Positive pole piece

By adding a decomposable lithium replenishing layer and a ceramic layer to the positive electrode sheet of a lithium-ion battery, the problems of safety and energy density of the lithium-ion battery are solved, and the puncture prevention capability and energy density of the battery are improved.

CN221861692UActive Publication Date: 2024-10-18东莞维科电池有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420115435.X
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-01-17
Publication Date
2024-10-18
Estimated Expiration
2034-01-17

AI Technical Summary

Technical Problem

Lithium-ion batteries are prone to heat, fire or even explosion due to internal abnormal reactions during use, affecting safety, and may reduce energy density when improving safety.

Method used

A cathode plate is designed, including a cathode current collector and a cathode active material layer, on which at least one lithium replenishing layer and a ceramic layer are added. The material in the lithium replenishing layer can decompose delithiation products with poor conductivity. To increase the thickness, a ceramic layer is coated on the outside of the lithium replenishing layer to improve puncture resistance.

Benefits of technology

The lithium-replenishing layer compensates lithium ions to increase the energy density of the battery, and reduces the risk of micro-short circuits through decomposition products, enhances the anti-puncture ability of the battery core, and avoids loss of energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221861692U_ABST
    Figure CN221861692U_ABST
Patent Text Reader

Abstract

The utility model relates to the technical field of energy storage devices, and particularly provides a positive pole piece. The positive electrode comprises a positive electrode current collector and a positive electrode active material layer positioned on the positive electrode current collector, the lithium supplementing layer is located on one side face of the positive electrode current collector in the length direction of the positive electrode current collector; or; the lithium supplementing layer is positioned between one side surface of the positive electrode current collector and the corresponding positive electrode active material layer; lithium ions in the positive electrode active material layer are compensated through the lithium supplementing layer, so that the energy density of the battery is improved. And meanwhile, the lithium supplement material is decomposed into a lithium removal product with relatively poor conductivity, so that the risk of micro short circuit caused by puncture can be reduced, and the anti-puncture capability of the battery cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of energy storage devices, and specifically relates to a positive electrode sheet. Background Art

[0002] Lithium-ion batteries have the advantages of high voltage, small size, light weight, environmental protection and long service life. The above advantages make lithium-ion batteries widely used in portable electronic products. Due to the runaway of lithium-ion batteries (abnormal reactions inside lithium-ion batteries cause them to heat up, and as the temperature continues to rise, more thermal side reactions are triggered, causing lithium-ion batteries to catch fire or even explode, which seriously threatens the safety of users' lives and property), lithium-ion battery safety accidents have occurred frequently in recent years, which has aroused people's attention and discouraged many potential buyers. Therefore, the safety issue of lithium-ion batteries is one of the biggest dilemmas they are currently facing.

[0003] As a result, some research directions have emerged in recent years targeting the safety of lithium-ion batteries, such as improving the thermal stability and flame retardancy of isolation membrane materials and adding safety coatings on electrode assemblies, etc. However, this will also reduce certain aspects of the performance of lithium-ion batteries, such as the energy density of the battery.

[0004] Based on this, it is urgent to invent a positive electrode plate to solve the above-mentioned technical problems. Utility Model Content

[0005] The technical problem to be solved by the utility model is how to avoid the loss of energy density of the battery. In view of the above problem, a positive electrode plate is provided.

[0006] The technical solution of the utility model to solve the above technical problems is to provide a positive electrode plate, including: a positive electrode collector and a positive electrode active material layer located on the positive electrode collector; characterized in that: it also includes at least one lithium replenishing layer, and along the length direction of the positive electrode collector, the lithium replenishing layer is located on one side surface of the positive electrode collector; or; the lithium replenishing layer is located between one side surface of the positive electrode collector and the corresponding positive electrode active material layer.

[0007] Specifically, the lithium supplement material in the lithium supplement layer is a decomposable lithium supplement material, and the lithium supplement material in the lithium supplement layer can decompose lithium desorption products to increase the thickness of the positive electrode plate. Specifically, the lithium supplement layer includes a conductive agent and a binder.

[0008] Specifically, the at least one lithium replenishing layer includes a first lithium replenishing layer and a second lithium replenishing layer respectively coated on both sides of the positive electrode current collector, and the length of the second lithium replenishing layer is greater than the length of the first lithium replenishing layer.

[0009] More specifically, a ceramic layer is also included, and the ceramic layer is coated on the empty foil area outside the lithium supplementing layer.

[0010] Specifically, the ceramic layer includes a conductive agent and a binder.

[0011] Preferably, the conductive agent in the lithium supplement layer and the ceramic layer is selected from one or more of conductive carbon black, graphene, acetylene black and carbon nanotubes.

[0012] Preferably, the binder in the lithium supplement layer and the ceramic layer is selected from one or more of polyethylene oxide, styrene-butadiene rubber, polyacrylate, epoxy resin, and polyvinylidene fluoride.

[0013] In terms of size, the thickness of the lithium replenishing layer is 0.3 μm to 30 μm.

[0014] In terms of size, the thickness of the ceramic layer is 0.3 μm to 30 μm.

[0015] The beneficial effect of the utility model is that the lithium ions in the positive electrode active material layer are compensated by the lithium supplement layer, thereby improving the energy density of the battery. At the same time, the lithium supplement material decomposes the lithium decomposition product with poor conductivity, which can reduce the risk of micro short circuit caused by puncture, thereby improving the anti-puncture ability of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions in the implementation modes of the present invention, the drawings required for use in the description of the implementation modes will be briefly introduced below. Obviously, the drawings described below are only some implementation modes of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 It is a structural schematic diagram of the positive electrode sheet of the utility model.

[0018] Reference numerals:

[0019] 1- positive electrode;

[0020] 10 - positive electrode current collector; 11 - lithium replenishing layer; 110 - first lithium replenishing layer; 111 - second lithium replenishing layer; 12 - ceramic layer. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the implementation of the utility model clearer, the technical solution in the implementation of the utility model will be clearly and completely described below in conjunction with the drawings in the implementation of the utility model. Obviously, the described implementation is a part of the implementation of the utility model, not all of the implementations. Based on the implementation of the utility model, all other implementations obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.

[0022] According to the current market development trend, power batteries (here refers to lithium batteries) are being used more and more widely. Power batteries are not only used in energy storage systems such as hydropower, thermal power, wind power and solar power stations, but also in electric vehicles such as electric bicycles, electric motorcycles and electric cars, as well as in military equipment and aerospace and other fields. Figure 1 As shown, the utility model provides a positive electrode plate 1, which is applied to a wound lithium battery. In other specific embodiments, the positive electrode plate 1 can also have other usage scenarios, which are not specifically limited here.

[0023] Implementation Method 1

[0024] like Figure 1 As shown, the positive electrode plate 1 includes a positive electrode collector 10 and a positive electrode active material layer located on the positive electrode collector 10, wherein the positive electrode active material layer is coated on both side surfaces of the positive electrode collector 10. In order to improve the energy density of the battery, specifically, in order to offset the irreversible lithium loss caused by the formation of a solid electrolyte interface film (SEI film) to the battery, that is, to maintain the total capacity and energy density of the battery, the positive electrode plate 1 also includes at least one lithium replenishment layer 11. Among them, along the length direction of the positive electrode collector 10, the lithium replenishment layer 11 is located on one side of the positive electrode collector 10, where one side here refers to any one of the two side surfaces of the positive electrode collector 10; or, the lithium replenishment layer 11 is located between one side of the positive electrode collector 10 and the corresponding positive electrode active material layer. It should be noted that in this specific embodiment, the lithium replenishment layer 11 is located on one side of the positive electrode collector 10. In other specific embodiments, the position of the lithium replenishment layer 11 is not limited.

[0025] Implementation Method 2

[0026] The difference between this embodiment and embodiment 1 is that in order to improve the anti-puncture function of the battery, specifically, by increasing the thickness of the positive electrode plate 1 to improve the anti-puncture function of the battery, the lithium supplement material in the lithium supplement layer 11 is a decomposable lithium supplement material, and the lithium supplement material in the lithium supplement layer 11 can decompose a lithium-depleted product with poor conductivity, which can reduce the risk of micro-short circuit caused by puncture, thereby improving the anti-puncture ability of the battery cell. It should be noted that the hardness of the lithium-depleted product is equivalent to the hardness of the ceramic layer 12 (see below for details), that is, the lithium-depleted product can reduce the risk of micro-short circuit in the battery caused by burrs piercing the plate. Among them, the lithium replenishing layer 11 is formed by coating the lithium replenishing material with a coating layer. Specifically, the material of the coating layer is selected from at least one of LiF, CaF2, AlF3, MgO, ZnO, CaO and Al2O3, and the lithium replenishing material is selected from one or more of Li5FeO4, Li2C2O4, Li6CoO4, Li2MoO3, Li2NiO2, Li2O, Li2O2, Co / LiO2, Co / LiF and Fe / LiF / LiO2.

[0027] In the charging and discharging process of lithium batteries, lithium ions and electrons need to participate together, which requires that the material of the electrode assembly of the lithium-ion battery must contain a mixed conductor of lithium ions and electrons, and the electrode reaction can only occur at the junction of the electrolyte, the conductive agent and the active material. Since the positive electrode active material usually uses transition metal oxides or transition metal phosphates, which are semiconductors or insulators with poor conductivity, a conductive agent must be added to improve the conductivity of the positive electrode active material. Therefore, in order to avoid affecting the flow direction of the current in the positive electrode plate 1 (if the lithium replenishment layer 11 does not contain a conductive agent, the current in the positive electrode plate 1 will bypass the lithium replenishment layer 11; in other words, the flow direction of the current in the positive electrode plate 1 is deflected), the lithium replenishment layer 11 includes a conductive agent and a binder. And the other parts of this embodiment are the same as embodiment 1, and will not be repeated here.

[0028] Implementation 3

[0029] The difference between this embodiment and embodiment 1 is that in order to prevent the battery energy density loss caused by the increase in the thickness of the electrode sheet (including the positive electrode sheet 1 and the negative electrode sheet), in this specific embodiment, the number of lithium replenishment layers 11 is two. For the convenience of description and understanding, the two lithium replenishment layers 11 are named as the first lithium replenishment layer 110 and the second lithium replenishment layer 111, and the first lithium replenishment layer 110 and the second lithium replenishment layer 111 are coated on the two side surfaces of the positive electrode current collector 10. Since one of the batteries including the positive electrode sheet 1 ends with the positive electrode sheet 1 during the winding process, that is, continue to refer to Figure 1The second lithium replenishing layer 111 exceeds the first lithium replenishing layer 110 and has no corresponding negative electrode sheet, so the length of the second lithium replenishing layer 111 is greater than the length of the first lithium replenishing layer 110. The other parts of this embodiment are the same as those of Embodiment 1 and will not be described here.

[0030] Implementation 4

[0031] The difference between this embodiment and embodiment 3 is that: in order to prevent lithium ions from precipitating in the aforementioned area, the positive electrode plate 1 further includes a ceramic layer 12, and the ceramic layer 12 is coated on the empty foil area outside the lithium supplement layer. Referring to the above, the ceramic layer 12 also includes a conductive agent and a binder. The other parts of this embodiment are the same as those of embodiment 3, and are not described here.

[0032] Implementation method 5

[0033] The difference between this embodiment and embodiment 3 and / or embodiment 4 is that: in order to ensure the conductivity of the aforementioned conductive agent, preferably, the conductive agent in the lithium supplement layer 11 and the ceramic layer 12 can be selected from one or more of conductive carbon black, graphene, acetylene black, and carbon nanotubes. Of course, in other specific embodiments, the material of the aforementioned conductive agent can also be other. And the other parts of this embodiment are the same as embodiment 3 and / or embodiment 4, and will not be repeated here.

[0034] Implementation 6

[0035] The difference between this embodiment and embodiment 3 and / or embodiment 4 is that: in order to ensure the bonding performance of the aforementioned binder, preferably, the binder in the lithium supplement layer 11 and the ceramic layer 12 can be selected from one or more of polyethylene oxide, styrene-butadiene rubber, polyacrylate, epoxy resin, and polyvinylidene fluoride. Of course, in other specific embodiments, the material of the aforementioned binder can also be other. And the other parts of this embodiment are the same as those of embodiment 3 and / or embodiment 4, and will not be repeated here.

[0036] Implementation 7

[0037] The difference between this embodiment and embodiment 3 is that in order to ensure the lithium replenishment effect through the lithium replenishment layer 11, preferably, the thickness of the lithium replenishment layer 11 can be 0.3 μm to 30 μm. The other parts of this embodiment are the same as those of embodiment 4 and will not be described here.

[0038] Implementation 8

[0039] The difference between this embodiment and the above embodiment is that in order to ensure the hardness of the ceramic layer 12, or in other words, to ensure the anti-puncture performance of the positive electrode plate 1, preferably, the thickness of the ceramic layer 12 is 0.3 μm to 30 μm. The other parts of this embodiment are the same as the above embodiment and will not be described here.

[0040] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be obvious to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features applied herein.

Claims

1. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode active material layer located on the positive electrode current collector; characterized in that: It also includes at least one lithium replenishing layer, and along the length direction of the positive electrode current collector, the lithium replenishing layer is located on one side of the positive electrode current collector; or; the lithium replenishing layer is located between one side of the positive electrode current collector and the corresponding positive electrode active material layer.

2. The positive electrode sheet according to claim 1, characterized in that: The lithium-supplementing material in the lithium-supplementing layer is a decomposable lithium-supplementing material, and the lithium-supplementing material in the lithium-supplementing layer can decompose lithium-removing products to increase the thickness of the positive electrode plate.

3. The positive electrode sheet according to claim 1, characterized in that: The lithium supplement layer includes a conductive agent and a binder.

4. The positive electrode sheet according to claim 1, characterized in that: The lithium replenishing layer comprises a first lithium replenishing layer and a second lithium replenishing layer respectively coated on both sides of the positive electrode current collector, and the length of the second lithium replenishing layer is greater than the length of the first lithium replenishing layer.

5. The positive electrode sheet according to claim 1, characterized in that: A ceramic layer is also included, and the ceramic layer is coated on the empty foil area outside the lithium supplementing layer.

6. The positive electrode sheet according to claim 5, characterized in that: The ceramic layer includes a conductive agent and a binder.

7. The positive electrode sheet according to claim 1, characterized in that: The thickness of the lithium supplement layer is 0.3 μm to 30 μm.

8. The positive electrode sheet according to claim 5, characterized in that: The thickness of the ceramic layer is 0.3 μm to 30 μm.