Method for measuring an extremely low oxygen concentration in a silicon wafer
By forming uniform films on silicon wafers and using FT-IR to subtract native oxide interference, the method addresses the challenge of measuring low oxygen concentrations, achieving sensitive and efficient detection comparable to SIMS.
Patent Information
- Application Number
- DE112019006252
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-17
- Filing Date
- 2019-12-04
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2039-12-04
AI Technical Summary
Existing methods like FT-IR, SIMS, and radioactivation analysis struggle to accurately measure extremely low oxygen concentrations (less than 1 × 10^16 atoms/cm^3) in silicon wafers due to interference from native oxide absorption, requiring large facilities and limited sample throughput.
Forming uniform SiO2, nitride, or polyethylene films on measurement, reference, and standard wafers, then using FT-IR to measure and subtract native oxide interference, allowing precise calculation of interstitial oxygen concentration based on standard wafer peaks.
Enables sensitive and easy measurement of extremely low oxygen concentrations, improving detection limits comparable to SIMS using FT-IR, without the need for large facilities.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] This invention relates to a method for measuring the interstitial oxygen concentration in a silicon wafer. BACKGROUND
[0002] Fourier transform infrared spectroscopy (FT-IR), secondary ion mass spectrometry (SIMS), and radioactivation analysis are conventionally used to measure oxygen concentration. Among these analytical techniques, radioactivation analysis is used to determine a range of 10 14 atoms / cm 3 available, and SIMS has a detection limit of 5 × 10 15 atoms / cm 3 . The FT-IR measurement is only available when the concentration is approximately 10 16 atoms / cm 3 FT-IR is no better than other methods because it requires a concentration of no less than 10 16 atoms / cm 3However, it is widely used to measure oxygen concentrations of not less than 1 × 10 16 atoms / cm 3 used because of its light and easy use.
[0003] In the conventional method of measuring oxygen concentration, FT-IR was considered not suitable for measuring oxygen concentration because the concentration of less than 1 × 10 16 atoms / cm 3 , i.e. a range of 10 15 atoms / cm 3is too low. However, techniques such as SIMS and radioactivation analysis require larger facilities than FT-IR, so consequently, few laboratories can meet this need. Another problem is that the number of samples that can be measured per hour is 1 / 10 to 1 / 100 of that using FT-IR. Therefore, there is a growing need for measuring oxygen concentration in silicon wafers with lower oxygen concentrations using FT-IR.
[0004] In the method for measuring the interstitial oxygen concentration in silicon wafers using FT-IR as described in NPL 1, the infrared absorption spectrum of a measurement wafer and that of a reference wafer (ie, a wafer containing no interstitial oxygen or having an extremely low interstitial oxygen concentration in a single-crystal silicon) are measured, and then the interstitial oxygen concentration in the measurement wafer is obtained.
[0005] When the absorption spectra of a silicon wafer with a low oxygen concentration are measured using FT-IR, a large reverse absorption of a convex downward shape is observed on the lower wavenumber side (1050 cm -1 ) than the infrared absorption due to the interstitial oxygen ( Fig. 1). This reverse absorption is attributed to native oxide adhering to an oxygen-free single-crystal silicon wafer (i.e., a wafer that contains no interstitial oxygen or has an extremely low interstitial oxygen concentration in single-crystal silicon) used as a reference. Due to the presence of the reverse absorption of the convex downward shape, a baseline around the interstitial oxygen is not straight but curved. As the absorption due to the interstitial oxygen becomes larger, the amount of absorption corresponding to the interstitial oxygen can be quantified using the baseline interpolation method described in PTL 1. As described in Fig. However, as shown in Figure 1, due to the interstitial oxygen in the silicon wafer with a low oxygen concentration, the infrared absorption is so low that the absorption amount is extremely difficult to quantify. If native oxides are removed to make the thicknesses of the silicon wafer as the measurement sample and the reference silicon wafer uniform, the influence due to the absorption of the native oxide can be removed. If the native oxides are removed every time before use, the reference may be damaged, so removing the native oxide is impractical. There is another idea of a native oxide film grown on the sample surface with the same thickness as the native oxide attached to the reference.However, the native oxide on single-crystal silicon has a thickness of approximately within 1 nm, as described in NPL 1, and it takes several years to grow the native oxide to the thickness of the native oxide on the reference. Additionally, the growth rate depends on environmental conditions such as humidity. Therefore, it is difficult to artificially adhere the same native oxide to the measurement wafer as on the reference. LIST OF PRINTED PUBLICATIONS Patent Literature PTL 1: Japanese unexamined patent application publication JP H06 - 3 268 A PTL 2: DE 693 16 434 T2 describes a determination of an interstitial oxygen concentration in monocrystalline silicon by means of the absorption in the infrared local vibration mode of the interstitial oxygen in the monocrystalline silicon, including obtaining the absorption peak of the interstitial oxygen at 1106 cm-1. PTL3: DE 691 30 245 T2 describes measuring an interstitial oxygen concentration in a pulled silicon wafer, including providing the pulled silicon wafer, wherein the pulled silicon wafer has an interstitial oxygen concentration to be measured and a front side and a back side, wherein the front side has one of a plurality of predetermined finishes and wherein the back side has one of the plurality of predetermined finishes. Non-patent literature
[0006] NPL 1: YANAGIUCHI, Katsuaki: Thickness measurement of native oxide layer on the polycrystal silicon exposed to the air for three years. In: Journal of surface analysis, Vol. 7, 2000, No. 2, pp. 218-227. – ISSN 1341-1756 SUMMARY OF THE INVENTIONTechnical Problem
[0007] An object of this invention is to provide a method for measuring an extremely low oxygen concentration of less than 1 × 10 16atoms / cm 3 in a silicon wafer easily and sensitively using FT-IR. Solution to the problem
[0008] The method for measuring the oxygen concentration in a single crystal silicon wafer according to this invention is that for measuring an interstitial oxygen concentration of less than 1.0 × 10 16 atoms / cm 3, which includes steps 1 to 4. In step 1, SiO2 films of the same thickness are formed on each surface of a silicon measurement wafer (simply referred to as the "measurement wafer"), a reference silicon wafer free of interstitial oxygen (hereinafter simply referred to as the "reference wafer"), and a standard silicon wafer with a known interstitial oxygen concentration (hereinafter simply referred to as the "standard wafer"). In step 2, infrared absorption spectra of the measurement wafer with the SiO2 film, the reference wafer with the SiO2 film, and the standard wafer with the SiO2 film are measured by Fourier transform infrared spectroscopy (FT-IR).In step 3, an infrared absorption spectrum (transmission spectrum) is obtained from the infrared absorption spectrum of the measurement wafer with SiO2 film and the infrared absorption spectrum of the reference wafer with SiO2 film, and the absorption peak intensity corresponding to interstitial oxygen is thereby obtained. In step 4, the interstitial oxygen concentration in the measurement wafer is calculated based on the interstitial oxygen concentration value of the standard wafer, and the peak intensity of interstitial oxygen is compared with the peak intensity of interstitial oxygen of the standard wafer with SiO2 film.
[0009] In step 1, the SiO2 film preferably has a thickness of 2 to 40 nm.
[0010] The method for measuring the oxygen concentration in a single crystal silicon wafer according to this invention is that for measuring an interstitial oxygen concentration of less than 1.0 × 10 16Atoms / cm 3, which includes steps 1 to 4. In step 1, nitride films of the same thickness are formed on each surface of a measurement wafer, a reference wafer free of interstitial oxygen, and a standard wafer with a known interstitial oxygen concentration. In step 2, infrared absorption spectra of the measurement wafer with the nitride film, the reference wafer with the nitride film, and the standard wafer with the nitride film are measured by Fourier transform infrared spectroscopy (FT-IR). In step 3, a transmission spectrum is obtained from the infrared absorption spectrum of the measurement wafer with the nitride film and the infrared absorption spectrum of the reference wafer with the nitride film, and the absorption peak intensity corresponding to interstitial oxygen is thereby determined.In step 4, the interstitial oxygen concentration in the measurement wafer is calculated based on the interstitial oxygen concentration value of the standard wafer, and the peak intensity of the interstitial oxygen is compared with the peak intensity of the interstitial oxygen of the standard wafer with nitride film.
[0011] In step 1, the nitride film preferably has a thickness of 1 to 10 nm.
[0012] The method for measuring the oxygen concentration of a single crystal silicon wafer according to this invention is that for measuring the interstitial oxygen concentration of less than 1.0 × 10 16 atoms / cm 3, which includes steps 1 to 4. In step 1, polyethylene films are formed on each surface of a measurement wafer, a reference wafer free of interstitial oxygen, and a standard wafer with a known interstitial oxygen concentration. In step 2, infrared absorption spectra of the measurement wafer with polyethylene film, the reference wafer with polyethylene film, and the standard wafer with polyethylene film are measured by Fourier transform infrared spectroscopy (FT-IR). In step 3, a transmission spectrum is obtained from the infrared absorption spectrum of the measurement wafer with polyethylene film and the infrared absorption spectrum of the reference wafer with polyethylene film, and the absorption peak intensity corresponding to interstitial oxygen is thereby determined.In step 4, the interstitial oxygen concentration in the measurement wafer is calculated based on the interstitial oxygen concentration value of the standard wafer, comparing the peak intensity of the interstitial oxygen with the peak intensity of the interstitial oxygen of the standard wafer with polyethylene film. Advantageous effects of the invention
[0013] According to the invention, the infrared absorption attributable to interstitial oxygen is observed better than in the prior art. The extremely low oxygen concentration of less than 1.0 × 10 16 atoms / cm 3 in a silicon wafer can be measured easily and sensitively. This invention enables the detection limit of interstitial oxygen to be improved to a value obtained by SIMS, even when FT-IR is used. Short description of drawings Fig. Figure 1 illustrates a conventional infrared absorption spectrum of a single-crystal silicon wafer. Fig. Figure 2 illustrates the infrared absorption spectra of a reference wafer. The native oxygen is removed, and the reference wafer is kept in air. After 0 hours, 7 hours, 21 hours, 2.8 days, 8.9 days, 16.8 days, and 33.1 days, the IR absorption spectrum was measured using the wafer from which the oxide film was removed as the reference wafer. Fig. Figure 3 illustrates a difference spectrum obtained by subtracting an infrared absorption spectrum of a reference wafer with a 2 nm thick SiO2 film from that of a measurement wafer with a 2 nm thick SiO2 film. Fig. 4 illustrates a difference spectrum obtained by subtracting an infrared absorption spectrum of a reference wafer having a 5 nm thick nitride film from that of a measurement wafer having a 5 nm thick nitride film. Description of implementation examples
[0014] The method for measuring the interstitial oxygen concentration in a single crystal silicon wafer according to this invention is that for measuring an extremely low oxygen concentration of less than 1.0 × 10 16 atoms / cm 3, which includes steps 1 to 4. In step 1, SiO2 films of the same thickness are formed on each surface of a measurement wafer, a reference wafer free of interstitial oxygen, and a standard wafer with a known interstitial oxygen concentration. In step 2, infrared absorption spectra of the measurement wafer with SiO2 film, the reference wafer with SiO2 film, and the standard wafer with SiO2 film are measured by Fourier transform infrared spectroscopy (FT-IR). In step 3, an infrared absorbance difference spectrum (transmission spectrum) is obtained using the infrared absorption spectrum of the measurement wafer with SiO2 film and the infrared absorption spectrum of the reference wafer with SiO2 film, and the absorption peak intensity corresponding to interstitial oxygen is thereby obtained.In step 4, the interstitial oxygen concentration in the measurement wafer is calculated based on the interstitial oxygen concentration value of the standard wafer, comparing the peak intensity of the interstitial oxygen with the peak intensity of the interstitial oxygen of the standard wafer with SiO2 film.
[0015] Known silicon wafers, or more specifically, wafers made from a sliced single-crystal silicon ingot grown by the Czochralski process, are used as measurement wafers, reference wafers, and standard wafers for use in this invention. The measurement wafer is a silicon wafer for measuring the interstitial oxygen concentration. The reference wafer is a silicon wafer free of interstitial oxygen, more specifically, a wafer free of interstitial oxygen, or a wafer with an extremely low interstitial oxygen concentration. The standard wafer is a silicon wafer with a known interstitial oxygen concentration.
[0016] In step 1, the method for forming SiO2 films on each surface of the measurement wafer, the reference wafer, and the standard wafer includes a method for depositing oxide films at a treatment temperature of 300°C or less by chemical vapor deposition (CVD) and a method for applying liquid glass by spin coating.
[0017] CVD is a process for heating wafer-holding plates to form oxide films on the wafers under the conditions of flowing reactant gases such as silane (SiH4) and oxygen. The film deposition temperature is 600°C or less, and preferably 50 to 300°C.
[0018] Spin coating is a process for producing glass (SiO2) on wafer surfaces by depositing liquid glass onto the wafers and allowing it to penetrate the wafers. The spin coating process can be performed at ambient temperature.
[0019] The thicknesses of the oxide films formed by the above methods are preferably 2 to 40 nm. It is more appropriate that SiO2 films of the measurement wafer with the SiO2 film, the reference wafer with the SiO2 film, and the standard wafer with the SiO2 film are stably adhered and do not change over time. Fig. Figure 2 shows a change in infrared absorption due to native oxygen over a period of 33.1 days immediately after the native oxide was removed from the reference wafer. The thicker the SiO2 film on the wafer, the smaller the change over time.
[0020] The thermal oxidation process, i.e. the process of growing oxide films (SiO2 films) on wafer surfaces by inserting wafers in a high-temperature reactor and then reacting silicon with oxygen or steam, may be included.
[0021] In step 1, instead of adhering SiO2 films having a thickness of 2 to 40 nm, nitride films having thicknesses of 0.1 nm or more or polyethylene (PE) films having thicknesses of 0.02 to 0.1 mm may be adhered to each surface of the measurement wafer, reference wafer, and standard wafer, which are other embodiments of this invention.
[0022] It is desirable that the nitride films of the measurement wafer with nitride film, the reference wafer with nitride film, and the standard wafer with nitride film adhere stably and do not change over time. The nitride film is specifically silicon nitride (Si3N4). It is formed by applying ammonia gas (NH3) and silane gas (SiH4) or dichlorosilane gas (SiH2Cl2) to the wafer at a flow rate ratio of 2 to 30 (ammonia / silane) and a deposition pressure of 13 to 133 Pa. The temperature and time are typically 1000°C and 1 hour, respectively.
[0023] When the silicon nitride film is deposited, a native oxide with a thickness of 0.2 to 1 nm grows simultaneously on the wafer, with a SiO2 film positioned beneath the silicon nitride film. Before depositing the nitride films, native oxides on the surfaces of the measurement wafer, the reference wafer, and the standard wafer should be removed. The removal process includes mechanical polishing and chemical polishing. Specific examples include the electrical heating process under vacuum and the cleaning process using a dilute aqueous solution of hydrofluoric acid or a mixture of hydrofluoric acid and ammonium fluoride.
[0024] The thicknesses of the nitride films are preferably 1 to 10 nm.
[0025] The polyethylene film is formed by the following process. A wafer is placed in a polyethylene bag, which is degassed under vacuum, and then fused to seal its opening. Polyethylene films of the measurement wafer with polyethylene film, the reference wafer with polyethylene film, and the standard wafer with polyethylene film formed in this way remain stable and do not change over time.
[0026] The thicknesses of the polyethylene films are usually preferably 0.02 to 0.1 mm.
[0027] Even when depositing nitride films or polyethylene films instead of the SiO2 films, these films can of course adhere to the measurement wafer, reference wafer, and standard wafer to measure infrared absorption spectra, respectively, as described later.
[0028] The thicknesses of the SiO2 film, the nitride film and the polyethylene film adhering to the surfaces of the silicon wafers can be measured using an ellipsometer.
[0029] In step 2, infrared absorption spectra of the measurement wafer with SiO2 film, the reference wafer with SiO2 film and the standard wafer with SiO2 film are measured by FT-IR.
[0030] When nitride films or polyethylene films are deposited on wafers, the methods for measuring the interstitial oxygen concentrations are the same as the method for measuring the interstitial oxygen concentration in the wafer with SiO2 film in steps 2 to 4. The method using the wafer with SiO2 film is described below as an example.
[0031] According to the invention, the interstitial oxygen concentration in the measurement wafer is measured using Fourier transform infrared spectroscopy (FT-IR). FT-IR is one of the infrared spectroscopic techniques for structural and quantitative analysis of a substance (sample) by applying infrared rays to the substance and measuring the light transmitted or reflected by it.
[0032] When measuring a sample using FT-IR, infrared light emitted from a light source passes through a Michelson interferometer in the optical path. The Michelson interferometer consists of a semi-transparent mirror (beam splitter), a mobile mirror, and a fixed mirror. The light is split into two parts by the semi-transparent mirror. After being reflected by both the mobile mirror and the fixed mirror, the two light beams (light waves) are recombined by the semi-transparent mirror. When the mobile mirror is moved back and forth, the optical path difference between the mobile mirror and the fixed mirror is caused. The Michelson interferometer can detect interference light, which is composed of the phase difference between the two light waves that vary over time.The interferogram is acquired by plotting the interference light intensity along the horizontal axis as the optical path difference. Data obtained directly from FT-IR corresponds to the interferogram, which is a recording of infrared light transmitted from the sample. Fourier transformation using a computer is used to calculate the infrared absorption spectrum with wavenumber (cm). -1 ) on the horizontal axis.
[0033] Because FT-IR measurement is a single-beam spectroscopy, the FT-IR spectrophotometer cannot directly measure the transmittance (%) of a sample. Therefore, the background should be measured first without introducing any sample, and then the sample should be measured. The ratio of the background spectrum to that of the sample is calculated using the following equation, which results in the transmittance of the sample. IR spectrum = log(sample / background)
[0034] The FT-IR method includes the transmission method, total reflection method, diffusion reflection method, normal incidence / transmission method, and infrared microspectrometry. Among these, the normal incidence / transmission method is preferred.
[0035] In step 3, the absorption peak intensity observed at a center wave number of 1106 cm -1 , which corresponds to interstitial oxygen, is calculated from a difference spectrum (transmission spectrum) obtained by subtracting the infrared absorption spectrum of the reference wafer with SiO2 film from the infrared absorption spectrum of the measurement wafer with SiO2 film. As in Fig. 1, the position of the absorption peak of interstitial oxygen is close to and partially overlaps the absorption peak of native oxygen, so that the absorption peak intensity of interstitial oxygen can be obtained by steps 1 to 3.
[0036] The absorption peak attributed to the SiO2 film, the native oxide, is successfully removed by subtracting the infrared absorption spectrum of the reference wafer with SiO2 film from the infrared absorption spectrum of the measurement wafer with SiO2. Because the reference wafer is free of interstitial oxygen, only the absorption peak attributed to the interstitial oxygen of the measurement wafer with SiO2 film is retained.
[0037] In step 4, the peak intensity of interstitial oxygen obtained in step 3 is compared with that of interstitial oxygen at a center wave number of 1106 cm -1in the infrared absorption spectrum of the standard wafer with SiO2 film. The interstitial oxygen concentration in the measurement wafer is determined by proportional calculation based on the interstitial oxygen concentration value of the standard wafer. Because the interstitial oxygen concentration of the standard wafer is known, the interstitial oxygen concentration in the measurement wafer can be calculated proportionally from the peak intensity. EXAMPLES
[0038] Hereinafter, this invention will be described in detail with reference to Examples, but this invention is not limited to these Examples. [Example 1]
[0039] A measurement silicon wafer, a reference wafer free of interstitial oxygen, and a standard silicon wafer with a known interstitial oxygen concentration were prepared.
[0040] The three wafer types were washed with hydrofluoric acid (HF) to remove native oxides. Then, 2 nm thick SiO2 films were deposited on each wafer surface by chemical vapor deposition (CVD).
[0041] The spectroscopic FT-IR infrared absorption measurements were performed on the three types of wafers with SiO2 film. A difference spectrum ( Fig. 3) was generated by subtracting the absorption spectrum of the reference wafer with SiO2 film from the absorption spectrum of the measurement wafer with SiO2 film. The interstitial oxygen concentration of the measurement wafer was determined by proportional calculation based on the difference spectrum and the absorption peak attributed to the interstitial oxygen of the standard wafer with SiO2 film. As a result, the interstitial oxygen concentration was 0.5 × 10 16 atoms / cm 3 .
[0042] The SIMS analysis was performed on the same wafer as the test silicon wafer whose interstitial oxygen concentration was determined. The wafer had an oxygen concentration of 0.5 × 10 16 atoms / cm 3 , which was in good agreement with the result of the FT-IR measurement. [Example 2]
[0043] Similarly to Example 1, a measurement silicon wafer, a reference wafer free of interstitial oxygen, and a standard silicon wafer with a known interstitial oxygen concentration were prepared.
[0044] The three types of wafers were washed with hydrofluoric acid (HF) to remove native oxides. Then, 10 nm thick nitride films were formed on each surface of the wafers by heating at 1000°C for 1 hour in an atmosphere of ammonia gas (NH3) and silane gas (SiH4).
[0045] Similarly to Example 1, FT-IR spectroscopic infrared absorption measurements were performed to determine the interstitial oxygen concentration of the measurement wafer. The interstitial oxygen concentration was found to be 0.5 × 10 16 atoms / cm 3 This concentration was in good agreement with the result of the SIMS measurement. Fig. 4 shows a difference spectrum generated by subtracting the absorption spectrum of the reference wafer with nitride film from that of the measurement wafer with nitride film. [Comparison example 1]
[0046] A measurement silicon wafer, a reference wafer free of interstitial oxygen, and a standard silicon wafer with a known interstitial concentration were prepared.
[0047] These three types of wafers were subjected to FT-IR infrared absorption spectroscopic measurements without removing native oxides by cleaning with hydrofluoric acid (HF), etc., and without adhering any SiO2 films, nitride films, and polyethylene films (in a state with adhering native oxides). A difference spectrum obtained by subtracting the absorption spectrum of the reference wafer from the absorption spectrum of the measurement wafer confirmed a spectrum of large inverse absorption of a convex downward shape by native oxygen on the lower wavenumber side (1050 cm-1). -1 ) than the absorption spectrum (central wave number: 1106 cm -1 ) by interstitial oxygen ( Fig.1). Because the large reverse absorption spectrum of a convex downward shape was an obstacle to drawing a baseline on the absorption spectrum of interstitial oxygen, the oxygen concentration could not be obtained with high accuracy. INDUSTRIAL APPLICABILITY
[0048] According to the invention, the extremely low oxygen concentration in a silicon wafer can be easily and sensitively measured by using FT-IR.
Claims
[1] Method for measuring an oxygen concentration in a single-crystal silicon wafer having an interstitial oxygen concentration of less than 1.0 × 10 16 atoms / cm 3 , the method comprising: a step 1 for forming SiO2 films of the same thickness on each surface of a measuring silicon wafer, a reference silicon wafer free of interstitial oxygen, and a standard silicon wafer with a known interstitial oxygen concentration, a step 2 for measuring infrared absorption spectra of the measuring silicon wafer with SiO2 film, the reference silicon wafer with SiO2 film and the standard silicon wafer with SiO2 film by Fourier transform infrared spectroscopy (FT-IR), a step 3 for obtaining an infrared absorption difference spectrum (transmission spectrum) from the infrared absorption spectrum of the measuring silicon wafer with SiO2 film and the infrared absorption spectrum of the reference silicon wafer with SiO2 film and obtaining the absorption peak intensity corresponding to interstitial oxygen, and a step 4 for calculating the interstitial oxygen concentration in the measuring silicon wafer based on the interstitial oxygen concentration value of the standard silicon wafer, comparing the peak intensity of the interstitial oxygen with the peak intensity of the interstitial oxygen of the standard silicon wafer with the SiO2 film. [2] A method for measuring the oxygen concentration in a single crystal silicon wafer according to claim 1, wherein in step 1, the SiO2 film thickness is 2 to 40 nm. [3] Method for measuring an oxygen concentration in a single-crystal silicon wafer having an interstitial oxygen concentration of less than 1.0 × 10 16 atoms / cm 3 , the method comprising: a step 1 for forming nitride films on each surface of a measuring silicon wafer, a reference silicon wafer free of interstitial oxygen, and a standard silicon wafer with a known interstitial oxygen concentration, a step 2 for measuring infrared absorption spectra of the measuring silicon wafer with nitride film, the reference silicon wafer with nitride film and the standard silicon wafer with nitride film by Fourier transform infrared spectroscopy (FT-IR), a step 3 for obtaining a transmission spectrum from the infrared absorption spectrum of the measuring silicon wafer with nitride film and the infrared absorption spectrum of the reference silicon wafer with nitride film and obtaining the absorption peak intensity corresponding to interstitial oxygen, and a step 4 for calculating the interstitial oxygen concentration in the measuring silicon wafer based on the interstitial oxygen concentration value of the standard silicon wafer, comparing the peak intensity of the interstitial oxygen with the peak intensity of the interstitial oxygen of the standard silicon wafer with nitride film. [4] A method for measuring the oxygen concentration in a single crystal silicon wafer according to claim 3, wherein in step 1, the nitride film thickness is 1 to 10 nm. [5] Method for measuring an oxygen concentration in a single-crystal silicon wafer having an interstitial oxygen concentration of less than 1.0 × 10 16 atoms / cm 3 , the method comprising: a step 1 for forming polyethylene films on each surface of a measuring silicon wafer, a reference silicon wafer free of interstitial oxygen, and a standard silicon wafer with a known interstitial oxygen concentration, a step 2 for measuring infrared absorption spectra of the measuring silicon wafer with polyethylene film, the reference silicon wafer with polyethylene film and the standard silicon wafer with polyethylene film by Fourier transform infrared spectroscopy (FT-IR), a step 3 for obtaining a transmission spectrum from the infrared absorption spectrum of the measuring silicon wafer with polyethylene film and the infrared absorption spectrum of the reference silicon wafer with polyethylene film and obtaining the absorption peak intensity corresponding to interstitial oxygen, and a step 4 for calculating the interstitial oxygen concentration in the measuring silicon wafer based on the interstitial oxygen concentration value of the standard silicon wafer, comparing the peak intensity of the interstitial oxygen with the peak intensity of the interstitial oxygen of the standard silicon wafer with polyethylene film.
Citation Information
Patent Citations
method of measuring interstitial oxygen concentration
DE69130245T2
Method and device for determining the interstitial oxygen concentration in monocrystalline silicon BACKGROUND OF THE INVENTION Field of the invention:
DE69316434T2
Infrared absorption spectroscopic method for interstitial oxygen or substituted carbon concentration of silicon wafer