An integrated method for segmented formation and venting of cylindrical aluminum-cased battery cells

By employing multi-parameter closed-loop control and micro-positive pressure transition design, the dynamic adjustment problem of formation and venting processes in the production of cylindrical aluminum-shell lithium-ion cells was solved, resulting in reduced cell internal resistance, uniform SEI film growth, and extended cycle life, thereby improving production consistency and yield.

CN123120939APending Publication Date: 2026-11-17GUIZHOU GRACE HUMMER NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611168875.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the current production process of cylindrical aluminum-shell lithium-ion cells, the formation and venting processes cannot be dynamically adjusted according to the real-time gas generation rate and surface temperature, resulting in problems such as internal gas expansion, uneven SEI film growth, electrolyte backflow, poor product consistency, and short cycle life. In particular, the adaptability to high gas generation materials and different structural specifications is insufficient.

Method used

Employing multi-parameter closed-loop control, combined with micro-positive pressure transition and gas production component monitoring, the charging current and exhaust parameters are dynamically adjusted by real-time acquisition of cell voltage, surface temperature, and gas production rate. Combined with positive pressure backflush and staged negative pressure design, intelligent management and control of the entire formation and exhaust process are achieved.

Benefits of technology

It achieves reduced cell internal resistance, uniform SEI film growth, elimination of electrolyte backflow, improved batch consistency, extended cycle life, and increased production yield. In particular, it significantly enhances adaptability to high-gas-producing materials and different structural specifications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120939A_ABST
    Figure CN123120939A_ABST
Patent Text Reader

Abstract

This invention discloses an integrated method for segmented formation and venting of cylindrical aluminum-shell battery cells, belonging to the field of lithium-ion battery manufacturing technology. This invention integrates electrolyte injection and settling, pre-charging and pre-venting, multi-parameter linked segmented formation, graded venting, constant voltage charging, post-settling, and re-inspection sealing into a single process flow. It employs closed-loop dynamic control of three parameters: voltage, surface temperature, and gas generation rate, and sets a micro-positive pressure holding transition section between each formation stage to prevent electrolyte backflow. Further optimization schemes include online detection of gas generation components, coordinated adaptation of venting structure and process, positive pressure backflushing, and dedicated parameter adjustment for silicon-carbon anodes. This invention solves the problems of fixed formation process parameters, easy venting blockage, weak side reaction control, and poor material and structural compatibility in traditional processes, effectively improving cell consistency, cycle life, and production yield, and is suitable for the large-scale production of various cylindrical aluminum-shell lithium-ion battery cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery manufacturing technology, specifically relating to an integrated method for segmented formation and venting of cylindrical aluminum-cased battery cells. Background Technology

[0002] In the production of cylindrical aluminum-cased lithium-ion cells, formation and venting are the core processes that determine the cell's electrochemical performance, cycle life, and safety. After the cell is filled with electrolyte, the electrodes and electrolyte undergo an electrochemical reaction to form an SEI film, accompanied by the generation of a large amount of gas. If the generated gas cannot be vented in a timely and effective manner, it can easily cause internal gas expansion within the cell, uneven SEI film growth, and blockage of the venting channels by electrolyte droplets or bubbles. Ultimately, this leads to problems such as high internal resistance, poor consistency, and rapid decay of cycle life.

[0003] Currently, the mainstream formation process in the industry mostly adopts a fixed current segmented formation + centralized negative pressure exhaust mode. The process parameters are fixed throughout the process, and production is completed by manually preset parameters, which has many defects: (1) It is impossible to dynamically adjust the charging and exhaust parameters according to the real-time gas production rate and surface temperature of the cell, and the side reactions of the cell are difficult to suppress; (2) After simple negative pressure exhaust, electrolyte backflow is likely to occur, which further damages the electrode interface; (3) For high gas production materials such as silicon-carbon composite negative electrode and aluminum shell cells with different structural specifications, the general process adaptability is poor; (4) Relying only on voltage and current for basic monitoring, it is impossible to identify the severity of the side reactions inside the cell, and the product yield is difficult to further improve.

[0004] In addition, although existing technologies include single improvement methods such as segmented formation, negative pressure exhaust, and pipeline dredging, they are all simple superpositions of conventional technologies, and there are obvious shortcomings in the degree of process refinement and adaptability. Summary of the Invention

[0005] In order to overcome the above-mentioned defects of the prior art, the present invention aims to provide an integrated method for segmented formation and degassing of cylindrical aluminum-shell battery cells. Through multi-parameter closed-loop control, micro-positive pressure transition, gas generation component monitoring, and structural process coordination, the invention achieves intelligent management and control of the entire formation and degassing process, thereby improving cell consistency, cycle life and production yield.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: A method for integrated segmented formation and venting of cylindrical aluminum-cased battery cells includes the following steps: Step 1: Vacuum settling after liquid injection; Place the cylindrical aluminum shell battery cell that has been injected with liquid into the formation cabinet and settling for 8 to 12 hours under the conditions of 25℃~35℃ and -30~-40kPa vacuum. Step 2: Pre-charge and pre-venting; charge the battery cell continuously for 5 to 10 minutes with a pre-charge current of 0.02C to 0.05C, and simultaneously open the venting valve to perform the first pre-venting. Step 3: Multi-parameter linkage segmented formation and graded exhaust; the battery cell formation voltage is used as the segmentation benchmark to divide the battery cell into three charging stages. The battery cell voltage, surface temperature and internal gas generation rate are collected in real time to form a closed-loop control. After each charging stage, the corresponding graded exhaust operation is performed, and a micro-positive pressure holding transition section is set between two adjacent charging stages. First stage formation: Charge the cell with a current of 0.10C to 0.15C until the cell voltage reaches 2.8V to 3.0V; after charging, apply a negative pressure of -40 to -50kPa for venting for 3 to 5 minutes; after venting, introduce dry inert gas at 0.02 to 0.05MPa and maintain the pressure for 1 to 2 seconds to form a slight positive pressure transition. The second stage of formation: continue charging with a current of 0.18C to 0.25C until the cell voltage reaches 3.2V to 3.4V; after charging is completed, apply a negative pressure of -50 to -60kPa to exhaust the air for 2 to 4 minutes; after exhausting the air, introduce dry inert gas of 0.02 to 0.05MPa and maintain the pressure for 1 to 2 seconds to form a slight positive pressure transition; The third stage of formation: continue charging at a current of 0.30C to 0.50C until the cell voltage reaches 3.65V to 4.20V; after charging is completed, apply a negative pressure of -30 to -40kPa to exhaust the air for 2 to 3 minutes. Specifically, when the real-time gas production rate exceeds the preset threshold (5 ml / min), the absolute value of the exhaust negative pressure increases by 5–8 kPa and the exhaust time is extended by 0.5–1 min in the corresponding stage; when the cell surface temperature exceeds 40°C, the charging current is reduced by 10% in the corresponding stage. Step 4: Constant voltage supplemental charging and continuous venting; using the termination voltage of the third stage of formation in step 3 as the constant voltage value, charge the cell at a constant voltage until the charging current drops below 0.02C; keep the venting valve open throughout the charging process, and maintain the venting negative pressure at -20 to -30 kPa. Step 5: Vacuum settling after formation; the battery cells that have been charged are settling at 30℃~40℃ and -20~-30kPa vacuum for 4~6 hours; Step 6: Re-inspection and sealing; Test the open circuit voltage and internal resistance of the battery cell, and seal the battery cell after passing the test.

[0007] Preferred configuration: After the completion of the second stage of formation in the third step and the completion of the micro-positive pressure transition, before the start of the third stage of formation, a positive pressure backflushing venting operation is added: 0.1-0.3 MPa of dry inert gas is introduced into the cell, the pressure is maintained for 2-5 seconds, and then the pressure is quickly released to use the instantaneous pressure difference between positive and negative pressure to clean the air bubbles and electrolyte droplets adhering to the inner wall of the venting channel; at the same time, the first discharge capacity is defined as the actual measured discharge capacity of the cell after the first stage of formation, and the nominal capacity is the design rated capacity of the cell. When the first discharge capacity is lower than 30% of the nominal capacity, the negative pressure of the venting in the third stage of formation is adjusted to -35 to -48 kPa.

[0008] Preferably, the cylindrical aluminum shell battery cell negative electrode material contains 5% to 15% silicon-carbon composite negative electrode material by mass; in view of the high gas production characteristics of silicon-carbon negative electrode, the formation current of the first stage and the second stage are reduced by 0.01C to 0.02C at the lower limit of the corresponding range, and the formation exhaust negative pressure of the third stage is adjusted to -35 to -45kPa.

[0009] Preferred option: The third step adds an online detection and linkage control step for gas-generating components: real-time detection of the volume percentage of CO, CO2, and alkane gases in the exhaust gas. When the volume percentage of alkane gases exceeds 15%, the overall charging current is reduced by 15%, and the absolute value of exhaust negative pressure in all stages is uniformly increased by 6-10 kPa.

[0010] Preferred: The diameter of the exhaust port of the cylindrical aluminum shell battery cell is limited to 0.8 to 1.2 mm, and the inert gas flow rate in the micro-positive pressure transition section is controlled to be 5 to 10 L / min, so that the process parameters and the battery cell exhaust structure are synergistically adapted.

[0011] Preferred conditions: The first step of settling conditions is a temperature of 30±2℃, a vacuum of -35kPa, and a settling time of 10 hours; the fifth step of settling conditions is a temperature of 35±2℃, a vacuum of -25kPa, and a settling time of 5 hours; in the third step, the first stage formation current is 0.12C~0.13C and the charging cutoff voltage is 2.9V, the second stage formation current is 0.20C~0.22C and the charging cutoff voltage is 3.3V, and the third stage formation current is 0.35C~0.45C.

[0012] Compared with the prior art, the present invention has the following advantages: 1. Multi-parameter closed-loop dynamic control: Relying on real-time monitoring of voltage, surface temperature, and gas production rate, the charging current and exhaust parameters are dynamically adjusted to accurately suppress the side reactions of the battery cell and avoid local overheating and gas accumulation problems.

[0013] 2. Micro-positive pressure transition design: After segmented venting, a micro-positive pressure holding process is added to completely solve the problem of electrolyte backflow caused by simple negative pressure venting, and ensure uniform and stable growth of the electrode SEI film.

[0014] 3. Online monitoring of gas production components: Upgraded from monitoring the single gas production rate to gas component analysis, accurately judging the severity of side reactions and adjusting parameters accordingly, significantly improving cell safety and cycle life.

[0015] 4. Structure-process synergistic adaptation: Matching specific gas flow rates to exhaust holes of specific diameters solves the problems of uneven exhaust and poor airflow in battery cells with different shell structures, significantly improving process versatility and adaptability.

[0016] 5. Multiple anti-clogging design: The combination of positive pressure backflushing and staged negative pressure exhaust effectively cleans the deposits in the exhaust channel, reduces the probability of channel blockage, and improves production yield.

[0017] 6. Adapted for silicon-carbon composite anodes: Customized adjustment of process parameters for high-gas-producing anode materials to solve industry pain points such as difficult formation and severe gas expansion of new anode materials. Attached Figure Description

[0018] Figure 1 This is an overall process flow diagram of Embodiment 1 of the present invention; Figure 2 This is a flowchart of the refined control process of Embodiment 2 of the present invention; Figure 3 This is a flowchart illustrating the structural and technological collaborative adaptation process of Embodiment 3 of the present invention. Detailed Implementation

[0019] The principles of the present invention will now be fully explained in conjunction with specific embodiments so that those skilled in the art can fully understand and implement them. Example

[0020] like Figure 1 As shown, the integrated method for segmented formation and venting of cylindrical aluminum-cased battery cells in this embodiment includes the following steps: Step 1: Vacuum settling after liquid injection: Place the cylindrical aluminum shell battery cell with liquid injection completed into the formation cabinet, at a temperature of 30℃ and a vacuum degree of -35kPa, and let it stand for 10 hours. Step 2: Pre-charging and pre-venting: Pre-charging current 0.03C, charging time 8min, and simultaneously opening the venting valve to complete pre-venting; Step 3: Multi-parameter linkage segmented formation and staged exhaust: Preset thresholds: Gas production rate threshold is 5 mL / min, temperature warning value is 40℃; ① First stage formation: current 0.12C, charge to voltage 2.9V; after completion, exhaust under -45kPa negative pressure for 4min; introduce 0.03MPa nitrogen and maintain pressure for 1.5s to complete the micro-positive pressure transition; ② Second stage formation: Current 0.21C, charge to voltage 3.3V; after completion, exhaust under -58kPa negative pressure for 3.5min; introduce 0.03MPa nitrogen and maintain pressure for 1.5s to complete the micro-positive pressure transition; ③ Third stage formation: current 0.40C, charging to voltage 4.0V; after completion, -36kPa negative pressure exhaust for 2.8min; Dynamic control: If the gas production rate is >5mL / min during production, the absolute value of the negative pressure in the corresponding stage will be increased by 6kPa and the exhaust time will be increased by 0.8min; if the cell surface temperature is >40℃, the current in the corresponding stage will be reduced by 10%. S4: Constant voltage supplemental charging: Charges at a constant voltage of 4.0V until the current drops below 0.02C; maintains -25kPa negative pressure for exhaust throughout the process; S5: Vacuum settling after formation: Temperature 35℃, vacuum degree -25kPa, settling for 5h; S6: Re-inspection and sealing: Check the open circuit voltage and internal resistance, and seal the opening after passing the test.

[0021] Implementation results: No electrolyte backflow occurred in the battery cells, and the SEI film grew uniformly; the average internal resistance of the battery cells was reduced by 8% compared with the traditional fixed parameter process, and batch consistency was improved by 12%. Example

[0022] like Figure 2 As shown, the specific steps of this embodiment are as follows: Step 1: Pre-processing: The basic parameters, operation sequence, and dynamic threshold of liquid injection and settling, pre-filling and pre-venting, three-stage formation, micro-positive pressure transition, constant pressure charging, settling after formation, and re-inspection and sealing are completely consistent with those of Example 1. Step 2: Add an online gas component detection process: Install online gas component analyzers in the exhaust pipelines at each stage to detect the volume percentage of CO, CO2, and alkane gases in real time; Step 3: Linkage Control Rules: Set Judgment Threshold: When the volume ratio of alkane gases is >15%, the following adjustments will be made: the overall charging current of the entire process will be reduced by 15%; the absolute value of the exhaust negative pressure in all formation stages will be uniformly increased by 8kPa; Step 4: The remaining procedures, parameters, and equipment are the same as in Example 1.

[0023] Implementation results: It can identify severe side reactions inside the battery cell in real time and quickly adjust parameters. The capacity retention rate of the battery cell after 500 cycles is improved by 4.5% compared with Example 1. The battery cell gas defect rate is reduced to below 0.3%, and the safety is significantly improved. Example

[0024] like Figure 3As shown, the cell structure in this embodiment is limited to: a standard cylindrical aluminum shell cell with a vent hole diameter of 1.0 mm; the steps and explanations are as follows: Step 1: Pre-processing: Liquid injection and settling, pre-charging and pre-venting, three-stage formation, dynamic parameter threshold, constant voltage charging, post-formation settling, and re-inspection and sealing are all consistent with Example 1; Step 2: Structural and process constraints: The flow rate of high-purity nitrogen in all micro-positive pressure transition sections is uniformly controlled at 7L / min; The rest of the operations remain unchanged.

[0025] Implementation results: It achieves precise coupling between cell structure parameters and formation venting process, the venting channel is less likely to retain electrolyte and air bubbles, the venting smoothness is greatly improved, the process stability is strong and the product yield is high under mass production conditions.

[0026] In summary, this invention, relying on three-parameter closed-loop control combined with micro-positive pressure transition timing design, solves fundamental industry pain points in traditional fixed-parameter formation processes, such as electrolyte backflow, uneven SEI film formation, and poor batch-to-batch consistency of battery cells. It overcomes the limitations of traditional methods that only monitor macroscopic physical parameters, achieving precise suppression of microscopic side reactions within the battery cell. This significantly improves process stability and product yield under large-scale mass production conditions. Compared to existing conventional formation venting processes, this invention, through multi-dimensional innovative coupling, effectively balances battery cell formation quality, production stability, and safety performance into an integrated solution.

[0027] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any equivalent substitutions or simple improvements made within the concept and protection scope of the present invention should fall within the protection scope of the present invention.

Claims

1. A method for integrated segmented formation and venting of cylindrical aluminum-cased battery cells, characterized in that, Includes the following steps: Step 1: Vacuum settling after liquid injection; Place the cylindrical aluminum shell battery cell that has been injected with liquid into the formation cabinet and settling for 8 to 12 hours under the conditions of 25℃~35℃ and -30~-40kPa vacuum. Step 2: Pre-charge and pre-venting; charge the battery cell continuously for 5 to 10 minutes with a pre-charge current of 0.02C to 0.05C, and simultaneously open the venting valve to perform the first pre-venting. Step 3: Multi-parameter linkage segmented formation and graded exhaust; the battery cell formation voltage is used as the segmentation benchmark to divide the battery cell into three charging stages. The battery cell voltage, surface temperature and internal gas generation rate are collected in real time to form a closed-loop control. After each charging stage, the corresponding graded exhaust operation is performed, and a micro-positive pressure holding transition section is set between two adjacent charging stages. First stage formation: Charge the cell with a current of 0.10C to 0.15C until the cell voltage reaches 2.8V to 3.0V; after charging, apply a negative pressure of -40 to -50kPa for venting for 3 to 5 minutes; after venting, introduce dry inert gas at 0.02 to 0.05MPa and maintain the pressure for 1 to 2 seconds to form a slight positive pressure transition. The second stage of formation: continue charging with a current of 0.18C to 0.25C until the cell voltage reaches 3.2V to 3.4V; after charging is completed, apply a negative pressure of -50 to -60kPa to exhaust the air for 2 to 4 minutes; after exhausting the air, introduce dry inert gas of 0.02 to 0.05MPa and maintain the pressure for 1 to 2 seconds to form a slight positive pressure transition; The third stage of formation: continue charging at a current of 0.30C to 0.50C until the cell voltage reaches 3.65V to 4.20V; after charging is completed, apply a negative pressure of -30 to -40kPa to exhaust the air for 2 to 3 minutes. Specifically, when the real-time gas production rate exceeds the preset threshold, the absolute value of the exhaust negative pressure increases by 5–8 kPa and the exhaust time is extended by 0.5–1 min in the corresponding stage; when the cell surface temperature exceeds 40°C, the charging current is reduced by 10% in the corresponding stage. Step 4: Constant voltage supplemental charging and continuous venting; using the termination voltage of the third stage of formation in step 3 as the constant voltage value, charge the cell at a constant voltage until the charging current drops below 0.02C; keep the venting valve open throughout the charging process, and maintain the venting negative pressure at -20 to -30 kPa. Step 5: Vacuum settling after formation; the battery cells that have been charged are settling at 30℃~40℃ and -20~-30kPa vacuum for 4~6 hours; Step 6: Re-inspection and sealing; Test the open circuit voltage and internal resistance of the battery cell, and seal the battery cell after passing the test.

2. The integrated method for segmented formation and venting of cylindrical aluminum-cased battery cells according to claim 1, characterized in that, After the completion of the second stage of formation in the third step and the completion of the micro-positive pressure transition, before the start of the third stage of formation, a positive pressure backflushing venting operation is added: 0.1-0.3 MPa of dry inert gas is introduced into the cell, the pressure is maintained for 2-5 seconds and then the pressure is quickly released, and the instantaneous pressure difference between positive and negative pressure is used to clean the air bubbles and electrolyte droplets adhering to the inner wall of the venting channel; at the same time, the first discharge capacity is defined as the actual measured discharge capacity of the cell after the first stage of formation, and the nominal capacity is the design rated capacity of the cell. When the first discharge capacity is lower than 30% of the nominal capacity, the negative pressure of the venting in the third stage of formation is adjusted to -35 to -48 kPa.

3. The method for integrated segmented formation and venting of a cylindrical aluminum-cased battery cell according to claim 2, characterized in that, The cylindrical aluminum shell battery cell negative electrode material contains 5% to 15% silicon-carbon composite negative electrode material by mass. In view of the high gas production characteristics of silicon-carbon negative electrode, the formation current of the first stage and the second stage are reduced by 0.01C to 0.02C at the lower limit of the corresponding range, and the formation exhaust negative pressure of the third stage is adjusted to -35 to -45kPa.

4. The integrated method for segmented formation and venting of cylindrical aluminum-cased battery cells according to claim 3, characterized in that, The third step adds an online detection and linkage control step for gas production components: real-time detection of the volume ratio of CO, CO2, and alkane gases in the exhaust gas. When the volume ratio of alkane gases exceeds 15%, the overall charging current is reduced by 15%, and the absolute value of exhaust negative pressure in all stages is uniformly increased by 6-10 kPa.

5. The method for integrated segmented formation and venting of a cylindrical aluminum-cased battery cell according to claim 4, characterized in that, The diameter of the exhaust port of the cylindrical aluminum shell battery cell is limited to 0.8 to 1.2 mm, and the inert gas flow rate in the micro-positive pressure transition section is controlled to be 5 to 10 L / min, so that the process parameters and the battery cell exhaust structure are synergistically adapted.

6. The method for integrated segmented formation and venting of a cylindrical aluminum-cased battery cell according to claim 5, characterized in that, The first step of the settling condition is a temperature of 30±2℃, a vacuum of -35kPa, and a settling time of 10 hours; the fifth step of the settling condition is a temperature of 35±2℃, a vacuum of -25kPa, and a settling time of 5 hours; in the third step, the first stage formation current is 0.12C~0.13C and the charging cutoff voltage is 2.9V, the second stage formation current is 0.20C~0.22C and the charging cutoff voltage is 3.3V, and the third stage formation current is 0.35C~0.45C.