Methods and applications for the separation and repair of mixed electrode powders in decommissioned sodium-ion batteries

By combining graded weak magnetic separation with electrostatic separation, along with composite sodium replenishing agents and coating agents, the problem of separation and repair of decommissioned sodium-ion battery materials has been solved, achieving efficient and high-purity material recycling and reuse.

CN123120949APending Publication Date: 2026-11-17WELNENG ENVIRONMENTAL TECH (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611250559.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for the recovery and treatment of sodium iron phosphate positive and hard carbon negative electrodes from sodium-ion batteries suffer from problems such as wastewater discharge, high reagent recovery costs, easy damage to the crystal structure of materials, low purity of separated products, and poor recovery rate. Furthermore, the single physical sorting method results in the inclusion of a large number of impurities.

Method used

A combination of graded weak magnetic separation and electrostatic separation is used to enhance the magnetic field strength and control the ambient humidity by using magnetic conductive components to accurately separate sodium iron pyrophosphate and hard carbon materials. Composite sodium replenishing agents and coating agents are then used for repair to ensure the purity and structural integrity of the materials.

Benefits of technology

This method enables efficient separation and repair of decommissioned sodium-ion battery materials, improving separation efficiency and recovery rate while ensuring material purity and structural stability. It is suitable for the preparation of sodium-ion battery electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120949A_ABST
    Figure CN123120949A_ABST
Patent Text Reader

Abstract

This application discloses a method and application for separating and repairing mixed electrode powder from retired sodium-ion batteries, relating to the technical field of sodium-ion batteries. The method involves pre-treating the electrodes of retired sodium-ion batteries and then sequentially passing the pre-treated powder through a magnetic separator equipped with a magnetic guide to perform primary magnetic separation, thereby obtaining conductive primary sodium iron pyrophosphate and insulating primary hard carbon material. Secondary magnetic separation is then performed to obtain crude sodium iron pyrophosphate and crude hard carbon. These crude materials are then subjected to electrostatic separation under specific environmental humidity and friction speed conditions, followed by repair to obtain repaired materials. By converging and enhancing the local magnetic field strength through the magnetic guide, the weak paramagnetism of sodium iron pyrophosphate is amplified, making it easier to adsorb. Combined with electrostatic separation, the positive and negative electrode materials are further precisely separated, and the separated materials are repaired to achieve the recycling of retired materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of sodium-ion batteries, specifically to a method for separating and repairing mixed electrode powder of retired sodium-ion batteries and its application. Background Technology

[0002] In some related technologies, wet separation methods, such as using flocculants and acids, are often employed in the recovery and treatment systems of sodium iron phosphate cathodes and hard carbon anodes from sodium-ion batteries. These processes suffer from wastewater discharge, high reagent recovery costs, and a tendency to damage the crystal structure of the materials. Other methods, primarily designed for lithium-ion battery systems or other sodium battery cathodes, fail to consider the weak magnetic properties of sodium iron phosphate and the low conductivity of hard carbon materials, resulting in low purity and poor recovery rates of the separated products. Furthermore, while existing single physical separation techniques can separate sodium iron phosphate cathodes and hard carbon anodes from sodium-ion batteries, the stability of the separated products varies, and they often contain a large number of impurities. Summary of the Invention

[0003] To address at least one of the problems mentioned in the background art, this application proposes a method and application for separating and repairing mixed electrode powder from retired sodium-ion batteries. The method combines graded weak magnetic separation with electrostatic separation to precisely separate sodium iron pyrophosphate and hard carbon materials from the mixed electrode powder. The separated materials are then repaired so that they can be directly used in the preparation of sodium-ion battery electrodes, thereby achieving the recycling and reuse of retired sodium-ion battery materials.

[0004] The specific technical solutions provided in this application are as follows: Firstly, a method for separating and repairing mixed electrode powder from retired sodium-ion batteries is provided, including the following steps: Collect retired battery electrode powder and pre-treat it to obtain mixed electrode powder; The mixed electrode powder is subjected to primary magnetic separation using a magnetic separator with a magnetic conductive element to obtain primary sodium iron pyrophosphate and primary hard carbon material. The primary hard carbon material and the primary sodium iron pyrophosphate are subjected to secondary magnetic separation to obtain crude sodium iron pyrophosphate and crude hard carbon. Under electrostatic separation conditions where the friction speed is positively correlated with the ambient humidity, the crude sodium pyrophosphate and the crude hard carbon are electrostatically separated to obtain sodium pyrophosphate recovery material and hard carbon recovery material, respectively. The recovered sodium ferric pyrophosphate material is mixed with a composite sodium supplement and heat-treated to obtain sodium ferric pyrophosphate repair material. The surface of the recovered hard carbon material is coated with a composite coating agent to obtain hard carbon repair material.

[0005] In one specific embodiment, the magnetic conductive element is a strip-shaped alloy sheet, and the alloy sheet is a silicon steel sheet; And / or, the magnetic guide has a flow guide on the side of the magnetic roller near the magnetic separator, and the length of the flow guide is 5mm~8mm; And / or, the magnetic guide is arranged parallel to the magnetic roller of the magnetic separator, and the distance between the magnetic guide and the magnetic roller is 3mm~5mm.

[0006] In one specific embodiment, the conditions for the primary magnetic separation are: magnetic field strength of 500 Gs to 900 Gs, feeding speed of 1 t / h to 2 t / h, and magnetic roller speed of 30 r / min to 50 r / min; And / or, the conditions for the secondary magnetic separation are: magnetic field strength of 1000Gs~1200Gs, feeding speed of 1t / h~2t / h, and magnetic roller speed of 30r / min~50r / min.

[0007] In one specific embodiment, under electrostatic separation conditions where the friction speed is positively correlated with ambient humidity, the crude sodium pyrophosphate and the crude hard carbon are electrostatically separated to obtain recycled sodium pyrophosphate and recycled hard carbon, specifically including: The electrostatic separation is performed using an electrostatic separator, with a friction speed of 800 r / min to 1000 r / min and an ambient humidity of 30% RH to 45% RH. The friction speed is positively correlated with the ambient humidity. The crude sodium ferric pyrophosphate is fed into the electrostatic separator and, after being separated by friction with the first friction medium, the recovered sodium ferric pyrophosphate is obtained. The crude hard carbon product is fed into the electrostatic separator, and the starting voltage is set to 5kV~8kV. After friction separation by the second friction medium, the recycled hard carbon material is obtained.

[0008] In one specific embodiment, the electrostatic separation voltage is 18kV~25kV, and the feeding speed is 0.5t / h~1t / h; And / or, the electrode spacing for electrostatic sorting is 5cm to 8cm; And / or, the friction medium for electrostatic sorting is one or more of polytetrafluoroethylene, perfluoroalkoxy fluoroplastics, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer, and polyvinylidene fluoride.

[0009] In one specific embodiment, the recovered sodium ferric pyrophosphate is mixed with a composite sodium supplement agent and then heat-treated to obtain a sodium ferric pyrophosphate remediation material, specifically comprising: The composite sodium supplement is obtained by mixing sodium carbonate and sodium fluoride at a mass ratio of (1~3):1. The recovered sodium ferric pyrophosphate material and the composite sodium supplement were mixed at a mass ratio of (100~110):(1~3) to obtain a mixture; The mixture is placed at a temperature of 300℃~400℃ in an inert gas atmosphere and heat-treated for 2h~3h to obtain the sodium iron pyrophosphate remediation material.

[0010] In one specific embodiment, a composite coating agent is used to coat the surface of the hard carbon recycled material to obtain a hard carbon remediation material, specifically including: The composite coating agent is obtained by mixing asphalt and graphene, wherein the mass ratio of graphene in the composite coating agent is 3%~7% based on the mass of the composite coating agent; the hard carbon recycled material and the composite coating agent are mixed at a mass ratio of 100:(5~8) to obtain a reactant; the reactant is heat-treated at a temperature of 350℃~450℃ in an inert gas atmosphere for 1h~2h to obtain the hard carbon repair material.

[0011] In one specific embodiment, the process of collecting retired battery electrode powder and pre-treating it to obtain mixed electrode powder specifically includes: Collect the retired battery electrode powder, sieve it for the first time to remove electrolyte impurities, and then grind it. Set the grinding speed to 1000 r / min to 1500 r / min and the grinding time to 5 min to 10 min to obtain the ground electrode powder. Sift the ground electrode powder for the second time, and then dry it for 1 h to 2 h under vacuum conditions of 80℃ to 100℃ and 0.05 MPa to 0.1 MPa to obtain the mixed electrode powder.

[0012] In one specific embodiment, the dust generated in the above steps is collected, and the dust is subjected to airflow screening to obtain effective dust with a particle size ≥1μm; the effective dust is added to the mixed electrode powder for magnetic separation.

[0013] Secondly, a sodium-ion battery is provided, which is prepared by processing sodium iron pyrophosphate repair material and hard carbon repair material obtained by the above-described method for separating and repairing mixed electrode powders from retired sodium-ion batteries.

[0014] The embodiments of this application have the following beneficial effects: When using a magnetic separator to process mixed electrode powder, a first-stage low magnetic field is used for coarse separation to remove most of the non-magnetic hard carbon impurities, resulting in primary sodium pyrophosphate and primary hard carbon material. Then, a higher magnetic field is used for further precise separation. At the same time, a magnetic conductor is placed in the magnetic separator. The magnetic conductor can converge and enhance the local magnetic field intensity, which is equivalent to forming multiple micro strong magnetic field regions inside the magnetic separator. This amplifies the weak paramagnetic effect of sodium pyrophosphate, making it easier to be adsorbed and separated, thus improving the magnetic separation efficiency of the mixed electrode powder. The magnetic separator with magnetic conductor and electrostatic separation work together to achieve precise and efficient separation of sodium pyrophosphate and hard carbon material in the mixed electrode powder.

[0015] By using a composite sodium replenishing agent to replenish sodium ferric phosphate recovered material after separation, sodium ion loss during the separation process is compensated. At the same time, sodium fluoride inhibits the lattice distortion of sodium ferric phosphate. Coating agents are used to coat the surface of hard carbon recovered material. Asphalt repairs the surface damage of hard carbon, and graphene improves the conductivity of hard carbon. The repaired material can be directly used to prepare sodium-ion battery electrodes, so as to realize the recycling and reuse of retired sodium-ion battery materials. Attached Figure Description

[0016] To more clearly illustrate the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This is a schematic diagram of a method for separating and repairing mixed electrode powder of a retired sodium-ion battery, provided in an embodiment of this application. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0019] The "range" disclosed herein is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also expected. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0020] Unless otherwise specified in this application, all embodiments and preferred embodiments mentioned herein can be combined to form new technical solutions.

[0021] Unless otherwise specified, all technical features and preferred features mentioned herein can be combined to form new technical solutions.

[0022] In this application, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if the method may also include step (c), it means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein in the specification of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0024] This application provides a method for separating and repairing mixed electrode powder from retired sodium-ion batteries, such as... Figure 1 As shown, it includes the following steps: S1. Collect retired battery electrode powder and pre-treat it to obtain mixed electrode powder. Specifically, this includes: S1.1 Collect retired battery electrode powder. Collect electrode powder mixed with sodium iron pyrophosphate and hard carbon. First sieve to remove electrolyte impurities. The first sieve refers to passing through a 200-mesh sieve to remove electrolyte residue and large metal foil impurities. Then, crush the powder using a grinding process. Then grind the powder. Set the grinding speed to 1000r / min~1500r / min and the grinding time to 5min~10min to obtain the ground electrode powder. Control the grinding speed and grinding time within an appropriate range to avoid excessive grinding of materials that will cause nanoscale mixing, and ensure that the positive electrode sodium iron pyrophosphate and hard carbon materials can be effectively separated.

[0025] S1.2. The ground electrode powder is sieved a second time, specifically through a 40-100 mesh sieve, to remove aluminum foil and copper foil fragments and large pieces of binder. Then, it is dried for 1-2 hours under vacuum conditions of 80℃-100℃ and 0.05MPa-0.1MPa to obtain mixed electrode powder. It should be noted that drying under vacuum conditions prevents the hard carbon material from being oxidized by oxygen in the air.

[0026] S2. A magnetic separator with a magnetic conductor is used to perform primary magnetic separation on the mixed electrode powder to obtain primary sodium iron pyrophosphate and primary hard carbon material. The primary hard carbon material and primary sodium iron pyrophosphate are then subjected to secondary magnetic separation to obtain crude sodium iron pyrophosphate and crude hard carbon, respectively. The magnetic field strength of the secondary magnetic separation is greater than that of the primary magnetic separation.

[0027] Specifically, the mixed electrode powder is fed into a magnetic separator. Based on the different magnetic properties of sodium ferric pyrophosphate and hard carbon material, the magnetic sodium ferric pyrophosphate is adsorbed and separated from the non-magnetic hard carbon material. The primary sodium ferric pyrophosphate-rich material and the primary hard carbon material are then collected separately. The primary hard carbon material is then fed back into the magnetic separator, and a higher field strength is set to adsorb the sodium ferric pyrophosphate inclusions, thus obtaining crude hard carbon. The primary sodium ferric pyrophosphate-rich material is then fed back into the magnetic separator, and a secondary magnetic separation field strength is set to be used for the same adsorption process as the primary hard carbon material. The magnetic separator adsorbs the sodium ferric pyrophosphate, and the non-magnetic hard carbon material falls down, resulting in the collection of crude sodium ferric pyrophosphate.

[0028] Furthermore, the conditions for primary magnetic separation are: magnetic field strength of 500 Gs to 900 Gs, feed rate of 1 t / h to 2 t / h, and magnetic roller speed of 30 r / min to 50 r / min; specifically, the magnetic field strength for primary magnetic separation is set to 500 Gs, 550 Gs, 600 Gs, 650 Gs, 700 Gs, 750 Gs, 800 Gs, 850 Gs, 900 Gs, or any combination of two of the above values. The conditions for secondary magnetic separation are: magnetic field strength of 1000 Gs to 1200 Gs, feed rate of 1 t / h to 2 t / h, and magnetic roller speed of 30 r / min to 50 r / min. The magnetic field strength of the secondary magnetic separation is greater than that of the primary magnetic separation. Specifically, the magnetic field strength of the secondary magnetic separation is set to 1000 Gs, 1050 Gs, 1100 Gs, 1150 Gs, 1200 Gs, or any combination of two of these values. The first stage, with its lower field strength, is used for coarse separation, removing most of the non-magnetic hard carbon impurities. The second stage, with its higher field strength, is used for precise enrichment of weakly paramagnetic sodium pyrophosphate particles. This sequentially increasing magnetic separation process avoids the mis-adsorption of hard carbon impurities that might occur with a single magnetic field strength, while also effectively capturing sodium pyrophosphate. The iron in sodium pyrophosphate does not exist in the form of elemental form or ferromagnetic oxides, but Fe... 3+ The presence of unpaired electrons gives it a weak paramagnetic property. Since this weak paramagnetism is relatively weak, it is necessary to configure the magnetic field strength of the primary magnetic separation field and the secondary magnetic separation field strength in combination with the magnetic conductive element to achieve coarse and precise separation of the electrode powder. The magnetic field strength, together with the magnetic conductive element, can form multiple micro strong magnetic field regions suitable for sodium iron pyrophosphate particles in the magnetic separator, and the field strength formed by these micro magnetic separation field regions can accurately collect sodium iron pyrophosphate particles.

[0029] In this embodiment, the magnetic guide is a fixed structural component, pre-installed and fixed inside the weak magnetic separator. The magnetic guide is located above the surface of the magnetic roller, parallel to the magnetic roller of the magnetic separator, and the surface distance between the magnetic guide and the magnetic roller is 3mm~5mm. Specifically, the surface distance between the magnetic guide and the magnetic roller is 3mm, 3.5mm, 4mm, 4.5mm, 5mm, or any two of the above values. The magnetic guide spans the flow width of the material fed into the magnetic separator and covers the effective area of ​​the magnetic field inside the magnetic separator. The material input into the magnetic separator flows under the magnetic guide, and the magnetic guide converges the magnetic lines of force, enhancing the local magnetic field gradient. This allows weakly paramagnetic sodium iron pyrophosphate particles to be strongly adsorbed when passing through this area, while diamagnetic hard carbon materials are unaffected and pass directly through the magnetic field area, thereby achieving the separate aggregation and separation of positive and negative electrode materials.

[0030] Furthermore, the magnetic guide is a strip-shaped alloy sheet. Preferably, in this embodiment, the alloy sheet is a silicon steel sheet, which is a high magnetic permeability material and has a rectangular cross-section. The magnetic guide has a flow guide on the side of the magnetic roller near the magnetic separator. The flow guide is a straight sheet-like structure extending laterally from the bottom of the main body of the magnetic guide. It is located on the side near the magnetic roller and is the core functional area of ​​the magnetic guide. The flow guide is a horizontally straight extension with a length of 5mm to 8mm and a thickness of 0.3mm to 0.5mm. The flow guide is used to gather, concentrate, and enhance the magnetic lines of force of the magnetic roller to form a local high-gradient micro-magnetic field area, thereby improving the capture ability of weakly paramagnetic iron sodium pyrophosphate.

[0031] The specific length of the guide section is set to 5mm, 5.5mm, 6mm, 6.5mm, 7mm, 7.5mm, 8mm, or any combination of two of the above values. The length of the guide section directly affects the residence time of the material to be separated in the magnetic field area. If the length of the guide section is too long, the residence time of the mixed electrode powder to be separated in the magnetic field area will be prolonged, which may cause some hard carbon material to be mistakenly adsorbed. If the length of the guide section is too short, the residence time of the mixed electrode powder to be separated in the magnetic field area will be reduced, resulting in some sodium iron pyrophosphate particles not being adsorbed and separated. Based on this, by installing the magnetic guide component in the corresponding position to ensure that the distance between the guide section and the magnetic roller is kept within the above range, and by controlling the shape and length of the guide section within an appropriate range, it can be ensured that when the material to be separated passes through the magnetic separator area with an appropriate residence time, the weakly paramagnetic sodium iron pyrophosphate and hard carbon material in the material to be separated can be accurately separated.

[0032] Meanwhile, in this embodiment, the magnetic conductive component made of silicon steel sheet, the guide section with a length of 5mm~8mm, and the distance between the magnetic component and the magnetic roller are 3mm~5mm. The synergistic effect of the magnetic conductive component made of silicon steel sheet and the guide section can converge and enhance the local magnetic field strength. This is equivalent to forming multiple "micro strong magnetic field regions" inside the magnetic separator to amplify the weak paramagnetic effect of sodium ferric pyrophosphate, making it easier to be adsorbed and separated, and improving the magnetic separation efficiency of mixed electrode powder.

[0033] S3. Under electrostatic separation conditions where the friction speed is positively correlated with ambient humidity, electrostatic separation is performed on crude sodium pyrophosphate and crude hard carbon to obtain recovered sodium pyrophosphate and recovered hard carbon, specifically including: S3.1 Electrostatic separation is performed using an electrostatic separator with a friction speed of 800r / min to 1000r / min and an ambient humidity of 30%RH to 45%RH. The friction speed is positively correlated with the ambient humidity.

[0034] In this embodiment, electrostatic adsorption separation is used. Under electrostatic separation in a dry environment, the interaction between material particles is minimized, and the particles can move more freely in the magnetic field, allowing the weakly paramagnetic sodium pyrophosphate to be separated from other substances. At the same time, during electrostatic separation, environmental parameters need to be strictly controlled: ambient temperature 25±10℃, ambient humidity 30%RH~45%RH. The friction speed is positively correlated with the ambient humidity; for every 1% decrease in ambient humidity, the friction speed decreases by 50 r / min. If the environment is too humid, the resistance of the liquid and the agglomeration effect of some particles will seriously interfere with the magnetic separation effect. By setting the environmental parameters, it is ensured that the material triboelectric charging is stable and the charge is not easily leaked. The material is pre-dried under vacuum to ensure that the moisture content of the material is ≤1%, thus ensuring the separation effect.

[0035] S3.2. The crude sodium ferric pyrophosphate is fed into an electrostatic separator. After friction separation by the first friction medium, recycled sodium ferric pyrophosphate is obtained. The specific separation principle and process are as follows: The first friction medium is a fluoropolymer, such as polytetrafluoroethylene. After the crude sodium ferric pyrophosphate enters the separator, the main material sodium ferric pyrophosphate particles and the entrained hard carbon fine powder collide violently in the fluoropolymer medium. Based on the strong electron-gaining ability of fluoropolymers, the hard carbon fine powder becomes positively charged due to losing electrons, while the sodium ferric pyrophosphate particles become negatively charged due to gaining electrons. Subsequently, the material enters the high-voltage electric field area. Under the combined action of electric field force, gravity, and centrifugal force, the positively charged hard carbon impurities deflect towards the negative electrode plate and are attracted away from the main material flow; while the main material sodium ferric pyrophosphate particles become negatively charged and fall into the collection area along the main trajectory, thereby achieving the removal of hard carbon impurities and obtaining recycled sodium ferric pyrophosphate.

[0036] S3.3. Feed the coarse hard carbon product into the electrostatic separator, set the auxiliary bias voltage to 5kV~8kV, and after friction separation by the second friction medium, obtain the hard carbon recycled material.

[0037] The specific sorting principle and process are as follows: The second friction medium is also preferably a fluoropolymer. Since hard carbon is semi-conductive, the positive charge generated by friction alone is easily leaked through contact conduction during transmission. Therefore, an additional auxiliary charging bias voltage of 5kV to 8kV needs to be applied to force the hard carbon particles to be induced to carry a stable and sufficient amount of positive charge. This bias voltage is different from the 18kV to 25kV sorting voltage applied to the subsequent sorting electrode plates.

[0038] After the coarse hard carbon enters the separator, the main material, hard carbon particles, and the entrained fine sodium ferric pyrophosphate powder are rubbed together by a second friction medium. The polarities of the two materials are opposite: the hard carbon is positively charged, and the fine sodium ferric pyrophosphate powder is negatively charged. Upon entering the high-voltage electric field, the negatively charged sodium ferric pyrophosphate impurities deflect towards the positive electrode plate and are attracted away from the main material flow; while the positively charged hard carbon particles follow the main trajectory into the collection area, thus removing the sodium ferric pyrophosphate impurities and obtaining the recovered hard carbon material.

[0039] In step S2, magnetic separation is used to enrich and roughly separate sodium iron pyrophosphate and hard carbon materials. The crude sodium iron pyrophosphate still contains a small amount of fine hard carbon powder, and the crude hard carbon also contains a small amount of sodium iron pyrophosphate. Electrostatic separation is then used to completely remove any remaining trace impurities, thereby improving the purity of the positive and negative electrode materials after separation.

[0040] It should be noted that in this step, crude sodium ferric phosphate and crude hard carbon are fed separately into an electrostatic separator for fine selection and impurity removal, rather than being electrostatically separated together. This separate feeding method utilizes the difference in charge characteristics of the two materials after friction with the fluoropolymer friction medium to specifically remove the trace amounts of opposite polarity material impurities they carry. This method differs from the existing combined separation process of waste lithium-ion battery crushed materials, which involves "first electrostatic separation of the mixture, then magnetic separation," in terms of the separation targets, process sequence, and the technical problems it solves.

[0041] In one specific embodiment, the electrostatic separation voltage is 18kV~25kV, and the feeding speed is 0.5t / h~1t / h; the electrode spacing of the electrostatic separation is 5cm~8cm; specifically, the friction medium of the electrostatic separation is one or more of polytetrafluoroethylene, perfluoroalkoxy fluoroplastics, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer, and polyvinylidene fluoride.

[0042] Crude sodium ferric phosphate and crude hard carbon are fed into a high-voltage electrostatic separator. After friction with the fluoropolymer friction medium, the two particles exhibit differences in charge quantity and polarity. In the electric field generated by the charging voltage, the particles move along different trajectories due to the combined effects of electric field force, gravity, and centrifugal force, thus removing and collecting the trace impurities they carry. These trace impurities include fine hard carbon powder carried in the crude sodium ferric phosphate and fine sodium ferric phosphate powder carried in the crude hard carbon, improving the purity of both hard carbon and sodium ferric phosphate. Specifically, the fine hard carbon powder carried in the crude sodium ferric phosphate becomes charged after friction and is attracted by the electrodes, detaching from the main material flow. The sodium ferric phosphate particles mainly fall along the main trajectory into the sodium ferric phosphate recovery material collection area. The fine sodium ferric phosphate powder carried in the crude hard carbon has a different charge characteristic after friction and is attracted by the electrodes, detaching from the main material flow. The hard carbon particles enter the hard carbon recovery material collection area. Meanwhile, the combination of magnetic separation by magnetic separator and electrostatic separator in this application ensures that the sodium iron pyrophosphate crystal phase structure is intact and free from lattice distortion, and that the surface of the hard carbon material is not further damaged and the pore structure is intact, laying the foundation for the subsequent application of positive and negative electrode materials.

[0043] S4. Mix the recovered sodium iron pyrophosphate with the composite sodium supplement agent and heat treat it to obtain sodium iron pyrophosphate repair material. Then, use a composite coating agent to coat the surface of the recovered hard carbon to obtain the hard carbon repair material.

[0044] The recovered sodium ferric pyrophosphate is mixed with a composite sodium supplement and then heat-treated to obtain a sodium ferric pyrophosphate remediation material, which specifically includes: Sodium carbonate and sodium fluoride are mixed at a mass ratio of (1~3):1 to obtain a composite sodium supplement; sodium ferric pyrophosphate recovery material is mixed with the composite sodium supplement at a mass ratio of (100~110):(1~3) to obtain a mixture; the mixture is placed at a temperature of 300℃~400℃ in an inert gas atmosphere, with nitrogen / argon gas, and a flow rate of 1L / min~2L / min for 2h~3h to obtain sodium ferric pyrophosphate repair material.

[0045] By using a combination of sodium carbonate and sodium fluoride for sodium replenishment and repair, sodium replenishment and lattice protection can be achieved. The use of sodium replenishing agent replenishes the sodium ion loss during the separation and purification process, while sodium fluoride inhibits the lattice distortion of sodium iron pyrophosphate.

[0046] Furthermore, a composite coating agent is used to coat the surface of the hard carbon recycled material to obtain a hard carbon remediation material, specifically including: A composite coating agent is obtained by mixing asphalt and graphene, with the graphene mass ratio in the composite coating agent being 3%~7%, based on the mass of the composite coating agent. Hard carbon recycled material and composite coating agent are mixed at a mass ratio of 100:(5~8) to obtain a reactant. The reactant is placed at a temperature of 350℃~450℃ in an inert gas atmosphere, with nitrogen / argon gas, and a flow rate of 1L / min~2L / min for 1h~2h to obtain a hard carbon repair material.

[0047] A pitch-graphene composite coating agent was used for surface coating repair. Pitch repaired the surface damage of hard carbon, while graphene improved the conductivity of hard carbon, so that the repaired material could be directly used in the preparation of sodium-ion battery electrodes.

[0048] After separating and repairing the sodium ferric pyrophosphate and hard carbon remediation materials, the dust generated in each stage is collected. The effective dust with a particle size ≥1μm is screened by air classification and then pretreated by 500Gs low-pressure magnetic separation to remove impurities. The effective dust is added to the mixed electrode powder so that the mixed electrode powder can be sent back to the weak magnetic separation stage for secondary separation, achieving efficient dust reflux and ensuring high recovery rates of sodium ferric pyrophosphate and hard carbon.

[0049] Corresponding to the above embodiments, this application provides a sodium-ion battery, which is prepared by processing sodium iron pyrophosphate repair material and hard carbon repair material obtained by the above-described method for separating and repairing mixed electrode powders from retired sodium-ion batteries.

[0050] Example 1 A method for separating and repairing mixed electrode powder from retired sodium-ion batteries is provided, including the following steps: S1. Collect 10 kg of mixed electrode powder from retired energy storage cells, first pass it through a 200-mesh sieve to remove electrolyte residue, then gently grind it at 1200 r / min for 8 min, pass it through a 60-mesh sieve to remove metal foil debris, and dry it at 90℃ and 0.08 MPa vacuum for 1.5 h to obtain 8.2 kg of pure mixed electrode powder. S2. The pure mixed electrode powder is fed into a weak magnetic separator. A silicon steel sheet magnetic guide (7mm guide section, 4mm distance from the magnetic roller) is added. The first-stage magnetic separation field strength is 700Gs, the feed speed is 1.5t / h, the magnetic roller speed is 40r / min, and the second-stage magnetic separation field strength is 1100Gs. The same parameters are maintained for the second magnetic separation to obtain 4.5kg of crude sodium iron pyrophosphate with a purity of 93.5% and 3.6kg of hard carbon-rich product. S3. The sorting environment temperature is controlled at 22℃ and the humidity at 35%RH. The matching friction speed is 900r / min, the sorting voltage is 22kV, the feeding speed is 0.8t / h, the electrode spacing is 6cm, and the friction medium is polytetrafluoroethylene. 4.3kg of sodium iron pyrophosphate with a purity of 95.2% and 3.4kg of hard carbon with a purity of 92.3% are obtained. S4. Mix the refined sodium ferric pyrophosphate with the composite sodium supplement (sodium carbonate:sodium fluoride = 2:1) at a mass ratio of 100:2, and heat-treat at 350℃ under nitrogen protection (flow rate 1.5L / min) for 2.5h; mix the refined hard carbon with the asphalt-graphene composite coating agent at a mass ratio of 100:6, and heat-treat at 400℃ under nitrogen protection for 1.5h. S5. Collect 1.2 kg of dust from each stage, and after air classification, 0.9 kg of dust with a particle size ≥1 μm is separated. After pretreatment by 500 Gs low-pressure magnetic separation, it is returned to the weak magnetic separation stage to finally obtain 4.25 kg of reconstituted iron sodium pyrophosphate and 3.35 kg of reconstituted hard carbon.

[0051] Test results: The initial discharge capacity of the repaired sodium iron pyrophosphate was 106.8 mAh / g, and the capacity retention rate after 300 cycles was 91.2%, with the crystal phase structure consistent with the original material; the initial coulombic efficiency of the repaired hard carbon was 79.5%, and the capacity retention rate after 300 cycles was 89.3%, with no obvious surface damage and a 9% improvement in conductivity; the total recovery rate of sodium iron pyrophosphate was 97.5%, and the total recovery rate of hard carbon was 96.8%.

[0052] Example 2 S1. Collect 8 kg of mixed electrode powder from production waste, gently grind it at 1000 r / min for 10 min, pass it through a 40 mesh sieve to remove metal foil debris, and dry it at 80℃ and 0.05 MPa vacuum for 2 h to obtain 6.8 kg of pure mixed electrode powder. S2. The pure mixed electrode powder is fed into a weak magnetic separator. A silicon steel sheet magnetic guide (5mm guide section, 3mm distance from the magnetic roller) is added. The first-stage magnetic separation field strength is 600Gs, the feeding speed is 1t / h, the magnetic roller speed is 30r / min, and the second-stage magnetic separation field strength is 1000Gs. The same parameters are maintained for the second magnetic separation to obtain 3.7kg of crude sodium iron pyrophosphate with a purity of 93.1% and 3.0kg of hard carbon-rich product. S3. The sorting environment temperature is controlled at 20℃ and humidity at 32%RH. The matching friction speed is 800r / min, the sorting voltage is 18kV, the feeding speed is 0.5t / h, the electrode spacing is 5cm, and the friction medium is polytetrafluoroethylene. 3.55kg of sodium pyrophosphate with a purity of 95.0% and 2.85kg of hard carbon with a purity of 92.0% are obtained. S4. Mix the refined sodium ferric pyrophosphate with the composite sodium supplement (sodium carbonate:sodium fluoride = 2:1) at a mass ratio of 100:1, and heat-treat at 300℃ under argon protection (flow rate 1L / min) for 3 hours; mix the refined hard carbon with the asphalt-graphene composite coating agent at a mass ratio of 100:5, and heat-treat at 350℃ under argon protection for 2 hours. S5. Collect 0.9 kg of dust from each stage, and after air classification, 0.7 kg of dust with a particle size ≥1 μm is separated. After pretreatment by 500 Gs low-pressure magnetic separation, it is returned to the weak magnetic separation stage to finally obtain 3.5 kg of reconstituted iron sodium pyrophosphate and 2.8 kg of reconstituted hard carbon.

[0053] Test results: The initial discharge capacity of the repaired sodium iron pyrophosphate was 105.2 mAh / g, and the capacity retention rate after 300 cycles was 90.1%; the initial coulombic efficiency of the repaired hard carbon was 78.2%, and the capacity retention rate after 300 cycles was 88.1%; the total recovery rate of sodium iron pyrophosphate was 97.1%, and the total recovery rate of hard carbon was 96.2%.

[0054] Example 3 Corresponding to the above embodiments, the difference between this embodiment and embodiment 1 is that the length of the flow guide of the magnetic conductor is set to 5mm, and the rest is the same as embodiment 1.

[0055] Example 4 Corresponding to the above embodiments, the difference between this embodiment and embodiment 1 is that the length of the flow guide of the magnetic conductor is set to 8mm, and the rest is the same as embodiment 1.

[0056] Example 5 Corresponding to the above embodiments, the difference between this embodiment and embodiment 1 is that the distance between the magnetic guide and the magnetic roller is set to 3mm, and the rest is the same as in embodiment 1.

[0057] Example 6 Corresponding to the above embodiments, the difference between this embodiment and embodiment 1 is that the distance between the magnetic guide and the magnetic roller is set to 5mm, and the rest is the same as embodiment 1.

[0058] Example 7 Corresponding to the above embodiments, the difference between this embodiment and embodiment 1 is that the distance between the magnetic guide and the magnetic roller is set to 2mm, and the length of the guide portion of the magnetic guide is 7mm, the rest is the same as embodiment 1.

[0059] Example 8 Corresponding to the above embodiments, the difference between this embodiment and embodiment 1 is that the distance between the magnetic guide and the magnetic roller is set to 4mm, and the length of the guide part of the magnetic guide is 10mm, the rest is the same as embodiment 1.

[0060] Example 9 Corresponding to the above embodiments, the difference between this embodiment and embodiment 1 is that the magnetic field strength of the first-stage magnetic separation is set to 500 Gs and the magnetic field strength of the second-stage magnetic separation is set to 1100 Gs, while the rest is the same as in embodiment 1.

[0061] Example 10 Corresponding to the above embodiments, the difference between this embodiment and embodiment 1 is that the magnetic field strength of the first-stage magnetic separation is set to 700 Gs and the magnetic field strength of the second-stage magnetic separation is set to 800 Gs, while the rest is the same as in embodiment 1.

[0062] Comparative Example 1 Corresponding to the above embodiments, the difference between this comparative example and Example 1 is that it adopts a combination of single-stage magnetic separation and electrostatic separation, specifically including the following steps: Take 10 kg of mixed electrode powder from the same batch of retired energy storage cells as in Example 1, and process it according to existing technology: directly pass it through a 60-mesh sieve, then use single-stage magnetic separation with a field strength of 1000 Gs, and then use conventional electrostatic separation. The conventional electrostatic separation conditions are no temperature and humidity control, separation voltage of 20 kV, and friction speed of 900 r / min. No gentle repair was carried out, and no dust was collected for closed-loop recycling.

[0063] Test results: Sodium iron pyrophosphate purity 88.3%, hard carbon purity 85.7%; Sodium iron pyrophosphate recovery rate 92.1%, hard carbon recovery rate 91.5%; Sodium iron pyrophosphate crystal phase partially damaged, initial discharge capacity 98.2 mAh / g, capacity retention rate 82.5% after 300 cycles; Hard carbon surface severely damaged, initial coulombic efficiency 72.3%, capacity retention rate 78.0% after 300 cycles.

[0064] Comparative Example 2 The difference between this comparative example and Example 1 is that no magnetic conductive component is added; otherwise, they are the same as Example 1.

[0065] Comparative Example 3 The difference between this comparative example and Example 1 is that conventional electrostatic separation is used. The conditions for conventional electrostatic separation are no temperature and humidity control, a separation voltage of 20kV, and a friction speed of 900r / min. The rest are the same as in Example 1.

[0066] The test conditions and test procedures for each data item in this embodiment are as follows: (1) Purity test Test methods: Inductively coupled plasma atomic emission spectrometry (ICP-AES) and carbon-sulfur analysis. Test procedure: 0.1g of the sample was digested, and the Fe, P, and Na content was determined using ICP, and the purity of sodium iron pyrophosphate was calculated. The carbon content was determined using a carbon-sulfur analyzer, and the purity of hard carbon was calculated. Test environment: Room temperature 25℃, humidity 40%RH~45%RH.

[0067] (2) Recovery rate test Recovery rate = (mass of target material in product / theoretical mass of target material in raw material) × 100%. Testing process: Weigh the raw material, intermediate product, and final product separately, and calculate the actual effective material mass based on purity data.

[0068] (3) X-ray diffraction analysis Testing instrument: X-ray diffractometer. Testing conditions: CuKα radiation, scanning range 10°~80°, scanning speed 2° / min. Judgment criteria: Compared with the standard sodium ferric pyrophosphate XRD pattern, the absence of impurity peaks, peak position shifts, and phase transitions indicates a complete crystalline phase.

[0069] (4) Conductivity test of hard carbon materials Test method: Four-probe tester. Test conditions: Room temperature, pressure 10 MPa, sample tablet thickness 2 mm. Calculation method: Improvement rate = (Conductivity after repair - Conductivity before repair) / Conductivity before repair × 100%.

[0070] (5) Sodium ion recovery rate Test method: ICPAES was used to determine the Na content. Calculation method: Sodium ion recovery rate = (Na content after repair / Na content of fresh material) × 100%.

[0071] (6) Electrochemical performance test (button cell) Battery type: CR2032 coin cell. Working electrode: Prepared by mixing the test material, conductive agent, and binder in a mass ratio of 8:1:1; Counter electrode: Sodium metal sheet. Electrolyte: 1.0M NaPF6 dissolved in EC / DEC, where the volume ratio of EC / DEC is 1:1; Charge / discharge regime: 0.1C constant current charge / discharge; Voltage range: Sodium iron pyrophosphate positive electrode 2.0V~4.0V, hard carbon negative electrode 0.005V~2.0V; Test temperature: 25℃ constant temperature.

[0072] Table 1. Basic test data of retired battery electrode powder

[0073] The mixed electrode powder from sodium-ion battery production waste, generated during the coating and cutting processes, is a non-recycled waste electrode powder with a complete material structure and high recycling value. It also has similar purity and residues to the mixed electrode powder from retired sodium-ion battery cells. Based on the above comparison, it can be concluded that this solution can process both the mixed electrode powder from retired sodium-ion battery cells and the mixed electrode powder from sodium-ion battery production waste, thereby achieving resource recycling of retired batteries and production waste.

[0074] Table 2. Processing products and test results of relevant data in this embodiment.

[0075] Combining the above embodiments 1, 3, and 4, it can be seen that the separation and repair method in this embodiment can achieve a purity of over 94% and a recovery rate of over 96% for sodium pyrophosphate after separation when the flow guide is set to different lengths, and a purity of over 91% and a recovery rate of over 95% for hard carbon material. This confirms that the magnetic conductive component added in this embodiment can increase the paramagnetic effect of sodium pyrophosphate during the magnetic separation process, making it easier for the two to separate.

[0076] Combining Examples 5 and 6, it can be seen that when the distance between the magnetic guide and the magnetic roller is set to different distances within the preferred range, the purity of the separated sodium iron pyrophosphate reaches about 94%, and the purity of the separated hard carbon material reaches about 91%, which means that the positive and negative electrode materials of the mixed electrode powder can still be effectively separated. Comparing Examples 7, 8, and 1, when the length of the guide section exceeds the preferred range or the distance between the guide and the magnetic roller exceeds the preferred range, the purity of the sodium iron pyrophosphate and hard carbon material separated from the mixed electrode powder of the retired sodium-ion battery is significantly lower than that of the separation control method in this example. Furthermore, when the length of the guide section of the magnetic guide exceeds the range of 5mm to 8mm, even if the distance between the magnetic guide and the magnetic roller meets the above range, the purity of the separated material is still lower than that of the scheme in this example. This proves that the addition of the magnetic guide and the control of the length of the guide section of the magnetic guide are essential technical solutions to achieve the separation effect of this example.

[0077] Comparative Example 1 uses a combination of single-stage magnetic separation and conventional electrostatic separation. However, the purity of both the separated sodium pyrophosphate and hard carbon material in Comparative Example 1 is lower than that of the separation method in this embodiment. The settings of Comparative Examples 2 and 3 allow for the simultaneous use of magnetic components and electrostatic separation to achieve high levels of purity for both the separated sodium pyrophosphate and hard carbon material. While adding only magnetic components or using only electrostatic separation can separate sodium pyrophosphate from hard carbon material, the purity of the separated substances is significantly lower.

[0078] Table 3. Physical property test data of the materials after separation and repair in this embodiment.

[0079] Based on the data in Table 3, it can be concluded that the sodium pyrophosphate crystal phase obtained by the separation and repair method is basically intact and without lattice distortion. However, when the mixed electrode powder is processed without adding magnetic conductive components or using conventional electrostatic sorting, although sodium ion repair is performed, the repaired sodium pyrophosphate still shows partial damage and lattice distortion. The hard carbon material also shows slight damage. The sodium ion recovery rate of sodium pyrophosphate and the conductivity improvement rate of the hard carbon material are also significantly lower than the test results obtained in Example 1.

[0080] Table 4 Electrochemical test data of the separated and repaired materials in this embodiment

[0081] Based on the electrochemical test results obtained from Table 4 for the separated and repaired sodium iron pyrophosphate positive electrode and hard carbon negative electrode, it can be seen that when the two-stage magnetic separation and electrostatic separation combined treatment method in this embodiment is adopted, and the magnetic field strength of the two-stage magnetic separation and the key parameters of the magnetic conductor are controlled within a reasonable range, the initial discharge capacity of the separated and repaired sodium iron pyrophosphate can reach more than 105 mAh / g, and the retention rate of sodium iron pyrophosphate after 300 cycles can basically reach more than 90%. However, when the length of the magnetic conductor in the separation process significantly exceeds the corresponding range, or the magnetic field strength in the magnetic separation process is too high or too low, the separation process of the positive and negative electrode materials is significantly affected. Even if the same repair scheme is used to repair the separated materials, the electrochemical performance of the repaired materials is still worse than that of the materials prepared by the scheme in this embodiment.

[0082] Although preferred embodiments have been described in this application, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the embodiments of this application.

[0083] Obviously, those skilled in the art can make various modifications and variations to this application without departing from the spirit and scope of this application. Therefore, if such modifications and variations fall within the scope of the claims of this application and their equivalents, this application also intends to include such modifications and variations.

Claims

1. A method for separating and repairing mixed electrode powder from retired sodium-ion batteries, characterized in that, Includes the following steps: Collect retired battery electrode powder and pre-treat it to obtain mixed electrode powder; The mixed electrode powder is subjected to primary magnetic separation using a magnetic separator with a magnetic conductive element to obtain primary sodium iron pyrophosphate and primary hard carbon material. The primary hard carbon material and the primary sodium iron pyrophosphate are subjected to secondary magnetic separation to obtain crude sodium iron pyrophosphate and crude hard carbon, respectively. The magnetic field strength of the secondary magnetic separation is greater than that of the primary magnetic separation. Under electrostatic separation conditions where the friction speed is positively correlated with the ambient humidity, the crude sodium pyrophosphate and the crude hard carbon are electrostatically separated to obtain sodium pyrophosphate recovery material and hard carbon recovery material, respectively. The recovered sodium ferric pyrophosphate material is mixed with a composite sodium supplement and heat-treated to obtain sodium ferric pyrophosphate repair material. The surface of the recovered hard carbon material is coated with a composite coating agent to obtain hard carbon repair material.

2. The method for separating and repairing mixed electrode powder of decommissioned sodium-ion batteries according to claim 1, characterized in that, The magnetic conductive element is a strip-shaped alloy sheet, and the alloy sheet is a silicon steel sheet; And / or, the magnetic guide has a flow guide on the side of the magnetic roller near the magnetic separator, and the length of the flow guide is 5mm~8mm; And / or, the magnetic guide is arranged parallel to the magnetic roller of the magnetic separator, and the distance between the magnetic guide and the magnetic roller is 3mm~5mm.

3. The method for separating and repairing mixed electrode powder of decommissioned sodium-ion batteries according to claim 1 or 2, characterized in that, The conditions for the first-stage magnetic separation are: magnetic field strength of 500 Gs to 900 Gs, feeding speed of 1 t / h to 2 t / h, and magnetic roller speed of 30 r / min to 50 r / min. And / or, the conditions for the secondary magnetic separation are: magnetic field strength of 1000Gs~1200Gs, feeding speed of 1t / h~2t / h, and magnetic roller speed of 30r / min~50r / min.

4. The method for separating and repairing mixed electrode powder of decommissioned sodium-ion batteries according to claim 1 or 2, characterized in that, Under electrostatic separation conditions where the friction speed is positively correlated with ambient humidity, the crude sodium pyrophosphate and the crude hard carbon are electrostatically separated to obtain recycled sodium pyrophosphate and recycled hard carbon, specifically including: The electrostatic separation is performed using an electrostatic separator, with a friction speed of 800 r / min to 1000 r / min and an ambient humidity of 30% RH to 45% RH. The friction speed is positively correlated with the ambient humidity. The crude sodium ferric pyrophosphate is fed into the electrostatic separator and, after being separated by friction with the first friction medium, the recovered sodium ferric pyrophosphate is obtained. The crude hard carbon product is fed into the electrostatic separator, and the starting voltage is set to 5kV~8kV. After friction separation by the second friction medium, the recycled hard carbon material is obtained.

5. The method for separating and repairing mixed electrode powder of decommissioned sodium-ion batteries according to claim 4, characterized in that, The electrostatic separation voltage is 18kV~25kV, and the feeding speed is 0.5t / h~1t / h; And / or, the electrode spacing for electrostatic sorting is 5cm to 8cm; And / or, the friction medium for electrostatic sorting is one or more of polytetrafluoroethylene, perfluoroalkoxy fluoroplastics, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer, and polyvinylidene fluoride.

6. The method for separating and repairing mixed electrode powder of decommissioned sodium-ion batteries according to claim 1 or 2, characterized in that, The recovered sodium ferric pyrophosphate material is mixed with a composite sodium supplement agent and then heat-treated to obtain a sodium ferric pyrophosphate remediation material, specifically comprising: The composite sodium supplement is obtained by mixing sodium carbonate and sodium fluoride at a mass ratio of (1~3):

1. The recovered sodium ferric pyrophosphate material and the composite sodium supplement were mixed at a mass ratio of (100~110):(1~3) to obtain a mixture; The mixture is placed at a temperature of 300℃~400℃ in an inert gas atmosphere and heat-treated for 2h~3h to obtain the sodium iron pyrophosphate remediation material.

7. The method for separating and repairing mixed electrode powder of decommissioned sodium-ion batteries according to claim 1 or 2, characterized in that, The hard carbon remediation material is obtained by coating the surface of the hard carbon recycled material with a composite coating agent, specifically including: The composite coating agent is obtained by mixing asphalt and graphene, wherein the mass ratio of graphene in the composite coating agent is 3% to 7%, based on the mass of the composite coating agent. The hard carbon recycled material and the composite coating agent are mixed at a mass ratio of 100:(5~8) to obtain the reactant; The reactants are heat-treated at 350℃~450℃ in an inert gas atmosphere for 1h~2h to obtain the hard carbon repair material.

8. The method for separating and repairing mixed electrode powder of decommissioned sodium-ion batteries according to claim 1 or 2, characterized in that, Collect retired battery electrode powder and preprocess it to obtain mixed electrode powder, specifically including: Collect the retired battery electrode powder, sieve it for the first time to remove electrolyte impurities, and then grind it. Set the grinding speed to 1000 r / min~1500 r / min and the grinding time to 5 min~10 min to obtain the ground electrode powder. The ground electrode powder is sieved a second time, and then dried for 1 to 2 hours under vacuum conditions of 80℃~100℃ and 0.05MPa~0.1MPa to obtain the mixed electrode powder.

9. The method for separating and repairing mixed electrode powder of decommissioned sodium-ion batteries according to claim 1 or 2, characterized in that, The method further includes: Collect the dust generated in the above steps, and perform airflow sieving on the dust to obtain effective dust with a particle size ≥1µm; The effective dust is added to the mixed electrode powder for magnetic separation.

10. A sodium-ion battery, characterized in that, The sodium-ion battery is prepared by processing sodium iron pyrophosphate repair material and hard carbon repair material obtained by the method of separating and repairing mixed electrode powder of retired sodium-ion batteries according to any one of claims 1 to 9.