Integrated preparation device for rare earth magnesium intermediate alloy

Through an integrated device that integrates molten salt electrolysis, multi-stage purification, and component modulation, the problems of uneven composition and high impurity content in the preparation of rare earth magnesium master alloys are solved, and the continuous production of high-quality rare earth magnesium master alloys is achieved to meet the high performance requirements. Demand for rare earth magnesium alloys.

CN221822355UActive Publication Date: 2024-10-11NANCHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202322880727.0
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2024-10-11
Estimated Expiration
2033-10-26

AI Technical Summary

Technical Problem

It is difficult to prepare rare earth magnesium master alloys with uniform composition and low impurity content using existing technology. Moreover, traditional methods have shortcomings such as high energy consumption, high cost, and segregation problems, and cannot meet the demand for high-performance rare earth magnesium alloys.

Method used

An integrated device integrating molten salt electrolysis, multi-stage purification and component modulation is used to realize the continuous production of rare earth magnesium master alloy through the combination of molten salt electrolysis chamber, multi-stage purification chamber and component modulation chamber. The raw materials are dissolved in high-temperature molten salts, followed by multi-stage purification and ingredient modulation to improve purity and uniformity.

Benefits of technology

It achieves high-quality continuous production of rare earth magnesium master alloys with uniform composition, low impurity content, simple operation, and short preparation process. It is suitable for large-scale continuous production and meets the raw material demand for high-performance rare earth magnesium alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221822355U_ABST
    Figure CN221822355U_ABST
Patent Text Reader

Abstract

The utility model discloses an integrated preparation device for a rare earth magnesium intermediate alloy. The device is an intermediate alloy preparation furnace body which integrates a fused salt electrolysis chamber, a first-stage purification chamber, a second-stage purification chamber, a third-stage purification chamber, a component modulation chamber and a pouring chamber, the six cabins are arranged in a step shape from top to bottom and are communicated with one another through pipelines, and the first five cabins are respectively provided with a heating element. The intermediate alloy prepared through molten salt electrolysis is subjected to multi-stage purification and then subjected to component modulation treatment, and finally, a high-quality rare earth magnesium intermediate alloy ingot is obtained through pouring. The device is suitable for short-process preparation of the rare earth magnesium intermediate alloy, and the high-quality rare earth magnesium intermediate alloy can be efficiently produced on a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the field of rare earth alloy production equipment, in particular to a rare earth magnesium intermediate alloy preparation device. Background Art

[0002] Rare earth magnesium alloy has the characteristics of low density, high specific strength and specific stiffness, strong corrosion resistance, excellent creep resistance, etc., so it has broad application prospects in the fields of aerospace, rail transportation, automobiles, communication equipment, etc. [The International Journal of Advanced Manufacturing Technology, 2008, 39 (9-10): 851-865]. At present, rare earth magnesium alloy is generally prepared by the doping method, that is, rare earth elements are added to the magnesium alloy melt under melting conditions. However, due to the large difference in melting point and density between rare earth and magnesium, it is difficult for rare earth metals to be uniformly dissolved in the alloy melt, thereby causing segregation. Therefore, it is necessary to prepare a rare earth magnesium master alloy first, and then add it to the alloy melt. The metal impurities (Fe, Si, Cu, etc.) and non-metallic inclusions (nitride oxides, carbides, etc.) in the rare earth magnesium master alloy have great harm to the quality of the terminal alloy material. To obtain high-performance rare earth magnesium alloy, it is necessary to first obtain a high-quality rare earth magnesium master alloy.

[0003] The key to producing rare earth magnesium master alloys with uniform composition and low impurity content is to choose a suitable preparation method. At present, the preparation methods of rare earth magnesium master alloys mainly include doping method, molten salt electrolysis method, etc. The doping method has low process conditions and can be mass-produced, but its production process has high energy consumption and requires high purity of mixed RE and Mg. The prepared product also needs to be re-dissolved and re-refined to remove impurities. The use of molten salt electrolysis to prepare master alloys has the following advantages:

[0004] (1) The raw materials for electrolysis are easily available, the process is short, the cost is low, and it meets environmental protection requirements. The raw materials for electrolysis are generally metal oxides or chlorides, and there is no need to go through a complicated purification process to obtain pure metals and then remelt them;

[0005] (2) The reaction process is rapid and energy consumption is low. Because the electrolytic raw materials have a high solubility in high-temperature molten salt, the exchange current between the metal and molten salt ion electrode interface is high, which makes the ion migration and diffusion speed high;

[0006] (3) Avoid metal burning and oxidation, and prepare a uniform composition of the intermediate alloy. Because the entire process is carried out in high-temperature molten salt, and the metal is electrolyzed while alloying, and the reaction is carried out in the electrolytic cell, the liquid metal Mg and RE can make full use of the magnetic field generated by the current to avoid the segregation problem caused by slow diffusion.

[0007] The purity of the intermediate alloy prepared by molten salt electrolysis [Transactions of Nonferrous Metals Society of China, 2013, 23(10): 3104-3111] is about 95%, which does not meet the requirements of high-performance rare earth magnesium alloys. Therefore, a purification method is needed to improve its purity.

[0008] The melting method is to dilute the impurity content of the master alloy by adding pure magnesium, thereby improving its purity; however, it has the disadvantages of high cost, easy burning of magnesium, difficulty in diffusion of magnesium in the master alloy, and easy segregation. The flux purification method is to use the physical adsorption or chemical reaction between impurities and flux to generate agglomerated particles or complexes with density differences, and use static suspension / sedimentation to achieve a better purification effect. In addition, by using the difference in solid solubility of impurities such as Fe and C in magnesium at different temperatures, and supplemented by multi-stage purification with a temperature system, the purification effect of the master alloy can be optimized.

[0009] Therefore, the utility model adopts molten salt electrolysis, multi-stage purification, and composition modulation integrated integrated device to prepare rare earth magnesium intermediate alloys, which can make the prepared intermediate alloys have uniform composition, low impurity and inclusion content, meet the demand for high-performance rare earth magnesium alloy raw materials, and use the device to prepare intermediate alloys with simple operation, short preparation process, and large-scale continuous production. Utility Model Content

[0010] The utility model provides an integrated preparation device for rare earth magnesium master alloy integrating molten salt electrolysis, multi-stage continuous purification and component modulation and a working method thereof, so as to realize the continuous production of high-quality rare earth magnesium master alloy; the device comprises a full set of functions including continuous feeding, molten salt heating and electrolysis, purification flux feeding and stirring, component modulation, alloy liquid flow and control, temperature control, continuous pouring, gas protection and the like.

[0011] The utility model provides an integrated preparation device for rare earth magnesium master alloy, which is a rare earth magnesium master alloy preparation furnace body in which six compartments, namely, a molten salt electrolysis chamber, a primary purification chamber, a secondary purification chamber, a tertiary purification chamber, a component modulation chamber and a casting chamber, are integrated; the six compartments are arranged in a stepped manner from top to bottom and are interconnected through pipelines, each compartment is introduced with protective gas, and heating elements are respectively installed in the first five compartments, wherein the primary purification chamber, the secondary purification chamber, the tertiary purification chamber and the component modulation chamber are separated by valves arranged at the pipe ports, a filter screen is installed behind the valve, and the filter screen adopts a MgO filter screen.

[0012] The molten salt electrolysis chamber is provided with an electrolysis feeding port, a cathode, an electrolysis stirring device, an electrolysis heating element, an electrolysis crucible, a collecting crucible, a molten salt / alloy liquid separator, and a valve; the molten salt electrolysis chamber is provided with an electrolysis crucible, the cathode and the electrolysis stirring device are installed in the electrolysis crucible, the collecting crucible is installed at the bottom of the electrolysis crucible, and the electrolysis heating element is installed around the electrolysis crucible; the molten salt / alloy liquid separator is connected to the bottom of the collecting crucible, the molten salt / alloy liquid separator adopts a solid-liquid separation device, and the molten salt / alloy liquid separator is connected to the primary purification chamber.

[0013] The primary purification chamber is provided with a stirring device, a flux feeding port, and a heating element;

[0014] The secondary purification chamber and the tertiary purification chamber are respectively provided with heating elements;

[0015] The component preparation chamber is provided with a stirring device, a pure magnesium feeding port, and a heating element;

[0016] The pouring chamber is provided with a mold and a furnace door;

[0017] The protective gas is an inert gas or an inert gas and SF 6 A mixed gas of the type described above, wherein the volume ratio of the inert gas to sulfur hexafluoride is (10-25):1;

[0018] The heating element can control the temperature of each compartment separately, and can achieve a temperature difference of 50°C to 100°C between the compartments.

[0019] The method for preparing rare earth magnesium master alloy using the device comprises the following steps:

[0020] Step 1, preparing molten salt and electrolysis raw materials, wherein the molten salt is GdF 3 and LiF mixture, the mass ratio is (80-95): (20-5); the electrolytic raw material is Gd 2 O 3 and MgO in a mass ratio of (70-85):(30-15);

[0021] Step 2, electrolysis of rare earth magnesium master alloy: a protective gas is introduced into the molten salt electrolysis chamber, the dried molten salt is added to the electrolysis crucible, the electrolysis temperature is heated to 1000-1200° C. to melt the molten salt, and the electrolysis raw materials are added and electrolyzed for 90-120 minutes; the rare earth magnesium master alloy obtained by electrolysis sinks to the bottom collection crucible, the molten salt and the alloy liquid are separated by a molten salt / alloy liquid separator, and the alloy liquid flows into the primary purification chamber through a valve;

[0022] Step 3, multi-stage purification of rare earth magnesium master alloy: the primary purification chamber is heated to 900-1100° C. under a protective atmosphere, a purification flux is added to the alloy liquid flowing into the primary purification chamber through the flux feeding port, and the alloy liquid is stirred for 3-5 minutes by a stirring device to make the alloy liquid fully contact with the flux, and the alloy liquid is allowed to stand for 30-60 minutes after the stirring is completed; the valve is opened to allow the alloy liquid to flow from the primary purification chamber to the secondary and tertiary purification chambers in turn; the temperature difference between each chamber is 50-100° C., and the melt is allowed to stand in each chamber for 30-60 minutes to make the impurities fully suspended and settled, and finally the purified rare earth magnesium master alloy is obtained in the tertiary purification chamber;

[0023] Step 4, rare earth magnesium master alloy composition modulation: the purified alloy liquid flows into the composition modulation chamber, pure magnesium is added to the alloy liquid through the pure magnesium feeding port, and stirred for 5 to 10 minutes by a stirring device to adjust the rare earth-rich magnesium master alloy to a magnesium-rich rare earth master alloy;

[0024] Step 5, rare earth magnesium master alloy pouring: pouring the alloy liquid after the composition is adjusted into the mold in the pouring chamber, taking it out through the furnace door and demoulding it to obtain the rare earth magnesium master alloy product.

[0025] In step 2 of the utility model, the collecting crucible is one of a corundum crucible, a molybdenum crucible or a magnesium oxide crucible.

[0026] Compared with the prior art, the beneficial effects of the utility model include:

[0027] Provided is an integrated preparation device and method for rare earth magnesium master alloys that integrates molten salt electrolysis, multi-stage purification, component modulation, and casting, to achieve continuous and large-scale production of high-quality rare earth magnesium master alloys; and the utility model is simple to use, simple to operate, has a short preparation process, and is easy to promote and apply. The utility model provides certain guidance for the production of rare earth magnesium master alloys, lays the foundation for large-scale, high-efficiency production of high-quality master alloys, and promotes the development of the rare earth magnesium master alloy industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a schematic diagram of an integrated preparation device for a rare earth magnesium master alloy proposed in the utility model;

[0029] Illustration, 1-gas outlet, 2-electrolysis feeding port, 3-cathode, 4-electrolysis stirring device, 5-protective gas inlet I, 6-electrolysis heating element, 7-electrolysis crucible, 8-molten salt electrolysis chamber, 9-collecting crucible, 10-molten salt / alloy liquid separator, 11-valve I, 12-protective gas inlet II, 13-stirring device I, 14-flux feeding port, 15-gas outlet, 16-purification heating element I, 17-primary purification chamber, 18-valve II, 19-filter, 20-secondary purification chamber, 21-purification heating element II, 22-tertiary purification chamber, 23-purification heating element III, 24-ingredient modulation chamber, 25-stirring device II, 26-pure magnesium feeding port, 27-heating element, 28-valve III, 29-pouring chamber, 30-mold, 31-furnace door. DETAILED DESCRIPTION

[0030] In the following embodiments, unless otherwise specified, functional components or structures are conventional components or conventional structures used in the art to achieve corresponding functions.

[0031] Example 1

[0032] like Figure 1 As shown, the integrated preparation device of rare earth magnesium master alloy is arranged, which includes six compartments arranged in a stepped manner from top to bottom, namely, molten salt electrolysis chamber 8, primary purification chamber 17, secondary purification chamber 20, tertiary purification chamber 22, component modulation chamber 24, and casting chamber 29, and the six compartments are integrated into an integrated furnace body. Heating elements are installed in the first five compartments respectively to control and adjust the temperature in different compartments.

[0033] In some specific embodiments, the molten salt electrolysis chamber 8 is provided with a gas outlet 1, an electrolysis feed port 2 and a protective gas inlet 15, and has a built-in cathode 3, an electrolysis stirring device 4, an electrolysis heating element 6, an electrolysis crucible 7, a collection crucible 9, and a molten salt / alloy liquid separator 10;

[0034] An electrolytic crucible 7 is built into the molten salt electrolysis chamber 8, a collecting crucible 9 is installed in the electrolytic crucible 7, a molten salt / alloy liquid separator 10 is connected to the bottom of the collecting crucible 9, and the molten salt / alloy liquid separator 10 adopts a solid-liquid separation device for separating the solid intermediate alloy obtained by electrolysis from the alloy liquid, wherein the solid intermediate alloy is deposited at the bottom of the collecting crucible 9, and the alloy liquid flows into the primary purification chamber 17 through a pipeline provided with a valve I11.

[0035] In some specific embodiments, the cathode 3 is a tungsten rod, the electrolytic crucible 7 is a graphite crucible, and the collecting crucible 9 is a corundum crucible, a molybdenum crucible or a magnesium oxide crucible, preferably a corundum crucible;

[0036] In some specific embodiments, a protective gas inlet II12 and a flux feeding port 14 are provided above the primary purification chamber 17, a stirring device I13 is built in the primary purification chamber, and purification heating elements I16 are arranged around the primary purification chamber 17;

[0037] In some specific embodiments, the secondary purification chamber 20 and the tertiary purification chamber 22 are respectively provided with a purification heating element II21 and a purification heating element III23; the secondary purification chamber 20 and the tertiary purification chamber 22 are also provided with a protective gas inlet.

[0038] In some specific embodiments, a stirring device II25 and a pure magnesium feeding port 26 are provided above the component preparation chamber 24, and heating elements 27 are arranged around it;

[0039] The primary purification chamber 17, the secondary purification chamber 20, the tertiary purification chamber 22, and the component modulation chamber 24 are connected in sequence by installing a connecting pipeline, on which a valve II18 and a filter screen 19 are installed; the filter screen 19 is a MgO filter screen.

[0040] In some specific embodiments, the pouring chamber 29 is provided with a mold 30 and an external furnace door 31 ; and a valve III28 is provided at the connection between the ingredient preparation chamber 24 and the pouring chamber 29 .

[0041] In some specific embodiments, the protective gas introduced into the molten salt electrolysis chamber 8 and the primary purification chamber 17 is an inert gas or an inert gas and SF 6 A mixed gas of the type described above, wherein the volume ratio of the inert gas to sulfur hexafluoride is (10-25):1;

[0042] In some specific embodiments, the heating elements (electrolysis heating element 6, purification heating element I16, purification heating element II21, purification heating element III23, heating element 27) can control the temperature of each compartment respectively, and can achieve a temperature difference of 50°C to 100°C between the compartments. The heating elements can use any heater allowed by the furnace body, such as electric arc heating or induction heating.

[0043] Example 2

[0044] This embodiment provides an integrated preparation method of the rare earth magnesium master alloy of the utility model, which includes:

[0045] Arrange the above-mentioned rare earth magnesium master alloy integrated preparation device;

[0046] Step 1, preparing molten salt and electrolysis raw materials, wherein the molten salt is GdF 3 and LiF mixture, mass ratio is 85:15; electrolytic raw material is Gd 2 O 3and MgO in a mass ratio of 85:15;

[0047] Step 2, electrolysis of rare earth magnesium master alloy: protective gas is introduced into the molten salt electrolysis chamber 8, the molten salt dried at 200°C for 30 minutes is added to the graphite crucible 7, the molten salt is heated to the electrolysis temperature of 1100°C to melt the molten salt, the electrolysis raw materials are added and electrolysis is carried out for 90 minutes; the Mg-90Gd master alloy obtained by electrolysis is sunk into the bottom corundum crucible 9, the molten salt and the alloy liquid are separated by the molten salt / alloy liquid separator 10, and the alloy liquid flows into the primary purification chamber 17 through the valve 11;

[0048] Step 3, multi-stage purification of rare earth magnesium master alloy: the first-stage purification chamber 17 is in SF 6 and N 2 The mixed gas volume ratio is 1:10 and heated to 1100°C in a protective atmosphere. A purification flux is added to the alloy liquid flowing into the primary purification chamber 17 through the flux feeding port 14, and stirred for 5 minutes through the stirring device 13 to make the alloy liquid fully contact with the flux. After the stirring is completed, the alloy liquid is allowed to stand for 30 minutes; the valve 18 is opened to allow the alloy liquid to flow from the primary purification chamber to the secondary and tertiary purification chambers in turn; the temperature difference between each chamber is 50°C, and the temperatures of the secondary and tertiary purification chambers are 1050°C and 1000°C respectively; the melt is allowed to stand in each chamber for 30 minutes to make the impurities fully suspended and settled, and finally the purified Mg-90Gd master alloy is obtained in the tertiary purification chamber;

[0049] Step 4, rare earth magnesium master alloy composition modulation: the purified alloy liquid flows into the composition modulation chamber 24, pure magnesium is added to the alloy liquid through the pure magnesium feeding port 26, and stirred for 10 minutes by the stirring device 25 and then kept warm for 30 minutes, so as to adjust the Mg-90Gd master alloy to Mg-30Gd master alloy;

[0050] Step 5, casting of rare earth magnesium master alloy: the alloy liquid with adjusted composition is cast into the mold 30 in the casting chamber 29, and is taken out through the furnace door 31 and demolded to obtain the Mg-30Gd master alloy product.

[0051] In some specific embodiments, the purification flux ratio of step 3 is MgCl 2 ~36.1wt%, KCl ~24.06wt%, BaCl 2 ~20.0wt%, B 2 O 3 ~0.61wt%, CaF 2 ~4.23wt%, GdCl 3 ~15.0wt%. The flux is fully dried before use and mixed and ball-milled evenly.

[0052] The above only expresses the preferred implementation of the utility model, and its description is relatively specific and detailed, but it cannot be understood as limiting the scope of the utility model patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the utility model, several modifications, improvements and substitutions can be made, which all belong to the protection scope of the utility model. Therefore, the protection scope of the utility model patent shall be based on the attached claims.

Claims

1. An integrated preparation device for rare earth magnesium master alloy, characterized in that: The device is a furnace body for preparing an intermediate alloy in which six chambers, namely, a molten salt electrolysis chamber (8), a primary purification chamber (17), a secondary purification chamber (20), a tertiary purification chamber (22), a component modulation chamber (24), and a casting chamber (29), are integrated into one. The six chambers are arranged in a stepped manner from top to bottom and are interconnected through pipelines, and each chamber is provided with a protective gas inlet. Heating elements are respectively installed in the five chambers of the molten salt electrolysis chamber (8), the primary purification chamber (17), the secondary purification chamber (20), the tertiary purification chamber (22), and the component modulation chamber (24); The molten salt electrolysis chamber (8) is used to heat and electrolyze the molten salt and electrolysis raw materials to separate the precipitate from the alloy liquid; The primary purification chamber (17), the secondary purification chamber (20), and the tertiary purification chamber (22) are used to remove impurities in the alloy liquid; The composition modulation chamber (24) is used to adjust the rare earth-rich magnesium master alloy liquid into a magnesium-rich rare earth master alloy liquid; The casting chamber (29) casts the magnesium-rich rare earth master alloy liquid and demoulds it to obtain a rare earth magnesium master alloy product.

2. The integrated preparation device for rare earth magnesium master alloy according to claim 1, characterized in that: The molten salt electrolysis chamber (8) has an electrolytic crucible (7) built in, a cathode (3) and an electrolytic stirring device (4) installed in the electrolytic crucible (7), a collecting crucible (9) installed at the bottom of the electrolytic crucible (7), and electrolytic heating elements (6) installed around the electrolytic crucible (7); a molten salt / alloy liquid separator (10) is connected to the bottom of the collecting crucible (9), the molten salt / alloy liquid separator (10) adopts a solid-liquid separation device, and the molten salt / alloy liquid separator (10) is connected to the primary purification chamber (17) through a pipeline provided with a valve I (11).

3. The integrated preparation device for rare earth magnesium master alloy according to claim 1, characterized in that: The primary purification chamber (17) and the component preparation chamber (24) are both provided with stirring devices.

4. The integrated preparation device for rare earth magnesium master alloy according to claim 1 or 3, characterized in that: The primary purification chamber (17) is provided with a flux feeding port (14) for feeding purified flux; the component modulation chamber (24) is provided with a pure magnesium feeding port (26) for feeding pure magnesium.

5. The integrated preparation device for rare earth magnesium master alloy according to claim 1, characterized in that: The pouring chamber (29) is provided with a mold (30) and a furnace door (31).

6. The integrated preparation device for rare earth magnesium master alloy according to claim 1, characterized in that: Valves and filters are provided at the points where the pipelines connect the primary purification chamber (17), the secondary purification chamber (20), and the tertiary purification chamber (22).

7. The integrated preparation device for rare earth magnesium master alloy according to claim 6, characterized in that: The filter screen adopts MgO filter screen.

8. The integrated preparation device for rare earth magnesium master alloy according to claim 1, characterized in that: The heating element is used to control the temperature of each chamber respectively. The temperature of each chamber, namely, the molten salt electrolysis chamber (8), the primary purification chamber (17), the secondary purification chamber (20), the tertiary purification chamber (22), and the component modulation chamber (24), gradually decreases, and the temperature difference between adjacent chambers is between 50°C and 100°C.

9. The integrated preparation device for rare earth magnesium master alloy according to claim 2, characterized in that: The collecting crucible (9) is one of a corundum crucible, a molybdenum crucible or a magnesium oxide crucible.