Light Emitting Diode Chips and Their Fabrication Methods

By introducing periodically alternating InGaN and GaN composite layers and a second quantum well layer into the light-emitting diode chip, the V-shaped pit defects and interface blurring problems caused by shallow multi-quantum well layers are solved, thereby improving electron utilization and luminous efficiency.

CN123124532APending Publication Date: 2026-11-17BOE HUACAN OPTOELECTRONICS (GUANGDONG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611544064.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, shallow quantum well layers are prone to V-shaped pit defects, which lead to leakage channels, affecting chip yield and limiting the improvement of luminous efficiency.

Method used

A composite layer consisting of a first sublayer and a second sublayer that alternate periodically is introduced into a light-emitting diode chip. The first sublayer is an InGaN layer and the second sublayer is a GaN layer. The In composition is gradually changed in the stacking direction to form a stepped potential energy difference structure. This is combined with a second quantum well layer to improve stress and interface ambiguity issues.

Benefits of technology

By forming a stepped potential energy difference structure, the electron flow velocity is effectively slowed down, the electron utilization rate is increased, and the luminescence efficiency is improved. At the same time, the problems caused by shallow quantum well layers are avoided, and the quality of the interface crystal is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124532A_ABST
    Figure CN123124532A_ABST
Patent Text Reader

Abstract

This disclosure provides a light-emitting diode (LED) chip and its fabrication method, belonging to the field of semiconductor fabrication technology. The LED chip includes: a first semiconductor layer, a composite layer, a first quantum well layer, and a second semiconductor layer stacked sequentially; the composite layer includes periodically alternating first and second sub-layers, the first sub-layer being an InGaN layer and the second sub-layer being a GaN layer, and in the stacking direction of the composite layer, the In content of each first sub-layer gradually increases or gradually decreases. This disclosure can effectively improve the luminous efficacy of the LED.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure belongs to the field of semiconductor fabrication technology, and specifically relates to a light-emitting diode chip and its fabrication method. Background Technology

[0002] With the gradual application of light-emitting diodes (LEDs) in general lighting, backlight displays and other fields, the market has increasingly higher requirements for the luminous efficacy of white and multi-color LEDs.

[0003] In related technologies, in order to improve the luminous efficiency of light-emitting diodes (LEDs), a structure combining shallow quantum well layers with light-emitting quantum well layers is often used to improve electron utilization, thereby achieving the goal of improving the luminous efficiency of LEDs.

[0004] However, shallow quantum well structures are prone to V-shaped pit defects, which can become leakage channels and severely affect chip yield. Summary of the Invention

[0005] This disclosure provides a light-emitting diode (LED) chip and its fabrication method, which can effectively improve the luminous efficacy of LEDs. The technical solution is as follows: In a first aspect, embodiments of this disclosure provide a light-emitting diode chip, comprising: a first semiconductor layer, a composite layer, a first quantum well layer, and a second semiconductor layer stacked sequentially; The composite layer includes a first sublayer and a second sublayer stacked alternately in a periodic manner. The first sublayer is an InGaN layer and the second sublayer is a GaN layer. In the stacking direction of the composite layer, the In content of each first sublayer gradually increases or gradually decreases.

[0006] In one implementation of this disclosure, the thickness of the first sublayer is 10~50nm, and the number of periods of the composite layer is 5~30.

[0007] In one implementation of this disclosure, the light-emitting diode chip further includes a second quantum well layer; The second quantum well layer is located on the side of the composite layer opposite to the first quantum well layer, and the In composition of the second quantum well layer is smaller than that of the first quantum well layer.

[0008] Secondly, embodiments of this disclosure provide a method for fabricating a light-emitting diode chip, comprising: Fabrication of the first semiconductor layer; A composite layer is prepared by periodically alternating the preparation of a first sub-layer and a second sub-layer, wherein the first sub-layer is an InGaN layer and the second sub-layer is a GaN layer, and the preparation temperature of each second sub-layer gradually increases or decreases in the preparation direction of the composite layer. Fabrication of the first quantum well layer; Prepare the second semiconductor layer.

[0009] In one implementation of this disclosure, the preparation of the first sublayer includes: The preparation temperature of the first sublayer is 750~820℃.

[0010] In one implementation of this disclosure, the preparation of the second sublayer includes: The preparation temperature of the second sublayer is 750~920℃.

[0011] In one implementation of this disclosure, the preparation of the second sublayer includes: The preparation time for the second sublayer is 30~150s.

[0012] In one implementation of this disclosure, the composite layer is prepared by: As the preparation temperature of the second sublayer gradually increases, the highest preparation temperature of the second sublayer is lower than that of the first sublayer. As the preparation temperature of the second sublayer gradually decreases, the minimum preparation temperature of the second sublayer is greater than that of the first sublayer.

[0013] In one implementation of this disclosure, the composite layer is prepared by: The number of cycles in the composite layer is 5 to 30.

[0014] In one implementation of this disclosure, before preparing the composite layer, the following steps are included: A second quantum well layer is prepared, wherein the In content of the second quantum well layer is less than that of the first quantum well layer.

[0015] The beneficial effects of the technical solutions provided in this disclosure include at least the following: The light-emitting diode chip provided in this disclosure effectively improves the stress and interface blurring problems caused by setting shallow multi-quantum-well layers in related technologies by introducing a composite layer composed of a first sub-layer and a second sub-layer that periodically alternates between the first semiconductor layer and the first quantum well layer.

[0016] In the light-emitting diode chip provided in this embodiment, since the In composition of each first sublayer of the composite layer exhibits a gradient change that gradually increases or decreases in the stacking direction, a step-like increasing or decreasing potential energy difference structure is formed between the InGaN layer and the GaN layer. This potential energy step can effectively slow down the flow speed of electrons, increase the probability of electrons staying and being bound before entering the first quantum well layer, and greatly improve the utilization rate of electrons and the overall luminous efficiency of the device.

[0017] In other words, the composite layer not only improves the luminous efficiency of the LED chip, but also effectively avoids the problems caused by shallow quantum well layers in related technologies. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of this disclosure, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 This is a schematic diagram of the structure of the light-emitting diode chip provided in the embodiments of this disclosure; Figure 2 This is a schematic diagram of the composite layer structure provided in the embodiments of this disclosure; Figure 3 This is a flowchart illustrating a method for fabricating a light-emitting diode chip according to an embodiment of this disclosure; Figure 4 This is a flowchart of another method for fabricating a light-emitting diode chip provided in this embodiment.

[0020] The symbols in the diagram represent the following meanings: 110. First semiconductor layer; 120. First quantum well layer; 130. Second semiconductor layer; 20. Composite layer; 210, First sublayer; 220, Second sublayer; 30. Second quantum well layer; 40. Substrate; 50. Buffer layer; 60. Transition layer; 70. Stress relief layer.

[0021] The accompanying drawings have illustrated specific embodiments of this disclosure, which will be described in more detail below. These drawings and descriptions are not intended to limit the scope of the concept in any way, but rather to illustrate the concepts of this disclosure to those skilled in the art through reference to particular embodiments. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this disclosure clearer, the embodiments of this disclosure will be described in further detail below with reference to the accompanying drawings.

[0023] This disclosure provides a light-emitting diode chip. Figure 1 See the schematic diagram of the structure of this light-emitting diode chip. Figure 1 In this embodiment, the light-emitting diode chip includes a first semiconductor layer 110, a composite layer 20, a first quantum well layer 120, and a second semiconductor layer 130 stacked sequentially.

[0024] Figure 2 This is a schematic diagram of the composite layer 20, combined with... Figure 2 In this embodiment, the composite layer 20 includes a first sub-layer 210 and a second sub-layer 220 that are periodically and alternately stacked. The first sub-layer 210 is an InGaN layer and the second sub-layer 220 is a GaN layer. In the stacking direction of the composite layer 20, the In composition of each first sub-layer 210 gradually increases or gradually decreases.

[0025] The light-emitting diode chip provided in this disclosure effectively improves the stress and interface blurring problems caused by setting shallow multiple quantum well layers in related technologies by introducing a composite layer 20 composed of a first sub-layer 210 and a second sub-layer 220 periodically alternating between the first semiconductor layer 110 and the first quantum well layer 120.

[0026] In the light-emitting diode chip provided in this embodiment, since the In composition of each first sub-layer 210 of the composite layer 20 exhibits a gradient change that gradually increases or decreases in the stacking direction, a step-like increasing or decreasing potential energy difference structure is formed between the InGaN layer and the GaN layer. This potential energy step can effectively slow down the flow speed of electrons, increase the probability of electrons staying and being bound before entering the first quantum well layer 120, and greatly improve the utilization rate of electrons and the overall luminous efficiency of the device.

[0027] In other words, the composite layer 20 not only improves the luminous efficiency of the LED chip, but also effectively avoids the problems caused by shallow quantum well layers in related technologies.

[0028] In this embodiment, the second sublayer 220 is formed naturally during the preparation of the first sublayer 210 when In atoms on the surface of the underlying InGaN layer overflow during a specific pause (stop In source) step, resulting in an extremely thin GaN capping layer. A barrier layer is formed between the InGaN layer and the GaN layer, which can block electrons.

[0029] This mechanism not only forms a clear barrier difference with the first sublayer 210 of the previous layer, but also eliminates the In floating layer on the surface of the first sublayer 210 through the pause step, allowing In atoms to migrate to stable positions with lower energy, protecting the In atoms that have been incorporated into the lattice, thereby making the barrier-well interface steeper, significantly improving the interface crystal quality, and enhancing the luminescence intensity.

[0030] In this embodiment, the first sub-semiconductor layer is an N-type GaN layer, the second semiconductor layer 130 is a P-type GaN layer, and the first quantum well layer 120 is a multiple quantum well (MQW) layer, which is composed of periodically alternating InGaN layers and GaN layers.

[0031] Of course, in other embodiments, the first sub-semiconductor layer may also be a P-type GaN layer, while the second semiconductor layer 130 may be an N-type GaN layer.

[0032] In this embodiment, the thickness of the first sublayer 210 is 10~50nm, and the number of periods of the composite layer 20 is 5~30.

[0033] In the above implementation, the thickness of the first sublayer 210 is controlled between 10 and 50 nm, and the number of alternating stacking cycles is controlled between 5 and 30 cycles, so that the composite layer 20 provides a sufficient number of potential energy steps while controlling the physical thickness of the single layer within the elastic critical thickness that can effectively release internal stress.

[0034] If the thickness of the first sublayer 210 is less than 10 nm or the number of periods is less than 5, the number and width of the potential energy steps are insufficient, and they cannot significantly slow down or block the high-speed injected electrons. If the thickness is greater than 50 nm or the number of periods is greater than 30, it will lead to the accumulation of excessive lattice mismatch stress inside the InGaN material, which can easily cause cracking of the epitaxial layer or induce through dislocations, thus reducing the lattice quality.

[0035] See again Figure 1 In this embodiment, the light-emitting diode chip further includes a second quantum well layer 30. The second quantum well layer 30 is located on the side of the composite layer 20 opposite to the first quantum well layer 120, and the In composition of the second quantum well layer 30 is less than the In composition of the first quantum well layer 120.

[0036] In the above implementation, a multi-level buffered electron injection channel is constructed by setting a second quantum well layer 30 below the composite layer 20.

[0037] Since the In composition of the second quantum well layer 30 is smaller than that of the first quantum well layer 120, electrons injected from the bottom layer upwards can first pass through a pre-buffered region with a lower potential energy before entering the gradient deceleration region constructed by the composite layer 20. This avoids electrons directly encountering huge potential barrier abrupt changes, improves the longitudinal transport uniformity of charge carriers, and alleviates the lattice stress extending upwards from the bottom layer to a certain extent.

[0038] For example, the second quantum well layer 30 is composed of periodically alternating layers of InGaN and GaN layers.

[0039] See also Figure 1 In this embodiment, the light-emitting diode chip includes a substrate 40, and a buffer layer 50 and a transition layer 60 sequentially stacked on the substrate 40. The buffer layer 50 is a low-temperature GaN layer or an AlN layer, and the transition layer 60 is an unintentionally doped GaN layer.

[0040] For example, the light-emitting diode chip includes a stress relief layer 70, which is located on the side of the first semiconductor layer 110 facing the composite layer 20. The stress relief layer 70 is an InGaN / GaN superlattice structure or an InGaN layer with low In content.

[0041] Figure 3 This is a flowchart illustrating a method for fabricating a light-emitting diode chip according to an embodiment of the present disclosure, in conjunction with... Figure 3 In this embodiment, the preparation method includes: Step 301: Prepare the first semiconductor layer 110.

[0042] Step 302: Prepare composite layer 20.

[0043] In this process, the first sublayer 210 and the second sublayer 220 are prepared alternately and periodically. The first sublayer 210 is an InGaN layer and the second sublayer 220 is a GaN layer. In the preparation direction of the composite layer 20, the preparation temperature of each second sublayer 220 gradually increases or decreases.

[0044] Step 303: Prepare the first quantum well layer 120.

[0045] Step 304: Prepare the second semiconductor layer 130.

[0046] The fabrication method provided in this disclosure, by introducing a composite layer 20 composed of a first sub-layer 210 and a second sub-layer 220 alternating periodically between the first semiconductor layer 110 and the first quantum well layer 120, effectively improves the stress and interface ambiguity problems caused by setting shallow multi-quantum well layers in related technologies.

[0047] In the fabrication method provided in this embodiment, since the fabrication temperature of the second sublayer 220 exhibits a gradual increase or decrease gradient, the In composition of the first sublayer 210 also exhibits a corresponding gradual increase or decrease gradient in the stacking direction. This creates a stepped potential energy difference structure between the InGaN and GaN layers. This potential energy step effectively slows down the electron flow rate, increases the probability of electrons remaining and being bound before entering the first quantum well layer 120, and significantly improves electron utilization and the overall luminous efficiency of the device.

[0048] In other words, the composite layer 20 not only improves the luminous efficiency of the LED chip, but also effectively avoids the problems caused by shallow quantum well layers in related technologies.

[0049] Figure 4 A flowchart illustrating another method for fabricating a light-emitting diode chip provided in this disclosure, in conjunction with... Figure 4 In this embodiment, the preparation method includes: Step 401: Provide a substrate 40.

[0050] For example, the substrate 40 can be a sapphire substrate, a Si substrate, etc., and can be selected according to actual needs. This disclosure does not limit it.

[0051] Step 402: Prepare buffer layer 50.

[0052] For example, the buffer layer 50 is a low-temperature GaN layer or an AlN layer.

[0053] In the above implementation, the buffer layer 50 is prepared on the substrate 40, and its main function is to absorb the lattice mismatch caused by the heterogeneous substrate 40 and provide preliminary nucleation centers.

[0054] Step 403: Prepare transition layer 60.

[0055] For example, the transition layer 60 is an unintentionally doped GaN layer.

[0056] In the above implementation, the transition layer 60 is fabricated on top of the buffer layer 50. Its main function is to cover up the three-dimensional fabrication defects of the bottom buffer layer 50, complete the transition to a high-quality two-dimensional single crystal plane, and reduce the density of penetrating dislocations.

[0057] Step 404: Prepare the first semiconductor layer 110.

[0058] For example, the first semiconductor layer 110 is an N-type GaN layer.

[0059] In the above implementation, the first semiconductor layer 110 is fabricated on the transition layer 60, and its main function is to provide sufficient electron carriers as the electron source for subsequent light-emitting recombination.

[0060] Step 405: Prepare the stress relief layer 70.

[0061] For example, the stress relief layer 70 is an InGaN / GaN superlattice structure or an InGaN layer with low In content.

[0062] In the above implementation, the stress relief layer 70 is fabricated on the first semiconductor layer 110. Its main function is to alleviate the physical stress accumulated between the bottom layer and the multi-quantum well light-emitting region due to the difference in lattice constant.

[0063] Step 406: Prepare the second quantum well layer 30.

[0064] For example, the In composition of the second quantum well layer 30 is less than that of the first quantum well layer 120, and the second quantum well layer 30 is composed of periodically alternating InGaN layers and GaN layers.

[0065] Since the In composition of the second quantum well layer 30 is smaller than that of the first quantum well layer 120, electrons injected from the bottom layer upwards can first pass through a pre-buffered region with a lower potential energy before entering the gradient deceleration region constructed by the composite layer 20. This avoids electrons directly encountering huge potential barrier abrupt changes, improves the longitudinal transport uniformity of charge carriers, and alleviates the lattice stress extending upwards from the bottom layer to a certain extent.

[0066] Step 407: Prepare composite layer 20.

[0067] In this embodiment, the first sublayer 210 and the second sublayer 220 are prepared alternately and periodically. The first sublayer 210 is an InGaN layer and the second sublayer 220 is a GaN layer. In the preparation direction of the composite layer 20, the preparation temperature of each second sublayer 220 gradually increases or decreases.

[0068] For example, step 407 includes: Step 4071: Prepare the first sublayer 210, which is an InGaN layer.

[0069] Step 4072: Stop the In source to consume some of the In in the first sublayer 210 through high temperature, thereby forming a thinner GaN layer, which is the second sublayer.

[0070] In other words, the preparation of the second sublayer 220 can be regarded as an intermittent insertion of a preparation stage to stop the In source during the preparation of the first sublayer 210, so that the In atoms are quantitatively overflowed through a set temperature gradient, forming a step-like potential barrier difference (increasing or decreasing) with the previous InGaN layer.

[0071] Periodic cyclic steps 4071 and 4072 are performed to obtain a periodically stacked first sublayer 210 and second sublayer 220.

[0072] In this embodiment, the number of cycles of the composite layer 20 is 5 to 30.

[0073] In the above implementation, if the number of cycles is less than 5, the overall stress release thickness is thin and a multi-level buffer barrier cannot be formed. If the number of cycles is greater than 30, the total deposition thickness is too large, making it easy for the wafer to accumulate a large amount of deformation potential energy due to the difference in thermal expansion coefficients during epitaxial cooling, increasing the risk of process scrap.

[0074] During the preparation of each first sublayer 210, the output In source and its various process parameters are the same, so theoretically the In content of each first sublayer 210 should be the same. However, in reality, there may be some differences. After step 4072, the In content of each first sublayer 210 changes differently. The differences in In content are mainly reflected in the following aspects: Firstly, the first sublayer 210 prepared earlier undergoes more steps of step 4072, resulting in a greater amount of In atoms overflowing. For example, if the composite layer 20 has 5 cycles, the first sublayer 210 prepared earlier will undergo 5 steps of step 4072, while the fifth sublayer 210 prepared later will only undergo 1 step of step 4072.

[0075] Secondly, the higher the preparation temperature of the second sublayer 220 in step 4072, the more In atoms will escape. This is because the In-N bond is relatively weak and easily broken at high temperatures. Therefore, the higher the preparation temperature of the second sublayer 220, the faster the decomposition rate of InGaN.

[0076] In this embodiment, as the preparation temperature of the second sublayer 220 gradually increases, the highest preparation temperature of the second sublayer 220 is lower than the preparation temperature of the first sublayer 210.

[0077] As the preparation temperature of the second sublayer 220 gradually decreases, the minimum preparation temperature of the second sublayer 220 is greater than the preparation temperature of the first sublayer 210.

[0078] In the above implementation, by ensuring that the highest or lowest temperature always maintains a certain symmetrical relationship with the preparation temperature of the first sublayer 210, the entire temperature control process is kept within a controllable and safe range. This avoids excessive temperature fluctuations or abrupt changes in In composition caused by directional reversal, thus guaranteeing the absolute continuity and smoothness of the constructed step-like increasing or decreasing potential energy difference.

[0079] For example, the preparation temperature of the first sublayer 210 is 750~820°C.

[0080] In the above implementation, the preparation temperature of the first sublayer 210 is controlled within the range of 750~820℃, so that In atoms in the gas phase can be stably incorporated into the gallium nitride lattice.

[0081] If the temperature is below 750℃, the pyrolysis efficiency of the precursor gas (such as trimethylgallium, ammonia, etc.) is low, resulting in insufficient surface atomic mobility and poor crystal quality and rough surface of the grown film. If the temperature is above 820℃, the pyrolysis adsorption rate of In atoms increases sharply, making it difficult for indium to be effectively incorporated into the lattice and preventing the formation of the InGaN layer required by the design.

[0082] For example, the preparation temperature of the second sublayer 220 is 750~920°C.

[0083] In the above implementation, the preparation temperature of the second sublayer 220 is controlled within a wide range of 750~920℃, so that this temperature range can fully cover and drive the appropriate overflow and evaporation of In atoms on the bottom surface.

[0084] If the temperature is below 750℃, the heat is insufficient to drive the free In atoms on the surface to escape, making it impossible to form a pure GaN capping layer, resulting in a blurred barrier interface. If the temperature is above 920℃, the excessive thermal shock will not only cause severe thermal degradation and decomposition of the underlying solidified InGaN layer, but will also cause stress imbalance in the epitaxial structure.

[0085] For example, the difference between the preparation temperatures of each second sublayer 220 is 5~10°C, and the difference in preparation temperatures is a constant value.

[0086] For example, the preparation time of the second sublayer 220 is 30~150s.

[0087] In the above implementation, the preparation time of the second sublayer 220 is also the time during which the In source is paused. This time is controlled between 30 and 150 seconds, allowing sufficient time for atomic rearrangement and surface layer removal on the InGaN material surface.

[0088] If the time is less than 30 seconds, the atomic surface migration and recombination process is insufficient, and the interface steepness cannot be effectively improved. If the time is more than 150 seconds, the excessively long pause in high-temperature baking will cause abnormal diffusion and aggregation of In atoms, which will not only increase the process time, but also cause irreversible damage to the overall photoelectric performance of the LED chip.

[0089] Step 408: Prepare the first quantum well layer 120.

[0090] For example, the first quantum well layer 120 is composed of periodically alternating layers of InGaN and GaN layers.

[0091] In the above implementation, a set potential energy difference is used to tightly bind a large number of electrons that have undergone "delayed" treatment inside the trap layer, thereby completing high-efficiency photoelectric recombination.

[0092] Step 409: Prepare the second semiconductor layer 130.

[0093] For example, the second semiconductor layer 130 is a P-type GaN layer.

[0094] In the above implementation, the second semiconductor layer 130 is fabricated on the first quantum well layer 120, and its main function is to provide hole carriers to the light-emitting region for combination with electrons.

[0095] Unless otherwise defined, the technical or scientific terms used herein shall have the ordinary meaning understood by one of ordinary skill in the art to which this disclosure pertains. The terms “first,” “second,” “third,” and similar terms used in this patent application specification and claims do not indicate any order, quantity, or importance, but are merely used to distinguish different components. Similarly, the terms “an” or “a” and similar terms do not indicate a quantity limitation, but rather indicate the presence of at least one. The terms “comprising” or “including” and similar terms mean that the elements or objects preceding “comprising” or “including” encompass the elements or objects listed following “comprising” or “including” and their equivalents, and do not exclude other elements or objects. The terms “connected” or “linked” and similar terms are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. The terms “upper,” “lower,” “left,” “right,” etc., are used only to indicate relative positional relationships; when the absolute position of the described objects changes, the relative positional relationship may also change accordingly.

[0096] The above description is merely an optional embodiment of this disclosure and is not intended to limit this disclosure. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the protection scope of this disclosure.

Claims

1. A light-emitting diode chip, characterized in that, include: A first semiconductor layer (110), a composite layer (20), a first quantum well layer (120), and a second semiconductor layer (130) are stacked sequentially. The composite layer (20) includes a first sub-layer (210) and a second sub-layer (220) stacked periodically and alternately. The first sub-layer (210) is an InGaN layer, and the second sub-layer (220) is a GaN layer. In the stacking direction of the composite layer (20), the In composition of each first sub-layer (210) gradually increases or gradually decreases.

2. The light-emitting diode chip according to claim 1, characterized in that, The thickness of the first sublayer (210) is 10~50nm, and the number of periods of the composite layer (20) is 5~30.

3. The light-emitting diode chip according to claim 1 or 2, characterized in that, The light-emitting diode chip also includes a second quantum well layer (30). The second quantum well layer (30) is located on the side of the composite layer (20) facing away from the first quantum well layer (120), and the In composition of the second quantum well layer (30) is smaller than that of the first quantum well layer (120).

4. A method for fabricating a light-emitting diode chip, characterized in that, include: Fabricate the first semiconductor layer (110); A composite layer (20) is prepared, wherein a first sublayer (210) and a second sublayer (220) are prepared alternately and periodically. The first sublayer (210) is an InGaN layer, and the second sublayer (220) is a GaN layer. In the preparation direction of the composite layer (20), the preparation temperature of each second sublayer (220) gradually increases or gradually decreases. Fabricate the first quantum well layer (120); Prepare a second semiconductor layer (130).

5. The preparation method according to claim 4, characterized in that, The preparation of the first sublayer (210) includes: The preparation temperature of the first sublayer (210) is 750~820℃.

6. The preparation method according to claim 4, characterized in that, The preparation of the second sublayer (220) includes: The preparation temperature of the second sublayer (220) is 750~920℃.

7. The preparation method according to claim 4, characterized in that, The preparation of the second sublayer (220) includes: The preparation time of the second sublayer (220) is 30~150s.

8. The preparation method according to claim 4, characterized in that, The preparation of the composite layer (20) includes: As the preparation temperature of the second sublayer (220) gradually increases, the highest preparation temperature of the second sublayer (220) is lower than the preparation temperature of the first sublayer (210); As the preparation temperature of the second sublayer (220) gradually decreases, the minimum preparation temperature of the second sublayer (220) is greater than that of the first sublayer (210).

9. The preparation method according to claim 4, characterized in that, The preparation of the composite layer (20) includes: The composite layer (20) has 5 to 30 cycles.

10. The preparation method according to claim 4, characterized in that, Before preparing the composite layer (20), the following steps are included: A second quantum well layer (30) is prepared, wherein the In composition of the second quantum well layer (30) is less than that of the first quantum well layer (120).