Preparation device for producing silicon-carbon negative electrode material of lithium battery by utilizing two-stage reactor method
The two-stage reactor method is used to prepare nano-silicon particles and coat them with online carbon, which solves the problems of expansion of silicon-carbon negative electrode materials and electrolyte consumption in lithium-ion batteries, achieves efficient and low-cost nano-material preparation, and improves battery cycle Stability and charge and discharge performance.
Patent Information
- Application Number
- CN202420177612.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2034-01-25
AI Technical Summary
It is difficult to effectively prepare high-purity, stable nano-silicon particles and achieve effective carbon coating in silicon-carbon negative electrode materials with existing technology, resulting in problems of expansion, pulverization and electrolyte consumption in lithium-ion batteries during the charge and discharge process. , affecting the cycle stability and capacity fading of the battery.
Using a two-stage reactor method, nanoscale silicon particles are generated through the first-stage reaction, and carbon coating is performed online in the second-stage reaction to form a protective layer. Combined with a vacuum system and a condensation device, the nanoparticles are efficiently prepared and integrated.
It achieves control of the diameter of nano-silicon particles between 50-800 nm, improves the charge and discharge efficiency and battery cycle stability of silicon anode materials, reduces preparation costs, and improves the purity and stability of nano-particles.
Smart Images

Figure CN221894724U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of nano material preparation, in particular to a preparation device for producing lithium battery silicon-carbon negative electrode materials by a two-stage reactor method. Background Art
[0002] In recent years, the preparation and performance research of nanoparticles has attracted widespread attention. Nanoparticles have the characteristics of small size effect, surface effect, quantum size effect and macro quantum tunneling effect, and show optical, electrical, thermal, magnetic and mechanical properties that are different from traditional materials. Therefore, they have important applications in many fields such as chemical engineering, materials, electronics, machinery, environmental protection and biomedical engineering.
[0003] Currently, the main methods for preparing nanoparticles include sol-gel method, electrochemistry, chemical precipitation method, pyrolysis method, ion implantation method, plasma method, self-assembly, template method, etc.
[0004] The sol-gel method can produce a large amount of nanopowders at a low cost, but it is very easy to agglomerate, which affects the actual application effect.
[0005] The purity, morphology and size of nanoparticles prepared by chemical precipitation are difficult to control. Template method can obtain large-area nanoparticle arrays, but the process is relatively cumbersome, especially the removal of templates is difficult. Ion implantation, pyrolysis, plasma, electrochemical and other methods require relatively complex experimental equipment and process procedures or high temperatures, which increase the preparation cost of nanoparticles. At the same time, due to their respective limitations, the practical application of nanoparticles is affected. Therefore, a simple and controllable method must be studied to obtain nanoparticles with high purity, good stability, and controllable morphology and size distribution, and to reduce the preparation cost and avoid the agglomeration of nanoparticles.
[0006] Silicon-carbon negative electrode materials are mainly used to replace the graphite negative electrode of traditional lithium-ion batteries, so that the energy density of the battery can break through the bottleneck of the graphite negative electrode and the performance can be greatly improved. Silicon-based negative electrode materials are considered to be the next generation of high energy density lithium-ion battery negative electrode materials with great potential due to their high theoretical specific capacity (4200mA·h / g at high temperature and 3580mA·h / g at room temperature), low delithiation potential (<0.5V), environmental friendliness, abundant reserves, and low cost. Silicon-based negative electrode materials need to solve the performance requirements of small silicon particle size and good dispersion, which can solve two important key problems in the process of large-scale use:
[0007] ① The silicon material repeatedly expands and contracts during the process of lithium insertion and extraction, causing the negative electrode material to pulverize and fall off, and eventually causing the negative electrode material to lose electrical contact and cause the battery to fail completely;
[0008] ② The continuous growth of SEI film on the surface of silicon material will continue to irreversibly consume the limited electrolyte in the battery and lithium from the positive electrode, eventually leading to rapid decay of battery capacity.
[0009] To solve the above two problems, first, it is necessary to synthesize nano-scale silicon particles, such as those with a size less than 150nm, which can effectively inhibit the expansion of the material and reduce the problem of crushing during repeated charge and discharge, thereby greatly extending the cycle stability of the battery. Although the high-energy ball milling method can obtain nanomaterials with a size of about 100nm, it consumes a lot of energy and the particles have serious agglomeration, which brings many problems to subsequent processing, and it is impossible to obtain particles with a size of less than 50nm;
[0010] Second, the synthesized silicon nanomaterials need to form an effective carbon coating on the surface to protect the silicon particles from direct contact and reaction with the electrolyte, while providing carbon materials with better conductive properties.
[0011] The utility model provides a preparation method for producing lithium battery silicon-carbon negative electrode materials using a two-stage reactor method, which can produce silicon particles of several nanometers to hundreds of nanometers, and can realize online in-situ carbon coating. Before the silicon particles leave the reaction area, they react with the introduced carbon precursor on the surface to generate a carbon protective layer, thereby effectively protecting the silicon surface, thereby improving the first coulomb efficiency of the silicon negative electrode material during charging and discharging. Utility Model Content
[0012] The purpose of the utility model is to provide a preparation device for producing lithium battery silicon-carbon negative electrode materials using a two-stage reactor method to solve the problems raised in the above background technology.
[0013] In order to solve the above technical problems, the utility model provides the following technical solutions:
[0014] A preparation device for producing lithium battery silicon-carbon negative electrode materials using a two-stage reactor method, comprising a reaction chamber, wherein a first reaction device and a second reaction device are installed in the reaction chamber according to a reaction sequence, and a coating nozzle is installed on the side of the reaction chamber channel, and the coating nozzle extends to the interior of the second reaction device;
[0015] The tail of the reaction chamber channel is connected to a collection chamber, a condensing device with an inclined angle is installed inside the collection chamber, a particle filtering system is installed below the condensing device, and the particle filtering system is connected to a vacuum system, a finished product collecting vessel is provided at the tail of the collection chamber to collect finished products, and a butterfly valve is installed between the collection chamber and the finished product collecting vessel.
[0016] Preferably, the first reaction equipment and the second reaction equipment are one or a combination of an RTP reactor, a plasma reactor, a microwave and an intermediate frequency reaction device.
[0017] Preferably, the coating nozzle comprises a nozzle tube body, and the outer surface of the nozzle tube body extending to the position of the second reaction device is provided with a plurality of fine diffusion holes.
[0018] Preferably, the condensation device includes a condensation plate with condensation water injected inside, and a cleaning scraper driven to reciprocate by a force is provided on the condensation plate. The condensation plate is in an inverted V shape to divide the top channel of the collection chamber, and the bottom of the diffusion hole is in contact with the outer surface of the nozzle tube body.
[0019] A method for preparing a lithium battery silicon-carbon negative electrode material using a two-stage reactor method comprises the following steps:
[0020] S1, introducing the gaseous precursor of nanoparticles into the first-stage reaction area, and controlling the internal temperature to 800°-1000°, the precursor is rapidly cracked into nano-sized particles under CVD reaction conditions;
[0021] S2, the particles generated in the first stage reaction area enter the second stage reaction chamber, and the internal temperature of the second stage reaction chamber is controlled to be 800°-1000°;
[0022] S3, spraying a carbon-containing precursor into the second-stage reaction chamber through a carbon precursor nozzle, so that the precursor and the first-stage particles are mixed, and then heated and cracked into high-energy particles by the second CVD reactor, and deposited on the surface of the silicon particles to form a film structure, thereby obtaining active nanoparticles coated with surface carbon;
[0023] S4, active nanoparticles are temporarily collected in a collector;
[0024] S5. Finally, the active nanoparticles in the collector are discharged through a butterfly valve and stored for future use.
[0025] Preferably, the gaseous precursor is a gaseous or liquid organic compound containing the desired nanoparticles, and the organic compound can be cracked under CVD reaction conditions.
[0026] Preferably, the first-stage and second-stage reactors are one or a combination of RTP reactors, plasma reactors, microwave and medium frequency reaction devices.
[0027] Preferably, when the gaseous precursor is introduced, a protective gas and a sensitizing gas should also be introduced.
[0028] Preferably, the protective gas is one of N2, He, Ar or H2 or a mixture thereof, which confines the reaction gas near the center of the reaction chamber to prevent it from accumulating in other corners of the reactor.
[0029] Preferably, the pressure in the reaction chamber is less than 700 torr.
[0030] Compared with the prior art, the beneficial effects achieved by the utility model are:
[0031] First, the utility model sets a first reaction device and a second reaction device. When preparing nanomaterials, the gaseous precursor of nanoparticles is introduced into the first-stage reaction area, and the precursor is quickly cracked into small nanoparticles under CVD reaction conditions, and is heated and cracked into high-energy particles in the second CVD reactor, so that the diameter of the prepared nanoparticles is in the range of 50-800nm, thereby achieving the purpose of nanomaterials less than 100nm.
[0032] Second, the two-stage nanomaterial synthesis device of the utility model can realize online in-situ carbon coating by spraying coating material into the interior of the second reaction device through the coating nozzle during the process of the material entering the second reaction device. Before the silicon particles leave the reaction area, they react with the introduced carbon precursor on the surface to generate a carbon protective layer, thereby effectively protecting the silicon surface, thereby improving the first coulomb efficiency of the silicon negative electrode material during charging and discharging;
[0033] Second, due to the low vacuum requirement during the preparation process, the production cost is greatly reduced, and the equipment is simple, the process stability is good, the prepared nanoparticles have high purity, good stability, uniform morphology and particle size, and high product quality reliability. At the same time, a higher nanoparticle yield can be obtained. The two-stage precursor injection device can perform surface carbon coating in situ after the nano-scale particles are obtained, thereby achieving the effect of reducing the preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic diagram of the structure of the utility model;
[0035] Figure 2 This is a schematic diagram of the structure of the coating nozzle of the utility model;
[0036] Figure 3 This is a schematic diagram of the structure of the condensing device of the utility model;
[0037] Figure 4 This is a scanning electron microscope photo of the silicon-carbon negative electrode material of the utility model;
[0038] Figure 5 This is a photo of the XRD diffraction spectrum of the silicon-carbon negative electrode material of the utility model;
[0039] Figure 6 This is a charge and discharge diagram of the silicon-carbon negative electrode material of the utility model;
[0040] Figure 7 This is the charge and discharge diagram of commercial graphite anode material.
[0041] Among them: 1. reaction chamber channel; 2. first reaction equipment; 3. second reaction equipment; 4. coated nozzle; 401. nozzle tube body; 402. diffusion hole; 5. collection chamber; 6. condensation device; 601. condensation plate; 602. cleaning scraper; 7. particle filtration system; 8. finished product collection container; 9. butterfly valve. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the utility model to clearly and completely describe the technical solutions in the embodiments of the utility model. Obviously, the described embodiments are only part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments in the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model. Specific implementation method 1
[0044] This embodiment is an embodiment of a method for producing a lithium battery silicon-carbon negative electrode material using a two-stage reactor method.
[0045] A two-stage method for preparing nanoparticles, wherein the gaseous precursor of the nanoparticles is introduced into the first-stage reaction area, and the precursor is rapidly cracked into nano-sized particles under CVD reaction conditions. The particles generated in the first-stage reaction area then enter the second-stage reaction chamber; there is a carbon precursor nozzle in the second-stage reaction chamber, and after the precursor and the first-stage particles are mixed, they are heated and cracked into high-energy particles by the second CVD reactor, and a film-like structure is deposited on the surface of the silicon particles to obtain active nanoparticles coated with surface carbon. The nanoparticles are collected by a collector.
[0046] The gaseous precursor is a gaseous or liquid organic compound containing the desired nanoparticles, which can be cracked under CVD reaction conditions. Generally speaking, any compound that can be used for MOCVD can be used as a precursor of this method.
[0047] The temperature in the reaction chamber is controlled by adjusting the RTP thermal power, and the temperature is controlled at 800°-1000°.
[0048] The first-stage and second-stage reactors can be RTP reactors, or plasma reactors such as ICP plasma devices, microwave and medium frequency reaction devices, etc.
[0049] In addition, while introducing the gaseous precursor, various gases such as protective gas and sensitizing gas should also be introduced. The protective gas is preferably N2 (ultra-passive grade), and can also be He, Ar or H2, or a mixture thereof; He and H2 confine the reaction gas near the center of the reaction chamber to prevent it from accumulating in other corners of the reactor. H2 can also increase the temperature of particle nucleation and prevent particle agglomeration.
[0050] Wherein, the pressure in the reaction chamber is less than 700torr;
[0051] The prepared active nanoparticles are temporarily collected in the collector, and at the same time, the active nanoparticles in the collector are discharged through the butterfly valve 9 for final storage for use.
[0052] The preparation of silicon nanoparticles is taken as an example to illustrate the method for preparing nanoparticles of the present invention.
[0053] Silicon nanoparticles are prepared from organic precursors of silicon, such as silane, for example but not limited to: SiH4, Si2H6, Si3H8, etc.; chlorosilane, such as SiH2Cl2, SiHCl3, SiCl4, Si2Cl6, etc. Carbon precursors are made from carbon-containing gas precursors, such as CH4; ethylene, acetylene, propane, propylene, etc.
[0054] The organic precursor gas of silicon enters the first stage reaction chamber through the gas introduction device, and generates nanoparticles after cracking reaction, and then enters the second stage reactor, and mixes with the carbon precursor sprayed from the nozzle, and enters the reaction area. In the first stage reaction chamber, the organic silicon is heated by the RTP furnace to crack and generate silicon nanoparticles;
[0055] In the second stage reaction chamber, the carbon precursor is heated by the second stage RTP furnace, and the carbon precursor is cracked and deposited on the surface of the silicon nanoparticles to form a carbon coating film. The carbon-coated silicon particles are collected by the collection device under the reaction chamber. The pressure in the reaction chamber is less than 700torr, and the diameter of the prepared silicon nanoparticles is about 50-800nm. Specific implementation method 2
[0057] This embodiment is an embodiment of a device for realizing a method for preparing silicon-carbon negative electrode materials for lithium batteries using a two-stage reactor method.
[0058] See also Figure 1-7 , a device for realizing a method for preparing a lithium battery silicon-carbon negative electrode material by a two-stage reactor method, comprising a reaction chamber channel 1, the reaction chamber channel 1 being a circular channel, a first reaction device 2 and a second reaction device 3 being installed on the reaction chamber 1 in accordance with a reaction sequence, the first reaction device 2 and the second reaction device 3 being one or a combination of an RTP reactor, a plasma reactor, a microwave and an intermediate frequency reaction device, a coating nozzle 4 being installed on the side of the reaction chamber channel 1, and the coating nozzle 4 extending to the interior of the second reaction device 3;
[0059] The tail of the reaction chamber channel 1 is connected with a collecting chamber 5, and a condensing device 6 with an inclined angle is installed inside the collecting chamber 5 for cooling particles and gas. A particle filtering system 7 is installed below the condensing device 6. The particle filtering system 7 is a circular bag collector. In the process of vacuuming the inside of the collecting chamber 5, the particles carried by the gas adhere to the outer surface of the particle filtering system 7. A rotatable brush is provided on the surface of the particle filtering system 7 for brushing the sediment attached to the surface of the bag collector to the inner bottom of the collecting chamber 5. A finished product collecting vessel 8 is provided at the tail of the collecting chamber 5 to collect the finished product, and a butterfly valve 9 is installed between the collecting chamber 5 and the finished product collecting vessel 8;
[0060] All air inlet and outlet pipe openings are equipped with individually controlled valves for on-off control.
[0061] The main principle of traditional CVD pyrolysis is to use the reactants to rapidly heat up under CVD conditions to decompose them into tiny particles, and quickly leave the reaction zone to obtain nanoparticles. However, the pyrolysis method has the disadvantages of serious agglomeration of the generated particles due to high reaction temperature and long reaction time. At the same time, the generated particles generally need to be further carbon-coated offline, and in-situ coating treatment cannot be performed. In the subsequent offline treatment process, surface protection at the single particle level cannot be formed, and coating protection is usually formed on the surface of the agglomerate, which cannot give full play to the advantages of nanomaterials. This device uses a two-stage reaction to crack the material into high-energy particles to prepare small-particle nanomaterials. Due to the low vacuum requirement during the preparation process, the equipment cost is greatly reduced, and the equipment is simple, the process stability is good, the prepared nanoparticles have high purity, good stability, uniform morphology and particle size, and high product quality reliability. At the same time, a higher nanoparticle yield can be obtained. The two-stage precursor injection device can perform surface carbon coating in situ after the nano-scale particles are obtained, achieving the effect of reducing the preparation cost.
[0062] Through the above technical scheme, a first reaction device 2 and a second reaction device 3 are set up. When preparing nanomaterials, the gaseous precursor of the nanoparticles is introduced into the first-stage reaction area. The precursor is quickly cracked into nanoscale small particles under CVD reaction conditions. In the process of the material entering the second reaction device 3, the coating material is sprayed into the interior of the second reaction device 3 through the coating nozzle 4, so that online in-situ carbon coating can be achieved. Before the silicon particles leave the reaction area, they react with the introduced carbon precursor on the surface to generate a carbon protective layer, thereby effectively protecting the silicon surface, thereby improving the first coulomb efficiency of the silicon negative electrode material during charging and discharging.
[0063] Specifically, the coating nozzle 4 includes a nozzle body 401 for transmitting the carbon precursor mixture. The outer surface of the nozzle body 401 extending to the position of the second reaction device 3 is provided with a plurality of small diffusion holes 402. The carbon precursor mixture diffuses rapidly over a large area inside the second reaction device 3 through the small diffusion holes 402. The carbon precursor is cracked under the action of the high temperature inside the second reaction device 3 and is deposited on the surface of the silicon nanoparticles to form a carbon coating film.
[0064] Specifically, the condensation device 6 includes a condensation plate 601 with condensed water injected inside. Under the action of the condensation plate 601, the particles are cooled and settled on the surface of the condensation plate 601 or fall to the bottom of the collection chamber 5 through the gap around the condensation plate 601. The condensation plate 601 is provided with a cleaning scraper 602 driven to reciprocate by a force. The cleaning scraper 602 is used to scrape the particles accumulated on the surface of the condensation plate 601 to the inner bottom of the collection chamber 5. The condensation plate 601 is an inverted V-shape, which divides the top channel of the collection chamber 5, reduces the direct adhesion of particles to the surface of the circular bag collector of the particle filtration system 7, and ensures the stability of the vacuum. The bottom of the diffusion hole 402 fits with the outer surface of the nozzle tube body 401.
[0065] The nanomaterials prepared by this device were observed using a transmission electron microscope to observe the microscopic morphology of the materials. It was found that the particle size of the material was about 10nm, the particle size distribution was uniform, the particles were spherical, and had good dispersion properties.
[0066] The XRD diffraction pattern 5 obtained by using an X-ray diffraction analyzer (D8ADVANCE model) shows that an obvious silicon diffraction front can be found through the pattern, which has good crystallinity.
[0067] The carbon content of the silicon-carbon material was analyzed using a carbon-sulfur analyzer, and the test data are shown in Table 1.
[0068] The first coulomb efficiency test. Silicon-carbon negative electrode material powder: SP (carbon black): CNT (carbon nanotube): PAA (polyacrylic acid) were mixed in a mass ratio of 80:9:1:10, and an appropriate amount of deionized water was added as a solvent. The mixture was stirred continuously with a magnetic stirrer until it became a paste. The stirred slurry was poured onto a copper foil with a thickness of 8 μm, coated with an experimental coating machine, and dried at 90 °C under vacuum for 3 h to obtain a negative electrode sheet. The electrode sheet was rolled to 150 μm on a manual roller machine, and then a circular electrode sheet with a diameter of 14 mm was obtained with a punching machine, and the weight of the active material was weighed and calculated. CR2032 button cells were assembled in a glove box, with a metal lithium sheet as the counter electrode, a polypropylene microporous membrane as the diaphragm, and a 1 mol LiPF6 solution (solvent is ethylene carbonate (EC) / dimethyl carbonate (DMC), volume ratio 1:1) as the electrolyte to form a button cell.
[0069] The LAND battery test system was used for constant current charge and discharge tests. The discharge cut-off voltage was 0.005V, the charge cut-off voltage was 1.5V, and the charge and discharge tests were performed at a current of 0.1C.
[0070] A commercial graphite negative electrode was used as comparative example 1. The test results of each embodiment are shown in Table 1.
[0071]
[0072] Table 1
[0073] From Table 1, it can be found that the silicon-carbon material has a charge capacity of 2600-2800mAh / g, which is equivalent to 8 times the charge capacity of 345.2mAh / g of the traditional graphite negative electrode material, and has a significant capacity advantage. As the carbon content of the silicon-carbon material increases, the specific capacity of the material will decrease, which is mainly due to the low capacity of carbon. As the carbon content increases, the silicon-carbon capacity will decrease. Among them, the first coulomb efficiency of the silicon-carbon material increased from 81.2% to 86.7%. Compared with the first coulomb efficiency of 92.0% of the traditional graphite negative electrode material, there is still a gap of 5%. At the same time, for silicon-carbon materials with high carbon content, high carbon content means that the coating will be comprehensive, which helps to reduce the surface activity of the silicon material, thereby improving the first coulomb efficiency. By comparing the parameters such as carbon content, charge capacity and first coulomb efficiency of Example 1 and Example 2 with the commercial graphite negative electrode comparative example 1, it is obvious that the preparation of materials with different carbon contents can be achieved in the silicon-carbon negative electrode material prepared by the two-stage reactor, and the charge capacity of the material is significantly improved.
[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A preparation device for producing lithium battery silicon-carbon negative electrode materials using a two-stage reactor method, characterized in that: The invention comprises a reaction chamber channel (1), wherein a first reaction device (2) and a second reaction device (3) are installed on the reaction chamber channel (1) in accordance with a reaction sequence, and a coating nozzle (4) is installed on the side of the reaction chamber channel (1), wherein the coating nozzle (4) extends into the interior of the second reaction device (3); The tail of the reaction chamber channel (1) is connected to a collecting chamber (5), a condensing device (6) with an inclined angle is installed inside the collecting chamber (5), a particle filtering system (7) is installed below the condensing device (6), and the particle filtering system is connected to a vacuum system, a finished product collecting vessel (8) is arranged at the tail of the collecting chamber (5) to collect finished products, and a butterfly valve (9) is installed between the collecting chamber (5) and the finished product collecting vessel (8); The coating nozzle (4) comprises a nozzle tube body (401), and the outer surface of the nozzle tube body (401) extending to the position of the second reaction device (3) is provided with a plurality of fine diffusion holes (402); The condensation device (6) includes a condensation plate (601) filled with condensed water, and a cleaning scraper (602) driven to reciprocate by a force is arranged on the condensation plate (601). The condensation plate (601) is in an inverted V shape and divides the top channel of the collection chamber (5). The bottom of the diffusion hole (402) is in contact with the outer surface of the nozzle tube body (401).
2. The preparation device for producing lithium battery silicon-carbon negative electrode materials using a two-stage reactor method according to claim 1, characterized in that: The first reaction device (2) and the second reaction device (3) are one or a combination of an RTP reactor, a plasma reactor, a microwave and an intermediate frequency reaction device.
Citation Information
Cited By
Preparation method and device for producing silicon-carbon negative electrode material of lithium battery by utilizing two-stage reactor method