Current 3D printing methods for concrete and mortar face issues such as high unreacted material waste, low strength due to high water/cement ratios, low packing density, poorly defined edges, and slow construction processes, particularly in powder-based systems and pellet-based methods.
A 3D printer system with an actively driven mixer and nozzle design that allows for precise and homogeneous mixing of accelerators with concrete or mortar, enabling rapid setting and precise dispensing, along with a smoothing element to address surface finish and reinforcement integration for improved mechanical stability.
Enables the creation of 3D printed objects with enhanced strength, reduced material waste, precise control over layer bonding, and improved surface finish, allowing for faster construction and increased mechanical stability through rapid setting and reinforcement integration.
Description
[0001] The present invention relates to a 3D printing system for dispensing concrete, mortar or the like, comprising a nozzle, a main opening for supplying the concrete, mortar or the like, at least one additional opening for supplying at least one additive, and a discharge opening for dispensing the concrete, mortar or the like mixed with the additive.
[0002] Several techniques are known for applying concrete. One commonly used method is to pour the concrete into concrete buckets, lift these with a crane over the area to be concreted (which is usually limited by formwork), and then open the bottom of the bucket so that the concrete flows out.
[0003] Shotcrete is frequently used, particularly in tunnel construction. In the wet shotcrete process, cement, aggregates, and water are mixed together and pumped to a spray nozzle. This nozzle uses separately supplied compressed air to atomize the mixture and accelerate it for application. An accelerator is added to the shotcrete at the nozzle. Due to the compressed air, the accelerator mixes with the shotcrete, partly within the nozzle, partly during its flight to the point of impact, and then, through the mechanical action of the impact (and the subsequent application of concrete), with the concrete itself.
[0004] Another option is the use of so-called (mobile) concrete pumps. With these systems, the concrete is pumped from the concrete mixer directly to the point of use through a hose line up to approximately 120 m long, with the open end of the hose positioned above the area to be concreted.
[0005] Usually, the ready-mixed concrete is pumped through the hose and delivered unchanged to the point of use. However, from DE 20215662 U1 and JP H04269299 A, it is also known that for placing fast-setting concrete into formwork, a mixer is provided at the end of a pipeline directly before the formwork. This mixer is designed to mix accelerator and liquid concrete. For this purpose, the mixer has separate inlets for concrete and accelerator, as well as an actively driven agitator.
[0006] This document describes a system for lining tunnels. The concrete is poured from below into the formwork, which has a hole at the appropriate location. The mixing unit is positioned horizontally beneath the formwork. The concrete is fed into the mixing unit from below, where it is deflected by 90°. After passing through the mixing unit, the concrete is deflected a second time by 90° so that it can enter the formwork vertically from below. The angle between the longitudinal axis of the mixing unit and the discharge direction of the nozzle is therefore 90°. The mixing unit's pipe can have a length between 30 and 100 cm and a diameter between 10 and 30 cm (see page 6 of this document, lines 9-11). This nozzle is designed to inject large quantities of still-liquid concrete into the formwork.
[0007] Finally, 3D printing for concrete and mortar has also attracted increasing interest in recent years. Most processes that can be considered market-ready operate on the principle of "powder printing": a layer of powdered, dry concrete, mortar, or binder is applied across the entire surface, and then water or liquid binder is selectively printed onto it using established inkjet printing technology. This causes the concrete or mortar to harden in these areas. The next layer of dry concrete, mortar, or binder is then applied across the entire surface and also printed with water or liquid binder. This process is repeated until the desired model is built up. The desired object is then created, and after the layer-by-layer process is complete, the surrounding powder must be removed. Such a process is described, for example, in DE 102011105688 A1.
[0008] The disadvantages are a) the high proportion of unreacted powdered concrete, mortar, or binder; b) the necessary high water / cement or water / binder ratios, which result in low strengths; c) the low packing density of the resulting hardened concrete or mortar layers due to the low density of the dry fill material during application; and d) poorly defined edges of the layers / strips, as water or binder is partially drawn outwards in an undefined manner. This manifests itself in rough outer and inner boundary surfaces of the constructed objects.
[0009] b) and c) result in low strength. This manifests itself on the one hand in longer waiting times until the printed component can be separated from the surrounding dry material, and on the other hand in low achievable final strengths (which would be important, for example, to achieve frost resistance or freeze-thaw resistance).
[0010] A similar principle applies to the system described in US 8211226 B2: there, a special concrete formula is provided for a ZPrinter®. However, the 3D printer sold under the ZPrinter® brand does return unused, excess powdered material to the storage container, thus at least reducing material consumption.
[0011] Finally, there is also a lack of attempts to apply the material directly in liquid form and harden it immediately afterwards. An example of this is described in WO 2016 / 024863 A1. According to this document, 3D models are produced from a mixture of clay and fly ash, which is transferred into a pellet mold. Pellet by pellet is then blown onto the desired location using compressed air, with each pellet being hardened immediately after application by hot air or laser.
[0012] It is obvious that this process is relatively slow because the desired model has to be built up and cured pellet by pellet.
[0013] A 3D printing system of the type mentioned above is known from CN 204354263 U.
[0014] The object of the present invention is to design a 3D printing system with a nozzle for dispensing plastic concrete, mortar or the like of the type mentioned above in such a way that 3D prints can be created directly and precisely with it.
[0015] This problem is solved according to the invention by a 3D printing system with a nozzle of the type mentioned above in that an actively driven mixing unit with a mixing tube is provided between the additional opening and the discharge opening and the inner diameter of the mixing tube is 2-8 cm, preferably 2-6 cm, particularly preferably 2-4 cm.
[0016] Due to its smaller size compared to the DE 20215662 U1, this nozzle is suitable for dispensing small quantities of concrete (mortar) with high precision, as required for 3D printing.
[0017] Numerous trials have shown that it is possible to add accelerators to the concrete in the nozzle in such a way and quantity that setting begins within 1-2 minutes and is complete after approximately 10 minutes. This allows the concrete or mortar to begin stiffening in the nozzle and to be rigid upon exiting. This makes it possible to briefly interrupt the material dispensing to move the nozzle to the next point where material is needed, without setting beginning in the nozzle. (These movements usually only last a few seconds.) Conversely, setting occurs so slowly that it is not yet complete when the next layer is applied (applying a layer takes at most a few minutes), so that the new layer forms a strong bond with the layer below it, i.e., a monolithic body is created through the intimate layer-to-layer bond.Nevertheless, due to its stiffness, the concrete or mortar remains dimensionally stable after application.
[0018] In contrast to shotcrete, however, it is necessary to provide an active mixing unit in the nozzle, as otherwise the homogeneous mixing of the concrete or mortar with the accelerator or other additives cannot be ensured, for example by passive guiding elements (static mixers) or other types of accelerator injection (e.g. injection via ring nozzles).
[0019] However, precise and homogeneous application of accelerators or additives into the concrete or mortar is essential for the exact execution of 3D objects and components according to the invention.
[0020] The nozzle makes it possible to precisely dose additives or admixtures into a continuously conveyed concrete or mortar stream shortly before 3D application and to mix them intensively and homogeneously in a very short time using an actively driven mixer.
[0021] It is obvious that the mixing tool used in the mixing tube is of paramount importance in this regard. Preferably, the mixing tube contains a mixing tool with mixing elements designed as blades, paddles, rods, or as one or more screw flights. The screw flights can be driven wholly or partially in the opposite or parallel to the material flow.
[0022] To implement an active mixing mechanism in a simple manner, one embodiment of the invention provides that the nozzle has a first section and a second straight section, with the main opening located at the beginning of the first section and the discharge opening at the end of the second section. The mixing mechanism has a shaft that is arranged coaxially in the second section and carries the mixing elements. The shaft extends through the second section opposite the discharge opening, and a motor is provided outside the nozzle to drive the shaft. In this way, a straight, rigid shaft can be provided, which is driven by a motor outside the nozzle, so that the motor does not need to be specially sealed to withstand the material flow.
[0023] In a preferred embodiment, the shaft is designed like a crankshaft. The transverse bars of the shaft, arranged perpendicular to the mortar flow, repeatedly interrupt the flow, thus ensuring intensive mixing. The longitudinal bars, which pass close to the mixing tube, generate high shear forces, further contributing to thorough mixing. It is advantageous if the shaft is additionally equipped with mixing elements in the form of transverse and / or longitudinal bars.
[0024] It is advantageous if the internal angle β between the first section and the second section is obtuse, preferably at least 120°. In this way, the concrete or mortar only needs to be deflected slightly, so that the risk of blockage is low.
[0025] Furthermore, it is advantageous if the angle between the longitudinal axis of the mixing tube and the discharge direction of the nozzle is a maximum of 75°, preferably a maximum of 30°, more preferably a maximum of 10°, and in particular approximately 0°.
[0026] Due to the necessary homogeneity and precision of the flow rate, the concrete or mortar, after being mixed with the accelerator and / or other additives in the mixing plant, should ideally not be subjected to any further mechanical stress, and for flow-related reasons, in particular, it should not be deflected. For this reason, the maximum deflection after the mixer should be significantly less than 90°; preferably, no deflection should occur at all.
[0027] Preferably, a valve for temporarily stopping the material flow is provided between the mixing unit and the discharge opening and / or the nozzle has an inlet for compressed air for blowing out the concrete, mortar or the like.
[0028] In this way, the material flow can be stopped at short notice as desired: either a valve is provided that is placed in front of the discharge opening; and / or the nozzle or the discharge opening is designed as a compressed air nozzle (spraying application method), so that an interruption of the material application can be stopped at short notice by interrupting the compressed air flow and / or also by an upstream valve.
[0029] Preferably, the valve is a pneumatically actuated pinch valve. Such valves are robust and can be closed quickly by supplying compressed air, and they also open quickly when the compressed air supply is interrupted.
[0030] As already mentioned, the setting of the concrete begins after contact with the accelerator within 1-2 minutes. Short interruptions of the pressing process are therefore problematic if no further precautions are taken. For this reason, a further embodiment of the invention provides for a 3-way valve, preferably a needle valve, in the area of the additional opening, which can interrupt the contact zone between the accelerator or additive and the concrete, mortar, or the like.
[0031] The accelerator and / or other additives are introduced via a 3-way injector valve, which, in a preferred embodiment, is actuated by compressed air and pneumatically opens, interrupts, and closes the contact zone of the accelerator or additive via a needle valve opening and closing mechanism. This prevents the accelerator or additive inlet opening from becoming blocked by hardening concrete / mortar in the immediate contact zone.
[0032] Preferably, a rinsing agent can also be supplied via the 3-way valve. The nozzle is then designed so that a cleaning process can be carried out during a longer stoppage of the printing process, in which the entire mixing tool and the corresponding mixer interior can be rinsed and cleaned with rinsing water.
[0033] According to a further embodiment of the invention, the nozzle consists of two half-shells for cleaning and maintenance purposes. Preferably, a wear sleeve is positioned within the half-shells, bearing against the mixing tube wall, to prevent abrasion and wear on the walls of the half-shells and thereby extend the service life of the nozzle components. The nozzle is thus designed so that it can be easily disassembled into two parts (half-shells), allowing access to all internal areas for cleaning and maintenance.
[0034] Concrete / mortar components or printed objects produced using additive manufacturing acquire a special surface structure due to the process's typical characteristics (filament printing, where individual layers are built up sequentially). This structure is grooved, ribbed, or layered because, as is typical for this process, the individual layers do not form a precise, seamless connection at their edges. Besides a slight mechanical weakening of the component structure caused by the grooves (notch effect), the inhomogeneous surface also presents an increased area of vulnerability to various external influences (exposure to water or other liquids, frost, freeze-thaw cycles, carbonation, chemical attack, microorganisms, deposits of various kinds, etc.).The described grooved surface structure can also be disadvantageous in terms of visual appearance, as it does not convey a perfectly homogeneous impression, unlike smooth surfaces.
[0035] Another disadvantage of grooved, ribbed or layered surfaces is that subsequent coatings and coatings can only be applied with increased material consumption or, due to the surface structure and more difficult accessibility for coatings, with increased technical effort compared to smooth surfaces.
[0036] In order to avoid or at least reduce the severity of this grooved, ribbed or layered surface, the nozzle preferably has a smoothing element that can be rotated without limitation around the discharge opening and whose angle of attack is adjustable in relation to the axis of the discharge opening.
[0037] Smoothing tools such as trowels, floats, etc., have smooth surfaces made of materials like metal, plastic, wood, ceramic, etc. With the help of such smoothing tools, soft-plastic materials, or materials still in the setting / hardening phase, such as concrete, mortar, screed, plaster, fillers, adhesives, etc., can be smoothed flat through mechanical action on the surface. This mechanical action (stropping, spreading, leveling) of the smoothing tool results in a uniformity, homogenization, and thus a smoothing of the component surface.
[0038] A smoothing element can only smooth one side of the component being manufactured, either the inside or the outside. Usually, smoothing the outside is sufficient. If the inside also needs to be smoothed, a second smoothing element can be positioned opposite the first, relative to the discharge opening.
[0039] Typically, the smoothing element, and possibly additional smoothing elements, are guided tangentially to the surface to be smoothed. For a substantially planar smoothing element, this means that there is a normal to this plane of the smoothing element that intersects the axis of the discharge opening. By positioning the smoothing element in the tangential plane with respect to any spatial point on the component surface, even complex geometries, such as singly or doubly curved freeform shapes, can be smoothed.
[0040] One of the essential basic properties of cement-bound mineral building materials (concretes and mortars) is that they exhibit high compressive strength but comparatively low tensile and flexural strength. Under load, statically or dynamically applied forces almost always exert tensile and flexural forces on the component, which, if the component's inherent strength is exceeded, are generally responsible for component failure / fracture. Therefore, when higher forces occur and static / dynamic loads are applied, it is currently state of the art to reinforce such cement-bound components. Reinforcement / component strengthening predominantly uses steel inserts, but also alternative materials made of fibrous base materials such as carbon, silicon carbide, basalt, ceramics, wollastonite, AR glass, or polymeric materials in the form of fibers, grids, rods, threads, fabrics, braids, beams, etc.
[0041] All these materials have the basic property that they can absorb very high tensile and flexural forces and therefore, in combination with the relatively brittle, cement-bound mineral building materials in components, achieve a significant improvement in the tensile and flexural strength properties.
[0042] To also utilize these advantages in a 3D print according to the invention, a further embodiment provides that the nozzle has two discharge openings spaced apart, allowing a reinforcement element in the form of strips, grids, bands, meshes, fabrics, mats, rods, or threads to be positioned between the discharge openings and completely encased in concrete / mortar from two sides by the material application. For space reasons, this reinforcement element can only have a relatively small height; it is essentially a band or strip. According to the invention, several strips, bands, meshes, fabrics, or mats can be arranged one above the other and overlapping each other, resulting in a planar reinforcement element.
[0043] The reinforcement element can be flexible, deformable, and deflectable, or rigid. It can be made of textile or fiber-like materials, as well as metallic, polymeric, or other non-metallic materials. Flexible deformation of the reinforcement element can also be achieved, for example, through a short-term thermal treatment.
[0044] Alternatively, two nozzles according to the invention can be provided in a 3D printing system for concrete, mortar, and the like, wherein a control system guides the two nozzles synchronously to both sides of a reinforcement element. In this case, the reinforcement element can be designed with a large surface area from the outset.
[0045] The nozzles are used to produce 3D-printed objects and components based on concrete, mortar, or similar materials, with a setting accelerator being added through the secondary opening. Preferably, an aluminum sulfate-based solution is used as the setting accelerator. In addition to the setting accelerator, at least one further additive, in particular water, color paste, air-entraining agent, plasticizer, retarder, thickener, binder, fillers, aggregates, and / or fibers, can be added either by mixing it with the accelerator or by adding it as a "pure substance" through a separate secondary opening.
[0046] Dry concrete or dry mortar is preferably used, which is mixed with water close to the nozzle and fed to the nozzle via a hose. Since the concrete or mortar in the hose does not yet contain the accelerator, the residence time in the hose is not critical. Only after the accelerator is added in the nozzle should the residence time be less than two minutes to reliably prevent setting in the nozzle.
[0047] As already explained regarding the smoothing organ, components or printed objects made of concrete / mortar, which are printed using additive manufacturing processes, acquire a grooved, ribbed or layered surface structure through the process typical of the procedure.
[0048] It is therefore preferred to use the nozzle in which, after the layer-by-layer application of concrete, mortar or the like, the resulting grooves are filled by spraying with a nozzle which has an inlet for compressed air to blow out the concrete, mortar or the like, with reinforcement elements, in particular reinforcement grids, optionally being laid down beforehand.
[0049] In this way, similar to the process used with shotcrete, concrete, mortar, or a similar material is sprayed onto the grooved surface, filling the grooves. A reinforcing mesh can be laid beforehand to improve the mechanical stability of the component.
[0050] If a reinforcement element is to be located in the component, it is advantageous if it is embedded or injected or sprayed coaxially from two sides by means of two independently spatially guided nozzles through the application of concrete / mortar.
[0051] Particularly when a reinforcement element is to be embedded not with two independently guided nozzles, but with a single nozzle with two discharge openings, the reinforcement element cannot be too tall (wide). It is therefore advantageous to create a homogeneous, reinforcing reinforcement network inside the component by overlapping individual reinforcement elements. Thus, even in this case, there is no structural disadvantage, although the reinforcement is composed of strip-shaped individual elements. Brief description of the drawing figures
[0052] The present invention is explained in more detail with reference to the accompanying drawings. They show: Fig. 1 a nozzle without an outlet-side valve and without compressed air supply, partially in cross-section; Fig. 2 the lower end of this nozzle, equipped with a valve; Fig. 3 the use, schematically illustrated, of a nozzle according to the Fig. 1 and 2 ; Fig. 4 the layered application of concrete or mortar with a nozzle according to Fig. 1 ; Fig. 5 the layered application of concrete or mortar using a nozzle with compressed air supply; Figs. 6 to 8 various preferred embodiments of mixer tools; Fig. 9 an exploded view of a nozzle; Fig. 10 a nozzle with a smoothing element; Fig. 11 the same, partly in cross-section; Fig. 12 various settings of this nozzle; Fig. 13 a view similar to Fig. 12 , each of a nozzle with two smoothing elements; Fig. 14The coating or smoothing of an already printed structure using a nozzle with compressed air supply; Fig. 15 the same, but using a reinforcement grid Fig. 16 a nozzle with two discharge openings in cross-section; Fig. 17 the same in perspective view; Fig. 18 and 19 nozzles show accordingly Fig. 16 and 17 , however, with compressed air supply; and Fig. 20 shows the use of secondary nozzles to produce a component with an embedded reinforcement grid. Description of the execution types
[0053] The nozzle 21 according to Fig. 1The nozzle has a first straight section 22 and a second straight section 23. At the upper end of the first straight section 22 is a main opening 2 through which concrete, mortar, or the like can be supplied. At the lower end of the second straight section 23, a discharge opening 6 is connected via a coupling 8', through which the supplied material can exit the nozzle. Between these two sections is at least one additional opening 3 through which an additive (liquid or paste-like) can be added. For 3D printing, this additive will contain a setting accelerator. The internal angle β between the first section 22 and the second section 23 is obtuse (for example, 135°), so that the material experiences only a slight change in direction as it passes through the nozzle 21 (for example, 45°).The second section 23 extends beyond the connection point between the first section 22 and the second section 23 to a connecting coupling 8. A shaft bearing 7 is coupled to a motor 9 via this connecting coupling 8. This motor 9 drives a shaft 4 on which mixing elements 5 in the form of blades are mounted. Paddles, rods, or screw flights can also be used instead of blades. This creates a mixing unit 24 in the area between the additional openings 3 and the discharge opening 6, so that the lower part of the second section 23 can also be referred to as a mixing tube 1.
[0054] Instead of the discharge opening 6, a valve 10 with discharge opening 6 can be coupled to the connecting coupling 8', as shown in Fig. 2This valve 10 is a pneumatic pinch valve; when compressed air is blown in through the inlet opening 25, the flexible hose 26 is compressed until its inner diameter becomes almost zero, thus stopping any material flow. If the supply of compressed air to the inlet opening 25 is stopped, the hose 26 returns to its original position. Fig. 2 The depicted shape and printing material can be dispensed through the discharge opening 6. With appropriate control, it is possible to produce a strand of any length or to apply the material point by point.
[0055] Based on Fig. 3The use of such a nozzle 21 is explained. Due to the relatively rapid onset of hardening, during longer periods of inactivity in the printing process, e.g., during periods of several minutes or after completion of the component printing, the material in the nozzle 21 would already begin to harden. In practice, the onset of rapid material hardening very quickly leads to heavy build-up on the mixer 24, to a blockage of the mixing tube 1, and in the worst case to a "concrete-filling" of the mixer tube interior and thus to irreversible damage to the nozzle 21. As a consequence, there is a risk of the accelerator or other additive supply lines becoming clogged at their inlet opening into the mixing tube 1, i.e., in the area of the additional opening 3.
[0056] A storage container holds pumpable concrete or mortar, mixed on-site from dry mortar and water. Alternatively, ready-mix concrete from a concrete plant, site-mixed concrete or mortar, or factory-mixed mortar can be used. The pumpable concrete or mortar is pumped by a mortar pump through an interrupter valve 36 to the main opening 2. A storage container for an accelerator is also provided, which is supplied to the auxiliary opening 3 via an accelerator pump, a solenoid valve 38, and a 3-way valve 13. It is understood that the accelerator pump must adjust its delivery rate to the mortar throughput. The mixing unit 24 distributes the accelerator evenly in the concrete or mortar, and the accelerator-mixed mortar can be precisely metered and dispensed from the discharge opening 6 using the valve 10.
[0057] Identical to the described process, three additional openings can be provided in the area surrounding the additional opening for dosing additional additives, as shown in Fig. 1 is shown.
[0058] The nozzle 21 is designed so that, in the event of a planned stop of the printing process, a cleaning process can be carried out by rinsing and cleaning the entire mixing unit 24 and the appropriate mixer interior using rinsing water.
[0059] The accelerator and / or other additives are introduced via the 3-way valve 13, to which not only additives can be supplied via the solenoid valve 38, but also rinsing agent (in particular, rinsing water 40) via a solenoid valve 39. In a preferred embodiment, the 3-way valve 13 is actuated by compressed air and pneumatically opens, interrupts, and closes the contact zone of the accelerator or additive via a needle valve opening and closing mechanism. This prevents the inlet opening of the accelerator or additive from becoming blocked by hardening concrete / mortar in the immediate contact zone.
[0060] Procedure for pressure interruption with cleaning: For cleaning, it is necessary to interrupt the flow of concrete or mortar material on the inlet side, thus preventing further material inflow. The interruptor valve 36 serves this purpose. Immediately below the interruptor valve 36, flushing water 40 is introduced into the mixing tube 1 through an inlet opening – controlled by a solenoid valve 37 – thereby flushing the first section of the nozzle, the entire mixing unit 24, and the mixing chamber. Furthermore, the supply line on the accelerator injection side, or when introducing other additional components / additives, is also cleaned by switching the 3-way injector valve 13 to a flushing solution 40. This ensures that no blockages occur in the supply line or the nozzle 21 in the immediate contact zone between the concrete / mortar and the accelerator or additional components.
[0061] By appropriately controlling the solenoid valves, it can be ensured, for example, when switching to the flushing process, that the concrete or mortar pump and the accelerator injection are stopped, the inlet-side interrupter valve 36 (preferably a pinch valve) located in the concrete line is closed, and the solenoid valves 37 and 39 of the flushing lines and the outlet-side valve 10 are open.
[0062] During the overrun period of the mixing unit 24, all areas of the nozzle 21 are rinsed. After the rinsing phase, this cleaning concept also allows for longer downtimes.
[0063] The advantage of the described rinsing and cleaning concept is that the printing process can be made significantly more flexible and variable than a continuous printing process by allowing short-term pressure interruptions.
[0064] After the standstill phase, the concrete or mortar pump and subsequently the accelerator or additive pumping and dosing devices are reactivated, and the printing process can be continued.
[0065] For short-term interruptions during printing, it is sufficient to briefly stop the concrete or mortar pump and the accelerator or additive injection, while the concrete / mortar remains in the mixing zone.
[0066] The following text describes in detail the possible system states and control sequences of nozzle 21:
[0067] In principle, nozzle 21 is designed for the individual material components that are in FIG. 3The described opening and closing mechanisms, which can be automatically switched by an electronic control system in the form of a series of different valves, enable various processes and system states such as starting, printing, stopping and cleaning steps.
[0068] With the in FIG. 3 The valves 36 to 39 shown, the 3-way valve (accelerator shut-off valve) 13, which is preferably designed as a needle valve, the pinch valve 10 at the nozzle end and the two lines for rinsing water 40 allow automatic switching between the following system states: Table 1 "Start-up / Filling" 36, 10 open; 37; 38, 39, 13 closed "Press" 36, 10; 38, 13, open; 37, 39 closed "Stop briefly" all listed valves closed "Flushing the injector" 39, 13, 10 open; 36, 37, 38 closed "Nozzle Flush" 37, 10 open; 36; 38, 39, 13 closed
[0069] The system state "Start operation / Fill" precedes the printing process. This ensures that the mixing zone is already filled with mortar / concrete when printing starts.
[0070] In the system state "Printing", all valves are open, except for solenoid valves 37 and 39 for the rinsing water, which are closed.
[0071] To change the nozzle's position between unconnected pressure paths without unwanted material leakage, the "Briefly Stop" system state closes all valves (36 to 39, 10 and 13). After a short standstill, the printing process must be resumed or a "Flush Injector" process initiated to prevent clogging of the printing system.
[0072] Before longer periods of inactivity, cleaning using both rinsing programs ("Injector Rinse" and "Nozzle Rinse") is necessary.
[0073] In Fig. 4The diagram shows a nozzle in operation, continuously dispensing a concrete / mortar strand or layer 15 from the discharge opening 6. If no particularly detailed shaping is required, the necessary material can be applied very quickly in this way, and the 3D printed object can be built up layer by layer. Each subsequent "wet-on-wet" layer of concrete / mortar 15 forms a strong bond with the material below it because the latter has not yet fully set.
[0074] In Fig. 5Finally, it is shown that a nozzle with a compressed air supply is used. A compressed air chamber 17 is provided, which can be supplied with compressed air via an inlet 16. The compressed air is used to blow out the supplied concrete or mortar 14, so that the material strikes the substrate in a spray jet 18 with relatively high energy. A bead 15 can also be applied in this way. The advantage of this application method is that the high kinetic energy that the concrete or mortar receives through the application process results in very high material homogeneity. A layered application is hardly perceptible in the finished workpiece.
[0075] Fig. 6Figure 1 shows a cross-section through a nozzle 21 with a preferred mixing tool. This tool has a shaft 4 in the form of a crankshaft. This shaft 4, which is rotatably mounted along the axis of the mixing tube 1, is repeatedly deflected eccentrically from the central axis, similar to the machine element crankshaft, as shown in Figure 2. FIG. 6 This results in effective mechanical and fluidic mixing effects, as the mortar flow running in the direction of the mixing tube axis and the additives dosed through the additional opening 3 are repeatedly "interrupted" and thus intensively mixed by the transverse bars of the shaft 4, which are arranged perpendicular to the mortar flow. Furthermore, test series have shown that the eccentric bar elements acting at the edge of the mixing tube 1 have a very positive effect on the mixing result due to their shearing action on the inner wall of the mixing tube 1.
[0076] Further test series showed that additionally installed crossbars 34, as in FIG. 7 shown, and transverse bars 34 with additional longitudinal bars 35, as shown in FIG. 8 shown, bring about a further improvement in the mixing result and therefore describe particularly preferred embodiments according to the invention.
[0077] An exploded view of a nozzle 21 with such a shaft 4 is shown in Fig. 9As shown, for easy maintenance and cleaning, the nozzle consists of two half-shells 51, 52. These can be quickly and easily separated from the parts of the nozzle 21 above and below (motor, not shown, and valve 10 with discharge opening 6) by means of two connecting couplings 8, 8', preferably in the form of quick-release clamps, and then fully opened. This allows all areas of the mixing zone, the mortar inlet opening, and the access zone for accelerators or additives to be freely accessible for cleaning and maintenance.
[0078] During prolonged use, the mixing process, with its abrasive concrete or mortar components such as aggregates, sands, etc., leads to material loss and significant wear on the inner wall of the mixing zone of the nozzle 21. This considerably reduces the service life of the nozzle 21 components. Therefore, a wear sleeve 41 is positioned within the half-shells 51 and 52 as a mixing tube to prevent abrasion and wear on the walls of the half-shells 51 and 52, thereby extending the service life of the nozzle 21 components.
[0079] As already mentioned in the introductory description, it can be desirable for a variety of reasons to avoid or at least reduce the grooves that typically result from the layer-by-layer application process. One way to achieve this is described in the Figs. 10 to 13As shown, a smoothing element 47 or a spatula is rotatably arranged around the discharge opening 6. This allows the component surface to be smoothed simultaneously during the printing process by a precisely controlled mechanical process.
[0080] Depending on whether only one surface or both surfaces ("outer" or "inner surface") of the component or printed object are to be smoothed, only the smoothing element 47 is available ( Figs. 10 to 12 ) or additionally another smoothing organ 47' ( Fig. 13 ) available.
[0081] As in FIG. 10 and 11As shown, the smoothing element 47 can perform movements in two directions. One direction of movement represents the rotation of the smoothing element 47 by 360° around the discharge opening 6 (double arrow 53). The second direction of movement controls the angle of attack of the smoothing element 47 with respect to the axis of the discharge opening 6 (double arrow 54). This enables the smoothing element to be positioned in the tangential plane with respect to any spatial point on the surface of the component to be smoothed, even with complex components / printed objects such as freeform shapes.
[0082] This applies to various printing options in FIG. 12 and FIG. 13 depicted.
[0083] The smoothing element 47 or smoothing elements 47, 47' are positioned by two motors 42, 42', which are electronically controlled synchronously with the nozzle guide. To ensure unlimited continuous rotation around the axis of the discharge opening 6, both motors 42, 42' are rigidly mechanically connected to the nozzle body.
[0084] The rotation around the axis of the discharge opening 6 (double arrow 53) is transmitted via a pinion 55 and a gear 56 to a cylindrically shaped and concentrically mounted rotating body 45.
[0085] For the tilting movement of the smoothing element 47 or smoothing elements 47, 47' (double arrow 54), a further gear 56' is rotated by means of a pinion 55'. This gear 56' has a bevel gear 46 on its underside, into which a bevel gear 44 engages. The rotational movement of the bevel gear 44 is transmitted to the smoothing element 47 via a linkage 43. If a further smoothing element 47' (see Fig. 13) is present, then a further linkage 43' is attached to this bevel gear 44, which tilts the further smoothing element 47'.
[0086] The length L (see Figs. 12 and 13 ) of the smoothing element 47 or smoothing elements 47, 47' corresponds at least to the height H of a printing layer, but the length dimension L can also be significantly greater and correspond to the height of several printing layers.
[0087] This provided a mechanical solution that allows unlimited rotation of the smoothing element 47 or smoothing elements 47, 47' around the axis of the discharge opening 6 and the setting of any desired angle of attack in relation to any spatial point of the component / object to be printed, while simultaneously providing a small, compact design for attachment to the discharge opening 6 of the nozzle.
[0088] If nozzles are used for the 3D printing process according to Fig. 4 (no-air operated nozzle) or Fig. 5(air-operated nozzle) can be used, unwanted groove structures can also be counteracted by using the nozzle 58 according to Fig. 5 subsequently sprayed with printing material. This is in FIG. 14 As shown, pressure concrete or mortar is applied using the method already demonstrated by FIG. 5The spray nozzle, as described in detail, is applied to the surface of a previously printed 3D component or object 57, thus homogeneously coating the surface. This gives the component 57 a completely new visual appearance, as the grooved or ribbed structure typical of the 3D printing filament process is no longer visible due to the uniform coating with the concrete or mortar, and the surface acquires a uniform, sprayed-on texture that can optionally be subsequently smoothed manually or mechanically (by varying the accelerator component) or otherwise textured (rubbed texture, etc.).
[0089] In particular, this method also makes it possible (see Fig. 15), a spatial or planar, two- or three-dimensional reinforcement element 30 made of reinforcement materials adapted to a 3D component or printed object 57, to be superficially applied or fixed to the already printed 3D component or object and then again as already described in FIG. 14 The process involves injecting materials to reinforce and strengthen the printed component or object. A reinforcement element can be understood as reinforcing strips, grids, tapes, meshes, fabrics, rods, or threads made of various materials such as metallic, polymeric, or non-metallic (e.g., fibrous) materials.
[0090] For both of the described spraying methods, it can be advantageous to reduce or completely omit the accelerator component. This results in longer processing and open times for the applied 3D-printed concrete or mortar, allowing for surface finishing of the sprayed concrete / mortar.
[0091] Following a further development, which in Figs. 16-20 As shown, it is also possible to integrate reinforcement elements directly during the initial 3D printing process. The discharge mechanism at the nozzle tip of the printing process is designed as follows:
[0092] The ready-mixed concrete / mortar 14 is divided into two strands 14a, 14b or chambers by the special geometry of the discharge element (which has the shape of "trousers" 29), with a discharge opening 6, 6' being provided for each strand 14a, 14b. The concrete / mortar is conveyed through these two discharge openings 6, 6' either continuously in a high-temperature flow process ( FIG 16 , 17 ) or in the case of the spraying method ( FIG. 18 , 19 pneumatically conveyed. In this case, nozzles are used accordingly. Fig. 5 for use, to which compressed air is supplied via compressed air lines 31, so that the concrete / mortar is "torn apart" into individual pieces by compressed air.
[0093] The discharge device is designed such that the two discharge openings 6, 6' are directed towards each other, so that the emerging mortar parts are deflected shortly before exiting the discharge openings (discharge angle α) in such a way that the two concrete / mortar strands are immediately reunited into a single strand 15 after exiting the discharge openings.
[0094] This method allows a predefined positioned reinforcement element 30 to be reliably encased on both sides by mortar / concrete, thus assuming the function of reinforcing reinforcement in the component.
[0095] The one in the Fig. 16 and 18 The depicted exit angle α can vary between 0-90°.
[0096] The reinforcement element can be flexible, deformable, and deflectable, or rigid. It can be made of textile or fiber-like materials, as well as metallic, polymeric, or other non-metallic materials. Flexible deformation of the reinforcement element can also be achieved, for example, through a short-term thermal treatment.
[0097] The reinforcement element 30 can be introduced automatically or manually during the application process via a mechanism of the nozzle in a continuous strand or in the form of individual strips / grids / bands / meshes / lays / mats / rods / threads, so that it is aligned exactly in the middle and is embedded on both sides by the concrete / mortar that emerges uniformly from both discharge openings 6.
[0098] Alternatively, the reinforcement element 30 can also be inserted manually or automatically, e.g. with a robot, and positioned appropriately.
[0099] By applying the mortar in layers during the application process, the individual reinforcement elements are embedded or injected layer by layer, resulting in a fully reinforced two- or three-dimensional component.
[0100] The positioning of the reinforcing element in relation to the mortar bead can also vary: it can be placed centrally, off-center, diagonally, vertically, horizontally, etc. It can also be dimensioned so that its width exceeds the width or height of the mortar bead / layer. This ensures that a portion of the reinforcing strip always protrudes from the freshly applied mortar layer, as shown in the [reference to relevant text]. Figs. 16 to 19 is shown.
[0101] After the next layer of reinforcing strips is inserted, the subsequent strips overlap and are then embedded or injected with the next layer of mortar to form a homogeneous component. This overlapping of the individual reinforcing strips, along with their subsequent mechanical fixation using embedded or injected and hardened concrete / mortar, creates a homogeneous reinforcement network within the component. This strengthens the component and allows it to withstand uniformly increased tensile forces across its entire surface.
[0102] Alternatively, two synchronously guided nozzles can be used, as shown in Fig. 20 as shown. Instead of a single 2-chamber spray head accordingly. Fig. 18 and Fig. 19Two individual nozzles 21, 21' are used, which are automatically guided spatially in such a way that they in turn embed a flexible, deformable and deflectable or rigid reinforcement element 30, by means of the spatially separated nozzle heads 21, 21' with identical structure as in Fig. 5 The described process involves embedding or spraying / injecting the reinforcement element 30 synchronously from two sides. This allows for the creation of components that incorporate printed objects, which are designed according to the instructions. Fig. 18 or 19 manufactured processes are equivalent. The two nozzles can be guided spatially automatically, for example, by two synchronously guided robots 32, 32'.
[0103] This method can also be used to spray or inject prefabricated, flat, single or double curved, rigid reinforcement elements (e.g. prefabricated metallic reinforcement cages or grids).
[0104] The following section discusses the formulation components of mortars / concretes suitable for 3D printing, which enable the production of optimized formulations suitable for 3D printing.
[0105] As a starting material for 3D printing according to this invention, both dry mortar or dry concrete and conventionally produced concrete (ready-mixed concrete from a ready-mix concrete plant or mixed on site) or a premixed ready-mix mortar (factory mortar), which was produced, for example, in a ready-mix concrete plant or similar mixing plant, can be used.
[0106] However, dry mortar or dry concrete is preferred. A.) DRY MORTAR / DRY CONCRETE RECIPE Sands / aggregates / fillers:
[0107] Based on limestone, dolomite or quartz sand or mixtures thereof, with a grain size range of 0 to X mm (X = variable maximum grain size in the range of 1 mm to 16 mm (preferably 0.1-4 mm, particularly preferred 0.1-2 mm)). Furthermore, all sands / aggregates / fillers suitable for concrete or mortar applications are also suitable. Usage range: 20-80% Preferred: 50-70% Binder:
[0108] based on Portland cement (CEM I or CEM II or CEM III), ground slag (blast furnace slag), fly ash, aluminate cements, sulfoaluminate cements, sulfate blast furnace cements, gypsum and hydrated lime or mixtures thereof. Usage range: 10-80% Preferred: 30-60% Additives:
[0109] latent hydraulic flour-fine pozzolanic additives such as microsilica, silicic acids, metakaolin, zeolites, trass, fine flours based on quartz, limestone, etc. Usage range: 0.5-15% Preferred: 1.5-10% Flow agent:
[0110] Based on polycarboxylate ether (PCE), naphthalenesulfonate, melaminesulfonate, lignosulfonate Usage range: 0.05-2% Preferred: 0.1-0.8% Extended opening hours:
[0111] Based on methylcellulose (MC) Usage range: 0.01-0.5% Preferred: 0.01-0.1% Stabilizers / Thickeners / Adjusting Agents:
[0112] Based on low-viscosity methylcelluloses, Welan Gum, Diutan Gum, Xanthan Gum, starch ethers, pectins, guar ether, polyvinyl alcohol, and silicates. Usage range: 0.01–0.5% Preferred: 0.01–0.1% Redispersion powder:
[0113] based on vinyl acetate-ethylene, styrene acrylate, styrene butadiene, pure acrylate, and copolymers of VeoVA, VAC / VeoVa, VAC / VeoVA / E, vinyl terpolymers, vinyl acetate-vinyl versatate, vinyl acetate-vinyl chloride, vinyl acetate-acrylic, VAC / VeoVA / Acryl, VAM / Acryl.
[0114] Redispersion powders act as an adhesive in 3D printed mortars or concretes, improving the bonding and adhesion of the individual printed layers, while also having an elasticizing effect and improving the tensile strength and impact resistance of the material. Usage range: 0.1-10% Preferred: 0.5-2.5% Defoamer:
[0115] based on mineral oil, non-ionic surfactants, silicone oil, polysiloxane, fatty alcohol alkoxylate, polyglycol, vegetable oil base, hydrophobic esters, ethoxylated alcohols Usage range: 0.02-0.5% Preferred: 0.05-0.2% Wetting and dispersing agents:
[0116] based on ethylene oxide / propylene oxide copolymers, polyglycol esters, glycol derivatives, modified polysiloxanes, mixtures of surfactants based on fatty alcohols (e.g. fatty alcohol polyethylene glycol ethers, methyl ester sulfonates, fatty alcohol sulfates, etc.), fatty acid amidoalkyl betaine, and sodium polynaphthyl methanesulfonate. Usage range: 0.005-0.2% Preferred: 0.01-0.1% Shrinkage-reducing agents:
[0117] organically based glycol compounds (glycols, glycol ethers, neopentyl glycol, dipropylene glycol), polyoxyalkylenes, alkyl ethers, monobutyl ethers, butoxyethoxyethanol or inorganically mineral based such as MgO, CaO, sulfoaluminate cements. Usage range: 0.1-7% Preferred: 0.3-5% Accelerator:
[0118] Based on alkali hydroxides, alkali carbonates, alkali aluminates, alkali silicates (e.g., water glasses), alkali and alkaline earth salts, in particular alkali and alkaline earth chlorides, alkali and alkaline earth formates, alkali and alkaline earth fluorides, and alkali and alkaline earth nitrides, e.g., calcium formate, calcium acetate, lithium carbonate, sodium carbonate, potassium carbonate. Also, aluminate compounds such as alumina cement (crystalline or amorphous), amorphous aluminum hydroxide, aluminum sulfate, etc., as well as modified calcium silicate hydrate nuclei, etc. Usage range: 0.05-2% Preferred: 0.1-1% Delayer:
[0119] based on hydroxycarboxylic acids such as tartaric acid, citric acid, malic acid or active ingredients based on phosphates, phosphonic acids, gluconates, gluconic acid, sulfonates, sugars, proteins, amino acids and salts of these compounds. Usage range: 0.01-0.5% Preferred: 0.02-0.3% Fibers:
[0120] Based on polypropylene, polyethylene, polyacrylic, polyacrylonitrile, polyamide, aramid, polyester, steel, alkali-resistant glass, quartz, silica, ceramic, silicon carbide, basalt, mineral wool, wollastonite, carbon, cellulose, cotton, flax, hemp, jute, bamboo. Usage range: 0.05-5% Preferred: 0.1-3% Pigments:
[0121] based on TiO₂, CaCO₃, dolomite, kaolin, Fe oxides and hydroxides, ZnO, ZnS, CoAl₂O₄, Cr oxides, (Ti, Ni, Sb)O₂, (Co, Ni, Zn)₂(Ti, Al)O₄, Co(Cr, Al)₂O₄, carbon black, flours from fired clay or bricks, organic pigments of various kinds Usage range: 0.05-20% Preferred: 0.1-5% B.) LIQUID ACCELERATOR FORMULA
[0122] The liquid or pasty accelerator supplied at the nozzle has as its active ingredient base aluminum sulfate, alkali aluminates, alkali aluminosulfates, aluminum formate, alumina cement (amorphous or crystalline alumina cement phases), sulfoaluminate cement, amorphous aluminum hydroxide, aluminum hydroxysulfate, alkanolamines, hydrofluoric acid, carboxy acids, phosphoric acids, water glass, ethanolamines such as diethanolamine (DEA) and triethanolamine (TEA) or mixtures thereof. Application range (referring to dry mortar) from - to: 0.5-10% Preferred: 1.0-7.0% C.) Pasty additives or additives
[0123] The additional additives supplied at the nozzle are based on the same active ingredients as described in A.), but must be in liquid, paste, or slurry form. Water, solvents, color or pigment pastes, air-entraining agents, flow agents, retarders, thickeners, binders, fillers, aggregates, and fibers are preferred. D.) Accelerated Mortar / Concrete
[0124] The intensive mixing of the dry mortar with the accelerator component in the active mixer of the printer nozzle results in an immediate reaction of the accelerator with the binder components, which leads to an initial immediate stiffening reaction in the area of the mixing tube (1) of the nozzle and results in a subsequent hardening reaction of the concrete / mortar immediately after exiting the discharge opening (6). Example: MORTAR:
[0125] 34% Portland cement CEM II AS 42.5 R (binder) 2% Metakaolin (additive) 0.2% PCE (flow agent) 0.04% low-viscosity MC (open time extender) 0.02% starch ether (thickener) 2.0% vinyl acetate-ethylene (redispersing powder) 0.15% mixture of fatty alcohol alkoxylate and polysiloxane (defoamer) 0.03% fatty alcohol-polyethylene glycol ether (wetting and dispersing agent) 3% sulfoaluminate swelling cement (shrinkage reducer) 0.5% calcium formate (accelerator) 0.03% citric acid (retarder) to 100% limestone granules and limestone flour 0-2 mm (approx. 58%) LIQUID ACCELERATOR:
[0126] 5% (based on dry mortar weight) aluminum sulfate solution (40%)
[0127] The given recipe example, with a water-to-dry mortar ratio of 16% ±1% points, results in the following fresh mortar properties when mixed (without the liquid accelerator component) using a standard mortar mixer: Fresh mortar: Spread with cylindrical sleeve (geometry: h = 5 cm, diameter = 3 cm): 9-10 cm. Setting times according to Vicat (conical needle): Setting start: 100-300 min; Setting end: 110-400 min. Strength profile (40 x 40 x 160 mm prism): DF 1 day: 5-10 MPa; BZF 1 day: 1.5-3.5 MPa; DF 28 days: 25-35 MPa; BZF 28 days: 5-7 MPa
[0128] The accelerated mortar / concrete exiting the nozzle tip has the following property profile for the example given: Fresh mortar: Spread with cylindrical sleeve (geometry: h = 5 cm, diameter = 3 cm): not measurable (mortar "stands" in the sleeve, i.e., stiff consistency). Setting times: Setting start: < 2 min; Setting end: < 10 min. Strength profile: DF 1 day: 6-11 MPa; BZF 1 day: 2-4 MPa; DF 28 days: 25-35 MPa; BZF 28 days: 6-8 MPa
[0129] The nozzle and the above-mentioned formula allow for highly precise results. Dimensional accuracy, resolution, and tolerance of the 3D printer can be used as quality parameters for assessing the precision of printed results (components, printed objects).
[0130] The dimensional accuracy of the component / printed object depends on Resolution of the 3D printer system: This refers to the ability of a 3D printer to move precisely from one spatial point to another during the additive manufacturing process of a component / printed object. Resolution is defined as the smallest possible spatial displacement of the nozzle, which in turn depends on the control software, the minimum displacement angle of the drive motors, and the transmission ratio to the moving elements. A fundamental distinction is made between Z-resolution (resolution along the vertical axis) and XY-resolution (the smallest movement the nozzle is capable of within a single layer). Z-resolution is simply another term for the layer thickness of the concrete or mortar strand (layer thickness is the measurement of the height of horizontally successive individual material layers or strands). Z-resolution, or layer thickness, is one of the essential technical characteristics of 3D printers.The number of layers required to produce a component / printed object also determines the object's production time. Other factors include the nozzle diameter of the dispensing opening from which the 3D printing material (concrete or mortar) emerges, the metering accuracy of the 3D printing material, the repeatability of the material placement / application, the flow or spray behavior of the 3D printing material after exiting the nozzle, the setting and hardening behavior of the printed 3D printing material, and the shrinkage, creep, and thermal behavior of the set or hardened 3D printing material.
[0131] The tolerance of the 3D printer system is the maximum deviation of the defined component / printed object dimensions in the digital drawing from the dimensions of the finished printed component / printed object.
[0132] The following values can be achieved with the present invention: 1.) Z-resolution:
[0133] for thick-current processes, contract processes acc. Fig. 4 Minimum layer thickness 1 mm, maximum layer thickness 50 mm for spraying and application methods according to [relevant standard / regulation]. Fig. 5 Minimum layer thickness 2 mm, maximum layer thickness 50 mm 2.) Tolerance:
[0134] for thick-current processes, contract processes acc. Fig. 4 : 0.5% (corresponds to 5 mm / 1000 mm) for spraying methods, application methods acc. Fig. 5 : 1.0% (corresponds to 10 mm / 1000 mm)
[0135] For conventional shotcrete nozzles, e.g. with nozzles for the dry spraying process, the following values can be assumed based on experience: 1.) Z-resolution:
[0136] Minimum layer thickness >50mm 2.) Tolerance:
[0137] >5.0% (corresponds to 50 mm / 1000 mm)
[0138] The lateral boundaries of the sprayed or printed "paths" are particularly problematic with a conventional shotcrete nozzle, making the nozzle unsuitable for precise 3D printing with concrete / mortar. This is primarily due to the undefined spray pattern resulting from the nozzle design (undefined edges of the spray pattern, no precise boundary possible). List of reference symbols
[0139] 1 Mixing tube 2 Main opening 3 Auxiliary opening 4 Shaft 5 Mixing elements 6, 6' Discharge opening 7 Shaft bearing 8, 8' Connection coupling 9 Motor 10 Valve 13 3-way valve 14 Incoming concrete / mortar 14a, 14b Strands 15 Concrete / mortar strand 16 Compressed air inlet 17 Compressed air chamber 18 Spray jet 21 Nozzle 22 First section 23 Second section 24 Mixer 25 Inlet opening 26 Hose 29 Hose 30 Reinforcing element 31 Compressed air lines 32, 32' Robot 34 Crossbars 35 Longitudinal bars 36 Interrupter valve 37 Solenoid valve 38 Solenoid valve 39 Solenoid valve 40 Rinsing water 41 Wear sleeve 42, 42' Motor 43, 43' Linkage 44 Bevel gear 45 Rotating body 46 Conical gear 47, 47' Smoothing element 51, 52 Half-shells 53 Double arrow 54 Double arrow 55, 55' Pinion 56, 56' Gear 57 Component 58 Grooves
Claims
1. A 3D printer system for dispensing concrete, mortar or the like with a nozzle (21) having a main opening (2) for supplying the concrete, mortar or the like, with at least one additional opening (3) for supplying at least one additive, as well as a discharge opening (6) for discharging the concrete mixed with the additive, mortar or the like, characterised in that an actively driven mixing mechanism (24) having a mixing tube (1) is provided between the additional opening (3) and the discharge opening (6), and the internal diameter of the mixing tube (1) is 2 - 8 cm, preferably 2 - 6 cm, most preferably 2 - 4 cm.
2. The 3D printer system according to claim 1, characterised in that in the mixing tube (1) a mixing tool having mixing elements (5) is provided which are formed as blades, paddles, rods or as a screw thread or as a plurality of screw threads.
3. The 3D printer system according to claim 2, characterised in that the nozzle has a first section (22) and a second straight section (23), wherein the main opening (2) is provided at the beginning of the first section (22) and the discharge opening (6) is provided at the end of the second section (23), in that the mixing mechanism (24) has a shaft (4) which is arranged coaxially in the second section (23) and carries the mixing elements (5), in that the shaft (4) penetrates the second section (23) opposite to the discharge opening (6), and in that a motor (9) is provided outside the nozzle (21) for driving the shaft (4).
4. The 3D printer system according to claim 3, characterised in that the shaft (4) is formed like a crankshaft and is preferably provided with mixing elements in the form of transverse rods (34) and / or longitudinal rods (35).
5. The 3D printer system according to claim 3 or 4, characterised in that the internal angle (β) between the first section (22) and the second section (23) is obtuse, preferably at least 120°.
6. The 3D printer system according to any of claims 1 to 5, characterised in that the angle between the longitudinal axis of the mixing tube (1) and the discharge direction of the nozzle is maximum 75°, preferably maximum 30°, more preferably maximum 10°, in particular about 0°.
7. The 3D printer system according to any of claims 1 to 6, characterised in that a valve (10), preferably a pinch valve which can be actuated pneumatically, is provided between the mixing mechanism (24) and the discharge opening (6) for short-term stopping the flow of material.
8. The 3D printer system according to any of claims 1 to 7, characterised in that the nozzle (21) includes an inlet (16) for compressed air for blowing out the concrete, mortar or the like.
9. The 3D printer system according to any of claims 1 to 8, characterised in that in the region of the additional opening (3) a 3 way valve (13), preferably a needle valve, is provided which can interrupt the contact zone of the additive to the concrete, mortar or the like, and in that a flushing fluid can be supplied via the 3 way valve (13), too.
10. The 3D printer system according to any of claims 1 to 9, characterised in that the nozzle consists of two half shells (51, 52) for the purpose of cleaning and maintenance work, wherein a wear sleeve (41) resting against the wall of the mixing tube is preferably placed within the two half shells (51, 52).
11. The 3D printer system according to any of claims 1 to 10, characterised in that the nozzle includes a smoothing member (47) which can be rotated around the discharge opening (6) without any limit and the pitch of which may be adjusted with respect to the axis of the discharge opening (6).
12. The 3D printer system according to claim 11, characterised in that with respect to the discharge opening (6) a further smoothing member (47') is provided opposite to the smoothing member (47).
13. The 3D printer system according to claim 11 or 12, characterised in that the smoothing member (47) and, optionally, also the further smoothing member (47') is substantially planar and a normal to this plane intersects the axis of the discharge opening (6).
14. The 3D printer system according to any of claims 1 to 13, characterised in that the nozzle includes two discharge openings (6, 6') which are spaced apart from one another such that a reinforcing element (30) in the form of strips, grids, ribbons, braids, laid webs, mats, rods or threads can be positioned between the discharge openings (6, 6') and can be deeply encased by concrete / mortar.
15. 3D printer system according to any of claims 1 to 13, characterised in that a second identical nozzle and a controller are provided which guides the two nozzles (21, 21') synchronously to both sides of a reinforcing element.
16. A use of a 3D printer system according to any of claims 1 to 15 for manufacturing of 3D printed objects and components based on concrete, mortar or the like, characterised in that a setting accelerator, preferably a solution based on aluminium sulphate, is fed through the additional opening (3) as an additive.
17. The use according to claim 16, characterised in that, in addition to the setting accelerator, at least one further additive, in particular water, colour paste, air-entraining agent, superplasticiser, retarder, thickener, binder, filler, aggregates and / or fibres, is fed.
18. The use according to claim 16 or 17, characterised in that a dry concrete or a dry mortar is used, which in close proximity to the nozzle is added by and mixed with water and fed to the nozzle via a hose.
19. The use according to any of claims 16 to 18, characterised in that after the application of concrete, mortar or the like layer by layer, the resulting grooves are filled by spraying with a nozzle of a 3D printer system according to claim 8, wherein optionally reinforcing elements, in particular reinforcing grids, are previously placed on the grooved surface for the purpose of reinforcing the component.
20. The use according to any of claims 16 to 19, characterised in that a reinforcing element (30) is coaxially embedded and injected and sprayed, respectively, by the application of concrete / mortar from two sides by means of two nozzles (21, 21') guided spatially independently from one another.
21. The use according to any of claims 16 to 20 of a 3D printer system according to claim 14, characterised in that a homogeneous, reinforcing reinforcement mesh is constructed inside the component by an overlapping positioning of individual reinforcement elements (30).