0013] After adding zinc salt and metal ions to deionized water and mixing them evenly, add buffer synergist, structural reinforcement agent and cycle stabilizer and stir evenly.
[0014] The present invention also discloses an aqueous zinc-ion battery, which uses a Prussian blue analogue as the positive electrode material and a zinc sheet as the negative electrode, and is assembled using a composite electrolyte.
[0015] The beneficial effects of this invention are as follows: The composite electrolyte, preparation method, and battery of this invention for Prussian blue and its analogues as positive electrode materials can in situ repair intrinsic defects in Prussian blue analogues and vacancies formed by metal ion dissolution, stabilizing the material's crystal structure. Simultaneously, a protective interface is formed in situ between the electrode and the electrolyte, inhibiting the dissolution reaction of metal ions and thus enhancing the material's cycle stability. By leveraging the synergistic effect of multiple components in the electrolyte, the system achieves three functions: in-situ repair of material defects, long-term stability of crystal structure, and protection of electrode interface. This completely solves core problems such as lattice collapse, ion dissolution, and structural distortion in Prussian blue analog cathodes. The integrity of the cathode crystal structure is significantly improved during long-term battery cycling, with no obvious structural damage. Through the dual mechanisms of in-situ defect repair and interface protection, the battery capacity decay rate is significantly reduced, effectively addressing the shortcomings of insufficient cycle stability in aqueous zinc-ion batteries and maintaining the battery's electrochemical performance for a long time. The synergistic regulation of the electrolyte's physicochemical properties and electrode interface state by multiple components balances high ionic conductivity, rapid ion transport, and low interfacial impedance, ensuring excellent rate performance and discharge capacity, and balanced electrochemical performance. Attached Figure Description
[0016] The present invention will be further described below with reference to the accompanying drawings and embodiments:
[0017] Figure 1The images show XRD patterns of aqueous zinc-ion batteries assembled in Example 1 and Comparative Example 1 using two different electrolytes at different cycling stages.
[0018] Figure 2 These are Raman images of an aqueous zinc-ion battery assembled in the electrolyte of Example 1 at different cycling stages;
[0019] Figure 3 This is a SEM image of an aqueous zinc-ion battery assembled in the electrolyte of Example 1 after cycling.
[0020] Figure 4 The rate performance diagrams show the assembled aqueous zinc-ion batteries of Example 1 and Comparative Example 1 using two different electrolytes.
[0021] Figure 5 The graph shows the long-cycle performance of aqueous zinc-ion batteries assembled in Example 1 and Comparative Example 1 using two different electrolytes at a current density of 5 A / g. Detailed Implementation
[0022] To better understand the present invention, the following embodiments are further illustrations of the present invention, but the content of the present invention is not limited to the following embodiments.
[0023] Unless otherwise specified, the experimental methods used in the embodiments are conventional methods, and the materials and reagents used are commercially available unless otherwise specified.
[0024] This embodiment presents a composite electrolyte for aqueous zinc-ion batteries. The composite electrolyte raw materials include zinc salts, metal ions, buffer synergists, structural reinforcing agents, and cycle stabilizers. The buffer synergists are one or more mixtures of ethylene glycol, glycerol, sorbitol, betaine, and ammonium acetate. The buffer synergists optimize the overall physicochemical properties of the electrolyte, regulate electrolyte viscosity, water molecule activity, and electrochemical stability window, and synergistically enhance the interfacial protection effect with ionic additives, suppressing aqueous side reactions. Simultaneously, they improve the compatibility of each component, avoiding the limitations of single additives and achieving multi-component synergistic enhancement. During the preparation and cycling of Prussian blue analogues, defects such as intrinsic lattice vacancies and missing coordination bonds inevitably occur. Furthermore, the dissolution of active metal ions at the positive electrode during charging and discharging continuously generates new structural vacancies, leading to a loose and collapsed crystal framework. The functional ionic additives in this electrolyte can dynamically migrate to defect sites in the cathode material during battery charge-discharge cycles, precisely filling lattice vacancies, repairing broken coordination bonds, and compensating for structural damage caused by intrinsic defects and ion dissolution in real time. This continuously reconstructs a regular and stable crystal framework, fundamentally suppressing lattice distortion and structural collapse. After filling defects, the functional additives can form strong coordination interactions with the Prussian blue analog crystal framework, enhancing the bonding strength and structural rigidity of the crystal structure, significantly improving the crystal framework's resistance to deformation, and effectively resisting the structural stress impact caused by repeated Zn²⁺ insertion / extraction. Simultaneously, this component can regulate the ion dissolution balance on the cathode surface, reducing the dissolution rate and amount of active metal ions, avoiding structural damage and capacity decay caused by continuous ion loss, and maintaining the structural integrity of the cathode material for a long time. During initial battery activation and cycling, the functional components of the electrolyte can generate a uniform, dense, and highly stable functional protective interface film in situ at the cathode-electrolyte interface. This interface film possesses excellent ion-selective permeability, ensuring normal Zn²⁺ intercalation-deintercalation transport while effectively blocking direct contact between active water molecules in the electrolyte and the cathode material. This inhibits adverse side reactions such as water decomposition, electrode corrosion, and byproduct deposition, preventing interface structure damage, further stabilizing the electrode interface state, and reducing the increase in interface impedance. Compared to traditional single-zinc salt electrolytes, this solution utilizes buffer synergists, structural reinforcing agents, and cycle stabilizers to achieve a complementary and synergistic effect with the core ion additives. On one hand, it reduces the activity of water molecules in the electrolyte, broadens the electrochemical stability window of the system, and reduces the inherent side reaction risks of aqueous electrolytes. On the other hand, it optimizes the ion transport environment, improves the migration rate and transport uniformity of Zn²⁺, alleviates localized stress concentration in the electrode, and helps enhance crystal structure stability. Simultaneously, the components exhibit excellent compatibility, with no aggregation, precipitation, or byproduct formation. This maximizes battery cycle stability without sacrificing rate performance or discharge capacity, achieving multiple benefits of "structural repair, interface protection, and performance optimization."
[0025] In this embodiment, the structural reinforcing agent is one or a mixture of two or more of borates, phosphates, and silicates; the lattice is anchored by the structural reinforcing agent.
[0026] In this embodiment, the circulating stabilizer is one or a mixture of two or more of the following: sulfonate betaine, xylitol, trace amounts of lithium nitrate, and sodium adipic acid salt;
[0027] In this embodiment, the zinc salt is one or a mixture of two or more of zinc sulfate, zinc chloride, and zinc trifluoromethanesulfonate. At least one of these three zinc salts is selected as the core conductive component to provide sufficient and stable Zn²⁺ for the battery charging and discharging process, ensuring excellent ionic conductivity of the electrolyte and guaranteeing the battery's basic electrochemical performance, such as rate discharge and ion transport. Simultaneously, it effectively maintains the electrolyte ion balance, avoiding electrode interface polarization problems caused by zinc ion concentration imbalance, and adapts to the ion intercalation / deintercalation characteristics of Prussian blue analog cathodes.
[0028] In this embodiment, the metal ion is at least one of Mn²⁺, Ni²⁺, Co²⁺, Cu²⁺, and Fe²⁺. The metal ion is the core functional component of this system. At least one of manganese (Mn), nickel (Ni), cobalt (Co), copper (Cu), and iron (Fe) metal ions (including but not limited to the above metal ion systems) is selected. It can accurately target and adapt to the crystal structure of Prussian blue analogues and has multiple characteristics such as defect filling, lattice repair, and interface regulation. It is the core key to achieving stable cathode structure, inhibiting the dissolution of active ions, and improving battery cycle performance.
[0029] In this embodiment, the metal ions are complexes of Mn²⁺-Ni²⁺, Mn²⁺-Co²⁺, and Ni²⁺-Co²⁺. In Mn²⁺-Ni²⁺, the ratio of Mn²⁺ to Ni²⁺ is 1:2; in Mn²⁺-Co²⁺, the ratio of Mn²⁺ to Co²⁺ is 1:1; and in Ni²⁺-Co²⁺, the ratio of Mn²⁺ to -Co²⁺ is 2:1. Preferably, complexes of metal ions are used. The form "Mn²⁺-Ni²⁺" represents a complex of manganese (Mn) ions and nickel (Ni) ions. "Mn²⁺-Co²⁺" represents a complex of manganese (Mn) ions and cobalt (Co) ions, and "Ni²⁺-Co²⁺" represents a complex of nickel (Ni) ions and cobalt (Co) ions. Based on the differences in vacancy size, coordination bond characteristics, and ion intercalation / deintercalation potentials in PBA crystals, a compounding logic of "large-radius ions filling vacancies, small-radius ions strengthening the framework, and highly active ions repairing defects" is followed to avoid problems such as ion competition and repulsion, lattice blockage, and interfacial precipitation, ensuring excellent compatibility of multiple ions coexisting. Different transition metal ions exhibit differentiated coordination characteristics in the PBA lattice. Mn ions adapt to large-sized lattice vacancies, quickly compensating for structural defects generated during preparation and cycling; Ni and Co ions have higher bonding energies and can be anchored at crystal framework nodes, improving overall structural rigidity and resistance to deformation; Fe and Cu ions can optimize charge transport at the electrode interface and reduce interfacial impedance. The multi-ion compounding can simultaneously achieve "defect filling, framework reinforcement, interface optimization, and dissolution suppression," solving the problems of incomplete repair and insufficient long-term stability of single-ion systems.
[0030] In this embodiment, the concentration of zinc salt is 2–4 mol / L, the concentration of metal ions is 0.05–2 mol / L, the concentration of buffer synergist is 0.05–0.2 mol / L, the concentration of structural reinforcing agent is 0.01–0.05 mol / L, and the concentration of cycling stabilizer is 0.01–0.05 mol / L. Low concentrations of buffer synergist can efficiently bind free water, avoiding the decrease in ionic conductivity caused by high viscosity; the amount of cycling stabilizer can better stabilize the interface, suppress side reactions, and alleviate interfacial polarization; only a trace amount of structural reinforcing agent is needed to complete lattice bonding reinforcement, while high concentrations can easily lead to salt precipitation and interfacial blockage.
[0031] These composite auxiliary components can synergistically enhance the performance of the main additives from multiple dimensions, thereby maximizing the long-term stability of the cathode crystal structure and the battery cycle life.
[0032] First, alcohols and xylitol polyols can bind free water molecules in the electrolyte at a high density, significantly reducing water molecule activity and fundamentally inhibiting continuous aqueous side reactions such as hydrogen release from water, positive electrode chemical corrosion, and zinc anode dendrite growth. This avoids interfacial failure and structural collapse caused by the accumulation of byproducts under long-term cycling, and broadens the long-term electrochemical stability window of the system. Second, organic buffer components such as betaine, sulfobetaine, ammonium acetate, and sodium adipic acid salt can precisely control the pH range of the electrolyte, resisting the dynamic pH fluctuations caused by ion deintercalation and micro-side reactions during long-term cycling, continuously maintaining the stability of the PBA positive electrode coordination framework, and preventing gradual framework deconstruction and chronic dissolution of metal ions under long-term cycling. Third, trace amounts of boron, phosphorus, and silicon-based structural reinforcement components can dynamically accumulate in the PBA positive electrode during charging and discharging. High-strength BO, PO, and Si-O inorganic coordination bonds are formed at lattice vacancies, defects, and grain boundaries, creating a double-layer rigid structure of "internal lattice anchoring + surface mesh protection." This significantly enhances the crystal framework's resistance to fatigue, deformation, and pulverization, effectively dissipating accumulated structural stress after thousands of cycles. Fourth, trace amounts of lithium nitrate can optimize the electrolyte ion migration configuration, induce uniform Zn²⁺ insertion / extraction, reduce local electrode polarization and stress concentration, and simultaneously assist in densifying the electrode interface film, improving the cycle durability of the interface structure. Fifth, multi-component synergistic adaptation to long-cycle conditions compensates for the insufficient long-term stability of single components, achieving multi-dimensional synergistic effects of "dynamic defect repair + lattice rigidity reinforcement + long-term interface locking + full-process suppression of side reactions," thus maximizing the battery's long-cycle stability.
[0033] This embodiment also discloses a method for preparing a composite electrolyte for aqueous zinc-ion batteries, comprising the following steps:
[0034] Zinc salts and metal ions are added to deionized water and mixed thoroughly. Then, buffer synergists, structural reinforcing agents, and cycle stabilizers are added and stirred until homogeneous. Deionized water, as an electrolyte dispersion solvent, has high purity and extremely low impurity ion content, effectively avoiding side reactions, electrode contamination, and self-discharge phenomena caused by impurity ions, ensuring the purity and stability of the battery system.
[0035] This embodiment also discloses an aqueous zinc-ion battery, which uses a Prussian blue analogue as the positive electrode material and a zinc sheet as the negative electrode, and is assembled using a composite electrolyte.
[0036] Example 1
[0037] S1, Preparation of zinc salt solution: Dissolve 10.9056g of zinc trifluoromethanesulfonate in 10mL of deionized water, and stir thoroughly with a glass rod at room temperature until completely dissolved. The concentration of the resulting solution is 3mol / L.
[0038] S2, Preparation of ionic additive solution: Dissolve 0.8451g of manganese sulfate in 10mL of deionized water, and stir magnetically for 30min at room temperature to obtain a completely dissolved and clear solution with a concentration of 0.5mol / L.
[0039] S3, take 4 mL of zinc salt solution from step S1 and 1 mL of ion additive solution from step S2, and mix them thoroughly at room temperature to obtain a zinc salt-manganese ion composite basic electrolyte system;
[0040] S4, a multifunctional additive formulation: A buffer synergist, structural reinforcing agent, and cycle stabilizer are sequentially added to the base electrolyte (S3). After standing at room temperature for 30 minutes, the solution is allowed to mature, eliminating localized concentration inconsistencies. This results in a highly stable composite aqueous zinc-ion battery electrolyte suitable for Prussian blue analog cathodes. The overall system exhibits excellent compatibility, with no precipitation, no stratification, and no byproducts. The concentrations of the buffer synergist (ethylene glycol) are 0.05 mol / L, the structural reinforcing agent (borate) is 0.01 mol / L, and the cycle stabilizer (sulfonate betaine) is 0.01 mol / L.
[0041] Example 2
[0042] S1, Preparation of zinc salt solution: Dissolve 10.9056g of zinc trifluoromethanesulfonate in 10mL of deionized water, and stir thoroughly with a glass rod at room temperature until completely dissolved. The concentration of the resulting solution is 3mol / L.
[0043] S2, Preparation of ionic additive solution: Dissolve 0.0845g of manganese sulfate in 10mL of deionized water, and stir magnetically for 30min at room temperature to obtain a completely dissolved and clear solution with a concentration of 0.05mol / L.
[0044] S3, take 4 mL of the zinc salt solution from step S1 and 1 mL of the ion additive solution from step S2, and mix them thoroughly at room temperature to obtain the basic electrolyte;
[0045] S4, a multifunctional additive formulation: A buffer synergist, structural reinforcing agent, and cycle stabilizer are sequentially added to the base electrolyte (S3). After standing at room temperature for 30 minutes, the solution is allowed to mature, eliminating localized concentration inconsistencies. This results in a highly stable composite aqueous zinc-ion battery electrolyte suitable for Prussian blue analogue cathodes. The overall system exhibits excellent compatibility, with no precipitation, no stratification, and no byproducts. The concentrations of the buffer synergist (glycerol) are 0.2 mol / L, the structural reinforcing agent (phosphate) is 0.05 mol / L, and the cycle stabilizer (xylitol) is 0.05 mol / L.
[0046] Example 3
[0047] S1, Preparation of zinc salt solution: Dissolve 10.9056g of zinc trifluoromethanesulfonate in 10mL of deionized water, and stir thoroughly with a glass rod at room temperature until completely dissolved. The concentration of the resulting solution is 3mol / L.
[0048] S2, Preparation of ionic additive solution: Dissolve 0.338g of manganese sulfate in 10mL of deionized water, and stir magnetically for 30min at room temperature to obtain a completely dissolved and clear solution with a concentration of 0.2mol / L;
[0049] S3, take 4 mL of the zinc salt solution from step S1 and 1 mL of the ion additive solution from step S2, and mix them thoroughly at room temperature to obtain a basic electrolyte;
[0050] S4, a multifunctional additive formulation: A buffer synergist, structural reinforcing agent, and cycle stabilizer are sequentially added to the base electrolyte (S3). After standing at room temperature for 30 minutes, the solution is allowed to mature, eliminating localized concentration inconsistencies. This results in a highly stable composite aqueous zinc-ion battery electrolyte suitable for Prussian blue analog cathodes. The overall system exhibits excellent compatibility, with no precipitation, no stratification, and no byproducts. The concentrations of the buffer synergist (sorbitol), structural reinforcing agent (silicate), and cycle stabilizer (lithium nitrate) are all 0.08 mol / L.
[0051] Example 4
[0052] S1, Preparation of zinc salt solution: Dissolve 10.9056g of zinc trifluoromethanesulfonate in 10 mL of deionized water, and stir thoroughly with a glass rod at room temperature until completely dissolved. The concentration of the resulting solution is 3mol / L.
[0053] S2, Preparation of ion additive solution: Dissolve 3.3804 g of manganese sulfate in 10 mL of deionized water, and stir magnetically for 30 min at room temperature to obtain a completely dissolved and clear solution with a concentration of 2 mol / L.
[0054] S3, take 4 mL of the zinc salt solution from step S1 and 1 mL of the ion additive solution from step S2, and mix them thoroughly at room temperature to obtain the basic electrolyte;
[0055] S4, a multifunctional additive compound: A buffer synergist, structural reinforcing agent, and cycle stabilizer are sequentially added to the base electrolyte (S3). After standing at room temperature for 30 minutes, the solution is allowed to mature, eliminating localized concentration inconsistencies. This results in a highly stable composite aqueous zinc-ion battery electrolyte suitable for Prussian blue analogue cathodes. The overall system exhibits excellent compatibility, with no precipitation, no stratification, and no byproducts. The concentrations of the buffer synergist (betaine and ammonium acetate) are 0.1 mol / L, the structural reinforcing agent (borate) is 0.03 mol / L, and the cycle stabilizer (sodium adipic acid salt) is 0.03 mol / L.
[0056] Comparative Example 1
[0057] This comparative example is basically the same as the above examples, except that: no metal ion additive solution is added to the electrolyte as in the examples, and the electrolyte is composed only of zinc salt, using a zinc trifluoromethanesulfonate solution with a concentration of 3 mol / L.
[0058] This invention is applied to an aqueous zinc-ion battery system using a Prussian blue analogue as the positive electrode. The electrolyte used is derived from all the examples and comparative examples. The positive electrode material in all the examples and comparative examples uses a vanadium-based Prussian blue analogue, and the specific preparation method includes the following steps:
[0059] S1, dissolve 0.3636g of vanadium pentoxide and 0.7564g of dihydrate and oxalic acid in 40mL of deionized water, and stir in a water bath at 75℃ until a clear blue solution is obtained;
[0060] S2, add 0.6585g of potassium ferricyanide to 40mL of deionized water and stir magnetically at room temperature to obtain a clear solution;
[0061] S3. Under magnetic stirring, slowly add the solution from step S1 to the solution from step S2 to obtain a mixed solution, then perform a co-precipitation reaction. After that, filter, wash, and dry the product to obtain a vanadium-based Prussian blue analog cathode material. The titration rate is 0.8-1.2 ml / min, and the temperature is controlled at room temperature. When using the co-precipitation method, the precipitation time is 18-24 h (e.g., 20 h). The vacuum drying temperature is 50-70℃, and the drying time is 12-18 h (e.g., 14 h).
[0062] Test Analysis
[0063] Taking Example 1 as an example, 70 wt% vanadium-based Prussian blue analogue was used as the positive electrode active material, and 20 wt% conductive agent SuperP and 10 wt% binder polyvinylidene fluoride were added and mixed and ground for 30 min. 1-methyl-2-pyrrolidone was added and the mixture was dispersed and stirred for 24 h to prepare a uniform slurry. The slurry was then coated onto a stainless steel mesh and placed in a vacuum drying oven at 60°C for 12 h to obtain the positive electrode sheet. Zinc sheet was used as the negative electrode and glass fiber as the separator. Electrolytes from all examples and comparative examples were selected and assembled into CR2032 coin cells.
[0064] The CR2032 coin cells assembled using the above method were subjected to cyclic voltammetry and constant current charge-discharge performance tests on a CS electrochemical workstation (provided by Wuhan Koster Instruments Co., Ltd.) and a LAND battery testing system (provided by Wuhan Landian Electronics Co., Ltd.). The voltage range was relative to Zn / Zn 2+ The voltage range is 0.2V to 2.0V.
[0065] Figure 1 XRD images of aqueous zinc-ion batteries assembled in Example 1 and Comparative Example 1 using the vanadium-based Prussian blue analogue as the positive electrode at different cycling stages. In the functional electrolyte of Example 1 (e.g.... Figure 1 a) As the cycle progressed, the formation of a new phase was observed, and the characteristic diffraction peaks corresponded to K2MnFe(CN)6·2H2O (PDF#51–1896). This is a new structural feature resulting from the electrochemically induced repair of vacancies in vanadium-based Prussian blue analogs by manganese ions, which is beneficial to the stability of the Prussian blue framework. The characteristic peaks of the manganese oxide protective layer were not observed in the figure; only a small and broad peak was observed near 22°, indicating that it is amorphous, resulting in an amorphous manganese oxide protective layer. However, in the ordinary electrolyte used in Comparative Example 1 (such as…),… Figure 1 (b) No new phase formation was observed under different cycle numbers.
[0066] Figure 2 Raman images of an aqueous zinc-ion battery assembled in the electrolyte of Example 1 using the vanadium-based Prussian blue analogue as the positive electrode at different cycling stages. 2093 cm⁻¹ -1 The peak at that point belongs to Fe-CN-V. As the cycle progresses, a characteristic peak of Fe-CN-Mn (2115 cm⁻¹) appears around cycle 10. -1 The CN peak shifts due to the inductive effect of different metal ions. Specifically, the electronegativity difference between substances causes a redistribution of the electronic energy spectrum of the nitrogen group and changes its absorption frequency, indicating a change in the electronic configuration around N, which explains the change in the bulk crystal structure.
[0067] Figure 3 SEM images of an aqueous zinc-ion battery assembled in the electrolyte of Example 1 using the vanadium-based Prussian blue analogue as the positive electrode after cycling are shown. A continuous protective layer is uniformly covered across the entire surface of the electrode material. This protective layer effectively encapsulates the underlying electrode material, preventing direct contact between the electrode and active water molecules in the electrolyte, reducing material dissolution, or buffering its volume changes during charge and discharge. Furthermore, the protective layer is tightly bonded to the bulk material, with no obvious gaps or detachment at the interface. This indicates good physical bonding and compatibility between the protective layer and the electrode substrate, which is crucial for maintaining interfacial stability and preventing protective layer detachment during electrochemical cycling.
[0068] Figure 4 The rate performance of aqueous zinc-ion batteries assembled using the vanadium-based Prussian blue analogue as the positive electrode under two electrolytes, Example 1 and Comparative Example 1, is shown in the graph. Using the electrolyte described in Example 1, the maximum discharge capacities obtained at current densities of 0.2, 0.5, 1.0, 2.0, 3.0, 5.0, 10, and 0.2 A / g are 180.2, 179.8, 168.5, 146.3, 129.8, 106.1, 77.2, and 172.8 mAh / g, respectively, demonstrating excellent rate performance.
[0069] Figure 5 The graph shows the long-term cycling performance of aqueous zinc-ion batteries assembled in Example 1 and Comparative Example 1 using the vanadium-based Prussian blue analogue as the positive electrode at a current density of 5 A / g. Comparative Example 1 shows a capacity of less than 50 mAh / g after 1000 cycles, exhibiting a significant decreasing trend. In contrast, Example 1 still maintains a specific capacity of 71.8 mAh / g after 6000 cycles, achieving a capacity retention of 73%, demonstrating excellent cycle stability.
[0070] Meanwhile, electrochemical tests were conducted on the aqueous zinc-ion batteries assembled in each embodiment and comparative example using the vanadium-based Prussian blue analogue as the positive electrode. The long-cycle test results at a current density of 5 A / g are as follows:
[0071]
[0072] Therefore, the functionalized aqueous zinc-ion battery electrolyte proposed in this invention demonstrates excellent improved cycle stability in aqueous zinc-ion battery systems using vanadium-based Prussian blue analog cathode materials. Under electrochemically induced reactions, ionic additives in situ repair intrinsic defects in the Prussian blue analog and vacancies formed by metal ion dissolution, stabilizing the material's crystal structure. Simultaneously, an in-situ protective interface is formed between the electrode and the electrolyte, inhibiting the dissolution reaction of metal ions and thus enhancing the material's cycle stability. Furthermore, all embodiments show that appropriate concentrations are beneficial for the synergistic optimization of capacity and cycle stability, resulting in a more significant improvement in the overall battery performance. The method of this invention also possesses advantages such as simplicity, versatility, environmental friendliness, low cost, and strong controllability, demonstrating significant application potential.
[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A composite electrolyte for aqueous zinc-ion batteries, characterized in that: The raw materials for the composite electrolyte include zinc salts, metal ions, buffer synergists, structural reinforcing agents, and cycle stabilizers; the buffer synergists are one or more mixtures of ethylene glycol, glycerol, sorbitol, betaine, and ammonium acetate.
2. The composite electrolyte for aqueous zinc-ion batteries according to claim 1, characterized in that: The structural reinforcing agent is one or a mixture of two or more of borates, phosphates, and silicates.
3. The composite electrolyte for aqueous zinc-ion batteries according to claim 1, characterized in that: The cycle stabilizer is one or a mixture of two or more of the following: sulfonate betaine, xylitol, trace amounts of lithium nitrate, and sodium adipic acid salt.
4. The composite electrolyte for aqueous zinc-ion batteries according to claim 1, characterized in that: The zinc salt is one or a mixture of two or more of zinc sulfate, zinc chloride, and zinc trifluoromethanesulfonate.
5. The composite electrolyte for aqueous zinc-ion batteries according to claim 4, characterized in that: The metal ion is at least one of Mn²⁺, Ni²⁺, Co²⁺, Cu²⁺, and Fe²⁺.
6. The composite electrolyte for aqueous zinc-ion batteries according to claim 5, characterized in that: The metal ions are a combination of Mn²⁺-Ni²⁺, Mn²⁺-Co²⁺, and Ni²⁺-Co²⁺. In Mn²⁺-Ni²⁺, the ratio of Mn²⁺ to Ni²⁺ is 1:2; in Mn²⁺-Co²⁺, the ratio of Mn²⁺ to Co²⁺ is 1:1; and in Ni²⁺-Co²⁺, the ratio of i²⁺ to -Co²⁺ is 2:
1.
7. The composite electrolyte for aqueous zinc-ion batteries according to claim 1, characterized in that: The concentrations of zinc salt, metal ions, buffer synergists, structural reinforcing agents, and cycle stabilizers are 2–4 mol / L, 0.05–2 mol / L, 0.05–0.2 mol / L, 0.01–0.05 mol / L, and 0.01–0.05 mol / L, respectively.
8. The method for preparing the composite electrolyte for an aqueous zinc-ion battery according to claim 1, characterized in that: Includes the following steps: After adding zinc salt and metal ions to deionized water and mixing them evenly, add buffer synergist, structural reinforcement agent and cycle stabilizer and stir evenly.
9. An aqueous zinc-ion battery, characterized in that: A water-based zinc-ion battery was assembled using a Prussian blue analogue as the positive electrode material and a zinc sheet as the negative electrode, along with a composite electrolyte.