Aqueous Cathode Artificial Electrolyte Interface Layer, Cathode Sheet and its Preparation Method, and Aqueous Battery
By constructing a three-dimensional cross-linked network on the surface of lithium iron phosphate cathode material to form an artificial electrolyte interface layer for aqueous cathodes, the problems of iron ion dissolution and interface instability in aqueous zinc-lithium hybrid batteries are solved, thereby improving the cycle stability and capacity retention of the battery.
Patent Information
- Application Number
- CN202611512169.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, lithium iron phosphate cathode materials in aqueous zinc-lithium hybrid batteries suffer from iron ion dissolution and interfacial instability during cycling, leading to rapid capacity decay.
A three-dimensional cross-linked network is constructed using carboxymethyl cellulose salt, phytic acid compounds, tannic acid compounds, and coordination cross-linking components to form a stable aqueous positive electrode artificial electrolyte interface layer. Through multi-point hydrogen bonding and coordination, the migration of iron ions is reduced, thereby enhancing interface stability and ion transport performance.
It effectively alleviates the iron ion dissolution problem of lithium iron phosphate cathode materials, improves the cycle stability and capacity retention of batteries, and enhances rate performance.
Smart Images

Figure CN123120928A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of battery materials technology, specifically relating to an aqueous positive electrode artificial electrolyte interface layer, a positive electrode sheet and its preparation method, and an aqueous battery. Background Technology
[0002] Aqueous zinc-based batteries have promising applications in large-scale energy storage due to their advantages such as high safety, low cost, environmental friendliness, and abundant zinc resources. Specifically, aqueous zinc-lithium hybrid batteries typically use lithium-containing cathode materials as the positive electrode and metallic zinc or zinc-based materials as the negative electrode. They employ an aqueous electrolyte containing both zinc and lithium salts, matching the zinc deposition / stripping reaction with the lithium ion insertion / extraction reaction in the cathode material, thus achieving both high safety and good energy output characteristics.
[0003] Lithium iron phosphate (LFP) batteries possess advantages such as structural stability, low cost, and high safety, and have been widely used in the lithium-ion battery field. Currently, incorporating LFP into aqueous zinc-lithium hybrid battery systems can help construct energy storage battery systems with high safety and long lifespan. However, in aqueous electrolyte environments, the surface and interfacial stability of LFP cathode materials after prolonged contact with water, zinc salts, lithium salts, and other components in the electrolyte still faces significant challenges. Especially under long-cycle, high-rate, or high-voltage window conditions, iron elements in LFP may dissolve and migrate, leading to gradual structural damage to the cathode material, loss of active materials, and potentially inducing electrolyte side reactions or anode interface degradation, ultimately resulting in battery capacity decay, reduced coulombic efficiency, and shortened cycle life.
[0004] In existing technologies, improvements to the capacity decay problem of aqueous zinc-based batteries are typically made through methods such as negative electrode protection, electrolyte additives, and positive electrode modification. For example, constructing a protective layer on the surface of the zinc negative electrode can suppress zinc dendrites and hydrogen evolution side reactions to a certain extent; or, introducing additives into the electrolyte can adjust water activity and zinc ion solvation structure; or, modifying the positive electrode material through carbon coating, element doping, or surface modification can improve the conductivity and structural stability of the material.
[0005] However, existing solutions still have shortcomings in addressing the iron ion dissolution problem of lithium iron phosphate cathodes in aqueous zinc-lithium hybrid batteries. Specifically, these shortcomings include the following aspects: Firstly, conventional carbon coatings are difficult to continuously capture iron ions dissolved from the cathode surface; secondly, simply adding complexing agents may cause the complexing agents to diffuse or migrate in the electrolyte, making it difficult for them to act stably at the cathode interface, and may even affect the bulk properties of the electrolyte and the stability of the anode reaction.
[0006] Therefore, how to construct a stable, hydrophilic, fast-transporting ion layer with iron ion complexing ability on the surface of lithium iron phosphate cathode material is a key issue in improving the cycle life and capacity retention of aqueous zinc-lithium hybrid batteries. Summary of the Invention
[0007] To address the shortcomings of existing technologies, this application aims to provide an aqueous positive electrode artificial electrolyte interface layer, a positive electrode sheet, a method for preparing the same, and an aqueous battery, in order to solve the problems of iron ion dissolution, positive electrode interface instability, and rapid capacity decay of lithium iron phosphate positive electrodes in existing aqueous zinc-lithium hybrid batteries during cycling.
[0008] To achieve this objective, the present application adopts the following technical solution: In a first aspect, this application provides an aqueous positive electrode artificial electrolyte interface layer, wherein the material of the aqueous positive electrode artificial electrolyte interface layer includes carboxymethyl cellulose salt, phytic acid compounds, tannic acid compounds, polyether compounds and coordination crosslinking components; The carboxymethyl cellulose salt and the phytic acid compound form a three-dimensional cross-linked network, the tannic acid compound is confined within the three-dimensional cross-linked network, and the coordination cross-linking component is distributed within the three-dimensional cross-linked network.
[0009] The technical solution of this application provides an artificial electrolyte interface layer suitable for aqueous cathodes, which can reduce the continuous dissolution and migration of iron ions in lithium iron phosphate cathodes without significantly hindering ion transport, stabilize the cathode / electrolyte interface, and thus improve the cycle stability of aqueous batteries.
[0010] Specifically, the hydroxyl and carboxyl groups on the carboxymethyl cellulose salt molecular chain and the phosphate and hydroxyl groups in phytic acid compounds can form a primary three-dimensional network through multi-site hydrogen bonding and molecular chain entanglement. Under the action of the precursor solution forming the coordination crosslinking component, polyvalent metal ions can further coordinate with carboxyl groups, phosphate groups, and / or phenolic hydroxyl groups in tannic acid compounds at multiple sites, further solidifying the primary three-dimensional network. Tannic acid compounds are confined within the three-dimensional crosslinking network, and their polyphenolic structure can complex with iron ions dissolved from the lithium iron phosphate cathode, thereby reducing the continuous migration of iron ions in the electrolyte and further inducing the dissolution of the cathode material. Polyether compounds can improve the hydrophilicity and flexibility of the artificial electrolyte interface layer, helping to maintain the wetting of the interface layer by the aqueous electrolyte and reduce ion transport resistance. The coordination crosslinking component can further enhance the crosslinking degree, water resistance, and interface stability of the artificial electrolyte interface layer.
[0011] Compared with aqueous cathode materials without an artificial electrolyte interface layer, the artificial cathode interface layer provided in this application can effectively alleviate the problem of iron ion dissolution in aqueous electrolytes of lithium iron phosphate cathode materials, reduce the loss of cathode active materials, suppress side reactions at the cathode / electrolyte interface, and thus improve the capacity retention, rate performance and cycle stability of aqueous batteries during long-term cycling.
[0012] In some embodiments, the aqueous positive electrode artificial electrolyte interface layer satisfies the following relationship: 0.03≤B / A≤0.5, 0.005≤C / A≤0.3, 0.01≤D / A≤0.3, 0.001≤E≤0.5; Wherein, A is the mass fraction of carboxymethyl cellulose salt in the aqueous positive electrode artificial electrolyte interface layer, B is the mass fraction of phytic acid compounds in the aqueous positive electrode artificial electrolyte interface layer, C is the mass fraction of tannic acid compounds in the aqueous positive electrode artificial electrolyte interface layer, D is the mass fraction of polyether compounds in the aqueous positive electrode artificial electrolyte interface layer, and E is the concentration of the coordination crosslinking agent solution used to form the coordination crosslinking component, in mol / L.
[0013] Specifically, B / A can be, for example, 0.03, 0.05, 0.1, 0.12, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28, 0.3, 0.32, 0.35, 0.38, 0.4, 0.42, 0.45, 0.48, or 0.5, etc.; C / A can be, for example, 0.005, 0.008, 0.01, 0.015, 0.02, 0.05, 0.1, 0.12, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28, or 0.3, etc.; and D / A can be, for example, 0.01, 0.015, 0.005, 0.01 ... The values can be 0.02, 0.05, 0.1, 0.12, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28, or 0.3, etc., and E can be, for example, 0.001, 0.005, 0.008, 0.01, 0.015, 0.02, 0.05, 0.1, 0.12, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28, 0.3, 0.32, 0.35, 0.38, 0.4, 0.42, 0.45, 0.48, or 0.5, etc., and are not limited to the listed values. Other unlisted values within this range also apply.
[0014] This application adjusts the ratios of B / A, C / A, D / A, and E to the aforementioned ranges, thereby matching the network crosslinking sites provided by phytic acid compounds, the iron ion complexing sites provided by tannic acid compounds, the hydrophilic and flexible regulatory effects provided by polyether compounds, and the secondary crosslinking strength provided by the coordination crosslinking components. This approach is beneficial for balancing the structural integrity, iron ion capture capacity, and ion transport performance of the aqueous cathode artificial electrolyte interface layer.
[0015] When the B / A or E ratio is low, the cross-linking degree of the formed aqueous positive electrode artificial electrolyte interface layer is insufficient, and swelling or component loss is likely to occur in the aqueous electrolyte. When the B / A or E ratio is high, the formed three-dimensional cross-linked network may be excessively dense and increase the ion transport resistance.
[0016] When the C / A ratio is low, the complexation capacity for iron ions is insufficient; when the C / A ratio is high, it may increase the ion transport resistance of the artificial electrolyte interface layer in the aqueous cathode or affect the network uniformity.
[0017] When the D / A ratio is low, the improvement effect on the wettability and flexibility of the artificial electrolyte interface layer of the aqueous cathode is limited; when the D / A ratio is high, it may lead to excessive swelling of the formed three-dimensional cross-linked network and reduce structural stability.
[0018] In some preferred embodiments, the aqueous positive electrode artificial electrolyte interface layer satisfies the following relationship: 0.05≤B / A≤0.2, 0.02≤C / A≤0.15, 0.03≤D / A≤0.15, 0.01≤E≤0.2; Wherein, A is the mass fraction of carboxymethyl cellulose salt in the aqueous positive electrode artificial electrolyte interface layer, B is the mass fraction of phytic acid compounds in the aqueous positive electrode artificial electrolyte interface layer, C is the mass fraction of tannic acid compounds in the aqueous positive electrode artificial electrolyte interface layer, D is the mass fraction of polyether compounds in the aqueous positive electrode artificial electrolyte interface layer, and E is the concentration of the coordination crosslinking agent solution used to form the coordination crosslinking component, in mol / L.
[0019] This application further regulates the interface layer of the aqueous cathode artificial electrolyte to satisfy the above-mentioned preferred relationship, making the proportions of each functional component more balanced. This is conducive to the formation of a continuous, uniform and stable three-dimensional cross-linked network. While ensuring the effective confinement of tannic acid compounds and the complexation ability of iron ions, it avoids the increase in ion transport resistance and network structure relaxation caused by excessive cross-linking or excessive hydrophilicity. This is more conducive to taking into account iron ion dissolution inhibition, interface stability, rate performance and long-cycle capacity retention.
[0020] In some embodiments, the carboxymethyl cellulose salt includes at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, potassium carboxymethyl cellulose, or ammonium carboxymethyl cellulose.
[0021] In some embodiments, the phytic acid compound includes at least one of phytic acid, sodium phytate, potassium phytate, lithium phytate, ammonium phytate, or zinc phytate.
[0022] In some embodiments, the tannic acid compounds include at least one of tannic acid, gallic acid, pyrogallic acid, catechins, or tea polyphenols.
[0023] In some embodiments, the polyether compound includes at least one of polyethylene glycol, polypropylene glycol, polyethylene glycol monomethyl ether, polyethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, or tetraethylene glycol dimethyl ether.
[0024] In some embodiments, the coordination crosslinking component is formed by the interaction of a coordination crosslinking agent solution with carboxymethyl cellulose salt, phytic acid compounds, or tannic acid compounds in the interface layer of the aqueous positive electrode artificial electrolyte.
[0025] In some embodiments, the coordination crosslinking agent solution includes, but is not limited to, an aqueous solution of zinc salt, which includes, but is not limited to, at least one of an aqueous solution of zinc sulfate, an aqueous solution of zinc trifluoromethanesulfonate, an aqueous solution of zinc perchlorate, an aqueous solution of zinc chloride, an aqueous solution of zinc acetate, or an aqueous solution of zinc nitrate.
[0026] In some embodiments, the thickness of the aqueous positive electrode artificial electrolyte interface layer is 0.05 μm to 10 μm, for example, it can be 0.05 μm, 0.08 μm, 0.1 μm, 0.2 μm, 0.5 μm, 1 μm, 2 μm, 5 μm, 8 μm or 10 μm, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable.
[0027] In some embodiments, the thickness of the aqueous positive electrode artificial electrolyte interface layer is 0.1 μm to 5 μm, for example, it can be 0.1 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable.
[0028] In a second aspect, this application provides a positive electrode sheet, including a positive current collector and a positive active material layer disposed on at least one side of the positive current collector, wherein an artificial electrolyte interface layer is disposed on the surface of the positive active material layer away from the positive current collector, and the artificial electrolyte interface layer includes the aqueous positive electrode artificial electrolyte interface layer according to the first aspect.
[0029] In some embodiments, the positive electrode active material of the positive electrode active material layer includes at least one of lithium iron phosphate, carbon-coated lithium iron phosphate, or doped and modified lithium iron phosphate.
[0030] In some preferred embodiments, the doping element in the doped modified lithium iron phosphate includes at least one of Mg, Ti, Al, Zr, Nb, V, Zn, Mn, Co, Ni, Na, K, Mo, W, B, F, N, or S.
[0031] Thirdly, this application provides a method for preparing a positive electrode sheet according to the second aspect, the method comprising the following steps: A positive electrode precursor containing a positive electrode active material layer is prepared. The positive electrode precursor includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector. A mixed slurry is obtained by mixing carboxymethyl cellulose salt, phytic acid compounds, tannic acid compounds, and polyether compounds with water; the mixed slurry is then coated onto the surface of the positive electrode active material layer in one step and pre-dried until there is no free liquid water on the surface to obtain a positive electrode intermediate. A coordination crosslinking agent solution is dropped onto the surface of the positive electrode intermediate to wet the positive electrode intermediate, and then dried to obtain the positive electrode.
[0032] In some embodiments, the preparation method of the positive electrode precursor includes the following steps: mixing and dispersing the positive electrode active material, conductive agent and binder in N-methylpyrrolidone solvent to obtain a positive electrode slurry; coating the positive electrode slurry onto at least one side of the surface of the positive electrode current collector, and obtaining the positive electrode precursor after drying and rolling.
[0033] As an example, the positive electrode active material includes at least one of lithium iron phosphate, carbon-coated lithium iron phosphate, or doped and modified lithium iron phosphate.
[0034] Specifically, the doping element in the doped modified lithium iron phosphate includes at least one of Mg, Ti, Al, Zr, Nb, V, Zn, Mn, Co, Ni, Na, K, Mo, W, B, F, N, or S.
[0035] As an example, the conductive agent includes, but is not limited to, at least one of conductive carbon black, acetylene black, carbon nanotubes, or graphene.
[0036] As an example, the adhesive includes, but is not limited to, at least one of polyvinylidene fluoride and polytetrafluoroethylene.
[0037] Fourthly, this application provides an aqueous battery, which includes a positive electrode, a negative electrode, an aqueous electrolyte, and a separator, wherein the positive electrode includes the positive electrode according to the second aspect.
[0038] In some embodiments, the negative electrode active material of the negative electrode sheet includes at least one of zinc foil, zinc sheet, zinc powder electrode, zinc alloy electrode, or surface-modified zinc electrode.
[0039] In some embodiments, the aqueous electrolyte includes zinc salt, lithium salt, and water.
[0040] In some embodiments, the zinc salt includes, but is not limited to, at least one of zinc sulfate, zinc trifluoromethanesulfonate, zinc perchlorate, zinc chloride, zinc acetate, or zinc nitrate.
[0041] In some embodiments, the lithium salt includes, but is not limited to, at least one of lithium sulfate, lithium trifluoromethanesulfonate, lithium perchlorate, lithium chloride, lithium acetate, lithium nitrate, lithium bis(trifluoromethanesulfonyl)imide, or lithium bis(fluorosulfonyl)imide.
[0042] In some embodiments, the concentration of zinc salt in the aqueous electrolyte is 0.1 mol / L to 5 mol / L, and the concentration of lithium salt is 0.1 mol / L to 5 mol / L.
[0043] Specifically, the concentration of zinc salt can be, for example, 0.1 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, or 5 mol / L, and the concentration of lithium salt can be, for example, 0.1 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, or 5 mol / L, and is not limited to the listed values; other unlisted values within this range are also applicable.
[0044] The numerical range described in this application includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values included in the range.
[0045] Compared with the prior art, this application has the following advantages: This application provides an artificial electrolyte interface layer suitable for aqueous cathodes, which can reduce the continuous dissolution and migration of iron ions in lithium iron phosphate cathodes without significantly hindering ion transport, stabilize the cathode / electrolyte interface, and thus improve the cycle stability of aqueous batteries.
[0046] Specifically, the hydroxyl and carboxyl groups on the carboxymethyl cellulose salt molecular chain and the phosphate and hydroxyl groups in phytic acid compounds can form a primary three-dimensional network through multi-site hydrogen bonding and molecular chain entanglement. Under the action of the precursor solution forming the coordination crosslinking component, polyvalent metal ions can further coordinate with carboxyl groups, phosphate groups, and / or phenolic hydroxyl groups in tannic acid compounds at multiple sites, further solidifying the primary three-dimensional network. Tannic acid compounds are confined within the three-dimensional crosslinking network, and their polyphenolic structure can complex with iron ions dissolved from the lithium iron phosphate cathode, thereby reducing the continuous migration of iron ions in the electrolyte and further inducing the dissolution of the cathode material. Polyether compounds can improve the hydrophilicity and flexibility of the artificial electrolyte interface layer, helping to maintain the wetting of the interface layer by the aqueous electrolyte and reduce ion transport resistance. The coordination crosslinking component can further enhance the crosslinking degree, water resistance, and interface stability of the artificial electrolyte interface layer.
[0047] Compared with aqueous cathode materials without an artificial electrolyte interface layer, the artificial cathode interface layer provided in this application can effectively alleviate the problem of iron ion dissolution in aqueous electrolytes of lithium iron phosphate cathode materials, reduce the loss of cathode active materials, suppress side reactions at the cathode / electrolyte interface, and thus improve the capacity retention, rate performance and cycle stability of aqueous batteries during long-term cycling. Attached Figure Description
[0048] Figure 1 This is a schematic diagram of the artificial electrolyte interface layer and the positive electrode containing it applied for by the applicant.
[0049] Figure 2 This is a comparison chart showing the iron ion dissolution rate calculated based on ICP results for the aqueous zinc-lithium hybrid batteries prepared in Examples 1 to 4, Example 9, Example 10, and Comparative Examples 1 to 6.
[0050] Figure 3 The curves show the comparison of the cycling performance of the aqueous zinc-lithium hybrid batteries prepared in Examples 1 to 3 and Comparative Example 1 at a 1C rate.
[0051] Figure 4 The curves show the rate performance comparison of the aqueous zinc-lithium hybrid batteries prepared in Example 1, Comparative Example 1, and Comparative Example 4 at different rates.
[0052] Figure 5 The graph shows a comparison of the capacity retention and average coulombic efficiency of the aqueous zinc-lithium hybrid batteries prepared in Examples 1, 4, 9, 10, and Comparative Examples 2, 5, and 6 after cycling. Detailed Implementation
[0053] The technical solution of this application will be further described below with reference to specific embodiments and accompanying drawings. Those skilled in the art should understand that the embodiments described are merely illustrative of this application and should not be considered as specific limitations thereof. Raw materials and equipment not specifically described can be obtained through conventional commercial means; experimental methods not specifically described are conventional methods in the art.
[0054] Unless otherwise stated, the mass percentages of each component relative to carboxymethyl cellulose salt in the following examples are based on the effective ingredient; the amount of phytic acid aqueous solution added is calculated based on the actual mass of phytic acid therein; the polyethylene glycol used is polyethylene glycol with an average molecular weight of 400; the thickness of the artificial electrolyte interface layer is the average thickness obtained by cross-sectional morphology testing after drying.
[0055] Example 1 This embodiment provides an aqueous positive electrode artificial electrolyte interface layer and a positive electrode sheet containing the interface layer. The materials of the aqueous positive electrode artificial electrolyte interface layer include sodium carboxymethyl cellulose, phytic acid, tannic acid, polyethylene glycol, and zinc salt coordination crosslinking components.
[0056] In this process, sodium carboxymethyl cellulose and phytic acid form a three-dimensional cross-linked network, tannic acid is confined within this network, and zinc salt coordination cross-linking components are distributed throughout the network. The zinc salt coordination cross-linking components are formed by the interaction of zinc sulfate aqueous solution with sodium carboxymethyl cellulose, phytic acid, and tannic acid in the interface layer of the aqueous positive electrode artificial electrolyte. Specifically, as shown... Figure 1 As shown.
[0057] This embodiment also provides a method for preparing the above-mentioned aqueous positive electrode artificial electrolyte interface layer and the positive electrode sheet containing it, which includes the following steps: Carbon-coated lithium iron phosphate cathode active material, Super-P conductive agent, and polyvinylidene fluoride binder were mixed and dispersed in N-methylpyrrolidone solvent at a mass ratio of 8:1:1, and the mixture was stirred evenly to obtain a cathode slurry with a solid content of 45%. This cathode slurry was coated onto the current collector side of a carbon-coated stainless steel foil, pre-dried at 80°C for 2 hours, rolled, and then vacuum-dried at 100°C for 8 hours to obtain the cathode precursor. The areal loading of the cathode active material in the cathode precursor was controlled to be 3.0 ± 0.2 mg / cm³. 2 .
[0058] Take 20.00 g of a 1.0% sodium carboxymethyl cellulose aqueous solution, wherein the mass of sodium carboxymethyl cellulose is 0.200 g; add 0.040 g of a 50% phytic acid aqueous solution to make the effective mass of phytic acid 0.020 g, i.e., B / A = 0.1; add 0.010 g of tannic acid to make C / A = 0.05; add 0.010 g of polyethylene glycol to make D / A = 0.05. Stir for 2 h and degas to obtain an artificial electrolyte interface layer slurry; uniformly coat the above artificial electrolyte interface layer slurry onto the surface of the positive electrode active material layer, and pre-dry at 40℃ for 10 min until there is no free liquid water on the surface to obtain the positive electrode intermediate.
[0059] According to 40 μL / cm 2 A zinc sulfate aqueous solution with a concentration of E=0.05mol / L was dropped onto the surface of the above-mentioned positive electrode intermediate to wet the positive electrode intermediate. After standing for 10 minutes, it was vacuum dried at 60°C for 6 hours to form an artificial electrolyte interface layer with an average thickness of 0.8±0.2μm, thus obtaining the positive electrode.
[0060] In summary, the interface layer of the artificial electrolyte in the aqueous cathode satisfies the following relationship: 0.03≤B / A=0.1≤0.5, 0.005≤C / A=0.05≤0.3, 0.01≤D / A=0.05≤0.3, 0.001≤E=0.05≤0.5.
[0061] Example 2 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of tannic acid added was adjusted to 0.020g, so that C / A=0.1, and the thickness of the final artificial electrolyte interface layer was 0.9±0.2μm. All other aspects are the same as in Example 1.
[0062] Example 3 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of tannic acid added was adjusted to 0.004g, so that C / A=0.02, and the thickness of the artificial electrolyte interface layer formed was 0.8±0.2μm. All other aspects are the same as in Example 1.
[0063] Example 4 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of phytic acid added is adjusted to 0.030g, the amount of tannic acid added is 0.010g, and the amount of polyethylene glycol added is 0.020g, so that B / A=0.15, C / A=0.05, and D / A=0.1, and the zinc sulfate aqueous solution is replaced with a zinc trifluoromethanesulfonate aqueous solution with a molar concentration of 0.10mol / L. The thickness of the artificial electrolyte interface layer formed is 2.0±0.3μm. All other aspects are the same as in Example 1.
[0064] Example 5 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of phytic acid added was adjusted to 0.010 g, the amount of tannic acid added to 0.004 g, the amount of polyethylene glycol added to 0.006 g, and the concentration of zinc sulfate aqueous solution to 0.01 mol / L, so that B / A=0.05, C / A=0.02, D / A=0.03, and E=0.01, and the thickness of the final artificial electrolyte interface layer was 0.6 ± 0.2 μm. All other aspects were the same as in Example 1.
[0065] Example 6 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of phytic acid added was adjusted to 0.040g, the amount of tannic acid added to 0.030g, the amount of polyethylene glycol added to 0.030g, and the concentration of zinc sulfate aqueous solution to 0.2mol / L, so that B / A=0.2, C / A=0.15, D / A=0.15, and E=0.2. The thickness of the artificial electrolyte interface layer formed in the end was 1.3±0.2μm. All other aspects were the same as in Example 1.
[0066] Example 7 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of phytic acid added was adjusted to 0.006 g, the amount of tannic acid added to 0.001 g, the amount of polyethylene glycol added to 0.002 g, and the concentration of zinc sulfate aqueous solution to 0.001 mol / L, so that B / A=0.03, C / A=0.005, D / A=0.01, and E=0.001. The thickness of the artificial electrolyte interface layer formed in the end is 0.5 ± 0.2 μm. All other aspects are the same as in Example 1.
[0067] Example 8 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of phytic acid added is adjusted to 0.100g, the amount of tannic acid added is 0.060g, the amount of polyethylene glycol added is 0.060g, and the concentration of zinc sulfate aqueous solution is 0.5mol / L, so that B / A=0.5, C / A=0.3, D / A=0.3, and E=0.5. The thickness of the artificial electrolyte interface layer formed is 1.8±0.3μm. All other aspects are the same as in Example 1.
[0068] Example 9 The difference between this embodiment and Embodiment 1 is that phytic acid is replaced with an equal mass of sodium phytate; otherwise, they are the same as in Embodiment 1.
[0069] Example 10 The difference between this embodiment and Example 1 is that sodium carboxymethyl cellulose is replaced with an equal mass of lithium carboxymethyl cellulose, tannic acid is replaced with an equal mass of gallic acid, polyethylene glycol is replaced with an equal mass of polyethylene glycol monomethyl ether (average molecular weight of 500), and zinc sulfate aqueous solution is replaced with zinc acetate aqueous solution of equal molar concentration. All other aspects are the same as in Example 1.
[0070] Example 11 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of phytic acid added was adjusted to 0.002g, so that B / A=0.01, and the thickness of the artificial electrolyte interface layer formed was 0.7±0.2μm. All other aspects are the same as in Example 1.
[0071] Example 12 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of phytic acid added was adjusted to 0.160g, so that B / A=0.8, and the thickness of the final artificial electrolyte interface layer was 1.5±0.3μm. All other aspects are the same as in Example 1.
[0072] Example 13 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of tannic acid added was adjusted to 0.120g, so that C / A=0.6, and the thickness of the final artificial electrolyte interface layer was 1.4±0.3μm. All other aspects are the same as in Example 1.
[0073] Example 14 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of polyethylene glycol added was adjusted to 0.001g, so that D / A=0.005, and the thickness of the final artificial electrolyte interface layer was 0.7±0.2μm. All other aspects are the same as in Example 1.
[0074] Example 15 The difference between this embodiment and Example 1 is that, during the preparation process, the amount of polyethylene glycol added was adjusted to 0.120g, so that D / A=0.6, and the thickness of the final artificial electrolyte interface layer was 1.4±0.3μm. All other aspects are the same as in Example 1.
[0075] Except for the differences in the types, amounts or parameters of components explicitly listed above, the preparation steps and process conditions in Examples 5-15 are the same as in Example 1.
[0076] Comparative Example 1 The difference between this comparative example and Example 1 is that no artificial electrolyte interface layer is provided on the surface of the positive electrode active material layer of the positive electrode sheet; otherwise, they are the same as in Example 1.
[0077] Comparative Example 2 The difference between this comparative example and Example 1 is that the material of the aqueous positive electrode artificial electrolyte interface layer does not include tannic acid, but only includes sodium carboxymethyl cellulose, phytic acid, polyethylene glycol and zinc salt coordination crosslinking components. Also, the artificial electrolyte interface layer slurry in the preparation method does not include tannic acid. All other aspects are the same as in Example 1.
[0078] Comparative Example 3 The difference between this comparative example and Example 1 is that the material of the aqueous positive electrode artificial electrolyte interface layer does not include phytic acid, but only includes sodium carboxymethyl cellulose, tannic acid, polyethylene glycol and zinc salt coordination crosslinking components. Also, the artificial electrolyte interface layer slurry in the preparation method does not include phytic acid. All other aspects are the same as in Example 1.
[0079] Comparative Example 4 The difference between this comparative example and Example 1 is that the material of the aqueous positive electrode artificial electrolyte interface layer does not include polyethylene glycol, but only includes sodium carboxymethyl cellulose, tannic acid, phytic acid and zinc salt coordination crosslinking components. Also, the artificial electrolyte interface layer slurry in the preparation method does not include polyethylene glycol. All other aspects are the same as in Example 1.
[0080] Comparative Example 5 The difference between this comparative example and Example 1 is that, in the preparation process, the positive electrode intermediate is not treated by adding zinc sulfate aqueous solution with a concentration of E=0.05mol / L, but is instead directly vacuum dried at 60°C for 6 hours. All other aspects are the same as in Example 1.
[0081] Application Example 1-15 and Comparative Application Example 1-5 The positive electrode sheets prepared in the above embodiments and comparative examples are assembled to obtain a coin cell. The preparation method is as follows: A mixed aqueous solution of zinc trifluoromethanesulfonate (1.0 mol / L) and lithium trifluoromethanesulfonate (1.0 mol / L) was used as the aqueous electrolyte. A glass fiber membrane was used as the separator, and zinc foil was used as the negative electrode. A CR2032 coin cell was assembled, with 100 μL of electrolyte added to each cell. The above-mentioned uniform electrolyte is only used to compare the embodiments with the comparative examples under the same conditions and does not constitute a limitation on the type of aqueous electrolyte used in this application.
[0082] Comparative Application Example 6 The difference between this comparative application example and Comparative Application Example 1 is that the aqueous electrolyte also contains 0.010g of tannic acid, while all other aspects are the same as in Comparative Application Example 1.
[0083] Test conditions The button cells assembled from the above application examples and comparative application examples were subjected to performance testing, and the testing methods are as follows: (1) Iron leaching test The coin cells assembled in the above application examples and comparative application examples were cycled 100 times at 1C, then disassembled, and the electrolyte was collected and diluted to volume with a 2% (w / w) nitric acid aqueous solution. The iron concentration was determined using ICP-OES. All samples used the same initial electrolyte volume, dilution factor, and instrument parameters, as detailed below. Figure 2 As shown.
[0084] (2) Cyclic performance test like Figure 3 As shown, the coin cells assembled in the above application examples and comparative application examples were left to stand at room temperature (25°C) for 12 hours, activated for 3 cycles at a 0.1C rate, and then subjected to constant current charge-discharge cycles at a 1C rate within a voltage range of 1.0V to 1.9V; 1C was defined as 170mA / g. The initial discharge specific capacity, the discharge specific capacity at the 500th cycle, the capacity retention rate, and the average coulombic efficiency were recorded. The capacity retention rate was calculated as the ratio of the discharge specific capacity at the 500th cycle to the initial discharge specific capacity. At least three parallel cells were tested for each sample group, and the average value was used as the result.
[0085] (3) Ratio performance test like Figure 4 As shown, within the voltage range of 1.0V to 1.9V, charge and discharge were performed in the order of 0.2C, 0.5C, 1C, 2C, 5C and 0.2C. Each rate was tested for 5 cycles, and the average discharge specific capacity at each rate and the capacity recovery rate after returning to 0.2C were recorded.
[0086] The test results are shown in Table 1.
[0087] Table 1 Depend on Figure 2 It can be seen that the iron dissolution rates in Application Examples 1-4, 9, and 10 are 0.022 mg / (g·d) to 0.058 mg / (g·d), which are significantly lower than the iron dissolution rates in Comparative Application Examples 1-6, i.e., 0.141 mg / (g·d) to 0.218 mg / (g·d). This indicates that the aqueous cathode artificial electrolyte interface layer provided in this application can effectively suppress the iron dissolution phenomenon in the lithium iron phosphate cathode. Among them, the iron dissolution rate in Application Example 4 is the lowest, specifically 0.022 mg / (g·d), and in Application Example 1 it is 0.032 mg / (g·d), both significantly lower than the 0.192 mg / (g·d) in Comparative Application Example 1 without an artificial electrolyte interface layer.
[0088] Depend on Figure 3It can be seen that after 500 cycles at 1C rate, the discharge specific capacity of Application Example 1, Application Example 2 and Application Example 3 remained at approximately 140 mAh / g, 119 mAh / g and 127 mAh / g, respectively, while that of Application Example 1 dropped to approximately 56 mAh / g. This indicates that setting an artificial electrolyte interface layer can significantly slow down the capacity decay during long-term cycling.
[0089] Depend on Figure 4 As can be seen, at a 5C rate, the discharge specific capacity of Application Example 1 remains at approximately 105 mAh / g, which is higher than approximately 72 mAh / g of Comparative Application Example 4 and approximately 53 mAh / g of Comparative Application Example 1. After recovering to 0.2C, the discharge specific capacity of Application Example 1 recovers to approximately 150 mAh / g, indicating that it has good rate reversibility.
[0090] Based on Table 1 Figure 5 As can be seen, the capacity retention rates of Application Examples 1, 4, 9, and 10 were 94.10%, 88.90%, 91.80%, and 90.60%, respectively, and the average coulombic efficiencies were 99.45%, 98.94%, 99.25%, and 99.10%, respectively, which are generally superior to those of Comparative Application Examples 2, 5, and 6. These results indicate that carboxymethyl cellulose salt, phytic acid compounds, tannic acid compounds, polyether compounds, and coordination crosslinking components can produce a synergistic effect, thereby balancing iron dissolution inhibition, cathode interface stability, and ion transport performance.
[0091] Comparing Application Examples 1 and 11-15, it can be seen that by adjusting B / A, C / A, D / A, and E to be within the above range, this application achieves a balance between the network crosslinking sites provided by phytic acid compounds, the iron ion complexing sites provided by tannic acid compounds, the hydrophilicity and flexibility adjustment provided by polyether compounds, and the secondary crosslinking strength provided by the coordination crosslinking components. This is beneficial for balancing the structural integrity, iron ion capture capacity, and ion transport performance of the aqueous positive electrode artificial electrolyte interface layer.
[0092] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.
Claims
1. An aqueous positive electrode artificial electrolyte interface layer, characterized in that, The material of the aqueous positive electrode artificial electrolyte interface layer includes carboxymethyl cellulose salt, phytic acid compounds, tannic acid compounds, polyether compounds, and coordination crosslinking components; The carboxymethyl cellulose salt and the phytic acid compound form a three-dimensional cross-linked network, the tannic acid compound is confined within the three-dimensional cross-linked network, and the coordination cross-linking component is distributed within the three-dimensional cross-linked network.
2. The aqueous positive electrode artificial electrolyte interface layer according to claim 1, characterized in that, The aqueous positive electrode artificial electrolyte interface layer satisfies the following relationship: 0.03≤B / A≤0.5, 0.005≤C / A≤0.3, 0.01≤D / A≤0.3, 0.001≤E≤0.5; Wherein, A is the mass fraction of carboxymethyl cellulose salt in the aqueous positive electrode artificial electrolyte interface layer, B is the mass fraction of phytic acid compounds in the aqueous positive electrode artificial electrolyte interface layer, C is the mass fraction of tannic acid compounds in the aqueous positive electrode artificial electrolyte interface layer, D is the mass fraction of polyether compounds in the aqueous positive electrode artificial electrolyte interface layer, and E is the concentration of the coordination crosslinking agent solution used to form the coordination crosslinking component, in mol / L.
3. The aqueous positive electrode artificial electrolyte interface layer according to claim 1 or 2, characterized in that, The aqueous positive electrode artificial electrolyte interface layer satisfies the following relationship: 0.05≤B / A≤0.2, 0.02≤C / A≤0.15, 0.03≤D / A≤0.15, 0.01≤E≤0.2; Wherein, A is the mass fraction of carboxymethyl cellulose salt in the aqueous positive electrode artificial electrolyte interface layer, B is the mass fraction of phytic acid compounds in the aqueous positive electrode artificial electrolyte interface layer, C is the mass fraction of tannic acid compounds in the aqueous positive electrode artificial electrolyte interface layer, D is the mass fraction of polyether compounds in the aqueous positive electrode artificial electrolyte interface layer, and E is the concentration of the coordination crosslinking agent solution used to form the coordination crosslinking component, in mol / L.
4. The aqueous positive electrode artificial electrolyte interface layer according to any one of claims 1 to 3, characterized in that, The carboxymethyl cellulose salt includes at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, potassium carboxymethyl cellulose, or ammonium carboxymethyl cellulose. And / or, the phytic acid compounds include at least one of phytic acid, sodium phytate, potassium phytate, lithium phytate, ammonium phytate, or zinc phytate; And / or, the tannic acid compounds include at least one of tannic acid, gallic acid, pyrogallic acid, catechins, or tea polyphenols; And / or, the polyether compound includes at least one of polyethylene glycol, polypropylene glycol, polyethylene glycol monomethyl ether, polyethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether or tetraethylene glycol dimethyl ether; And / or, the coordination crosslinking component is formed by the reaction of a coordination crosslinking agent solution with carboxymethyl cellulose salt, phytic acid compounds, or tannic acid compounds in the interface layer of the aqueous positive electrode artificial electrolyte.
5. The aqueous positive electrode artificial electrolyte interface layer according to any one of claims 1 to 4, characterized in that, The thickness of the aqueous positive electrode artificial electrolyte interface layer is 0.05 μm to 10 μm.
6. A positive electrode sheet, comprising a positive current collector and a positive active material layer disposed on at least one side of the positive current collector, characterized in that, An artificial electrolyte interface layer is provided on the surface of the positive electrode active material layer along the side away from the positive electrode current collector, and the artificial electrolyte interface layer includes the aqueous positive electrode artificial electrolyte interface layer according to any one of claims 1 to 5.
7. The positive electrode sheet according to claim 6, characterized in that, The positive electrode active material of the positive electrode active material layer includes at least one of lithium iron phosphate, carbon-coated lithium iron phosphate, or doped and modified lithium iron phosphate. The doping element in the doped modified lithium iron phosphate includes at least one of Mg, Ti, Al, Zr, Nb, V, Zn, Mn, Co, Ni, Na, K, Mo, W, B, F, N, or S.
8. A method for preparing a positive electrode sheet according to claim 6 or 7, characterized in that, The preparation method includes the following steps: A positive electrode precursor containing a positive electrode active material layer is prepared, wherein the positive electrode precursor includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector; A mixed slurry is obtained by mixing carboxymethyl cellulose salt, phytic acid compounds, tannic acid compounds, and polyether compounds with water; the mixed slurry is then coated onto the surface of the positive electrode active material layer in one step and pre-dried until there is no free liquid water on the surface to obtain a positive electrode intermediate. A coordination crosslinking agent solution is dropped onto the surface of the positive electrode intermediate to wet the positive electrode intermediate, and then dried to obtain the positive electrode.
9. A water-based battery, characterized in that, The aqueous battery includes a positive electrode, a negative electrode, an aqueous electrolyte, and a separator, wherein the positive electrode includes the positive electrode according to claim 6 or 7.
10. The aqueous battery according to claim 9, characterized in that, The negative electrode active material of the negative electrode sheet includes at least one of zinc foil, zinc sheet, zinc powder electrode, zinc alloy electrode or surface-modified zinc electrode. And / or, the aqueous electrolyte comprises zinc salt, lithium salt and water; The concentration of zinc salt in the aqueous electrolyte is 0.1 mol / L to 5 mol / L, and the concentration of lithium salt is 0.1 mol / L to 5 mol / L.