Electrolytic capacitor
By using porous electrode foils formed from aluminum and aluminum alloy powder sintered bodies and low resistivity electrolytes, the existing electrolytic capacitors solve the problem of balancing electrostatic capacity and environmental load, achieving high electrostatic capacity and low environmental pollution.
Patent Information
- Application Number
- CN202190000954.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2031-07-15
AI Technical Summary
Existing electrolytic capacitors are difficult to balance between increasing electrostatic capacity and reducing environmental load, especially when the electrostatic capacity decreases at high frequencies and the etching process causes environmental pollution.
A sintered body composed of aluminum and aluminum alloy powder is used as the electrode foil, and a porous structure is formed through sintering. Combined with a low resistivity electrolyte, a high electrostatic capacity electrolytic capacitor without etching treatment is realized.
It achieves a higher electrostatic capacity than the etching method, reduces environmental pollution, suppresses the increase in leakage current under high-temperature loads, and optimizes the electrostatic capacity characteristics at high frequencies.
Smart Images

Figure CN221861469U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to an electrolytic capacitor. Background Art
[0002] Electrolytic capacitors are small, have large capacity, and are inexpensive, and are widely used as one of the important components of electronic equipment, electrical equipment, vehicle-mounted equipment, and the like.
[0003] Conventional electrolytic capacitors, such as the most widely used aluminum electrolytic capacitors, can be manufactured as follows: After electrochemically etching a high-purity aluminum foil to increase its surface area, an anode foil having a film formed on the surface of the aluminum foil by anodic oxidation and a cathode foil having an etched surface are used to manufacture it. Then, the obtained anode foil and cathode foil are arranged opposite to each other, and a separator is further sandwiched between these foils and wound to form an element of the structure, and the electrolyte is impregnated into the element of the structure. The element impregnated with the electrolyte is housed in a housing and sealed with an elastic sealing body to complete the electrolytic capacitor.
[0004] The high capacity of electrolytic capacitors is an important market demand directly related to the miniaturization of the mounted devices, and the high capacity is gradually realized based on the increase of etching rate. However, there is a theoretical limit to the increase of surface area based on etching, and it is gradually becoming unable to meet the increasing demand for high capacity year by year. In addition, in order to reduce the environmental load caused by hydrochloric acid containing sulfuric acid, phosphoric acid, nitric acid, etc. used in etching, it is also expected to replace the surface area increase method of etching foil.
[0005] Here, as a method of increasing the surface area instead of etching the foil, a capacitor using a metal sintered body as an anode has been proposed (Patent Document 1: Japanese Utility Model Application Laid-Open No. 59-140430).
[0006] However, a capacitor of this shape has a long distance from the anode to the cathode current collector, so the resistance component through the electrolyte becomes large, and there is a disadvantage that the electrostatic capacitance at high frequencies decreases.
[0007] As another method for increasing the surface area, an aluminum electrolytic capacitor has been proposed, which is characterized by using a foil having fine aluminum powder attached to the surface of the electrode foil (Patent Document 2: Japanese Patent Application Laid-Open No. 2-267916, and Patent Document 3: Japanese Patent Application Laid-Open No. 2006-108159).
[0008] However, the aluminum powder of the electrode foil disclosed in these documents has a small particle size, so there are the following disadvantages when forming an anodic oxide coating: there is sometimes a concern that the gaps between the sintered particles will be filled and the electrostatic capacitance will be reduced. In addition, when using an electrolyte for medium and high voltage capacitors with a high viscosity and resistivity, the electrostatic capacitance at high frequencies is reduced.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Utility Model Publication No. 59-140430
[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 2-267916
[0013] Patent Document 3: Japanese Patent Application Publication No. 2006-108159 Utility Model Content
[0014] Problems to be solved by utility models
[0015] The utility model is made in view of the above-mentioned need for high capacity and reduction of environmental load, and its purpose is to provide an electrolytic capacitor that does not require etching of electrode materials and can achieve a higher electrostatic capacitance than the conventional electrolytic capacitor using electrode foil whose surface area is increased only by etching.
[0016] Solutions for solving problems
[0017] The electrolytic capacitor of the utility model is characterized in that it comprises a capacitor element and an electrolyte, wherein the capacitor element comprises: an anode foil, a cathode foil and a separator sandwiched between the anode foil and the cathode foil, the electrolyte is impregnated in the capacitor element, the anode foil or the cathode foil comprises: a sintered body composed of sintered particles containing powder of at least one of aluminum and an aluminum alloy, and the aluminum purity of the aluminum contained in the sintered body is 99.8% by weight or more.
[0018] The anode foil or the cathode foil preferably comprises the sintered body and a substrate for supporting the sintered body, and the aluminum purity of the aluminum contained in the sintered body and the substrate is 99.99% by weight or more. In addition, it is suitable that the resistivity of the electrolyte is 1500Ω·cm or less, and the average particle size (D50) of the powder or the sintered particles is 6μm or less.
[0019] In addition, the aforementioned electrolyte solution is suitable for containing: a solvent including an organic solvent, or a solvent including a mixture of water and an organic solvent; and at least one electrolyte selected from the group consisting of an organic acid or an organic acid salt, an inorganic acid or an inorganic acid salt, and a mixture of an organic acid or an organic acid salt and an inorganic acid or an inorganic acid salt.
[0020] Effect of utility model
[0021] According to the electrolytic capacitor of the utility model, the surface area of the electrode foil is larger than the pit area of the conventional etched foil, so a large electrostatic capacitance can be achieved. In addition, etching of the electrode foil is not necessarily required, and the environmental load can be reduced as a result. In addition, the increase of leakage current to high temperature load can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic cross-sectional view showing an example of the electrolytic capacitor according to the present embodiment.
[0023] Figure 2 This is an explanatory diagram for explaining an example of the capacitor element according to the present embodiment.
[0024] Figure 3 Graph showing the leakage current values of the electrolytic capacitors of Example 13 and Example 14 in the high temperature load test. DETAILED DESCRIPTION
[0025] Hereinafter, although the suitable embodiment of this invention is described, this invention is not limited to these aspects.
[0026] Figure 1 A schematic cross-sectional view showing the overall structure of the electrolytic capacitor according to the present embodiment is shown in FIG. Figure 2 A diagram illustrating capacitor elements.
[0027] The electrolytic capacitor 10 is constructed as follows: a capacitor element 1 is arranged inside a bottomed cylindrical outer casing 4 formed of a metal such as aluminum, and the opening of the outer casing 4 is sealed by an elastic sealing body 3, and the elastic sealing body 3 is fixed by fitting the opening edge (curl 14), thereby forming the structure.
[0028] The capacitor element 1 is a wound capacitor element 1 formed by winding an anode foil 20 having a sintered body 22 of aluminum powder formed on the surface of a core material (substrate) 21, a cathode foil 23, a first separator 24 disposed between the anode foil 20 and the cathode foil 23, and a second separator 25, and is sealed in an exterior case 4 after being impregnated with an electrolyte. It should be noted that reference numeral 2 is a lead wire mounted on each of the anode foil 20 and the cathode foil 23.
[0029] The sintered body 22 is formed on both surfaces or one surface of the substrate 21. Alternatively, the sintered body 22 may be formed on the cathode foil 23 (not shown).
[0030] It should be noted that substrate 21 is not necessarily required, and anode foil 20 or cathode foil 23 may be constituted only by sintered body 22 of aluminum powder.
[0031] According to the present embodiment, the surface area of the electrode foil is larger than the pit area of the conventional etched foil, and therefore, a large electrostatic capacitance can be achieved. In addition, for the aluminum sintered body capacitor proposed in the past (e.g., Patent Document 1), the present embodiment is a structure in which the sintered body is formed into a foil shape and wound, so that the distance between the anode and cathode collectors becomes closer, thereby reducing the resistance component across the electrolyte, and the electrostatic capacitance at high frequency (about 10kHz) is excellent. In addition, for electrolytic capacitors using foils with fine aluminum powder attached (e.g., Patent Documents 2 or 3), the electrostatic capacitance at high frequency (about 10kHz) of the present embodiment is also excellent.
[0032] Here, the powder sintered body 22 refers to a sintered body composed of sintered particles of the powder. The sintered particles refer to sintered particles (referred to as "sintered particles" in the present application) obtained by sintering particles of the powder (referred to as "powder particles" in the present application).
[0033] The sintered body 22 of the aluminum powder of the present embodiment is composed of sintered particles of powder containing at least one of aluminum and aluminum alloy. For the aluminum in the aluminum and aluminum alloy, from the viewpoint of preventing adverse conditions caused by impurities, the aluminum purity is preferably 99.8% by weight or more, and in particular, in order to suppress the increase of leakage current under high temperature load, the aluminum purity is more preferably 99.99% by weight or more. In addition, in the case of aluminum alloy, for example, an alloy containing one or more elements such as silicon (Si), iron (Fe), copper (Cu), manganese (Mn), magnesium (Mg), chromium (Cr), zinc (Zn), titanium (Ti), vanadium (V), gallium (Ga), nickel (Ni), boron (B) and zirconium (Zr) can be used. In this case, the content of these elements is preferably set to 100 ppm by weight or less, and particularly preferably set to 50 ppm by weight or less.
[0034] The sintered body 22 is formed by sintering sintered particles of powder of at least one of aluminum and aluminum alloy while maintaining pores with each other. That is, the sintered particles are connected with each other while maintaining pores, and have a three-dimensional network structure. By forming such a porous sintered body, the desired electrostatic capacitance can be obtained even without etching. The porosity at this time can be appropriately set within a range of usually more than 10% according to the desired electrostatic capacitance, etc. In addition, the porosity can be controlled, for example, according to the particle size of the powder of aluminum or aluminum alloy of the starting material, the composition of the paste composition containing the powder (resin binder), etc.
[0035] The shape of the sintered body 22 is not particularly limited, but is generally in the form of a foil having an average thickness of preferably 5 μm to 100 μm, particularly preferably 5 μm to 60 μm on one side when including the substrate 21. The average thickness can be calculated by a weight method.
[0036] It should be noted that the average particle size of the sintered particles is preferably 80 μm or less. If the average particle size is larger than 80 μm, a desired electrostatic capacitance may not be obtained.
[0037] The average particle size of the sintered particles is preferably 1 μm or more. If the average particle size is less than 1 μm, there is a concern that the desired withstand voltage cannot be obtained. It should be noted that a small average particle size is advantageous when the surface area is increased, but if the average particle size is excessively reduced, there is a concern that the electrostatic capacitance may be reduced by filling the gaps between the sintered particles when an anodic oxide film is formed as required. From the perspective of preventing such a reduction in electrostatic capacitance, it is more preferred to have an average particle size of 2.5 μm or more.
[0038] From the viewpoint of improving the electrostatic capacitance characteristics at around 10 kHz, the average particle size is particularly preferably 2.5 μm or more and 6 μm or less.
[0039] The substrate 21 is not particularly limited, and aluminum foil can be preferably used. The substrate 21 may be used without being subjected to etching treatment, but may be subjected to etching treatment as necessary.
[0040] Aluminum or aluminum alloy having the same composition as the aluminum or aluminum alloy powder can be used as the aluminum foil of the substrate 21. In order to suppress the increase of leakage current under high temperature load, the aluminum purity is preferably 99.99 wt % or more.
[0041] The thickness of the aluminum foil as the substrate 21 is not particularly limited, but is preferably within a range of 5 μm to 100 μm, and particularly preferably within a range of 5 μm to 60 μm.
[0042] The method of forming the sintered body 22 on the substrate 21 to produce the electrode foil 20 (23) is based on the following method. That is, it includes the following steps:
[0043] 1. A first step of forming a coating formed of a composition containing a powder of at least one of aluminum and an aluminum alloy on a substrate 21; and,
[0044] 2. A second step of sintering the film at a temperature of 560°C to 660°C.
[0045] Step 1
[0046] In the first step, a coating film made of a composition including powder of at least one of aluminum and an aluminum alloy is formed on the substrate 21 .
[0047] As the composition and ingredients of aluminum or aluminum alloy, those described above can be used.
[0048] The particle shape of the powder, that is, the powder particles, is not particularly limited, and spherical, amorphous, flaky, etc. shapes can be suitably used. Spherical powder particles are particularly suitably used.
[0049] The average particle size of the powder, ie, the powder particles, is preferably 80 μm or less. If the average particle size is larger than 80 μm, the desired electrostatic capacitance may not be obtained.
[0050] The average particle size of the powder, i.e., the powder particles, is preferably 1 μm or more. If the average particle size is less than 1 μm, there is a concern that the desired withstand voltage cannot be obtained. It should be noted that when the surface area is increased, a small average particle size is advantageous, but if the average particle size is excessively reduced, there is a concern that the electrostatic capacitance will decrease due to the gaps between the sintered particles being filled when the anodized film is formed as required. From the perspective of preventing such a decrease in electrostatic capacitance, it is more preferable to make the average particle size 2.5 μm or more.
[0051] From the viewpoint of improving the electrostatic capacitance characteristics at around 10 kHz, the average particle size is particularly preferably 2.5 μm or more and 6 μm or less.
[0052] It should be noted that the particle size of the powder particles does not change significantly even after the sintering in the second step, and the average particle size of the sintered particles can be adjusted to the same level by adjusting the average particle size of the powder particles.
[0053] The aforementioned composition may include a resin binder, a solvent, a sintering aid, a surfactant, etc. as required. They may all use known or commercially available ones. It is particularly preferred to contain at least one of a resin binder and a solvent and use it as a paste-like composition. Thus, a coating may be formed efficiently.
[0054] In addition, a known solvent can be used. For example, in addition to water, an organic solvent such as ethanol, toluene, ketones, and esters can be used.
[0055] Step 2
[0056] In the second step, the film is sintered at a temperature of 560° C. or higher and 660° C. or lower.
[0057] The sintering temperature is 560° C. to 660° C., preferably 560° C. to less than 660° C., more preferably 570° C. to 659° C. The sintering time varies depending on the sintering temperature, etc., but can be appropriately determined in the range of about 5 to 24 hours.
[0058] The sintering atmosphere is not particularly limited, and may be, for example, a vacuum atmosphere, an inert gas atmosphere, an oxidizing gas atmosphere (atmosphere), a reducing atmosphere, etc., but it is particularly preferred to be a vacuum atmosphere or a reducing atmosphere. In addition, regarding the pressure conditions, it may be normal pressure, reduced pressure, or pressurized.
[0059] It should be noted that, when the aforementioned composition contains an organic component such as a resin binder, it is preferred that after the first step and before the second step, a heat treatment (degreasing treatment) is performed in advance within a temperature range of 100° C. to 600° C. for a holding time of more than 5 hours. The heat treatment atmosphere is not particularly limited, and for example, it can be a vacuum atmosphere, an inert gas atmosphere, or an oxidizing gas atmosphere. In addition, the pressure condition can also be normal pressure, reduced pressure, or pressurized.
[0060] In the second step, the electrode material of the present invention can be obtained. The electrode material can be used as an electrode (electrode foil 20 (23)) for the aluminum electrolytic capacitor 10 without being subjected to etching treatment, but can also be subjected to etching treatment as needed.
[0061] Step 3
[0062] The electrode material may be subjected to anodization treatment as a third step as necessary to form a dielectric. For example, a dielectric oxide film having withstand voltage may be formed by a predetermined anodization treatment to form anode foil 20 for electrolytic capacitor 10 having a desired withstand voltage.
[0063] Next, the electrolytic solution will be described.
[0064] In the present invention, the resistivity of the electrolyte is preferably 1500Ω·cm or less. As a result, the ratio of the electrostatic capacitance at 10kHz to the electrostatic capacitance at 120Hz becomes closer to 1 than before, and good electrostatic capacitance characteristics are obtained in a wide frequency range. In addition, from the perspective of ensuring the desired withstand voltage, the resistivity of the electrolyte is preferably 100Ω·cm or more.
[0065] The electrolyte of the utility model contains at least an electrolyte and a solvent. In addition, additives described below may also be added. As a solvent for dissolving the electrolyte and the additive, an organic solvent is preferably used alone, or a solvent of a water-organic solvent system, i.e. a mixture of an organic solvent and water, may be used.
[0066] As an organic solvent, a protic solvent or an aprotic solvent can be used alone or by mixing two or more thereof. As required, one or more protic solvents can be used in any combination with one or more aprotic solvents. As a suitable protic solvent, for example, an alcohol compound can be cited. As a specific example of an alcohol compound that can be advantageously used herein, it is not particularly limited, and the following can be cited, diols (glycols) such as methanol, ethanol, propanol, butanol, triols such as ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, 1,4-butanediol, 1,3-butanediol, triols such as glycerol, or their derivatives, etc. In addition, suitable aprotic solvents are not particularly limited, and examples thereof include lactone compounds such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, sulfolane, methylsulfolane, dimethylsulfolane, propylene carbonate, butylene carbonate, isobutylene carbonate, methylpyrrolidone, imidazolidinone, pyrrolidinenitrile, pyrrolidone, methylpyrrolidone, tetrahydrofuran, acetonitrile, N-methylformamide, N,N-dimethylformamide, nitrobenzene, their derivatives, and other intramolecular polar compounds.
[0067] In the electrolyte solution related to the present embodiment, as described above, a water-organic solvent system may be used instead of using an organic solvent alone. By using such a water-organic solvent system solvent, the freezing point of the solvent is lowered, thereby improving the resistivity characteristics of the electrolyte solution at low temperatures, and achieving good low-temperature characteristics shown by a small difference in resistivity between low temperature and normal temperature.
[0068] When describing in further detail, if ethylene glycol is used as an organic solvent, the boiling point of this proton-based organic solvent is 198°C and the melting point is about -13°C. The temperature range required for capacitors is generally -40°C to 105°C, so the electrolyte using this solvent has a margin of characteristics at high temperatures, but at low temperatures, there is a concern that the electrical characteristics may be reduced due to the increase in viscosity and solidification of the electrolyte.
[0069] The electrolyte of the present embodiment is used alone or mixed with a plurality of organic solvents having excellent temperature characteristics. On the other hand, when an organic solvent with a high freezing point is used, a water-organic solvent system is used by adding water, so that the freezing point of the solvent can be lowered to ensure the electrical characteristics at low temperatures. The electrolyte solubility and ion mobility of the water-organic solvent system electrolyte are very large, so a relatively low resistivity can be achieved compared to an electrolyte with an organic solvent alone. In addition, at low temperatures, the characteristics of the solvent are improved, so that an electrolyte having a breakthrough characteristic of a small difference in resistivity at low temperatures and at room temperature is obtained. Therefore, the electrolytic capacitor 10 using this electrolyte can certainly reflect the characteristics of the electrolyte and has good temperature characteristics.
[0070] As electrolyte, an organic acid, preferably a carboxylic acid or its salt, a dicarboxylic acid or a hydroxycarboxylic acid boron complex or its salt, and an inorganic acid or its salt are used. These electrolyte components can be used alone, or two or more electrolyte components can be used in combination. If a carboxylic acid or its salt, a dicarboxylic acid or a hydroxycarboxylic acid boron complex or its salt and an inorganic acid or its salt are used as electrolyte components, it is expected that the freezing point of the electrolyte is reduced, and therefore, the low temperature characteristics of the electrolyte can be further improved.
[0071] Examples of carboxylic acids that can be used as electrolyte components are not limited to the following, but can include monocarboxylic acids or derivatives thereof represented by formic acid, acetic acid, propionic acid, butyric acid, p-nitrobenzoic acid, salicylic acid, benzoic acid, methylbenzoic acid, ethylbenzoic acid, isobutylbenzoic acid, sec-butylbenzoic acid, tert-butylbenzoic acid, etc., and dicarboxylic acids or derivatives thereof represented by oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, fumaric acid, maleic acid, phthalic acid, azelaic acid, sebacic acid, octanoic acid, 1,6-decanedicarboxylic acid, 5,6-decanedicarboxylic acid, methyladipic acid, ethyladipic acid, isobutyladipic acid, sec-butyladipic acid, tert-butyladipic acid, etc. In addition, carboxylic acids containing hydroxyl groups, such as citric acid, can also be used.
[0072] Moreover, the dicarboxylic acids or hydroxycarboxylic acids in the boron complexes of dicarboxylic acids or hydroxycarboxylic acids that can be used as the same electrolyte components should not be limited to those listed below, but examples include boron dioxalic acid, boron dimalonic acid, boron disuccinic acid, boron diadipic acid, boron dimaleic acid, boron diglycolic acid, boron dilactic acid, boron dimalic acid, boron ditartaric acid, boron dicitric acid, boron disalicylic acid, boron diphthalic acid, boron di(2-hydroxy)isobutyric acid, boron dimandelic acid, boron di(3-hydroxy)propionic acid, etc.
[0073] And then, as the example of the inorganic acid that can be used as the same electrolyte component, it is not limited to the following enumerators, but phosphoric acid, phosphorous acid, hypophosphorous acid, alkyl phosphoric acid, phosphomolybdic acid, boric acid, sulfamic acid etc. can be enumerated. In addition, the derivative of this inorganic acid can also be used as required.
[0074] Furthermore, as the salt of the above-mentioned carboxylic acid or inorganic acid, a large amount of commonly known salts can be used. As the example of suitable salt, it is not particularly limited, and can be selected from sodium salt, potassium salt, ammonium salt, alkylammonium salt, amine salt listed below, one or more of amidine salts. As amine salts, dimethylamine, diethylamine, trimethylamine, triethylamine, ethyldimethylamine, diethylmethylamine, methanolamine, ethanolamine, dimethanolamine, diethanolamine, trimethanolamine, triethanolamine, pyrrolidinecarbonitrile, piperidine, piperazine, morpholine, methylmorpholine, ethylmorpholine, oxazolidine, thiomorpholine, thiazolidinemorpholine, methylmorpholine, ethylmorpholine, oxazolidine, thiomorpholine, thiazolidine salts such as morpholine. Examples of amidine salts include salts such as 1,3-dimethylimidazoline, 1,3-diethylimidazoline, 1,2,3-trimethylimidazoline, 1,2,3,4-tetramethylimidazoline, 1,3-dimethyl-2-ethylimidazoline, 1,2-dimethyl-3-ethylimidazoline, 1,2-dimethyl-3-ethylimidazoline, 1,2,3-triethylimidazoline, and 1,2,3,4-tetraethylimidazoline. Examples of amidine salts include tetraalkylammonium salts and imidazolium salts.
[0075] Furthermore, if an inorganic acid or a salt thereof is used as an electrolyte component, the freezing point of the electrolyte can be expected to decrease, which can contribute to the improvement of the low-temperature characteristics of the electrolyte. In addition, when an inorganic acid or a salt thereof is used, when a nitro compound is used as an additive, there is a hydrogen absorption effect derived from the nitro compound.
[0076] Furthermore, by using such an electrolyte component such as an inorganic acid or a salt thereof in combination with the electrolyte component such as the above-mentioned carboxylic acid or a salt thereof, the life of the electrolytic capacitor 10 is significantly extended compared to the case where the carboxylic acid or a salt thereof is used alone.
[0077] In the electrolyte solution related to the present embodiment, the amount of electrolyte contained therein can be appropriately determined according to the characteristics required by the electrolyte solution, the type of solvent used, the type of electrolyte used, and other conditions. Generally speaking, for example, when a carboxylic acid or a salt thereof is used as an electrolyte, its amount is preferably about 3 to 30% by mass of the total weight of the electrolyte solution. When the amount of the above-mentioned electrolyte is less than 3% by mass, the desired conductivity cannot be fully ensured. If it exceeds 30% by mass, the effect gradually reaches saturation, and in addition, it becomes difficult to dissolve in the solvent.
[0078] When an inorganic acid or its salt is used as an electrolyte, its amount is preferably about 0.1 to 15% by mass of the total amount of the electrolyte. When the amount of the above electrolyte is less than 0.1% by mass, the desired conductivity cannot be fully ensured. If it exceeds 15% by mass, the effect gradually becomes saturated, and it becomes difficult to dissolve in the solvent. When a carboxylic acid or its salt is used in combination with an inorganic acid or its salt, it can also be used within the above range.
[0079] Furthermore, in the electrolyte solution according to the present embodiment, additives such as (1) chelate, (2) sugar or its derivative, (3) gluconic acid and / or gluconolactone, (4) the above-mentioned nitro compound, and (5) polymer compound are preferably added as needed. These additives may be used alone or in combination of two or more. Each additive is described below.
[0080] (1) Chelate
[0081] As the chelate, for example, ethylenediaminetetraacetic acid (EDTA), trans-1,2-diaminocyclohexane-N,N,N',N',N'-tetraacetic acid-hydrate (CyDTA), dihydroxyethylglycine (DHEG), ethylenediaminetetra(methylenephosphonic acid) (EDTPO), diethylenetriamine-N,N,N',N",N"-pentaacetic acid (DTPA), diaminopropanoltetraacetic acid (DPTA-OH), ethylenediaminediacetic acid (EDDA), ethylenediamine-N,N'-bis(methylenephosphonic acid) 1 / 2 hydrate (EDDPO), glycol ether diaminetetraacetic acid (GEDTA), hydroxyethylethylenediaminetriacetic acid (EDTA-OH), etc. can be used. The chelate is usually preferably added in the range of 0.01 to 3 mass%. This chelate complex can bring about effects such as extending the life of the capacitor 10 by suppressing the hydration reaction of the aluminum (Al) electrode foil of the low-impedance capacitor, improving the low-temperature characteristics of the electrolytic capacitor 10 (the solvent has a composition close to an antifreeze state, so the change in impedance at room temperature and low temperature becomes smaller), and improving corrosion resistance.
[0082] (2) Sugar or its derivatives
[0083] As sugar or its derivative, for example, monosaccharides such as glucose, fructose, xylose, galactose, ribose, mannose, arabinose, lyxose, allose, aldose, gulose, idestarose and their derivatives, sugar alcohols such as erythritol, xylitol, mannitol, maltose, sucrose, fructose, cellobiose, sucrose, agarose and their derivatives, trisaccharides such as maltotriose and their derivatives, starch, glycogen, alginic acid, agar, polysaccharides such as polymannose and their derivatives, etc. can be cited. Sugar or its derivative is usually preferably added in the range of 0.01 to 5 mass%. Such sugar or its derivative can bring about the effect of extending the life of the capacitor 10 by suppressing the hydration reaction of the electrode foil of the low-impedance capacitor, suppressing the decomposition and activation of electrolytes such as carboxylic acids by adding sugar or its derivative, and improving the low-temperature characteristics of the electrolytic capacitor 10 (the solvent is a composition close to the antifreeze state, so the impedance change at room temperature and low temperature becomes small).
[0084] (3) Gluconic acid and / or gluconolactone
[0085] The electrolyte solution according to the present embodiment may contain gluconic acid, gluconolactone, etc. alone or in combination as necessary. Such additives are usually preferably added in an amount of 0.01 to 5% by mass.
[0086] (4) Nitro compounds
[0087] The electrolyte solution according to the present embodiment may contain at least one nitro compound selected from the group consisting of nitrophenols such as p-nitrophenol, nitrobenzoic acid such as p-nitrobenzoic acid, dinitrobenzoic acid, nitroacetophenones such as p-nitroacetophenone, nitroanisole, and nitrobenzyl alcohol, as required.
[0088] In the electrolyte of the present embodiment, when two or more nitro compounds are mixed and the above nitro compounds are used, a further preferred effect can be expected. In addition, the nitro compound is preferably added and used in an amount of 0.01 to 5% by mass, based on the total amount of the electrolyte. If the amount of the nitro compound added is less than 0.01% by mass, the desired effect is basically not obtained. On the contrary, even if it is more than 5% by mass, further improvement of the desired effect cannot be expected, and it is also considered that it may have an adverse effect on other characteristics depending on the situation.
[0089] When the use of the nitro compound is further described, when the nitro compound is used alone, the water content in the solvent used gradually increases, and there is a tendency for the absorption effect to decrease. In addition, this tendency to decrease the absorption effect becomes significant when the electrolyte is placed in a high temperature environment. However, the problems caused by the use of such a nitro compound alone can be eliminated by using two or more nitro compounds in combination.
[0090] (5) Polymer compounds
[0091] As the polymer compound, for example, water-soluble silicone, polyacrylic acid or its derivatives, polymethacrylic acid or its derivatives, polyacrylamide or its derivatives, polyglutamic acid or its derivatives, polyglycerol or its derivatives, polyethylene glycol or its derivatives, polypropylene glycol or its derivatives, polyvinyl alcohol or its derivatives, etc. can be used. Such a polymer compound can bring about the effects corresponding to the functions of each polymer compound, such as improvement of the withstand voltage characteristics of the electrolytic capacitor 10 and extension of the life of the electrolytic capacitor 10.
[0092] The molecular weight of the polymer compound can be widely used, ranging from a relatively low molecular weight (oligomer) to a high molecular weight, depending on the function of each polymer compound, solubility / dispersibility in a solvent, or desired effect.
[0093] Furthermore, the electrolyte solution according to the present embodiment may contain additives commonly used in the field of aluminum electrolytic capacitors or other electrolytic capacitors in addition to the above-mentioned additives. Suitable additives include, for example, silane coupling agents, polymer electrolytes, colloidal silica, and the like.
[0094] The separators 24 and 25 of the present embodiment are not particularly limited, but preferably, naturally produced cellulose materials, such as Manila hemp and plant pulp, can be used as raw materials, and the raw pulp is manufactured through dust removal, cleaning, beating, papermaking, etc. In addition, woven fabrics, non-woven fabrics, sheets, films, etc. made of synthetic fibers such as rayon, nylon, polyester, polyvinyl compounds, aramid, propionic acid, and polyurethane can also be used. In addition, mixed products and blended products of natural fibers and synthetic fibers can also be used.
[0095] The outer casing 4 for housing the capacitor element 1 can be made of aluminum that is commonly used in the past. When strength is required, non-heat-treated aluminum with a purity of 99.0% or more (such as non-heat-treated aluminum 1100), heat-treated aluminum with a purity of 99.0% or more (such as H22 material of 1000 series aluminum), tuning materials of aluminum alloys containing manganese (Mn) and (or) magnesium (Mg) (such as O material of aluminum alloy 3003, 22 material of 3000 series aluminum alloy, O material of aluminum alloy 3004), etc. can be used.
[0096] The sealing body 3 used in the electrolytic capacitor 10 in the present embodiment can be formed of a variety of commonly used materials as long as the material has high hardness, moderate rubber elasticity, is impermeable to the electrolyte, and has good airtightness as the sealing body 3. As suitable materials for the sealing body 3, elastic rubbers such as natural rubber (NR), styrene-butadiene rubber (SBR), ethylene-propylene dimer (EPT), and isobutylene-isoprene rubber (IIR) can be cited. In particular, isobutylene-isoprene rubber (IIR) has high airtightness and the electrolyte does not pass through as vapor, so it is suitable. In addition, it is further preferred to use IIR with better heat resistance, such as sulfur vulcanization, quinone vulcanization, resin vulcanization, peroxide vulcanization, etc.
[0097] Furthermore, in order to suppress mechanical stress, there is also a method of using high-hardness rubber. As hardness, a sealing rubber having a rubber hardness measurement (30-second value) of 80 (IRHD / M) or more based on an IRHD hardness tester is used, so that mechanical stress is not easily applied, and the increase in leakage current can be suppressed.
[0098] Furthermore, a composite material of a resin material plate having airtightness and sufficiently high strength (for example, a fluororesin plate such as a PTFE plate) and elastic rubber bonded together may be advantageously used instead of the above-mentioned sealing body 3 material.
[0099] Furthermore, the lead 2 used as an external connection terminal or an external electrode terminal and inserted into the lead through hole of the sealing body 3 can be formed of various metal materials such as iron, copper, tin, lead, silver, gold, zinc, bismuth, tungsten, nickel, titanium, and chromium. For the purpose of reducing the ESR of the capacitor 10, it is advantageous to form the lead 2 from a highly conductive metal material such as copper, silver, iron, and gold, and it is particularly advantageous to form it from a copper wire or a silver wire. It is also effective to further use a chemical conversion lead. By using a chemical conversion lead, not only can the leakage current of the capacitor 10 be reduced, but also the chemical conversion of the lead 2 by phosphoric acid chemical conversion or adipic acid chemical conversion can be performed, so that a material with good chemical conversion properties can be arranged between the lead tab and the electrode foil 20 (23), so that the coating can be repaired in a shorter time, and even when mechanical stress is applied, the increase of the leakage current can be prevented.
[0100] Example
[0101] Next, the present invention will be further described based on examples. The examples listed here illustrate the present invention and are not intended to limit the present invention. It should be noted that "parts" and "%" represent "parts by weight" and "mass %" respectively.
[0102] Example 1
[0103] In this example, a wound aluminum electrolytic capacitor was manufactured according to the following steps.
[0104] The anode foil of the aluminum powder sintered body is produced by the manufacturing method disclosed above (the first step to the third step), and then the electrode lead wire is installed. In addition, another aluminum foil is electrochemically etched to produce a cathode foil, and then the electrode lead wire is installed. Then, a separator (separation paper) is clamped between the anode foil and the cathode foil and wound to produce a capacitor element. On the other hand, based on the composition table shown in Table 1 below, a solvent component and an electrolyte component are added in sequence in a constant container, and then stirred to dissolve and prepare an electrolyte solution.
[0105] After the capacitor element is impregnated with the electrolyte prepared by the above-mentioned preparation method, the electrode lead wires are housed in a bottomed aluminum case so as to protrude outside the case, and the opening of the case is sealed with an elastic sealing body, followed by aging treatment to produce an electrolytic capacitor with a wound structure.
[0106] Comparative Example 1
[0107] In Comparative Example 1, an aluminum foil was electrochemically etched and then anodized to form an oxide film on the surface, which was used as an anode foil. The other methods for preparing an electrolytic capacitor were the same as those described in Example 1.
[0108] In both Example 1 and Comparative Example 1, samples were produced so that the foil withstand voltage became equivalent to 400 WV in terms of capacitor withstand voltage.
[0109] Then, the electrostatic capacitance of the electrolytic capacitors prepared in Example 1 and Comparative Example 1 was measured at 25° C., a frequency of 120 Hz, and 10 kHz, and the measured values described in the following Table 1 were obtained.
[0110] [Table 1]
[0111]
[0112] Comparing the electrostatic capacitance of the capacitors of Example 1 and Comparative Example 1, it is found that the electrostatic capacitance of the capacitors of Example 1 using the anode foil of the sintered aluminum powder is larger than that of Comparative Example 1 using the etched anode foil.
[0113] Embodiments 2 to 12
[0114] Next, for the capacitors made by the same method as in Example 1, the relationship between the resistivity of the electrolyte and the electrostatic capacitance of the capacitor is compared at an average powder particle size of 2.5 μm and 6 μm. The method for making the electrolytic capacitors of Examples 2 to 12 repeats the same method as in Example 1, and in the method for making the electrolyte, the components are made the same as in Example 1, and the composition is adjusted to make resistivities of 100 Ω·cm, 30°C to 2000 Ω·cm, 30°C, respectively. It should be noted that the samples made with an average powder particle size of 2.5 μm have a foil withstand voltage equivalent to 400 WV on a capacitor withstand voltage meter, and the samples made with an average powder particle size of 6 μm have a foil withstand voltage equivalent to 450 WV on a capacitor withstand voltage meter.
[0115] Comparative Examples 2 to 12
[0116] The method for preparing the capacitors of the aluminum etched foil used in Comparative Examples 2 to 12 was the same as that in Comparative Example 1, and the method for preparing the electrolyte was the same as that described in Examples 2 to 12. In the same manner as in Examples 2 to 12, samples with a foil withstand voltage equivalent to 400 WV and a foil withstand voltage equivalent to 450 WV were prepared in the capacitor withstand voltage meter.
[0117] Then, the electrostatic capacitance of the electrolytic capacitors prepared in Examples 1 to 12 and Comparative Examples 1 to 12 was measured at 25° C., a frequency of 120 Hz, and 10 kHz, and the measured values described in the following Tables 2 and 3 were obtained.
[0118] [Table 2]
[0119] Average particle size of aluminum powder sintered body: 2.5 μm
[0120] The capacitor withstand voltage is equivalent to 400WV
[0121]
[0122] [Table 3]
[0123] Average particle size of aluminum powder sintered body: 6μm
[0124] The capacitor withstand voltage is equivalent to 450WV
[0125]
[0126] Tables 2 and 3 show the electrostatic capacitance at 120 Hz and 10 kHz. As a representative use of capacitors, they are used for primary-side smoothing of switching power supplies. In addition to smoothing the input voltage from the commercial power line, they also have the function of absorbing current noise from components such as MOS-FETs that repeatedly switch at a frequency of around 10 kHz in the later stage of the circuit. This noise is called EMI, and it has an adverse effect on other electrical equipment through the commercial power line, so it is subject to regulation according to the EMC Directive (89 / 336 / EEC). In order to help reduce this noise, it is important to increase the electrostatic capacitance around 10 kHz. When the "ratio" of the electrostatic capacitance at 120 Hz and 10 kHz is recorded here, it is compared with the electrostatic capacitance at 10 kHz itself. The electrolytic capacitor using the aluminum powder sintered body foil with a large foil capacitance will naturally become a value larger than the electrolytic capacitor using the etched foil. Therefore, by recording the "ratio", it is usually used to compare the ease of generating the 10 kHz electrostatic capacitance relative to the electrostatic capacitance limited at 120 Hz.
[0127] If the ratio of the electrostatic capacitance at 120Hz and 10kHz recorded in Tables 2 and 3 is observed, when the electrolyte resistivity is 100Ω·cm to 1500Ω·cm, the aluminum powder sintered body foil shows a value higher than the etched foil. At 2000Ω·cm, the powder sintered body foil shows a value lower than the etched foil, but it is believed that this is because the structure of the aluminum powder sintered body foil is formed by the aggregation of particles rather than the tunnel-shaped etching pits seen in the previous etching foil, until the passage deep in the pit is longer, so it becomes difficult to generate capacitance at high frequencies when using a high-resistivity electrolyte. That is, in an aluminum electrolytic capacitor, if the aluminum powder sintered body foil is combined with an electrolyte with a resistivity of less than 1500Ω·cm, it is easier to generate a 10kHz capacity relative to the 120Hz capacity compared to the aluminum etching foil used in the past.
[0128] Embodiment 13, 14
[0129] Next, the correlation between the purity of the aluminum substrate and the life of the capacitor was compared.
[0130] The electrolytic capacitor of Example 13 was produced using an aluminum powder sintered foil having an aluminum purity of 99.99 wt % or more in the base material and an aluminum purity of 99.99 wt % or more in the powder. The capacitor production method otherwise repeated the method described in Example 1.
[0131] In addition, the electrolytic capacitor of Example 14 is produced using an aluminum powder sintered foil whose aluminum purity of the base material is 99.8 wt % or more and less than 99.95 wt % and whose aluminum purity of the powder is 99.99 wt % or more. The capacitor production method otherwise repeats the method described in Example 1.
[0132] Then, the electrolytic capacitors of Examples 13 and 14 were subjected to a high temperature load test at 425 V and 105° C. Figure 3 The leakage current value of the electrolytic capacitor in the high temperature load test is shown. The leakage current of the capacitor of any embodiment is suppressed to less than 12μA, but in particular, in the capacitor with a substrate purity of 99.99% by weight or more (Example 13), there is no tendency for the leakage current to increase after 3000 hours and thereafter, and the increase in leakage current is suppressed. The increase in leakage current leads to an increase in the amount of gas generated inside the capacitor, and the internal pressure rises slowly, which increases the risk of valve operation at an early stage. Therefore, in order to form good life characteristics, it is more preferred that the aluminum purity of the substrate is 99.99% by weight or more. In addition, for the aluminum powder electrically bonded to the substrate, it is also understood that the aluminum purity is preferably 99.99% by weight or more for the same reason.
[0133] In addition, in this specification, "average particle diameter (D50)" refers to the particle diameter at a cumulative value of 50% in a volume-based particle size distribution determined by a laser diffraction / scattering method.
Claims
1. An electrolytic capacitor, characterized in that: A capacitor element and an electrolyte are provided, wherein the capacitor element includes an anode foil, a cathode foil, and a separator interposed between the anode foil and the cathode foil, and the electrolyte is impregnated in the capacitor element. The anode foil or the cathode foil has a sintered body composed of sintered particles containing powder of at least one of aluminum and an aluminum alloy. The aluminum contained in the sintered body has an aluminum purity of 99.8% by weight or more, The resistivity of the electrolyte is less than 1500 Ω·cm, The powder or the sintered particles may have an average particle size D50 of 6 μm or less.
2. The electrolytic capacitor according to claim 1, characterized in that: The anode foil or the cathode foil includes the sintered body and a substrate for supporting the sintered body. The aluminum contained in the sintered body and the substrate has an aluminum purity of 99.99% by weight or more.