A method for preparing a dual transition metal sulfide-heteroatom doped rod-shaped composite material
By constructing rod-shaped composite materials doped with dual transition metal sulfides and heteroatoms, the problems of poor impedance matching and single loss mechanism in carbon-based composite materials at extremely thin thicknesses were solved, and high efficiency performance of broadband electromagnetic wave absorption was achieved.
Patent Information
- Application Number
- CN202611146291.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing carbon-based composite absorbing materials suffer from poor impedance matching, a single loss mechanism, and difficulty in finely controlling their microstructure, making it difficult to achieve broadband absorption at extremely thin thicknesses.
A rod-shaped composite material with a hierarchical heterostructure was constructed by using a bimetallic organic framework (MOF) template method combined with in-situ construction of an organic coating layer and subsequent sulfidation heat treatment. The composite material includes a dual transition metal sulfide and a heteroatom-doped carbon matrix.
Excellent performance of broadband electromagnetic wave absorption under ultra-thin coating was achieved. The specific surface area and multiple scattering performance of the material were improved, and the microwave loss capability was greatly improved by multidimensional heterogeneous interface and synergistic loss mechanism.
Smart Images

Figure CN123124318A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of microwave absorption and electromagnetic shielding materials technology, specifically to a method for preparing a dual transition metal sulfide-heteroatom doped rod-shaped composite material. Background Technology
[0002] With the rapid development of 5G / 6G high-frequency communication, radar detection technology, and the aerospace industry, electromagnetic radiation not only seriously interferes with the normal operation of high-precision electronic equipment, but also poses a huge threat to human health and national defense security. Therefore, developing high-performance electromagnetic wave absorbing materials with the characteristics of "thin, light, wide, and strong" (i.e., thin matching thickness, low density, wide effective absorption bandwidth, and strong reflection loss) has become a research hotspot in the field of materials science.
[0003] Traditional magnetic absorbing materials (such as ferrites, magnetic metals and their alloys) have good magnetic loss capabilities, but they suffer from drawbacks such as high density, easy oxidation, and susceptibility to the snooker limit at high frequencies. Carbon-based nanomaterials (such as carbon nanotubes, graphene, and porous carbon) have excellent properties such as low density, good conductivity, and large specific surface area, thus attracting considerable attention from researchers. However, single carbon materials typically have excessively high dielectric constants, leading to a severe impedance mismatch between electromagnetic waves and the material. This causes most electromagnetic waves to be reflected at the material surface and unable to penetrate the material interior for loss, resulting in generally weak minimum reflection loss (typically worse than -30 dB) and failing to meet broadband absorption requirements.
[0004] To address this issue, multi-component composites and microstructure designs involving magnetic and dielectric loss components with a carbon matrix are currently the mainstream strategy. However, existing conventional composite or single-structure materials, lacking fine-tuning of micro-level interfaces and resonant cavity design, typically exhibit minimum reflection losses concentrated between -30 dB and -50 dB under thin coatings of around 2.0 mm, with effective bandwidth generally maintained at 2.5–3.8 GHz, making it difficult to simultaneously achieve strong absorption and ultra-wideband coverage at extremely thin thicknesses. Transition metal sulfides (such as FeS, MoS2, CoS, NiS, etc.) not only possess excellent semiconductor properties and dielectric / magnetic field response capabilities but can also introduce abundant heterointerfaces and dipole polarization defects into composite systems. Simultaneously, doping with heteroatoms (such as N, B, P, S, F, etc.) can effectively modulate the electronic structure of the carbon matrix, optimize its dielectric constant, and enhance dipole polarization. Therefore, the ability to uniformly assemble multiple components (dual transition metal sulfides and heteroatom-doped carbon) at the nanoscale using a simple process and construct a rod-like structure with hierarchical heterogeneous characteristics to achieve multiple synergistic effects on electromagnetic loss mechanisms is of great significance for promoting the development of next-generation high-performance electromagnetic wave absorbing materials. Summary of the Invention
[0005] The purpose of this invention is to address the shortcomings of existing carbon-based composite microwave absorbing materials, such as poor impedance matching, a single loss mechanism, and difficulty in finely controlling the microstructure, by providing a method for preparing a rod-shaped composite material of dual transition metal sulfide-heteroatom doped materials. This invention successfully constructs a rod-shaped composite material with a hierarchical heterostructure through a bimetallic organic framework (MOF) template method combined with in-situ construction of an organic coating layer and subsequent sulfidation heat treatment, achieving excellent broadband electromagnetic wave absorption performance.
[0006] The technical solution of this invention is: a method for preparing a dual transition metal sulfide-heteroatom-doped rod-shaped composite material, characterized by the following specific steps:
[0007] (1) Synthesis of bimetallic MOF precursor: The first magnetic transition metal salt and the second group VIB transition metal salt were dissolved in deionized water to form solution A; the polycarboxylic acid organic ligand and surfactant were dissolved in an organic solvent to form solution B; solution A and solution B were mixed evenly in equal volumes and then transferred to a reaction vessel for solvothermal reaction. After the reaction was completed, the precipitate was collected, washed and dried to obtain the bimetallic MOF precursor.
[0008] (2) In-situ construction of organic coating layer and introduction of heteroatoms: The bimetallic MOF precursor and organic carbon source prepared in step (1) are dispersed in a buffer solution containing heteroatom source and stirred continuously. An organic coating layer is formed on the MOF surface through physical adsorption, self-polymerization or chemical cross-linking reaction. After the reaction is completed, the product is collected, centrifuged, washed and dried to obtain a core-shell structured composite material.
[0009] (3) High-temperature sulfidation heat treatment: The composite material obtained in step (2) is placed in a tube furnace and subjected to high-temperature calcination heat treatment with sulfur-containing compounds placed upstream as sulfur source under a protective atmosphere; after natural cooling, a double transition metal sulfide-heteroatom doped rod-shaped composite material is obtained.
[0010] The preferred first magnetic transition metal salt in step (1) is one or more of iron salt, cobalt salt, nickel salt or manganese salt, and the mass ratio of its added mass to deionized water is (2-8):100; the preferred second group VIB transition metal salt is one or more of molybdenum salt or tungsten salt, and the mass ratio of its added mass to deionized water is (1-5):100.
[0011] The preferred first magnetic transition metal salt in step (1) is one or more of anhydrous ferric chloride, anhydrous ferric nitrate, anhydrous cobalt chloride, anhydrous cobalt nitrate, anhydrous nickel chloride, or anhydrous nickel nitrate; the preferred second Group VIB transition metal salt is one or more of anhydrous sodium molybdate, ammonium tetrathiomolybdate, ammonium molybdate, sodium tungstate, or ammonium tungstate.
[0012] The preferred step (1) uses one or more of the following: aromatic polycarboxylic acids or aliphatic polycarboxylic acids, with a mass-to-volume ratio of 15-60 g / L to the organic solvent; the surfactant is one or more of the following: nonionic polymer, anionic surfactant, cationic surfactant, or natural macromolecular dispersant, with a mass-to-volume ratio of 10-50 g / L to the organic solvent; and the organic solvent is one or more of the following: amide solvent, sulfoxide solvent, alcohol solvent, or ketone solvent.
[0013] More preferably, the polycarboxylic acid organic ligand in step (1) is one or more of terephthalic acid, 2-aminoterephthalic acid, isophthalic acid, trimesoic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, or fumaric acid; the surfactant is one or more of polyvinylpyrrolidone (PVP), polyethylene glycol (PEG), polyvinyl alcohol (PVA), triblock copolymer F127, hexadecyltrimethylammonium bromide (CTAB), or sodium dodecylbenzenesulfonate (SDBS); and the organic solvent is one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), anhydrous ethanol, or ethylene glycol.
[0014] The preferred temperature for the solvothermal reaction in step (1) is 100-140 °C, and the holding time is 1-3 hours.
[0015] The preferred organic carbon source in step (2) is one or more of dopamine hydrochloride, tannic acid, catechol, pyrrole, aniline, resorcinol-formaldehyde resin, glucose, cyclodextrin or chitosan, and the mass ratio of the added organic carbon source to the volume of the buffer solution is 0.5-10 g / L; the heteroatom source is one or more of inorganic heteroatom precursors and organic heteroatom precursors, and the mass ratio of the added heteroatom source to the volume of the buffer solution is 1-20 g / L.
[0016] More preferably, the heteroatom source mentioned in step (2) is one or more of urea, melamine, dicyandiamide, polyaniline, polypyrrole, boric acid, sodium borate, sodium tetraphenylborate, phytic acid, phosphoric acid, ammonium dihydrogen phosphate, triphenylphosphine, thiourea, thioacetamide, sublimed sulfur, ammonium fluoride, sodium fluoride, and polyvinylidene fluoride.
[0017] The preferred step (2) is to add the bimetallic MOF precursor at a mass ratio of 0.5-5 g / L to the volume of the buffer solution; and to continue stirring for 12-24 hours.
[0018] The sulfur-containing compound mentioned in step (3) is preferably thiourea or sulfur, and the mass ratio of the sulfur-containing compound to the composite material is (2-5):1; the heat treatment protective atmosphere mentioned in step (3) is any one of nitrogen, argon and helium, the calcination temperature is 450-600 ℃, the holding time is 2-4 hours, and the heating rate is 2-5 ℃ / min.
[0019] Beneficial effects:
[0020] (1) Unique rod-shaped heterostructure and multiple scattering performance: The one-dimensional rod-shaped structure effectively increases the specific surface area of the material. The tube structure, as a micro-resonant cavity for electromagnetic waves, enables electromagnetic waves to undergo multiple reflections and scatterings inside the material, thus extending the propagation and attenuation path of electromagnetic waves.
[0021] (2) Multidimensional heterogeneous interfaces and synergistic loss mechanism: This invention generates dual transition metal sulfides and heteroatom-doped carbon matrix in situ by calcining the organic coating layer and the bimetallic MOF precursor. The deep coupling of the magnetic phase, high dielectric phase and conductive carbon network not only optimizes the impedance matching of the material, but also constructs a rich array of multidimensional heterogeneous interfaces. The introduction of heteroatoms results in a large number of electron traps and polarization centers in the material, leading to strong polarization relaxation loss, thereby significantly improving microwave loss capability.
[0022] (3) The preparation process is simple and the composition is adjustable: This invention utilizes heteroatom buffer solution and gas-phase sulfidation method to achieve in-situ derivatization of multiple components and co-doping of multiple heteroatoms. The preparation process is easy to control, and the elements and carbon sources are highly expandable, showing good engineering prospects. Attached Figure Description
[0023] Figure 1 The image shows the microstructure of the FeS / MoS2@N / B co-doped carbon rod-shaped heterostructure composite material prepared in Example 1. Detailed Implementation
[0024] The present invention will now be described in detail with reference to specific embodiments and comparative examples.
[0025] Example 1
[0026] Solution A was prepared by dissolving 1.2 g of anhydrous ferric chloride and 0.6 g of anhydrous sodium molybdate in 30 mL of deionized water; solution B was prepared by dissolving 0.9 g of terephthalic acid and 0.9 g of polyvinylpyrrolidone in 30 mL of N,N-dimethylformamide (DMF). After mixing and stirring for 30 minutes, the mixture was transferred to a reaction vessel and incubated at 120 °C for 2 hours. The mixture was washed and dried to obtain the bimetallic MOF precursor. 0.4 g of the prepared bimetallic MOF precursor and 0.2 g of dopamine hydrochloride were dispersed in 200 mL of borate buffer (5 g / L) and stirred continuously for 16 hours. After centrifugation, washing, and drying, the composite material precursor was obtained. 0.5 g of the obtained precursor and 1.75 g of thiourea were heat-treated under a nitrogen atmosphere at a heating rate of 3 °C / min to 550 °C for 3 hours to obtain the FeS / MoS2@N / B co-doped carbon rod-shaped heterostructure composite material.
[0027] like Figure 1 As shown in the scanning electron microscope (SEM) images, the prepared FeS / MoS2@N / B co-doped carbon composite material exhibits a regular and uniformly dispersed one-dimensional rod-like structure. The rods have a good aspect ratio, a smooth and dense surface, and uniform size (cross-sectional dimensions in the range of approximately 1-3 μm), demonstrating that a complete and structurally stable rod-like heterostructure composite material was successfully constructed using the MOF template method combined with in-situ coating and sulfidation strategies.
[0028] Example 2
[0029] Solution A was prepared by dissolving 0.9 g of anhydrous ferric nitrate and 0.54 g of ammonium tetrathiomolybdate in 30 mL of deionized water; solution B was prepared by dissolving 1.8 g of terephthalic acid and 0.9 g of sodium dodecylbenzenesulfonate in 30 mL of N,N-dimethylacetamide (DMAc). After mixing and stirring for 30 minutes, the mixture was transferred to a reaction vessel and incubated at 140 °C for 1.5 hours. The mixture was washed and dried to obtain the bimetallic MOF precursor. 0.6 g of the prepared bimetallic MOF precursor and 0.1 g of tannic acid were dispersed in 200 mL of urea salt buffer (3 g / L) and stirred continuously for 16 hours. After centrifugation, washing, and drying, the composite material precursor was obtained. 0.5 g of the obtained precursor and 1 g of thiourea were heat-treated under nitrogen atmosphere at a heating rate of 4 °C / min to 550 °C for 2 hours to obtain the FeS / MoS2@N / B co-doped carbon rod-shaped heterostructure composite material.
[0030] Example 3
[0031] Solution A was prepared by dissolving 1.6 g of anhydrous cobalt nitrate and 0.8 g of anhydrous sodium molybdate in 30 mL of deionized water; solution B was prepared by dissolving 0.9 g of isophthalic acid and 0.3 g of polyvinylpyrrolidone in 30 mL of N,N-dimethylformamide (DMF). After mixing and stirring for 30 minutes, the mixture was transferred to a reaction vessel and incubated at 120 °C for 2 hours. The mixture was washed and dried to obtain the bimetallic MOF precursor. 0.5 g of the prepared bimetallic MOF precursor and 1 g of dopamine hydrochloride were dispersed in 200 mL of phosphate buffer (1 g / L) and stirred continuously for 12 hours. After centrifugation, washing, and drying, the composite material precursor was obtained. 0.5 g of the precursor and 2.5 g of thiourea were heat-treated under nitrogen atmosphere at a heating rate of 3 °C / min to 450 °C for 4 hours to obtain the FeS / MoS2@N / B co-doped carbon rod-shaped heterostructure composite material.
[0032] Example 4
[0033] Solution A was prepared by dissolving 1.2 g of anhydrous ferric chloride and 0.6 g of sodium tungstate in 30 mL of deionized water; solution B was prepared by dissolving 0.45 g of fumaric acid and 0.6 g of hexadecyltrimethylammonium bromide in 30 mL of dimethyl sulfoxide (DMSO). After mixing and stirring for 30 minutes, the mixture was transferred to a reaction vessel and incubated at 100 °C for 3 hours. The mixture was washed and dried to obtain the bimetallic MOF precursor. 0.1 g of the prepared bimetallic MOF precursor and 2 g of aniline were dispersed in 200 mL of thioacetamide buffer (10 g / L) and stirred continuously for 24 hours. After centrifugation, washing, and drying, the composite material precursor was obtained. 0.5 g of the precursor and 1.5 g of thiourea were heat-treated under nitrogen atmosphere at a heating rate of 2 °C / min to 550 °C for 2 hours to obtain the FeS / MoS2@N / B co-doped carbon rod-shaped heterostructure composite material.
[0034] Example 5
[0035] 2.4 g of anhydrous ferric chloride and 0.96 g of anhydrous sodium molybdate were dissolved in 30 mL of deionized water as solution A; 1.2 g of 2,6-naphthalenedicarboxylic acid and 1.5 g of polyvinyl alcohol were dissolved in 30 mL of ethylene glycol as solution B. After mixing and stirring for 30 minutes, the mixture was transferred to a reaction vessel and kept at 110 °C for 2 hours. The mixture was washed and dried to obtain the bimetallic MOF precursor. 0.3 g of the prepared bimetallic MOF precursor and 1 g of glucose were dispersed in 200 mL of thioacetamide buffer (12 g / L) and stirred continuously for 20 hours. After centrifugation, washing, and drying, the composite material precursor was obtained. 0.5 g of the obtained precursor and 1.75 g of sulfur were heat-treated under a nitrogen atmosphere at a heating rate of 3 °C / min to 500 °C for 2 hours to obtain the FeS / MoS2@N / B co-doped carbon rod-shaped heterostructure composite material.
[0036] Example 6
[0037] Solution A was prepared by dissolving 1.8 g of anhydrous nickel chloride and 0.99 g of anhydrous sodium molybdate in 30 mL of deionized water; solution B was prepared by dissolving 0.8 g of terephthalic acid and 0.9 g of polyethylene glycol in 30 mL of anhydrous ethanol. The mixture was stirred for 30 minutes and then transferred to a reaction vessel, where it was kept at 120 °C for 1 hour. After washing and drying, the bimetallic MOF precursor was obtained. 1.0 g of the prepared bimetallic MOF precursor and 0.5 g of chitosan were dispersed in 200 mL of borate buffer (6 g / L) and stirred continuously for 16 hours. After centrifugation, washing, and drying, the composite material precursor was obtained. 0.5 g of the precursor and 2.5 g of sulfur were heat-treated under a nitrogen atmosphere at a heating rate of 5 °C / min to 600 °C for 2 hours to obtain the FeS / MoS2@N / B co-doped carbon rod-shaped heterostructure composite material.
[0038] Comparative Example 1
[0039] In this comparative example, anhydrous sodium molybdate was not added, and other operations were the same as in Example 1, which will not be repeated here.
[0040] Comparative Example 2
[0041] In this comparative example, an excess of terephthalic acid (4 g) was added, and other operations were the same as in Example 1, which will not be repeated here.
[0042] Comparative Example 3
[0043] In this comparative example, dopamine hydrochloride was not added, and other operations were the same as in Example 1, which will not be repeated here.
[0044] Comparative Example 4
[0045] In this comparative example, thiourea was not added during the high-temperature heat treatment, and other operations were the same as in Example 1, which will not be repeated here.
[0046] Comparative Example 5
[0047] In this comparative example, the heat treatment temperature was 700 ℃, and other operations were the same as in Example 1, which will not be repeated here.
[0048] Performance testing:
[0049] Electromagnetic parameters were tested by mixing each example and comparative sample with paraffin wax (filling amount 30 wt%). The test results are shown in Table 1 below:
[0050] Table 1 Performance test results of the examples and comparative samples
[0051] Group / Performance Coating matching thickness (mm) Minimum reflection loss (dB) Effective bandwidth (GHz) Example 1 2.0 -62.1 5.2 Example 2 2.0 -63.4 5.8 Example 3 2.0 -61.6 5.1 Example 4 2.0 -60.9 5.5 Example 5 2.0 -62.4 5.3 Example 6 2.0 -62.7 5.8 Comparative Example 1 2.0 -36.7 3.2 Comparative Example 2 2.0 -32.2 3.9 Comparative Example 3 2.0 -29.7 3.8 Comparative Example 4 2.0 -28.6 3.2 Comparative Example 5 2.0 -30.8 2.7
[0052] Table 1 compares the coating matching thickness, minimum reflection loss, and effective bandwidth of the samples prepared in Examples 1-6. The composite materials prepared in Examples 1-6, with an ultra-thin matching thickness of 2.0 mm, all achieved a minimum reflection loss below -60 dB (between -60.9 dB and -63.4 dB), and maintained an effective bandwidth above 5.0 GHz (up to 5.8 GHz). This lays a solid foundation for achieving efficient and wide-band electromagnetic wave absorption with lightweight and thin materials. Test results show that each example effectively optimized the impedance matching of the material through the synergistic construction of multi-dimensional heterogeneous interfaces and the fine control of the microstructure, achieving superior electromagnetic loss capability and extremely wide frequency band coverage with an extremely thin coating thickness.
[0053] In Comparative Example 1, the lack of a molybdenum source prevented the construction of a bimetallic sulfide heterostructure, resulting in insufficient dielectric loss and a significantly increased minimum reflection loss. Adding organic ligands can adjust the precursor structure; for example, adding excessive terephthalic acid in Comparative Example 2 disrupts the coordination balance, causing the tubular structure to collapse and significantly weakening the multiple reflections and resonance effects of electromagnetic waves. Furthermore, even with a complete precursor structure, without carbon coating (as in Comparative Example 3), the lack of a heteroatom-doped carbon shell makes the metal sulfide prone to severe aggregation during sulfidation, and the absence of a conductive network further reduces dielectric loss and leads to impedance mismatch. In Comparative Example 4, sulfidation is not performed during heat treatment, preventing the transition metal from transforming into a bimetallic sulfide with high dielectric / magnetic field response. This results in an extremely simplistic loss mechanism and poor absorption performance. In addition, temperature control during the sulfidation heat treatment is also crucial. In Comparative Example 5, the excessively high temperature (700 °C) caused grain coarsening and partial melting of the tubular structure, weakened interfacial polarization, and electrical mismatch caused by excessively high electrical conductivity, ultimately leading to an increase in minimum reflection loss and a significant decrease in effective bandwidth.
[0054] The above description of the embodiments is only for illustrating the technical concept and features of the present invention. Its purpose is to enable those skilled in the art to understand the content of the present invention and implement it accordingly. Those skilled in the art can obviously easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative effort. Therefore, the above embodiments should not be used to limit the scope of protection of the present invention. All improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing a double transition metal sulfide-heteroatom doped rod-like composite material, characterized in that, The specific steps are as follows: (1) Synthesis of bimetallic MOF precursor: The first magnetic transition metal salt and the second group VIB transition metal salt were dissolved in deionized water to form solution A; the polycarboxylic acid organic ligand and surfactant were dissolved in an organic solvent to form solution B; solution A and solution B were mixed evenly in equal volumes and then transferred to a reaction vessel for solvothermal reaction. After the reaction was completed, the precipitate was collected, washed and dried to obtain the bimetallic MOF precursor. (2) In-situ construction of organic coating layer and introduction of heteroatoms: The bimetallic MOF precursor and organic carbon source prepared in step (1) are dispersed in a buffer solution containing heteroatom source and the reaction is continuously stirred; after the reaction is completed, the product is collected, centrifuged, washed and dried to obtain a core-shell structured composite material. (3) High-temperature sulfidation heat treatment: The composite material obtained in step (2) is placed in a tube furnace and subjected to high-temperature calcination heat treatment with sulfur-containing compounds placed upstream as sulfur source under a protective atmosphere; after cooling, a double transition metal sulfide-heteroatom doped rod-shaped composite material is obtained.
2. The production method according to claim 1, characterized by, The first magnetic transition metal salt mentioned in step (1) is one or more of iron salt, cobalt salt, nickel salt or manganese salt, and the mass ratio of its added mass to deionized water is (2-8):100; the second group VIB transition metal salt is one or more of molybdenum salt or tungsten salt, and the mass ratio of its added mass to deionized water is (1-5):
100.
3. The production method according to claim 2, characterized by, The first magnetic transition metal salt mentioned in step (1) is one or more of anhydrous ferric chloride, anhydrous ferric nitrate, anhydrous cobalt chloride, anhydrous cobalt nitrate, anhydrous nickel chloride, or anhydrous nickel nitrate; the second group VIB transition metal salt is one or more of anhydrous sodium molybdate, ammonium tetrathiomolybdate, ammonium molybdate, sodium tungstate, or ammonium tungstate.
4. The method of claim 1, wherein, The polycarboxylic acid organic ligands mentioned in step (1) are one or more of aromatic polycarboxylic acids or aliphatic polycarboxylic acids, and the mass-to-volume ratio of the added ligands to the organic solvent is 15-60 g / L; the surfactants are one or more of nonionic polymers, anionic surfactants, cationic surfactants or natural macromolecular dispersants, and the mass-to-volume ratio of the added surfactants to the organic solvent is 10-50 g / L; the organic solvents are one or more of amide solvents, sulfoxide solvents, alcohol solvents or ketone solvents.
5. The preparation method according to claim 4, characterized in that, The polycarboxylic acid organic ligands mentioned in step (1) are one or more of terephthalic acid, 2-aminoterephthalic acid, isophthalic acid, trimesoic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, or fumaric acid; the surfactants are one or more of polyvinylpyrrolidone, polyethylene glycol, polyvinyl alcohol, triblock copolymer F127, hexadecyltrimethylammonium bromide, or sodium dodecylbenzenesulfonate; and the organic solvents are one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, anhydrous ethanol, or ethylene glycol.
6. The method of claim 1, wherein The temperature of the solvothermal reaction in step (1) is 100-140 ℃, and the holding time is 1-3 hours.
7. The method of claim 1, wherein The organic carbon source mentioned in step (2) is one or more of dopamine hydrochloride, tannic acid, catechol, pyrrole, aniline, resorcinol-formaldehyde resin, glucose, cyclodextrin or chitosan, and the mass ratio of the added organic carbon source to the volume of the buffer solution is 0.5-10 g / L; the heteroatom source is one or more of inorganic heteroatom precursors and organic heteroatom precursors, and the mass ratio of the added heteroatom source to the volume of the buffer solution is 1-20 g / L.
8. The method of claim 1, wherein The heteroatom source mentioned in step (2) is one or more of the following: urea, melamine, dicyandiamide, polyaniline, polypyrrole, boric acid, sodium borate, sodium tetraphenylborate, phytic acid, phosphoric acid, ammonium dihydrogen phosphate, triphenylphosphine, thiourea, thioacetamide, sublimed sulfur, ammonium fluoride, sodium fluoride, and polyvinylidene fluoride.
9. The method of claim 1, wherein The mass ratio of the added bimetallic MOF precursor to the volume of the buffer solution in step (2) is 0.5-5 g / L; the stirring time is 12-24 hours.
10. The method of claim 1, wherein The sulfur-containing compound mentioned in step (3) is thiourea or sulfur, and the mass ratio of the sulfur-containing compound to the composite material is (2-5):1; the heat treatment protective atmosphere mentioned in step (3) is any one of nitrogen, argon and helium, the calcination temperature is 450-600 ℃, the holding time is 2-4 hours, and the heating rate is 2-5 ℃ / min.