Methods for fabricating solar cells and solar cells

By using a specific ratio of In2O3 and SnOx conductive layers and optimizing the thickness of the metal seed layer in solar cells, the problem of high dark film rate in the copper interconnect process was solved, and the yield and chemical corrosion resistance of solar cells were improved.

CN123124483APending Publication Date: 2026-11-17TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510622545.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing solar cell manufacturing processes, the copper interconnect process results in a high probability of dark spots, which affects the yield of solar cells.

Method used

A conductive layer of In2O3 and SnOx with a mass ratio of 97-99:0.8-3 is used. Combined with annealing treatment and thickness optimization of the metal seed layer, metal gate lines are formed to enhance the chemical corrosion resistance of the conductive layer and avoid damage to the PN junction by chemical solutions.

Benefits of technology

It effectively improves the yield of solar cells, reduces the corrosive effect of chemical solutions on the conductive layer, and avoids the dark spot problem in luminescence detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124483A_ABST
    Figure CN123124483A_ABST
Patent Text Reader

Abstract

This application relates to a method for fabricating solar cells and the solar cells themselves. The method for fabricating solar cells includes providing a solar cell substrate, the surface of which has a doped layer; and forming a conductive layer on the doped layer, the conductive layer comprising In₂O₃ and SnO in a mass ratio of 97–99:0.8–3. x A metal seed layer is formed on the conductive layer; metal grid lines are formed in the grid line region of the metal seed layer. This application can effectively improve the chemical corrosion resistance of the conductive layer and improve the yield of solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of solar cell manufacturing technology, and in particular to a method for preparing a solar cell and a solar cell. Background Technology

[0002] The copper interconnect process involves sputtering a metal seed layer onto the surface of an ITO (Indium Tin Oxide) transparent conductive film, followed by coating with a photosensitive material. The photosensitive material is then exposed using light with a specific pattern, causing material denaturation in the exposed areas. In the unexposed areas, grooves with a specific pattern are formed under the action of chemicals. Metal grid lines are then fabricated within these grooves using electroplating. Finally, the photosensitive material and the metal seed layer in the non-grid area areas are removed through a stripping and etching process.

[0003] However, when performing luminescence detection on solar cells prepared using the above process, the probability of dark spots is relatively high, which affects the yield of solar cells. Summary of the Invention

[0004] This application provides a method for preparing a solar cell and a solar cell, which can effectively improve the chemical corrosion resistance of the conductive layer and improve the yield of the solar cell.

[0005] In a first aspect, the method for preparing a solar cell provided in the embodiments of this application includes:

[0006] A solar cell substrate is provided, wherein the surface of the solar cell substrate has a doped layer;

[0007] A conductive layer is formed on the doped layer, the conductive layer comprising In₂O₃ and SnO in a mass ratio of 97–99:0.8–3. x ;

[0008] A metal seed layer is formed on the conductive layer;

[0009] Metal grid lines are formed in the grid line region of the metal seed layer.

[0010] In some embodiments, the conductive layer comprises In₂O₃ and SnO in a mass ratio of 99:0.8–1. x .

[0011] In some embodiments, the solar cell substrate includes a silicon substrate, a first intrinsic amorphous silicon layer and a first doped layer sequentially stacked on a first surface of the silicon substrate, and a second intrinsic amorphous silicon layer and a second doped layer sequentially stacked on a second surface of the silicon substrate, wherein the conductivity type of the first doped layer is the same as that of the silicon substrate, and the conductivity type of the second doped layer is opposite to that of the silicon substrate.

[0012] The step of forming a conductive layer on the doped layer includes forming a first conductive layer on the side of the first doped layer away from the silicon substrate, and forming a second conductive layer on the side of the second doped layer away from the silicon substrate;

[0013] The formation of the metal seed layer on the conductive layer includes forming a first metal seed layer on the side of the first conductive layer away from the silicon substrate, and forming a second metal seed layer on the side of the second conductive layer away from the silicon substrate, wherein the mass of the second metal seed layer on a unit area of ​​the second conductive layer is 0.18 mg / cm³. 2 ~0.2mg / cm 2 .

[0014] In some embodiments, the mass of the first metal seed layer on a unit area of ​​the first conductive layer is 0.16 mg / cm³. 2 ~0.2mg / cm 2 .

[0015] In some embodiments, forming metal gate lines in the gate line region of the metal seed layer includes:

[0016] A first metal gate line is formed in the gate line region of the first metal seed layer;

[0017] A second metal gate line is formed in the gate line region of the second metal seed layer, and the width of the second metal gate line is greater than the width of the first metal gate line.

[0018] In some embodiments, the silicon substrate is of the N-type conductivity.

[0019] In some embodiments, forming a conductive layer on the doped layer includes:

[0020] A conductive layer is deposited on the doped layer;

[0021] The conductive layer is then annealed.

[0022] In some embodiments, the annealing temperature is 180°C to 200°C.

[0023] In some embodiments, the annealing process lasts for 15 to 20 minutes.

[0024] Secondly, the solar cells provided in the embodiments of this application are obtained by using the solar cell preparation method provided in any of the above embodiments.

[0025] Compared with the prior art, the beneficial effects of the embodiments of this application are as follows: The method for preparing the solar cell and the solar cell include providing a solar cell substrate, the surface of which has a doped layer; forming a conductive layer on the doped layer, the conductive layer comprising In2O3 and SnO in a mass ratio of 97-99:0.8-3. x A metal seed layer is formed on the conductive layer; metal grid lines are formed in the grid line region of the metal seed layer. Through the embodiments of this application, the chemical corrosion resistance of the conductive layer can be effectively improved, thereby reducing the impact of chemical solutions used in subsequent processes on the conductive layer, effectively avoiding damage to the PN junction, solving the problem of dark spots in light emission detection, and improving the yield of solar cells. Attached Figure Description

[0026] Figure 1 This is a schematic flowchart illustrating a method for fabricating a solar cell according to an embodiment of this application.

[0027] Figure 2 This is a schematic diagram of the solar cell substrate structure provided in step S11 of one embodiment of this application.

[0028] Figure 3 This is a schematic diagram of the structure of the intermediate obtained in step S121 in one embodiment of this application.

[0029] Figure 4 This is a schematic diagram of the structure of the intermediate obtained in step S13 of one embodiment of this application.

[0030] Figure 5 This is a comparison chart showing the chemical resistance test results of the conductive layer of the solar cells prepared in Example 1, Example 2, and Comparative Example 1.

[0031] Figure 6 This is an EL panel rendering of the solar cell of Comparative Example 1 of the present invention.

[0032] Figure 7 This is an EL dark sheet effect diagram of the solar cell of Comparative Example 1 of the present invention.

[0033] Figure 8 This is a schematic diagram of the solar cell of Comparative Example 2 of the present invention.

[0034] Figure 9 This is a PL dark sheet effect diagram of the solar cell of Comparative Example 2 of the present invention.

[0035] Figure 10 This is a schematic diagram of the solar cell of Comparative Example 3 of the present invention.

[0036] Figure 11 This is a PL dark sheet effect diagram of the solar cell of Comparative Example 4 of the present invention. Detailed Implementation

[0037] To facilitate understanding of this application, a more complete description will be provided below with reference to the accompanying drawings. Preferred embodiments of this application are shown in the drawings. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of this application.

[0038] It should be noted that when a component is said to be "fixed to" another component, it can be directly attached to the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.

[0040] As used in this article, the description of "a1~a2" means "greater than or equal to a1" and "less than or equal to a2". For example, if x is 0~1, it means: 0≤x≤1.

[0041] like Figure 1 As shown, this is a method for preparing a solar cell according to one embodiment of this application.

[0042] like Figure 1 The method for fabricating this solar cell includes the following steps S11 to S14:

[0043] Step S11: Provide a solar cell substrate 100. The surface of the solar cell substrate 100 has a doped layer. Please refer to [reference needed]. Figure 2 As shown.

[0044] In some embodiments, the solar cell substrate 100 includes a silicon substrate 110, a first intrinsic amorphous silicon layer 120 and a first doped layer 130 sequentially stacked on a first surface of the silicon substrate 110, and a second intrinsic amorphous silicon layer 140 and a second doped layer 150 sequentially stacked on a second surface of the silicon substrate 110. The conductivity type of the first doped layer 130 is the same as that of the silicon substrate 110, and the conductivity type of the second doped layer 150 is opposite to that of the silicon substrate 110.

[0045] In one implementation, the silicon substrate 110 is an N-type single-crystal silicon wafer. The first doped layer 130 is an N-type doped amorphous silicon layer, and the second doped layer 150 is a P-type doped amorphous silicon layer.

[0046] In one implementation, step S11 may specifically include steps S111 to S112:

[0047] Step S111: The silicon substrate 110 is subjected to texturing and cleaning treatment to form a uniform "positive pyramid" textured surface on the surface of the silicon substrate 110. The base dimension (side length of the square base) of the pyramid structure of the textured surface can be 2μm to 8μm.

[0048] In step S112, a first intrinsic amorphous silicon layer 120 and a first doped layer 130 (N-type doped amorphous silicon layer) are sequentially deposited on the first surface of the texturized silicon substrate 110 using a PECVD (plasma enhanced chemical vapor deposition) plasma deposition equipment. Then, a second intrinsic amorphous silicon layer 140 and a second doped layer 150 (P-type doped amorphous silicon layer) are sequentially deposited on the second surface of the texturized silicon substrate 110 using the same PECVD equipment to form a PN junction.

[0049] The thickness of the first intrinsic amorphous silicon layer 120 can be 3nm to 6nm, the thickness of the second intrinsic amorphous silicon layer 140 can be 3nm to 9nm, the thickness of the first doped layer 130 can be 5nm to 10nm, and the thickness of the second doped layer 150 can be 5nm to 15nm.

[0050] Step S12: A conductive layer is formed on the doped layer, the conductive layer comprising In2O3 and SnO in a mass ratio of 97-99:0.8-3. x As examples, In2O3 and SnO x The mass ratio can be, but is not limited to, 97:3, 98:3, 99:3, 97:2, 99:2, 98:1, 99:1, 97:0.8 or 99:0.8.

[0051] Please refer to the conductive layer chemical resistance test below. The applicant found that reducing the SnO content in the conductive layer... x The appropriate doping ratio can effectively reduce crystal defects in the conductive layer, improve its resistance to chemical corrosion, solve the problem of dark spots in luminescence detection, and improve the yield of solar cells.

[0052] In this embodiment, the conductive layer comprises In₂O₃ and SnO in a mass ratio of 97–99:0.8–3. x This can effectively improve the chemical corrosion resistance of the conductive layer, avoiding corrosion of the conductive layer by chemical solutions such as developing solutions (Na2CO3 solution) and electroplating solutions (copper sulfate solution) in subsequent preparation steps. It can effectively avoid damage to the PN junction, solve the problem of dark spots in light emission detection, and improve the yield of solar cells.

[0053] In some implementations, step S12 includes step S121:

[0054] Step S121: Using a PVD (Physical Vapor Deposition) magnetron sputtering apparatus, a first conductive layer 210 and a second conductive layer 220 are formed on the side of the first doped layer 130 away from the silicon substrate 110 and the side of the second doped layer 150 away from the silicon substrate 110, respectively. Please refer to [reference needed]. Figure 3 As shown. The first conductive layer 210 comprises In2O3 and SnO in a mass ratio of 97-99:0.8-3. x The second conductive layer 220 comprises In2O3 and SnO in a mass ratio of 97–99:0.8–3. x .

[0055] The first conductive layer 210 and the second conductive layer 220 can each be a TCO (Transparent Conductive Oxides) thin film. For example, the first conductive layer 210 and the second conductive layer 220 can each be an ITO (Indium Tin Oxide) transparent conductive thin film. The thickness of the first conductive layer 210 and the second conductive layer 220 can each be 90 nm to 110 nm.

[0056] In one embodiment, the first conductive layer 210 comprises In2O3 and SnO in a mass ratio of 99:0.8 to 1. x The second conductive layer 220 comprises In2O3 and SnO in a mass ratio of 99:0.8~1. x As examples, In2O3 and SnO x The mass ratio can be, but is not limited to, 99:1, 99:0.9 or 99:0.8.

[0057] In this embodiment, the conductive layer comprises In₂O₃ and SnO in a mass ratio of 99:0.8 to 1. x This ensures the chemical corrosion resistance of the conductive layer and more effectively solves the problem of dark spots in luminescent detection.

[0058] In some implementations, step S12 further includes step S122:

[0059] Step S122: Anneal the first conductive layer 210 and the second conductive layer 220.

[0060] In this embodiment, annealing the conductive layer before forming the metal seed layer can effectively improve the crystallinity of the conductive layer.

[0061] As one implementation, the annealing temperature is 180°C to 200°C. For example, the annealing temperature can be, but is not limited to, 180°C, 185°C, 190°C, 195°C, or 200°C.

[0062] As one implementation method, the annealing process takes 15 to 20 minutes. As an example, the annealing process can take, but is not limited to, 15 minutes, 16 minutes, 17 minutes, 18 minutes, 19 minutes, or 20 minutes.

[0063] Step S13: Form a metal seed layer on the conductive layer.

[0064] Step S13 may specifically include: forming a first metal seed layer 310 and a second metal seed layer 320 respectively on the side of the first conductive layer 210 away from the silicon substrate 110 and the side of the second conductive layer 220 away from the silicon substrate 110 using a PVD magnetron sputtering device. Please refer to [reference needed]. Figure 4 As shown.

[0065] In some embodiments, the mass of the second metal seed layer 320 on the second conductive layer 220 per unit area is 0.18 mg / cm². 2 ~0.2mg / cm 2 As an example, the mass of the second metal seed layer 320 on the second conductive layer 220 per unit area can be, but is not limited to, 0.18 mg / cm². 2 0.19 mg / cm 2 Or 0.2 mg / cm 2 .

[0066] At the PN junction, a built-in electric field is generated due to the diffusion of electrons and holes. The applicant discovered that, due to the effect of this built-in electric field, H in the chemical solution... + Chemicals accumulate on the P-side (second surface) of the solar cell, leading to a difference in chemical resistance between the N-side (first surface) and the P-side (second surface). The P-side exhibits decreased chemical resistance, resulting in dark spots during luminescence testing. Please refer to the luminescence testing section below for details. The applicant discovered that increasing the thickness of the metal seed layer (second metal seed layer 320) on the P-side can block chemical solutions, weaken the difference in chemical resistance between the N-side and P-side caused by the PN junction, improve the dark spot problem in luminescence testing, and increase the yield of the solar cell.

[0067] In this embodiment, the mass of the second metal seed layer 320 on the second conductive layer 220 per unit area is 0.18 mg / cm². 2 ~0.2mg / cm 2 This allows the second metal seed layer 320 to have sufficient thickness to block chemical solutions, improve the chemical resistance of the P-side, and solve the problem of dark spots in luminescent detection.

[0068] In some embodiments, the mass of the first metal seed layer 310 on the first conductive layer 210 per unit area is 0.16 mg / cm². 2 ~0.2mg / cm 2 As an example, the mass of the first metal seed layer 310 on the first conductive layer 210 per unit area is 0.16 mg / cm². 2 0.17 mg / cm 2 0.18 mg / cm 2 0.19 mg / cm 2 Or 0.2 mg / cm 2 .

[0069] Step S14: Form metal grid lines in the grid line region of the metal seed layer.

[0070] Specifically, a first metal gate line is formed in the gate line region of the first metal seed layer 310, and a second metal gate line is formed in the gate line region of the second metal seed layer 320.

[0071] In some embodiments, the first surface of the solar cell substrate 100 is the light-receiving surface, and the second surface of the solar cell substrate 100 is the back-lighting surface; that is, the first metal grid line is located on the light-receiving surface, and the second metal grid line is located on the back-lighting surface. The width of the second metal grid line is greater than the width of the first metal grid line, which can optimize current transmission and mechanical support performance.

[0072] In some embodiments, the preparation method further includes step S15 before step S14:

[0073] Step S15: A photosensitive adhesive layer is formed on the metal seed layer. The photosensitive adhesive layer has patterned grooves, and the grid line area of ​​the metal seed layer is exposed in the patterned grooves.

[0074] In one implementation, step S15 specifically includes steps S151 to S153:

[0075] In step S151, photosensitive adhesive layers are coated onto the first metal seed layer 310 and the second metal seed layer 320 respectively, completely covering both layers. The thickness of the photosensitive adhesive layers is controlled between 10 μm and 15 μm.

[0076] Step S152: The designed grid pattern is laser-printed onto the photosensitive emulsion layer and then exposed.

[0077] In step S153, the unexposed photosensitive adhesive layer (grid line area) is cleaned and removed using a sodium carbonate solution to form a patterned groove, exposing the grid line area of ​​the first metal seed layer 310 and the grid line area of ​​the second metal seed layer 320.

[0078] In this embodiment, after step S14, the preparation method further includes step S16:

[0079] Step S16: First, remove the remaining photosensitive emulsion in an alkaline solution (NaOH, KOH, etc.), and then remove the first metal seed layer 310 in the non-grid area and the second metal seed layer 320 in the non-grid area in a dilute sulfuric acid solution.

[0080] The solar cell provided in this application embodiment is obtained by using the solar cell preparation method provided in any of the above embodiments.

[0081] The present application will be further illustrated below through specific embodiments and comparative examples.

[0082] Example 1

[0083] This embodiment provides a method for fabricating a solar cell, including the following steps:

[0084] Step 1-1: The silicon substrate 110 is texturized and cleaned to form a uniform "positive pyramid" textured surface on the silicon wafer. The silicon substrate 110 is an N-type monocrystalline silicon wafer, and the base size of the pyramid structure of the textured surface is 2μm to 8μm.

[0085] Steps 1-2: Using a PECVD plasma deposition system, a first intrinsic amorphous silicon layer 120 and an N-type doped amorphous silicon layer are sequentially deposited on the first surface of the texturized silicon substrate 110. Then, using the same PECVD system, a second intrinsic amorphous silicon layer 140 and a P-type doped amorphous silicon layer are sequentially deposited on the second surface of the texturized silicon substrate 110. The thickness of the first intrinsic amorphous silicon layer 120 is 3 nm to 6 nm, the thickness of the second intrinsic amorphous silicon layer 140 is 3 nm to 9 nm, the thickness of the N-type doped amorphous silicon layer is 5 nm to 10 nm, and the thickness of the P-type doped amorphous silicon layer is 5 nm to 15 nm.

[0086] Steps 1-3 involve depositing a first conductive layer 210 and a second conductive layer 220 on the N-type doped amorphous silicon layer and the P-type doped amorphous silicon layer, respectively, using a PVD magnetron sputtering apparatus. The first conductive layer 210 and the second conductive layer 220 are both ITO transparent conductive films. The first conductive layer 210 comprises In₂O₃ and SnO in a mass ratio of 99:1. x The second conductive layer 220 comprises In2O3 and SnO in a mass ratio of 99:1. x .

[0087] Steps 1-4 involve depositing a first copper seed layer and a second copper seed layer on the first conductive layer 210 and the second conductive layer 220, respectively, using a PVD magnetron sputtering apparatus. The mass of the first copper seed layer on the first conductive layer 210 per unit area is 0.16 mg / cm³. 2~0.2mg / cm 2 The mass of the second copper seed layer on the second conductive layer 220 per unit area is 0.11 mg / cm³. 2 ~0.13mg / cm 2 .

[0088] Steps 1-5: Apply photosensitive emulsion to the first and second copper seed layers respectively, completely covering both layers. The thickness of the photosensitive emulsion layer is controlled between 10 μm and 15 μm.

[0089] Steps 1-6: Print the designed grid pattern onto the photosensitive emulsion layer using laser and then expose it.

[0090] Steps 1-7: Use sodium carbonate solution to clean and remove the unexposed photosensitive emulsion layer (grid area) to form patterned grooves, exposing the first copper seed layer and the second copper seed layer.

[0091] Steps 1-8: Wrap the four edges and corners with edge-sealing tape. The width of the edge-sealing tape should be less than or equal to 50μm, and the thickness should be 10μm to 15μm.

[0092] Steps 1-9 involve electroplating the first and second copper grid lines in a copper sulfate plating solution. The heights of the first and second copper grid lines are controlled between 8 μm and 10 μm, respectively.

[0093] Steps 1-10: First, remove the remaining photosensitive emulsion in an alkaline solution (NaOH, KOH, etc.). Then, remove the first copper seed layer in the non-grid area and the second copper seed layer in the non-grid area in a dilute sulfuric acid solution to obtain a battery cell with a copper seed layer only in the grid area.

[0094] Example 2

[0095] This embodiment provides a method for fabricating a solar cell, including the following steps:

[0096] Step 2-1: The silicon substrate 110 is texturized and cleaned to form a uniform "positive pyramid" textured surface on the silicon wafer surface. The silicon substrate 110 is an N-type monocrystalline silicon wafer, and the base size of the pyramid structure of the textured surface is 2μm to 8μm.

[0097] Step 2-2: Using a PECVD plasma deposition system, a first intrinsic amorphous silicon layer 120 and an N-type doped amorphous silicon layer are sequentially deposited on the first surface of the texturized silicon substrate 110. Then, using the same PECVD system, a second intrinsic amorphous silicon layer 140 and a P-type doped amorphous silicon layer are sequentially deposited on the second surface of the texturized silicon substrate 110. The thickness of the first intrinsic amorphous silicon layer 120 is 3 nm to 6 nm, the thickness of the second intrinsic amorphous silicon layer 140 is 3 nm to 9 nm, the thickness of the N-type doped amorphous silicon layer is 5 nm to 10 nm, and the thickness of the P-type doped amorphous silicon layer is 5 nm to 15 nm.

[0098] Steps 2-3 involve depositing a first conductive layer 210 and a second conductive layer 220 on the N-type doped amorphous silicon layer and the P-type doped amorphous silicon layer, respectively, using a PVD magnetron sputtering apparatus. The first conductive layer 210 and the second conductive layer 220 are both ITO transparent conductive films. The first conductive layer 210 comprises In₂O₃ and SnO in a mass ratio of 97:3. x The second conductive layer 220 comprises In2O3 and SnO in a mass ratio of 97:3. x .

[0099] Steps 2-4 involve depositing a first copper seed layer and a second copper seed layer on the first conductive layer 210 and the second conductive layer 220, respectively, using a PVD magnetron sputtering apparatus. The mass of the first copper seed layer on the first conductive layer 210 per unit area is 0.16 mg / cm³. 2 ~0.2mg / cm 2 The mass of the second copper seed layer on the second conductive layer 220 per unit area is 0.11 mg / cm³. 2 ~0.13mg / cm 2 .

[0100] Steps 2-5: Apply photosensitive emulsion to the first and second copper seed layers respectively, completely covering both layers. The thickness of the photosensitive emulsion layer is controlled between 10 μm and 15 μm.

[0101] Steps 2-6: Print the designed grid pattern onto the photosensitive emulsion layer using laser printing, and then expose it.

[0102] Steps 2-7: Use sodium carbonate solution to clean and remove the unexposed photosensitive emulsion layer (grid area) to form patterned grooves, exposing the first copper seed layer and the second copper seed layer.

[0103] Steps 2-8: Wrap the four corner edges and corner positions with edge-sealing tape. The width of the edge-sealing tape should be less than or equal to 50μm, and the thickness of the edge-sealing tape should be 10μm to 15μm.

[0104] Steps 2-9 involve electroplating the first and second copper grid lines in a copper sulfate plating solution. The heights of the first and second copper grid lines are controlled between 8 μm and 10 μm, respectively.

[0105] Steps 2-10: First, remove the remaining photosensitive emulsion in an alkaline solution (NaOH, KOH, etc.). Then, remove the first copper seed layer in the non-grid area and the second copper seed layer in the non-grid area in a dilute sulfuric acid solution to obtain a battery cell with a copper seed layer only in the grid area.

[0106] Example 3

[0107] This embodiment provides a method for fabricating a solar cell, including the following steps:

[0108] Step 3-1: The silicon substrate 110 is texturized and cleaned to form a uniform "positive pyramid" textured surface on the silicon wafer. The silicon substrate 110 is an N-type monocrystalline silicon wafer, and the base size of the pyramid structure of the textured surface is 2μm to 8μm.

[0109] Step 3-2: Using a PECVD plasma deposition system, a first intrinsic amorphous silicon layer 120 and an N-type doped amorphous silicon layer are sequentially deposited on the first surface of the texturized silicon substrate 110. Then, using the same PECVD system, a second intrinsic amorphous silicon layer 140 and a P-type doped amorphous silicon layer are sequentially deposited on the second surface of the texturized silicon substrate 110. The thickness of the first intrinsic amorphous silicon layer 120 is 3 nm to 6 nm, the thickness of the second intrinsic amorphous silicon layer 140 is 3 nm to 9 nm, the thickness of the N-type doped amorphous silicon layer is 5 nm to 10 nm, and the thickness of the P-type doped amorphous silicon layer is 5 nm to 15 nm.

[0110] Step 3-3: A first conductive layer 210 and a second conductive layer 220 are deposited on the N-type doped amorphous silicon layer and the P-type doped amorphous silicon layer, respectively, using a PVD magnetron sputtering apparatus. The first conductive layer 210 and the second conductive layer 220 are both ITO transparent conductive films. The first conductive layer 210 comprises In₂O₃ and SnO in a mass ratio of 97–99:0.8–3. x The second conductive layer 220 comprises In2O3 and SnO in a mass ratio of 97–99:0.8–3. x .

[0111] Steps 3-4 involve depositing a first copper seed layer and a second copper seed layer on the first conductive layer 210 and the second conductive layer 220, respectively, using a PVD magnetron sputtering apparatus. The mass of the first copper seed layer on the first conductive layer 210 per unit area is 0.16 mg / cm³. 2 ~0.2mg / cm 2 The mass of the second copper seed layer on the second conductive layer 220 per unit area is 0.18 mg / cm³. 2~0.2mg / cm 2 .

[0112] Steps 3-5: Apply photosensitive emulsion to the first and second copper seed layers respectively, completely covering both layers. The thickness of the photosensitive emulsion layer is controlled between 10 μm and 15 μm.

[0113] Steps 3-6: Print the designed grid pattern onto the photosensitive emulsion layer using laser printing, and then expose it.

[0114] Steps 3-7: Use sodium carbonate solution to clean and remove the unexposed photosensitive emulsion layer (grid area) to form patterned grooves, exposing the first copper seed layer and the second copper seed layer.

[0115] Steps 3-8: Wrap the four corner edges and corner positions with edge-sealing tape. The width of the edge-sealing tape should be less than or equal to 50μm, and the thickness of the edge-sealing tape should be 10μm to 15μm.

[0116] Steps 3-9 involve electroplating the first and second copper grid lines in a copper sulfate plating solution. The heights of the first and second copper grid lines are controlled between 8 μm and 10 μm, respectively.

[0117] Steps 3-10: First, remove the remaining photosensitive emulsion in an alkaline solution (NaOH, KOH, etc.). Then, remove the first copper seed layer in the non-grid line region and the second copper seed layer in the non-grid line region in a dilute sulfuric acid solution to obtain a battery cell with a copper seed layer only in the grid line region.

[0118] Comparative Example 1

[0119] This comparative example provides a method for fabricating a solar cell, including the following steps:

[0120] Step 4-1 involves texturing and cleaning the silicon substrate to form a uniform "positive pyramid" textured surface on the silicon wafer. The silicon substrate is an N-type monocrystalline silicon wafer, and the base dimensions of the pyramid structure on the textured surface range from 2μm to 8μm.

[0121] Step 4-2: Using a PECVD plasma deposition system, a first intrinsic amorphous silicon layer and an N-type doped amorphous silicon layer are sequentially deposited on the first surface of the texturized silicon substrate. Then, using the same PECVD system, a second intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer are sequentially deposited on the second surface of the texturized silicon substrate. The thickness of the first intrinsic amorphous silicon layer is 3 nm to 6 nm, the thickness of the second intrinsic amorphous silicon layer is 3 nm to 9 nm, the thickness of the N-type doped amorphous silicon layer is 5 nm to 10 nm, and the thickness of the P-type doped amorphous silicon layer is 5 nm to 15 nm.

[0122] Step 4-3: A first conductive layer and a second conductive layer are deposited on the N-type doped amorphous silicon layer and the P-type doped amorphous silicon layer, respectively, using a PVD magnetron sputtering apparatus. The first and second conductive layers are both ITO transparent conductive films. The first conductive layer comprises In₂O₃ and SnO in a mass ratio of 90:10. x The second conductive layer comprises In₂O₃ and SnO in a mass ratio of 90:10. x .

[0123] Step 4-4: A first copper seed layer and a second copper seed layer are deposited on the first conductive layer and the second conductive layer, respectively, using a PVD magnetron sputtering apparatus. The mass of the first copper seed layer per unit area on the first conductive layer is 0.16 mg / cm³. 2 ~0.2mg / cm 2 The mass of the second copper seed layer on the second conductive layer per unit area is 0.11 mg / cm². 2 ~0.13mg / cm 2 .

[0124] Steps 4-5: Apply photosensitive emulsion to the first and second copper seed layers respectively, completely covering both layers. The thickness of the photosensitive emulsion layer is controlled between 10 μm and 15 μm.

[0125] Steps 4-6: Print the designed grid pattern onto the photosensitive emulsion layer using laser printing, and then expose it.

[0126] Steps 4-7: Use sodium carbonate solution to clean and remove the unexposed photosensitive emulsion layer (grid line area) to form patterned grooves, exposing the first copper seed layer and the second copper seed layer.

[0127] Steps 4-8: Wrap the four corner edges and corner positions with edge-sealing tape. The width of the edge-sealing tape should be less than or equal to 50μm, and the thickness of the edge-sealing tape should be 10μm to 15μm.

[0128] Steps 4-9 involve electroplating the first and second copper grid lines in a copper sulfate plating solution. The heights of the first and second copper grid lines are controlled between 8 μm and 10 μm, respectively.

[0129] Steps 4-10: First, remove the remaining photosensitive emulsion in an alkaline solution (NaOH, KOH, etc.). Then, remove the first copper seed layer in the non-grid line region and the second copper seed layer in the non-grid line region in a dilute sulfuric acid solution to obtain a battery cell with a copper seed layer only in the grid line region.

[0130] Comparative Example 2

[0131] This comparative example provides a method for fabricating a solar cell, including the following steps:

[0132] Step 5-1 involves texturing and cleaning the silicon substrate to form a uniform "positive pyramid" textured surface on the silicon wafer. The silicon substrate is an N-type monocrystalline silicon wafer, and the base dimensions of the pyramid structure on the textured surface range from 2μm to 8μm.

[0133] Step 5-2: Using a PECVD plasma deposition system, a first intrinsic amorphous silicon layer and an N-type doped amorphous silicon layer are sequentially deposited on the first surface of the texturized silicon substrate. Then, using the same PECVD system, a second intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer are sequentially deposited on the second surface of the texturized silicon substrate. The thickness of the first intrinsic amorphous silicon layer is 3 nm to 6 nm, the thickness of the second intrinsic amorphous silicon layer is 3 nm to 9 nm, the thickness of the N-type doped amorphous silicon layer is 5 nm to 10 nm, and the thickness of the P-type doped amorphous silicon layer is 5 nm to 15 nm.

[0134] Step 5-3: A first conductive layer and a second conductive layer are deposited on the N-type doped amorphous silicon layer and the P-type doped amorphous silicon layer, respectively, using a PVD magnetron sputtering apparatus. The first and second conductive layers are both ITO transparent conductive films. The first conductive layer comprises In₂O₃ and SnO in a mass ratio of 90:10. x The second conductive layer comprises In₂O₃ and SnO in a mass ratio of 90:10. x .

[0135] Step 5-4: A first copper seed layer and a second copper seed layer are deposited on the first conductive layer and the second conductive layer, respectively, using a PVD magnetron sputtering apparatus. The mass of the first copper seed layer per unit area on the first conductive layer is 0.16 mg / cm³. 2 ~0.2mg / cm 2 The mass of the second copper seed layer on the second conductive layer per unit area is 0.11 mg / cm². 2 ~0.13mg / cm 2 .

[0136] Step 5-5: Coat the first and second copper seed layers with photosensitive emulsion, completely covering both layers. The thickness of the photosensitive emulsion layer should be controlled between 10 μm and 15 μm.

[0137] Steps 5-6 involve laser printing the first grid line pattern onto the photosensitive adhesive layer and then exposing it. Note that the grid line area of ​​the first grid line pattern occupies only half of the pre-defined grid line area of ​​the solar cell. Please refer to [reference needed]. Figure 8 and Figure 9 As shown, only the right half of the solar cell has grid lines, while the left half has no grid lines.

[0138] Steps 5-7: Use sodium carbonate solution to clean and remove the unexposed photosensitive emulsion layer (the grid area of ​​the first grid pattern) to form patterned grooves, exposing the first copper seed layer and the second copper seed layer.

[0139] Steps 5-8: Wrap the four corner edges and corner positions with edge-sealing tape. The width of the edge-sealing tape should be less than or equal to 50μm, and the thickness of the edge-sealing tape should be 10μm to 15μm.

[0140] Steps 5-9 involve electroplating the first and second copper grid lines in a copper sulfate plating solution. The heights of the first and second copper grid lines are controlled between 8 μm and 10 μm, respectively.

[0141] Steps 5-10: First, remove the remaining photosensitive emulsion in an alkaline solution (NaOH, KOH, etc.). Then, remove the first copper seed layer in the non-grid area and the second copper seed layer in the non-grid area in a dilute sulfuric acid solution to obtain a solar cell test piece with a copper seed layer only in the grid area.

[0142] Comparative Example 3

[0143] This comparative example provides a method for fabricating a solar cell, including the following steps:

[0144] Step 6-1 involves texturing and cleaning the silicon substrate to form a uniform "positive pyramid" textured surface on the silicon wafer. The silicon substrate is an N-type monocrystalline silicon wafer, and the base dimensions of the pyramid structure on the textured surface range from 2μm to 8μm.

[0145] Step 6-2: Using a PECVD plasma deposition system, a first intrinsic amorphous silicon layer and an N-type doped amorphous silicon layer are sequentially deposited on the first surface of the texturized silicon substrate. Then, using the same PECVD system, a second intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer are sequentially deposited on the second surface of the texturized silicon substrate. The thickness of the first intrinsic amorphous silicon layer is 3 nm to 6 nm, the thickness of the second intrinsic amorphous silicon layer is 3 nm to 9 nm, the thickness of the N-type doped amorphous silicon layer is 5 nm to 10 nm, and the thickness of the P-type doped amorphous silicon layer is 5 nm to 15 nm.

[0146] Step 6-3: A first conductive layer and a second conductive layer are deposited on the N-type doped amorphous silicon layer and the P-type doped amorphous silicon layer, respectively, using a PVD magnetron sputtering apparatus. The first and second conductive layers are both ITO transparent conductive films. The first conductive layer comprises In₂O₃ and SnO in a mass ratio of 90:10. x The second conductive layer comprises In₂O₃ and SnO in a mass ratio of 90:10. x .

[0147] Step 6-4: A first copper seed layer and a second copper seed layer are deposited on the first conductive layer and the second conductive layer, respectively, using a PVD magnetron sputtering apparatus. The mass of the first copper seed layer per unit area on the first conductive layer is 0.16 mg / cm³. 2 ~0.2mg / cm 2 The mass of the second copper seed layer on the second conductive layer per unit area is 0.11 mg / cm². 2 ~0.13mg / cm 2 .

[0148] Step 6-5: Apply photosensitive emulsion to the first and second copper seed layers respectively, completely covering both layers. The thickness of the photosensitive emulsion layer is controlled between 10 μm and 15 μm.

[0149] Step 6-6: Print the designed grid pattern onto the photosensitive emulsion layer of the first copper seed layer using laser printing, and then expose it.

[0150] Steps 6-7 involve using a sodium carbonate solution to clean and remove the unexposed photosensitive emulsion layer (grid area), forming patterned grooves and exposing the first copper seed layer.

[0151] Steps 6-8: Wrap the four corner edges and corner positions with edge-sealing tape. The width of the edge-sealing tape should be less than or equal to 50μm, and the thickness of the edge-sealing tape should be 10μm to 15μm.

[0152] Steps 6-9 involve electroplating the first copper grid line in a copper sulfate plating solution. The height of the first copper grid line is controlled between 8 μm and 10 μm.

[0153] Steps 6-10: First, remove the remaining photosensitive emulsion in an alkaline solution (NaOH, KOH, etc.), and then remove the first copper seed layer in the non-grid area in a dilute sulfuric acid solution.

[0154] Comparative Example 4

[0155] This comparative example provides a method for fabricating a solar cell, including the following steps:

[0156] Step 7-1 involves texturing and cleaning the silicon substrate to form a uniform "positive pyramid" textured surface on the silicon wafer. The silicon substrate is an N-type monocrystalline silicon wafer, and the base dimensions of the pyramid structure on the textured surface range from 2μm to 8μm.

[0157] Step 7-2: Using a PECVD plasma deposition system, a first intrinsic amorphous silicon layer and an N-type doped amorphous silicon layer are sequentially deposited on the first surface of the texturized silicon substrate. Then, using the same PECVD system, a second intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer are sequentially deposited on the second surface of the texturized silicon substrate. The thickness of the first intrinsic amorphous silicon layer is 3 nm to 6 nm, the thickness of the second intrinsic amorphous silicon layer is 3 nm to 9 nm, the thickness of the N-type doped amorphous silicon layer is 5 nm to 10 nm, and the thickness of the P-type doped amorphous silicon layer is 5 nm to 15 nm.

[0158] Step 7-3: A first conductive layer and a second conductive layer are deposited on the N-type doped amorphous silicon layer and the P-type doped amorphous silicon layer, respectively, using a PVD magnetron sputtering apparatus. The first and second conductive layers are both ITO transparent conductive films. The first conductive layer comprises In₂O₃ and SnO in a mass ratio of 90:10. x The second conductive layer comprises In₂O₃ and SnO in a mass ratio of 90:10. x .

[0159] Step 7-4: A first copper seed layer and a second copper seed layer are deposited on the first conductive layer and the second conductive layer, respectively, using a PVD magnetron sputtering apparatus. The mass of the first copper seed layer per unit area on the first conductive layer is 0.16 mg / cm³. 2 ~0.2mg / cm 2 The mass of the second copper seed layer on the second conductive layer per unit area is 0.11 mg / cm². 2 ~0.13mg / cm 2 .

[0160] Step 7-5: Apply photosensitive emulsion to the first and second copper seed layers respectively, completely covering both layers. The thickness of the photosensitive emulsion layer is controlled between 10 μm and 15 μm.

[0161] Steps 7-6: Print the designed grid pattern onto the photosensitive emulsion layer of the second copper seed layer using laser printing, and then expose it.

[0162] Step 7-7: Use sodium carbonate solution to clean and remove the unexposed photosensitive emulsion layer (grid area) to form patterned grooves and expose the second copper seed layer.

[0163] Steps 7-8: Wrap the four edges and corners with edge-sealing tape. The width of the edge-sealing tape should be less than or equal to 50μm, and the thickness should be 10μm to 15μm.

[0164] Steps 7-9 involve electroplating the second copper grid line in a copper sulfate plating solution. The height of the second copper grid line is controlled between 8 μm and 10 μm.

[0165] Steps 7-10: First, remove the remaining photosensitive emulsion in an alkaline solution (NaOH, KOH, etc.), and then remove the second copper seed layer in the non-grid area in a dilute sulfuric acid solution.

[0166] Chemical resistance test of conductive layer

[0167] The solar cells prepared in Example 1, Example 2, and Comparative Example 1 were immersed in an acidic solution to test the acid resistance (H2O) of each solar cell. + Corrosion resistance. Please refer to [reference needed]. Figure 5 As shown, the conductive layer of the solar cell prepared in Example 1 remained normal during immersion for 0–350 min, without discoloration or peeling. The conductive layer of the solar cell prepared in Example 2 remained normal during immersion for 0–120 min; after immersion exceeding 120 min, the conductive layer discolored; and after immersion exceeding 270 min, the conductive layer peeled off. The conductive layer of the solar cell prepared in Comparative Example 1 remained normal during immersion for 0–30 min; after immersion exceeding 30 min, the conductive layer discolored; and after immersion exceeding 90 min, the conductive layer peeled off. Therefore, the solar cell prepared in Example 1 exhibits the best chemical corrosion resistance, while the solar cell prepared in Comparative Example 1 exhibits the worst chemical corrosion resistance.

[0168] Luminescence test

[0169] EL (Electroluminescence) testing

[0170] EL tests were performed on multiple solar cells prepared in Comparative Example 1, and the results were as follows: Figure 6 and Figure 7 The diagrams shown illustrate the light and dark conditions. Some solar cells showed normal EL test results, as shown in Figure 6 (bright EL sheet). Other solar cells showed abnormal EL test results, as shown in Figure 7 (dark EL sheet).

[0171] In addition, the electrical performance of the solar cells prepared in Comparative Example 1, which were tested with EL bright film and EL dark film, was tested. The test results are shown in Table 1. The tested electrical performance parameters include: conversion efficiency (Eta), open circuit voltage (Uoc), short circuit current (Isc), fill factor (FF), performance filling factor (PFF), series resistance (Rser), parallel resistance (Rshunt), reverse leakage current (IRev2), standard deviation of conversion efficiency (Eta std.), and maximum conversion efficiency (Eta-Max). Among them, the solar cells with EL dark film showed severe leakage, indicating that the PN junction of the solar cells was damaged during the solar cell preparation process.

[0172] Table 1 Comparison of Solar Cell Electrical Performance Tests

[0173]

[0174] PL (Photoluminescence) test

[0175] PL tests were performed on the solar cell test pieces prepared in Comparative Example 2, and the results were as follows: Figure 8 and Figure 9 The diagram shows a contrast profile. 2% of the test pieces showed abnormal PL test results; the portion of the test piece with the grid lines (the right half of the test piece) appeared dark in the PL test. Figure 9 As shown. The PL test results of the remaining test pieces are normal, as shown. Figure 8 As shown.

[0176] PL tests were performed on multiple solar cell test pieces prepared in Comparative Example 3 and Comparative Example 4, respectively, and the results were as follows: Figure 10 and Figure 11 The diagram shows the contrast between light and dark areas. The PL test results of the test piece prepared in Comparative Example 3 were all normal. Figure 10 The PL test strips shown are as follows. In Comparative Example 4, 5% of the test strips obtained showed abnormal PL test results. Figure 11 The PL film shown.

[0177] The above EL and PL test results indicate that during the fabrication of solar cells, prolonged contact with chemical solutions can lead to corrosion and damage to the conductive layer, and the chemical solutions cause greater damage to the P-side than to the N-side.

[0178] EL tests were performed on multiple solar cells prepared in Example 3. The EL test results of all solar cells were normal, and the test results were similar to those of other solar cells. Figure 6 The EL sheet is shown. PL tests were performed on multiple solar cells prepared in Example 3, and the PL test results for all solar cells were normal.

[0179] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0180] The above embodiments merely illustrate preferred implementations of this application, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the scope of protection of this application. Therefore, the scope of protection of this patent application should be determined by the appended claims.

Claims

1. A method for fabricating a solar cell, characterized in that, include: A solar cell substrate is provided, wherein the surface of the solar cell substrate has a doped layer; forming a conductive layer on the doped layer, the conductive layer comprising In2O3 and SnO in a mass ratio of 97-99:0.8-3 x ; A metal seed layer is formed on the conductive layer; Metal grid lines are formed in the grid line region of the metal seed layer.

2. The method for preparing a solar cell as described in claim 1, characterized in that, The conductive layer comprises In₂O₃ and SnO in a mass ratio of 99:0.8–1. x .

3. The method for preparing a solar cell as described in claim 1, characterized in that, The solar cell substrate includes a silicon substrate, a first intrinsic amorphous silicon layer and a first doped layer sequentially stacked on a first surface of the silicon substrate, and a second intrinsic amorphous silicon layer and a second doped layer sequentially stacked on a second surface of the silicon substrate. The conductivity type of the first doped layer is the same as that of the silicon substrate, and the conductivity type of the second doped layer is opposite to that of the silicon substrate. The step of forming a conductive layer on the doped layer includes forming a first conductive layer on the side of the first doped layer away from the silicon substrate, and forming a second conductive layer on the side of the second doped layer away from the silicon substrate; The formation of the metal seed layer on the conductive layer includes forming a first metal seed layer on the side of the first conductive layer away from the silicon substrate, and forming a second metal seed layer on the side of the second conductive layer away from the silicon substrate, wherein the mass of the second metal seed layer on a unit area of ​​the second conductive layer is 0.18 mg / cm³. 2 ~0.2mg / cm 2 .

4. The method for preparing a solar cell as described in claim 3, characterized in that, The mass of the first metal seed layer on the first conductive layer per unit area is 0.16 mg / cm³. 2 ~0.2mg / cm 2 .

5. The method for preparing a solar cell as described in claim 3, characterized in that, The formation of metal gate lines in the gate line region of the metal seed layer includes: A first metal gate line is formed in the gate line region of the first metal seed layer; A second metal gate line is formed in the gate line region of the second metal seed layer, and the width of the second metal gate line is greater than the width of the first metal gate line.

6. The method for preparing a solar cell as described in claim 3, characterized in that, The silicon substrate has an N-type conductivity.

7. The method for preparing a solar cell as described in claim 1, characterized in that, The formation of a conductive layer on the doped layer includes: A conductive layer is deposited on the doped layer; The conductive layer is then annealed.

8. The method for preparing a solar cell as described in claim 7, characterized in that, The annealing temperature is 180℃~200℃.

9. The method for preparing a solar cell as described in claim 7, characterized in that, The annealing process takes 15 to 20 minutes.

10. A solar cell, characterized in that, The solar cell is obtained by the method described in any one of claims 1-9.