METHOD FOR THE PRODUCTION OF MAGNESIUM HYDROXIDE

DE502021005691D1Active Publication Date: 2024-11-28NABALTEC AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502021005691
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-29
Publication Date
2024-11-28
Estimated Expiration
2041-06-29

AI Technical Summary

Technical Problem

Current processes for producing magnesium hydroxide often result in products with high specific surface areas and salt contamination, making them unsuitable for flame retardant applications in plastics due to high processing costs and inefficiencies.

Method used

A process involving the rehydration of caustic magnesium oxide added to an aqueous medium at a controlled rate, followed by stirring, separation, and drying, to produce magnesium hydroxide with a low specific surface area and minimal salt impurities, using a simple synthesis apparatus and avoiding pressure conditions.

Benefits of technology

This method effectively reduces salt contamination and achieves crystalline magnesium hydroxide with a low specific surface area, suitable for plastics processing, while eliminating the need for saline wastewater and allowing for a pressure-free reaction.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a process for producing magnesium hydroxide by rehydrating caustic magnesium oxide while adding the magnesium oxide to an aqueous medium.

[0002] Magnesium hydroxide (MDH) is used, among other things, as a flame retardant in plastics. Both naturally occurring and ground MDH and synthetic MDH are used. Crystallized synthetic MDHs offer advantages in processing and in the mechanical and flame-retardant properties of the final product.

[0003] Magnesium hydroxide has advantages, especially at processing temperatures, which already cause the decomposition of aluminum hydroxide, the halogen-free flame retardant currently used most frequently.

[0004] The relatively low market share of magnesium hydroxide in this application area is due to its high market price, which is due to expensive starting materials or expensive process management. For example, EP 0 791 559 B1 describes the hydrothermal production of magnesium hydroxide. The disadvantage here is the need to operate the process under pressure.

[0005] Magnesium hydroxides are produced commercially by precipitation from magnesium chloride solutions with a base or by rehydration of magnesium oxide with water. However, each method yields different products with different uses and applications. For example, it is advantageous for magnesium hydroxide to have a low specific surface area as a flame retardant.

[0006] The addition of a base, such as sodium hydroxide, to magnesium chloride results in the precipitation of magnesium hydroxide. Due to the rapid precipitation process, this results in very high specific surface areas, usually greater than approximately 20 m² / g.

[0007] DE 103 04 314 A1 describes processes for producing magnesium hydroxide with a defined particle size and shape by hydroxide formation. This is achieved by continuously feeding the reactants into a system consisting of a loop reactor and an associated clarification device. A concentrated to saturated magnesium salt solution, in which magnesium chloride is the main component, is used as a reactant. The magnesium hydroxide thus obtained has a comparatively high particle size distribution and a specific surface area of ​​more than 8 m² / g. Further publications describing the precipitation of magnesium hydroxide using magnesium salts and a base include US 4,695,445 A, US 2010 / 0011993 A1, and US 4,098,762 A.

[0008] US 2021 / 114891 A1 describes a material containing magnesium hydroxide in which a surface treatment agent is added to a suspension of the material.

[0009] A disadvantage of the processes described above is the presence of salts, particularly chlorides, as impurities in the resulting magnesium hydroxide. Furthermore, the magnesium hydroxides obtained have a high specific surface area.

[0010] In addition to the precipitation of magnesium salt solutions, rehydration of magnesium oxide is also possible. This can be achieved by dehydrating or calcining a precipitated magnesium hydroxide or a naturally occurring magnesium-containing mineral in calcination units, or by spray roasting or pyrohydrolysis of a magnesium chloride solution. This process is similar to spray drying. The difference lies in the significantly higher process temperature, which leads to the decomposition of the MgCl2 into MgO and HCl. The HCl produced during the decomposition can be used to produce additional magnesium chloride (DE 103 04 314 A1).

[0011] In the rehydration of magnesium oxide to produce magnesium hydroxide, it was found in EP 0 568 488 A2 that the use of magnesium oxide with a BET surface area of ​​3-10 m 2 / g leads to a particulate magnesium hydroxide with a specific surface area of ​​13-30 m 2 / g. In this process, magnesium oxide is added to deionized water at 90°C at a concentration of 200 g / l. However, lower specific surface areas would be advantageous for applications in flame retardant applications.

[0012] There is therefore a need for improved processes for the production of magnesium hydroxide with a low specific surface area and the lowest possible amounts of salt impurities. Furthermore, the reaction should be simple and preferably crystallized products should be obtained, which are more suitable than ground products, for example, because they can be processed more effectively in plastics.

[0013] An object of the present invention is therefore to provide such a method.

[0014] The object is achieved by a process for the preparation of magnesium hydroxide by rehydration of caustic magnesium oxide comprising the steps a) adding the magnesium oxide to an aqueous medium with stirring; b) continuing stirring after the addition of the magnesium oxide without further addition; c) separating the resulting magnesium hydroxide; d) drying the magnesium hydroxide, characterized in that the addition is carried out at a rate of not more than 500 grams of MgO / (liter × hour).

[0015] It has been surprisingly discovered that by rehydrating magnesium oxide to magnesium hydroxide, hydroxides with the desired low specific surface area can be obtained by controlling the addition rate. This also avoids or at least reduces salt contamination by avoiding magnesium salts as starting materials. Furthermore, the production can be carried out using a simple synthesis apparatus and a simple reaction procedure. Furthermore, crystalline products are obtained. Furthermore, no saline wastewater is produced, and a pressureless reaction is possible.

[0016] The magnesium oxide used is caustic magnesium oxide. This can be obtained by calcination at a temperature in the range of 600°C to 1000°C, preferably 800°C to 900°C. The starting material is typically magnesium carbonate. Caustic magnesium oxide typically has a specific surface area according to the BET method (DIN ISO 9277:2014-01) of 1 m² / g to 200 m² / g, so that in the context of the present invention, caustic magnesium oxide is understood in particular to mean a magnesium oxide with a BET surface area in this range. Preferably, however, in the context of the present invention, caustic magnesium oxide is understood to mean a magnesium oxide which has a specific surface area according to the BET method in the range from 1 m 2 < / g to 30 m 2 < / g, preferably in the range from 2 m 2 < / g to 20 m 2 < / g, more preferably in the range from 3 m 2 < / g to 15 m 2 < / g.

[0017] Caustic magnesium oxide typically exhibits small crystallites with moderate to high activity. It is characterized by its comparatively good solvency and differs from hard-burned magnesium oxide (1100°C - 1650°C) and dead-burned magnesium oxide (up to 2200°C) ("THE EFFECTS OF HYDRATING AGENTS ON THE HYDRATION OF INDUSTRIAL MAGNESIUM", OXIDEKGABO PHILLEMON MATABOLA, Master's thesis, University of South Africa, November 2006).

[0018] The activity of magnesium oxide is largely determined by the degree of calcination (temperature, residence time) and is also reflected in the BET surface area. "Dead-burned" MgO is dead-burned and can no longer be hydrated (calcination temperatures from approximately 1600-1700°C). Caustic MgO is still active and can react with water to form magnesium hydroxide. However, if the MgO is too active, hydroxides with a low BET cannot be produced. This MgO hydrates so quickly that only high BET surface areas result. Furthermore, the magnesium hydroxide is present in the form of relatively large and stable aggregates. Increasing the calcination temperature thus leads to weaker activity and hydration rates.

[0019] While the specific surface area provides indirect information about the reactivity of magnesium oxide, a direct determination is also possible. Two methods exist for determining activity. The most commonly used method uses citric acid, the other uses acetic acid. The underlying test is described in C.A. Strydom et al., Journal of Thermal Analysis and Calorimetry, 80 (2005), 659-662, and "THE EFFECTS OF HYDRATING AGENTS ON THE HYDRATION OF INDUSTRIAL MAGNESIUM," OXIDEKGABO PHILLEMON MATABOLA, Master's thesis, University of South Africa, November 2006, especially page 44.

[0020] In the context of the present invention, the activity was determined as follows. A 0.40 N citric acid solution was prepared. To prepare this solution, 28 g of citric acid and 2 ml of phenolphthalein were placed in a measuring cylinder. The measuring cylinder was then filled to one liter with distilled water. A sodium hydroxide solution was also prepared. For this purpose, 40 g of NaOH platelets were dissolved in distilled water, and the solution was then filled to exactly one liter with distilled water. For standardization, 100 ml of the prepared citric acid solution was titrated with sodium hydroxide solution. From 40 ml of sodium hydroxide solution added, the solution should turn pink, due to the added indicator. In this case, the solution was prepared correctly and can be used for the activity test. To carry out the activity test, 100 ml of the citric acid solution was placed in a beaker. The solution was then heated to 30°C.A temperature deviation of 0.2 °C is within the tolerance range. The stirrer speed is set to 500 rpm. Then, 2 g of the magnesium oxide sample to be tested is weighed onto a watch glass. A deviation of 0.05 g is the tolerance range. The weighed sample is then added in one portion to the citric acid solution, and the time is recorded until the solution turns pink. This time is given in seconds.

[0021] In the context of the present invention, the magnesium oxide used preferably has an activity in the range of 30 seconds to 600 seconds, more preferably from 70 s to 400 s, further more preferably from 90 s to 300 s.

[0022] The magnesium oxide can be added dry in powder form, so that only the aqueous medium needs to be used to determine the volume and the addition rate. Preferably, however, the magnesium oxide is added in the form of a suspension. In this case, the volume of the suspension must also be added to calculate the addition rate. The suspension is preferably well dispersed. This can be achieved, for example, using a dispersing stirrer or a stirred ball mill.

[0023] The aqueous medium into which the magnesium oxide is added can be water, an aqueous solution, or an aqueous suspension that already contains magnesium hydroxide, for example. However, water, especially demineralized water, is preferably used.

[0024] The aqueous medium preferably has a temperature in the range of 1°C to 250°C, more preferably in the range of 20°C to 150°C, even more preferably in the range of 60°C to 100°C, even more preferably in the range of 60°C to <100°C. The rehydration can be carried out under elevated or reduced pressure. However, it is preferred to carry out the rehydration without elevated pressure, so that it takes place at atmospheric pressure.

[0025] Preferably, the addition rate is in the range of 0.1 g / (l×h) to 500 g / (l×h), more preferably in the range of 1 g / (l×h) to 200 g / (l×h), further more preferably in the range of 3 g / (l×h) to 30 g / (l×h).

[0026] The magnesium oxide can be added continuously or discontinuously. If the process according to the invention is carried out discontinuously, it is preferred that the total amount to be introduced be added in at least 2, preferably at least 3, more preferably at least 4, more preferably at least 5, portions. It is further preferred that all portions have the same quantitative proportion. Furthermore, it is preferred that the time intervals between two consecutive additions of portions be equal. This time interval is further preferably at least 0.5 hours.

[0027] It is preferred that after complete addition of the magnesium oxide, a calculated total concentration of magnesium oxide is in the range of 10 g / l to 500 g / l, more preferably in the range of 50 g / l to 400 g / l, further more preferably in the range of 150 g / l to 300 g / l.

[0028] The term "calculated concentration" takes into account the fact that some of the magnesium oxide has already been converted into magnesium hydroxide before the magnesium oxide is completely added. Therefore, the calculated concentration is composed of the added amount of MgO and the total volume of the aqueous medium and, if applicable, the MgO suspension.

[0029] After step a), further steps are carried out resulting in the process according to the invention, the further steps comprising b) continuing stirring after the addition of the magnesium oxide without further addition; c) separating the resulting magnesium hydroxide; d) drying the magnesium hydroxide.

[0030] Stirring in step b) is preferably continued for a period of at least 3 hours, preferably at least 5 hours, more preferably at least 10 hours, further more preferably at least 15 hours, and further more preferably at least 20 hours. For example, the separation in step c) can be carried out by filtration. The magnesium hydroxide in step d) is preferably dried using a mill-dryer. Due to the low milling power, the crystalline primary crystals are largely retained. However, any coarse agglomerates and aggregates present are very reliably comminuted and reduced.

[0031] The magnesium hydroxide obtained preferably has a BET specific surface area of ​​less than 8 m 2 / g.

[0032] The present invention is described using the following examples, without the invention being exclusively limited thereto. Examples

[0033] All reported particle size distributions were determined using a Cilas 1064. Prior to measurements, 0.1% sodium pyrophosphate was added to each sample as a dispersant and subjected to ultrasonic treatment for 140 seconds. Measurements were performed using the Fraunhofer method.

[0034] The specific surface area was determined using a Tristar II 3020 including a degasser FlowPrep 060 from Micromeritics GmbH.

[0035] To determine the activity of the magnesium oxide samples used, a 0.40 N citric acid solution was prepared. To prepare this solution, 28 g of citric acid and 2 ml of phenolphthalein were placed in a measuring cylinder. The measuring cylinder was then filled to one liter with distilled water. A sodium hydroxide solution was also prepared. For this purpose, 40 g of NaOH platelets were dissolved in distilled water and the solution was then filled to exactly one liter with distilled water. To carry out the activity test, 100 ml of the citric acid solution was placed in a beaker. The solution was then heated to 30°C. The stirrer speed was set to 500 rpm. 2 g of the magnesium oxide sample to be tested was then weighed onto a watch glass. The weighed sample was then added all at once to the citric acid solution and the time was recorded until the solution turned pink.This time is given in seconds.

[0036] The following magnesium oxides were used in the experiments: Designation MgO 1 MgO2 BET (m 2 < / g) 3 - 4 10 - 15 Activity(s) 240 - 280 110 - 210 Loss on ignition (%) 1,7 - 3,0 0,5 - 1,8 Example 1

[0037] To 1.5 liters of demineralized water, which was continuously stirred at 80°C, 30 g of magnesium oxide MgO 1 were added every hour until a total of 150 g was reached. The magnesium oxide was added at a rate of 20 g per hour per liter until a quantity of 100 g of magnesium oxide per liter of water was reached. After the final addition, the suspension was stirred for a further 3 hours at 80°C, then filtered and dried. The BET measurement gave a value of 5.2 m 2 / g. The loss on ignition was 30.4 wt.%. Example 2

[0038] To 1.5 liters of demineralized water, which was continuously stirred at 80°C, 30 g of magnesium oxide (MgO2) were added every hour until a total of 150 g was reached. The magnesium oxide was added at a rate of 20 g per hour per liter until a quantity of 100 g of magnesium oxide per liter of water was reached. After the final addition, the suspension was stirred for a further 3 hours at 80°C, then filtered and dried. The BET measurement gave a value of 6.9 m2 / g. The loss on ignition was 27.1 wt.%. Example 3

[0039] To 1.5 liters of demineralized water, which was continuously stirred at 80°C, 30 g of magnesium oxide (MgO2) were added every three hours until a total of 150 g was reached. The magnesium oxide was added at a rate of 6.7 g per hour per liter until a quantity of 100 g of magnesium oxide per liter of water was reached. After the final addition, the suspension was stirred for a further 20 hours at 80°C, then filtered and dried. The BET measurement gave a value of 5.4 m2 / g. The loss on ignition was 28.9 wt.%. Example 4

[0040] To 1.5 liters of demineralized water, which was continuously stirred at 80 °C, 30 g portions of magnesium oxide MgO 1 were added every three hours until a total amount of 300 g was reached. The magnesium oxide was thus added at a rate of 6.7 g per hour and per liter until a quantity of 200 g of magnesium oxide per liter of water was reached. After the last addition, the suspension was stirred for a further 36 hours at 80 °C, then filtered and dried. The BET measurement gave a value of 4.8 m 2 < / g. The grain size distribution had a D10 of 0.7 µm, a D50 of 2.5 µm and a D90 of 15.6 µm. The loss on ignition was 30.7 wt.%. Example 5

[0041] To 1.5 liters of demineralized water, which was continuously stirred at 80 °C, 30 g portions of magnesium oxide MgO 2 were added every three hours until a total of 300 g was reached. The magnesium oxide was thus added at a rate of 6.7 g per hour and per liter until a quantity of 200 g of magnesium oxide per liter of water was reached. After the last addition, the suspension was stirred for a further 36 hours at 80 °C, then filtered and dried. The BET measurement gave a value of 4.8 m 2 / g. The grain size distribution had a D10 of 0.7 µm, a D50 of 1.8 µm and a D90 of 14.6 µm. The loss on ignition was 29.6 wt.%. Comparison example 6

[0042] 375 g of magnesium oxide MgO 1 (250 g / l) were added to 1.5 liters of demineralized water, which was continuously stirred at 80 °C. After the final addition, which took place after the usual 5 minutes for this amount, the suspension was stirred at 80 °C for two days, then filtered and dried. This results in an addition rate of 3000 grams per liter per hour. The BET measurement gave a value of just 8.4 m 2 < / g. The grain size distribution showed a D10 of 1.2 µm, a D50 of 3.6 µm and a D90 of 11.0 µm. The loss on ignition was 30.8 wt.%. Example 7 (Upscale of Example 4 to pilot plant scale)

[0043] To 700 liters of demineralized water, which was continuously stirred at 80 °C, 14 kg portions of magnesium oxide (MgO 1) were added every three hours until a total of 140 kg was reached. Thus, the magnesium oxide was added at a rate of 6.7 g per hour per liter until a quantity of 200 g of magnesium oxide per liter of water was reached. After the final addition, the suspension was stirred for another 36 hours at 80 °C, then filtered and dried.

[0044] Filtration was performed using a chamber filter press. The filter cake was then dried and ground on a mill-dryer. During this process, four samples were taken and analyzed.

[0045] The analysis before the 4th magnesium oxide addition showed a BET of 5.1 m² / g and a loss on ignition of 31 wt%. The analysis before the 7th magnesium oxide addition showed a BET of 4.4 m² / g and a loss on ignition of 31 wt%. The analysis after complete addition and subsequent maturation for 36 h showed a BET of 3.3 m² / g and a loss on ignition of 31.1 wt%. The grain size distribution showed a D10 of 1.09 µm, a D50 of 5.07 µm, and a D90 of 12.09 µm. The final product after mill-drying had a BET of 3.9 m² / g and a loss on ignition of 31.1 wt%. The grain size distribution showed a D10 of 0.76 µm, a D50 of 2.08 and a D90 of 5.29 µm.

Claims

1. Method for producing magnesium hydroxide by rehydration of caustic magnesium oxide, comprising the steps of a) adding the magnesium oxide to an aqueous medium with stirring; b) continuing the stirring after addition of the magnesium oxide has taken place, without further adding; c) removing the magnesium hydroxide obtained; d) drying the magnesium hydroxide; characterized in that the adding takes place with a rate of addition of at most 500 g of MgO / (litre × hour).

2. Method according to Claim 1, characterized in that the magnesium oxide has a specific surface area according to the BET method in the range from 1 m2 / g to 30 m2 / g.

3. Method according to Claim 1 or 2, characterized in that the magnesium oxide has an activity in the range from 30 seconds to 600 seconds, preferably from 70 s to 400 s, more preferably from 90 s to 300 s.

4. Method according to one or more of Claims 1 to 3, characterized in that the magnesium oxide is added in the form of a suspension.

5. Method according to one or more of Claims 1 to 4, characterized in that the aqueous medium is water, an aqueous solution or an aqueous suspension, preferably fully demineralized water.

6. Method according to one or more of Claims 1 to 5, characterized in that the aqueous solution has a temperature in the range from 1°C to 250°C, preferably from 20°C to 150°C, more preferably from 60°C to 100°C, more preferably still in the range from 60°C to < 100°C.

7. Method according to one or more of Claims 1 to 6, characterized in that the rate of addition is in the range from 0.1 g / (l × h) to 500 g / (l × h), preferably from 1 g / (l × h) to 200 g / (l × h), more preferably from 3 g / (l × h) to 30 g / (l × h).

8. Method according to one or more of Claims 1 to 7, characterized in that the adding of the magnesium oxide takes place continuously or discontinuously.

9. Method according to Claim 8, characterized in that the magnesium oxide is added discontinuously in at least 2, preferably at least 3, more preferably at least 4, more preferably at least 5 portions.

10. Method according to one or more of Claims 1 to 9, characterized in that after complete addition of the magnesium oxide, a calculated total concentration of magnesium oxide in the range from 10 g / l to 500 g / l, preferably from 50 g / l to 400 g / l, more preferably from 150 g / l to 300 g / l is obtained.

11. Method according to Claim 10, characterized in that the continuing of the stirring in step b) takes place over a period of at least 3 hours, preferably at least 5 h, more preferably at least 10 h, more preferably at least 15 h, more preferably at least 20 h.

12. Method according to Claim 10 or 11, characterized in that the removing in step c) takes place by filtration.

13. Method according to one or more of Claims 10 to 12, characterized in that the drying of the magnesium hydroxide in step d) takes place with the aid of a mill dryer.

14. Method according to one or more of Claims 10 to 13, characterized in that the magnesium hydroxide obtained has a BET specific surface area of less than 8 m2 / g.