Method for manufacturing optical products with encapsulated microstructures

By using an injection molding process combining imidized acrylic polymers and high-refractive-index materials, the problem of microstructure deformation was solved, resulting in a double-layer composite lens that is aesthetically pleasing and effectively controls myopia.

CN123125101APending Publication Date: 2026-11-17ESSILOR INTERNATIONAL(COMPAGNIE GENERALE D OPTIQUE)
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202580027682.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-20
Filing Date
2025-06-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to maintain the shape integrity and optical design of microstructures while simultaneously meeting aesthetic requirements and myopia control effects when manufacturing optical products with encapsulated microstructures, especially when using high-refractive-index materials as lens layers, as the microstructures are prone to deformation.

Method used

An imidized acrylic polymer is used as the cover layer material, combined with a high-refractive-index transparent thermoplastic material as the support layer. A double-layer composite lens is formed through injection molding. This ensures that the glass transition temperature of the cover layer is higher than that of the support layer. Microstructure deformation is avoided by controlling injection parameters such as melt temperature, viscosity and pressure.

Benefits of technology

It achieves the goal of maintaining the shape integrity and optical design of the microstructure while reducing the overall thickness, effectively controlling myopia development, and is suitable for various microstructure arrangements and smooth outer surfaces, while being compatible with existing transition transfer bonding processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125101A_ABST
    Figure CN123125101A_ABST
Patent Text Reader

Abstract

A method for manufacturing an optical article (64) having an encapsulated microstructure, the method comprising the steps of: - forming a capping layer (56) having a microstructure (58) on a concave surface, the capping layer (56) comprising a first transparent thermoplastic material (52); - depositing a second transparent thermoplastic material (60) on the microstructured surface, the second transparent thermoplastic material having a refractive index (RI) 镜片 The refractive index (RI) is higher than that of the first transparent thermoplastic material (52). 晶片 And the glass transition temperature (Tg) 镜片 The glass transition temperature (Tg) of the first transparent thermoplastic material (52) is equal to or lower than that of the corresponding glass transition temperature. 晶片 Thus, a support layer (62) for the encapsulated microstructure (58) is obtained, which together with the cover layer (56) forms the optical article (64) with the encapsulated microstructure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing optical articles with encapsulated microstructures, such as ophthalmic lenses, and particularly for myopia control. Background Technology

[0002] Ophthalmic lenses with microstructures (typically microlenses) have been shown to effectively slow the progression of myopia in children and adolescents. These microstructures are placed on the anterior surface to provide peripheral defocus for light incident on the retina of an individual eye. However, the presence of these microstructures on the lens surface presents significant challenges to the overall manufacturing of the lens.

[0003] The term "lens" will be used in the following description, but other known optical products with encapsulated microstructures on the surface, such as wafers or thin films, may also be considered.

[0004] Injection molding methods for manufacturing lenses with microstructures are known. These methods typically involve injecting a first optical thermoplastic material into a mold to obtain an optical thermoplastic wafer layer (TP) of uniform thickness and microstructures on its surface. 晶片 (Also known as a cover layer).

[0005] TP wafer layer with microstructure 晶片 It can be produced by injection molding, roll-to-roll hot stamping, or other means.

[0006] Then through the wafer layer TP 晶片 Different second optical thermoplastic materials are injected onto the microstructured surface to encapsulate the microstructure, thereby obtaining the lens layer TP that forms the lens body. 镜片 (Also known as the main layer).

[0007] The resulting final lens is a double-layer composite lens, which has a TP layer encapsulated in the wafer layer. 晶片 With lens layer TP 镜片 Microstructures at the interface between them.

[0008] like Figure 1 (As shown in the cross-sectional view depicting a lens 2 with microstructure 4), when a hard coating 6 is deposited on lens 2 to protect it from scratches and other damage, the geometry of lens 2 is altered. This shape change causes a shift in the optical design of lens 2. Typically, several additional design steps in the coating process are required to compensate for this problem, and this is a time-consuming and expensive process. Furthermore, these design compensation steps must be repeated for each different coating applied to lens 2.

[0009] Methods including lamination, overmolding, and injection molding are known to encapsulate the microstructure 4 within the lens body to eliminate dependence on coatings while providing protection for the microstructure 4.

[0010] Figure 2 The wafer layer TP disclosed above is shown. 晶片 The steps of the injection encapsulation process for microstructure 4 on the surface.

[0011] exist Figure 2 The image shows a top view of the open die 8, in which the wafer layer TP is inserted. 晶片 (exist Figure 2 The wafer is marked as 10, such as a PC (polycarbonate) wafer with microstructures 4 on its concave surface. Then, the mold 8 is closed, and the wafer layer TP is... 晶片 An open space 12 is left between 10 and mold 8. A hot melt of a second optical thermoplastic material, such as PMMA (polymethyl methacrylate), is injected into the open space 12 through filler 14, thereby creating the lens layer TP. 镜片 (exist Figure 2 (Marked as 16 in the middle). Finally, mold 8 is opened, thus allowing the final lens 18 (made of wafer layer TP) to be obtained. 晶片 10 and lens layer TP 镜片 (A double layer consisting of 16).

[0012] As detailed above, the injection molding process involves injecting a hot-melt second optical thermoplastic material into the wafer layer TP. 晶片 On a relatively cold, microstructured surface.

[0013] Chip layer TP 晶片 The microstructure 4 softens and deforms under the high heat and pressure of the overmolding process. This leads to the loss of shape integrity of the microstructure 4 and the deterioration of its optical design, resulting in poorer control over myopia progression.

[0014] Furthermore, careful selection of the first and second optical thermoplastic materials is required to form a clear interface for good optical fidelity and lens sharpness, and to achieve a robust bond. The resulting final lens 18 should theoretically pass through subsequent known Rx processing steps without problems; therefore, material selection is particularly challenging. A very specific property relationship is required between the two different thermoplastic materials.

[0015] Figure 3 Cross-sectional views of two different types of final lenses 18 are shown: a first final lens 18a with a convex microstructure 4 and a second final lens 18b with a concave microstructure 4. The encapsulated microstructure 4 must have a predetermined optical power to facilitate peripheral defocusing. To achieve the appropriate optical power, a wafer layer TP is required. 晶片 The refractive index RI of the wafer layer 晶片 Unlike the TP lens layer 镜片The refractive index RI of the lens layer 镜片 That is, the two refractive indices RI 晶片 and RI 镜片 The difference ΔRI must be different from zero.

[0016] For myopia control, the microlens power of the final lens 18 must be positive to provide peripheral defocus that slows myopia progression. When ΔRI is greater than zero (i.e., RI...), 晶片 Greater than RI 镜片 When ), the wafer layer TP 晶片 The microstructure 4 on the lens must be convex to have positive focal power (first final lens 18a). When ΔRI is less than 0 (i.e., RI... 晶片 Less than RI 镜片 When ), the wafer layer TP 晶片 The microstructure 4 on it must be concave to have positive focal length (second final lens 18b).

[0017] To maintain the shape integrity of microstructure 4, the wafer layer TP 晶片 The heat resistance must be greater than that of the lens layer TP. 镜片 The heat resistance of the wafer layer is crucial to withstand the high heat and pressure of injection molding. For thermoplastic materials, heat resistance can be characterized by the glass transition temperature (Tg): a higher Tg corresponds to better heat resistance. Therefore, the wafer layer TP... 晶片 glass transition temperature Tg 晶片 It must be higher than the lens layer TP 镜片 glass transition temperature Tg 镜片 In order to prevent the microstructure 4 from deforming.

[0018] Generally, high-refractive-index amorphous thermoplastics inherently possess good heat resistance due to their chemical structure. Therefore, a high glass transition temperature (Tg) corresponds to a high refractive index (RI).

[0019] Since the main body of the final lens 18 is composed of lens layer TP 镜片 Formed thus reducing the overall thickness of the final lens 18 to make it aesthetically pleasing and appealing to consumers, preferably, the lens layer TP 镜片 The second optical thermoplastic material is the lens layer refractive index RI 镜片 Above the wafer layer TP 晶片 The refractive index RI of the wafer layer 晶片 High refractive index materials. In this case, the wafer layer TP 晶片 The first optical thermoplastic material will be a low refractive index material.

[0020] However, as explained above, this would imply the lens layer TP. 镜片 The glass transition temperature Tg of the second optical thermoplastic material 镜片It is also higher than the chip layer TP. 晶片 The glass transition temperature of the first optical thermoplastic material.

[0021] On the other hand, in order to maintain the wafer layer TP during subsequent injection molding of the second optical thermoplastic material 晶片 The shape integrity of the microstructure 4, the wafer layer TP 晶片 The heat resistance of the first optical thermoplastic material must be greater than that of the second optical thermoplastic material that is injected to encapsulate the microstructure 4.

[0022] Therefore, high refractive index materials are used as the lens layer TP. 镜片 The second optical thermoplastic material (which will preferably reduce the total thickness of the final lens 18) will not work because of the wafer layer TP 晶片 The microstructure 4 generated on the low refractive index material will be severely deformed.

[0023] Existing technologies do not provide a working solution for constructing composite lenses with encapsulated microstructures, where the lens layer TP... 镜片 The refractive index RI of the lens layer 镜片 Above the wafer layer TP 晶片 The refractive index RI of the wafer layer 晶片 It is made of a second optical thermoplastic material, and the microstructure 4 therein does not deform.

[0024] In fact, there is no such thermoplastic material pair in which the wafer layer TP 晶片 The glass transition temperature (Tg) of the first optical thermoplastic material 晶片 Above the lens layer TP 镜片 The glass transition temperature of the second optical thermoplastic material, and simultaneously, the refractive index RI 晶片 The refractive index RI of the second optical thermoplastic material is lower than that of the second optical thermoplastic material. 镜片 These materials are further compatible with each other to construct double-layer composite lenses.

[0025] Therefore, there is a need for an innovative method for manufacturing optical articles with encapsulated microstructures that have a reduced overall thickness to be aesthetically pleasing and attractive to consumers, while maintaining the shape integrity of the contained microstructures and optical design to better control the development of myopia in individuals, thereby overcoming the problems of the prior art. Summary of the Invention

[0026] This article provides a method for manufacturing optical articles with encapsulated microstructures, the method comprising the following steps:

[0027] - A cover layer with a microstructure is provided on a concave surface, the cover layer comprising a first transparent thermoplastic material;

[0028] - A second transparent thermoplastic material with a refractive index RI is deposited on the microstructured surface. 镜片 The refractive index RI is higher than that of the first transparent thermoplastic material. 晶片 And the glass transition temperature Tg 镜片 The glass transition temperature (Tg) of the first transparent thermoplastic material is equal to or lower than the corresponding glass transition temperature (Tg) of the first transparent thermoplastic material. 晶片 This results in a support layer for the encapsulated microstructure, which together with the cover layer forms the optical article with the encapsulated microstructure.

[0029] In this embodiment, the microstructure is concave.

[0030] In one embodiment, depositing the second transparent thermoplastic material includes injection overmolding.

[0031] In the embodiments, the first transparent thermoplastic material is an imidized acrylic polymer, which comprises imide units having the following structural formula:

[0032]

[0033] R1, R2 and R3 independently include hydrogen or unsubstituted or substituted C1 to C20 alkyl, aryl, or aralkyl, alkylaryl, or mixtures thereof.

[0034] In the embodiments, the imidized acrylic polymer comprises the following chain structure:

[0035]

[0036] In the embodiments, the imidized acrylic polymer comprises both an ester group -OC(=O)- and an amide group -C(=O)-N=.

[0037] In the embodiments, the second transparent thermoplastic material includes polycarbonate, aromatic thermoplastic polyurethane, aromatic polyamide, polysulfone, polyphenylsulfone, polyetherimide, copolyester, copolymer thereof, or derivatives or mixtures thereof.

[0038] In the embodiments, the thickness of the microstructured capping layer is between 0.25 mm and 2.0 mm, and preferably between 0.4 mm and 1.5 mm.

[0039] In this embodiment, the thickness of the support layer is in the range of 0.25 mm to 15 mm or more.

[0040] This article also provides an optical article with a packaged microstructure, which includes finished lenses, semi-finished lenses, wafers or thin films.

[0041] The aforementioned optical products with encapsulated microstructures can be designed to control myopia in individuals. Attached Figure Description

[0042] Further features and advantages of the invention will become apparent from the following description, provided only by way of non-limiting example and with reference to the accompanying drawings, in which:

[0043] Figure 1 A cross-sectional view of a lens with microstructure is depicted;

[0044] Figure 2 The steps of an injection overmolding process for encapsulating microstructures on the surface of a wafer layer are shown.

[0045] Figure 3 Cross-sectional views of two different types of final lenses are shown;

[0046] Figure 4 The steps of a method for manufacturing an optical article having an encapsulated microstructure according to an example of the present invention are shown;

[0047] Figure 5 This is a top view image of the overlay layer according to a first embodiment of the present invention;

[0048] Figure 6 This is a top view of an optical article with an encapsulated microstructure according to a first embodiment of the present invention;

[0049] Figure 7 This is a bottom view of the overlay layer according to a second embodiment of the present invention; and

[0050] Figure 8 This is a top view of an optical article with an encapsulated microstructure according to a second embodiment of the present invention. Detailed Implementation

[0051] In the following description, the drawings are not necessarily drawn to scale, and some features may be shown in a generalized or schematic form for clarity and brevity or for informational purposes. The embodiments discussed herein are merely illustrative and do not limit the scope of the invention. It will also be apparent to those skilled in the art that all technical features defined relative to the method can be transposed individually or in combination to the apparatus, and conversely, all technical features relative to the apparatus can be transposed individually or in combination to the method. To avoid unnecessary details for practicing the invention, certain information known to those skilled in the art may be omitted from this specification.

[0052] The method for manufacturing optical articles with encapsulated microstructures according to the present invention is based on utilizing a novel set of polymers having high glass transition temperatures (Tg) and low refractive indices (RI) to serve as a capping layer (corresponding to the wafer layer TP disclosed above). 晶片 ).

[0053] The thermoplastic polymer according to the present invention contains an imide unit having the following structural formula (I):

[0054] (I)

[0055] R1, R2 and R3 independently include hydrogen or unsubstituted or substituted C1 to C20 alkyl, aryl, or aralkyl, alkylaryl, or mixtures thereof.

[0056] Thermoplastic polymers containing imide units with the above structural formula can be obtained by imidizing acrylic polymers using fully disclosed methods (such as those disclosed in US 2,146,209, DE 1,077,872, DE 1,242,369, and US 3,284,425). Imidized acrylic polymers possess the optical properties of acrylic acid and the high heat resistance of polyimide.

[0057] Depending on the degree of imidization, the refractive index RI of the thermoplastic polymer can range from 1.50 to 1.55 or higher, and the glass transition temperature Tg is much higher than 150°C, making it suitable for producing optical articles with encapsulated microstructures for use. Figure 2 The injection molding process shown encapsulates the lens layer using a high-refractive-index substrate material.

[0058] Examples of commercially available thermoplastic polymers containing imide units of structural formula (I) include Roehm America ACRYMID® TT50 (RI = 1.53 and Tg = 151°C) and TT70 (RI = 1.54 and Tg = 175°C), which are highly heat-deformable poly(n-methylmethacrylimide) (PMMI) containing the following chain structural formula (II):

[0059] (II)

[0060] Imidinated acrylic polymers contain both ester groups -OC(=O)- and amide groups -C(=O)-N=, thus they are compatible with a variety of high refractive index thermoplastics, including polycarbonate, aromatic thermoplastic polyurethane, and aromatic polyamide.

[0061] Figure 4The steps of a method for manufacturing an optical article having an encapsulated microstructure according to an example of the present invention are shown.

[0062] In the first step 100, a mold 50 is provided, comprising a shaped portion 50a having a microstructured surface and a smooth portion 50b having a smooth surface. In the next step 102, a first transparent thermoplastic material 52, preferably an imidized acrylic polymer as disclosed above, such as ACRYMID® TT50 or TT70, is injected into the mold 50 through a filler 54. In the next step 104, the mold 50 is opened, and a cover layer 56 having microstructures 58 on a concave surface (corresponding to the wafer layer TP disclosed above) is obtained. 晶片 10). Advantageously, the microstructure 58 is concave. The microstructure 58 is generated in a manner known per se.

[0063] Injection molding of imidized acrylic polymers is very challenging because the materials are not very thermally stable in the molten state. Therefore, it is necessary to minimize the residence time and melt temperature of such materials inside the filler 54 to avoid degradation that could lead to foaming problems.

[0064] Advantageously, the cycle time is less than or equal to 120 seconds. More preferably, the cycle time is less than or equal to 75 seconds, and even more preferably, the cycle time is less than or equal to 50 seconds. The cycle time is the time required to complete both steps 102 and 104 and to prepare for repeating the same operation again.

[0065] The melting temperature of the imidized acrylic polymer 52 is preferably less than or equal to 550°F, more preferably less than or equal to 530°F, and even more preferably less than or equal to 515°F.

[0066] Considering the desired final thickness of the resulting optical article (preferably a lens, preferably for myopia control), the thickness of the microstructured cover layer 56 should be between 0.25 mm and 2.0 mm, and preferably between 0.4 mm and 1.5 mm.

[0067] Advantageously, optical products can be used for applications other than myopia control.

[0068] In a further step 106, the microstructured cover layer 56 is reinserted into the mold 50, which was closed in step 108, and then in step 110, a second transparent thermoplastic material 60, preferably a high-refractive-index thermoplastic material, is overmolded and injected onto the concave surface of the microstructured cover layer 56 through a filler 54 to form a support layer 62 (corresponding to the lens layer TP disclosed above). 镜片 16).

[0069] Thermoplastic material 60 includes polycarbonate (PC), aromatic thermoplastic polyurethane, aromatic polyamide, polysulfone, polyphenylsulfone, polyetherimide, copolymers thereof, or derivatives or mixtures thereof.

[0070] The refractive index RI of imidized acrylic polymer 52 晶片 The refractive index RI is lower than that of high refractive index thermoplastics 60. 镜片 The glass temperature Tg of imidized acrylic polymer 52 晶片 The glass temperature Tg is 60°C higher than that of high refractive index thermoplastics. 镜片 (Tg) 镜片 Equal to or lower than Tg 晶片 ).

[0071] Special care is required when injection molding the high-refractive-index thermoplastic material 60 onto the imidized acrylic polymer coating 56, as the imidized acrylic polymer coating is relatively brittle and deforms and / or cracks under high shear and high pressure.

[0072] The viscosity of the high-refractive-index thermoplastic material 60 must be limited during injection to avoid the aforementioned problems. Viscosity can be reduced by increasing the melt temperature; however, this will cause deformation of the microstructure 58 around the gate region of the mold 50 due to the high heat. The gate region (which is known in itself) is the entry point for the molten material into the mold 50. Viscosity is directly related to the molecular weight of the high-refractive-index thermoplastic material 60: lower molecular weight is associated with lower viscosity.

[0073] In the embodiments, a high refractive index thermoplastic material 60 with a weight-average molecular weight (Mw) of no more than 40,000 and preferably no more than 30,000 is used.

[0074] For practical purposes, the thickness of the support layer 62 is in the range of 0.25 mm to 15 mm or more.

[0075] In the final step 112, the mold 50 is opened, and a double-layer composite optical product 64 with encapsulated microstructure 58 for myopia control is obtained.

[0076] The optical product 64 with the encapsulated microstructure can be a lens, a finished lens or a semi-finished (SF) lens, a wafer or a thin film.

[0077] In a first embodiment according to the invention, a planar PMMI wafer with a diameter of 76 mm and a center thickness of 1.1 mm is produced in a known manner in a first step using a Fanucα-S110i injection molding machine with a Roehm America ACRYMID® TT70 imidized acrylic polymer having a refractive index of 1.54 and a glass transition temperature Tg of about 175°C. The wafer has a concave bifocal microstructure 58 on a concave surface.

[0078] The injection molding parameters have been set as follows: melt temperature 265°C, mold temperature 125°C, injection speed 100mm / s, holding pressure 9000 psi, and cooling time 20 seconds.

[0079] Bifocal microlens 58 Figure 5 The figure shows a continuous configuration arrangement, and is a top view of the cover layer 56 of the first example.

[0080] In the second step, the microlens 58 obtained in the first step is encapsulated in a known manner using Sabic Lexan® OQ1022 polycarbonate resin with a refractive index of 1.586, a glass transition temperature Tg of about 145°C and a molecular weight of about 17,000 using a Krauss Maffei KM150 injection molding machine, thereby obtaining a PMMI / PC lens 64, particularly a semi-finished (SF) lens.

[0081] The melt temperature and mold temperature for the injection overmolding process were set to 245°C and 120°C, respectively. The injection speed was 7 mm / s, and the holding pressure was 1,160 psi.

[0082] The resulting PMMI / PC lens 64 (optical product with encapsulated microstructure) has a thickness of 10.0 mm, of which the PC layer is 8.9 mm.

[0083] The microstructure 58 of the package was characterized using a known imaging device, and Figure 6 A top view of the PMMI / PC lens 64 of the first example is shown, which has very well-defined boundaries between the microstructures 58, indicating that the shape integrity of the microlens is preserved. Furthermore, the PMMI / PC lens 64 undergoes Rx surface treatment and edge grinding without causing layer separation, indicating a strong bond between the PMMI capping layer 56 and the PC support layer 62.

[0084] In a second embodiment according to the invention, a planar PMMA wafer with a diameter of 76 mm and a center thickness of 1.1 mm was produced using a Roehm America ACRYLITE® hw55 PMMA copolymer having a refractive index of 1.510 and a glass transition temperature Tg of approximately 120°C using a Nissei FN4000 injection molding machine. This wafer has concave microlenses 58 on its concave surface. The melt temperature and mold temperature for the injection process were set to 480°F and 245°F, respectively. The injection speed was 45%, and the holding pressure was 48%. The microlenses 58 were arranged as follows: Figure 7 The concentric ring configuration shown in the figure is a bottom view of the overlay layer 56 of the second example.

[0085] In the second step, the microlens 58 obtained in the first step is encapsulated in a known manner using Lexan® OQ3820 PC (bisphenol A polycarbonate) with a refractive index of 1.586 and a glass transition temperature Tg of about 147°C using a Nissei FN4000 injection molding machine, thereby obtaining a PMMA / PC lens 64.

[0086] The melt temperature and mold temperature for the injection overmolding process were set to 270°C and 110°C, respectively.

[0087] like Figure 8 As shown, this figure is a top view of the PMMA / PC lens 64 of the second example. Unlike the PMMA / PC lens 64 of the first example, the image of the lens shows a very blurred boundary between the microlens 58 and the substrate lens. This indicates that the microlens 58 has been deformed and interdiffusion has occurred at the PMMA / PC interface, because the heat resistance of hw55 PMMA is insufficient to withstand the high heat and pressure of PC overmolding to maintain the integrity of the microlens 58. However, the PMMA / PC lens 64 does not delaminate after the Rx surface treatment / edge grinding process, indicating a strong bond between PMMA and PC due to the similar ester groups in their repeating chemical structural units.

[0088] Some advantages of the present invention include:

[0089] - Obtain a high-refractive-index composite optical product 64 with an encapsulated microstructure, particularly for myopia control;

[0090] - This solution is suitable for encapsulating various microstructures in different arrangements (such as concentric rings or adjacent hexagonal arrays), including single-focus microlenses and double-focus microlenses, π-Fresnel microstructures, diffractive micropillars, etc.

[0091] - This method is compatible with existing transition bonding processes because the microstructure 58 is encapsulated and the outer surface of the optical article 64 is smooth.

[0092] Obviously, the principles of the present invention remain the same, and the embodiments and details of production may vary significantly from those described and shown by way of non-limiting example only, without departing from the scope of protection of the present invention as defined in the appended claims.

Claims

1. A method for manufacturing an optical article (64) having an encapsulated microstructure, the method comprising the following steps: - A cover layer (56) having a microstructure (58) is provided on a concave surface, the cover layer (56) comprising a first transparent thermoplastic material (52); - A second transparent thermoplastic material (60) is deposited on the microstructured surface, the refractive index (RI) of the second transparent thermoplastic material is... 镜片 The refractive index (RI) is higher than that of the first transparent thermoplastic material (52). 晶片 And the glass transition temperature (Tg) 镜片 The glass transition temperature (Tg) of the first transparent thermoplastic material (52) is equal to or lower than that of the corresponding glass transition temperature. 晶片 Thus, a support layer (62) is obtained to encapsulate the microstructure (58), and the support layer (62) together with the cover layer (56) forms the optical article (64) with the encapsulated microstructure.

2. The method as described in claim 1, wherein, The microstructure (58) is concave.

3. The method as described in claim 1, wherein, Depositing a second transparent thermoplastic material (60) includes injection overmolding.

4. The method as described in any of the preceding claims, wherein, The first transparent thermoplastic material (52) is an imidized acrylic polymer, which contains imide units having the following structural formula: R1, R2 and R3 independently include hydrogen or unsubstituted or substituted C1 to C20 alkyl, aryl, or aralkyl, alkylaryl, or mixtures thereof.

5. The method of claim 4, wherein, The imidized acrylic polymer comprises the following chain structure.

6. The method as described in claims 4 and 5, wherein, The imidized acrylic polymer contains both ester groups -OC(=O)- and amide groups -C(=O)-N=.

7. The method as described in any of the preceding claims, wherein, The second transparent thermoplastic material (60) includes polycarbonate, aromatic thermoplastic polyurethane, aromatic polyamide, polysulfone, polyphenylsulfone, polyetherimide, copolyester, copolymer thereof, or derivatives or mixtures thereof.

8. The method as described in any of the preceding claims, wherein, The thickness of the microstructured capping layer (56) is between 0.25 mm and 2.0 mm, and preferably between 0.4 mm and 1.5 mm.

9. The method as described in any of the preceding claims, wherein, The thickness of the support layer (62) is in the range of 0.25 mm to 15 mm or more.

10. An optical article having an encapsulated microstructure, manufactured according to any one of claims 1 to 9 for manufacturing an optical article having an encapsulated microstructure.

11. The optical article with an encapsulated microstructure as described in claim 10, wherein, The optical product with encapsulated microstructure includes at least one of finished lens, semi-finished lens, wafer or film.

12. The optical article with encapsulated microstructure as claimed in claim 11, which is designed for controlling myopia in an individual.

Citation Information

Patent Citations

  • Process for preparing nitrogen-containing derivatives of polymethacrylic acid

    DE1077872A

  • Process for preparing N-alkylated polymethacrylic acid imides

    DE1242369A

  • Preparation of resinous imides of substituted acrylic acids

    US2146209A

  • Conversion of polymethacrylate to polymethacrylimide in an aqueous system

    US3284425A