METHOD FOR RECOVERING PLATINOID PARTICLES CONTAINED IN AN ELECTRICALLY INSULATING CARRIER ELEMENT

DE602020042410T2Active Publication Date: 2024-12-04CENT NAT DE LA RECH SCI (C N R S) +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602020042410
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-31
Filing Date
2020-10-29
Publication Date
2024-12-04
Estimated Expiration
2040-10-29

AI Technical Summary

Technical Problem

Current methods for recovering platinum from proton exchange membrane fuel cells, such as pyrometallurgical and hydrometallurgical processes, are energy-intensive, generate harmful gases, and pose safety risks, while alternative processes using solvents are flammable and require high temperatures, increasing costs and complexity.

Method used

A process involving immersion of an electrically insulating support in an ionic liquid solution, comprising specific ionic liquids that stabilize and extract platinum nanoparticles without electrochemical steps, allowing for direct recovery and recycling of the support.

Benefits of technology

This method avoids high temperature and pressure treatments, reduces toxic gas emissions, optimizes safety, and enables efficient platinum recovery with reusable ionic liquids, making the process more economical and environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a method for recovering particles of platinum or another platinoid contained in an electrically insulating material, for example a fuel cell membrane.

[0002] The present invention finds, in particular, an application in the recycling of fuel cells that have reached the end of their life, in particular proton exchange membrane fuel cells, with a view to recovering the platinum present in the latter. The invention is also particularly interesting in the field of heterogeneous chemical catalysis. STATE OF THE PRIOR ART

[0003] Proton Exchange Membrane Fuel Cells (PEMFCs) convert chemical energy into electrical energy using the following half-equations: H 2 → 2H +< + 2e -< 4H +< + 4e -< + O 2 → 2H 2 O

[0004] PEMFC batteries consist of a stack of elementary electrochemical cells separated from each other by bipolar plates. These elementary electrochemical cells, also called membrane electrode assemblies and abbreviated as MEA, are formed of a membrane placed between two electrodes; this membrane is electrically insulating and ionically conductive. The electrodes of these MEAs include a catalyst, generally based on noble metals such as platinum, to catalyze the oxidation reaction of dihydrogen.

[0005] If we consider all the components that make up a PEMFC fuel cell, the cost of platinum alone represents 25% of the overall cost of such a cell.

[0006] Also, and so that the cost of platinum does not constitute an obstacle to the development of PEMFC type battery technology, there is a strong interest in setting up an efficient and economically viable process for recovering noble metals and / or platinoids, in particular, the platinum contained in the MEAs of end-of-life fuel cells and / or production scrap.

[0007] Currently, only pyrometallurgical and hydrometallurgical processes are used on an industrial scale to recover noble metals in fuel cells.

[0008] The recovery of platinum by the pyrometallurgical route consists of heating to a very high temperature (typically to a temperature ranging from 1400°C to 1700°C), in a plasma arc furnace, a mixture comprising the different components (including the catalysts) previously ground, and a flux (CaO or MgO).

[0009] Pyrometallurgical processes are effective for recovering platinum, but they have the disadvantage of consuming a lot of energy and leading to the release of significant quantities of gases that are harmful to humans and the environment. In particular, these pyrometallurgical processes can lead to the formation of carbon dioxide (CO 2 ) and toxic gases. These toxic gases include sulfur dioxide (SO 2 ) and hydrogen fluoride (HF). These two gases come from the combustion of the MEA membrane, when it is made of a perfluorocarbon polymer containing sulfonated groups. In addition, pyrometallurgical processes do not allow the recovery of the other components that make up MEAs.

[0010] The recovery of platinum by the hydrometallurgical route consists of bringing the previously crushed membrane electrode assembly into contact with a solution capable of dissolving platinum. The solution that is currently recognized as being the most effective for dissolving platinum is aqua regia, which is formed by a concentrated mixture of hydrochloric acid and nitric acid in a 1 / 3 ratio. This process makes it possible to recover, in addition to platinum, other constituent components of MEAs and, in particular, membranes, graphite or carbon electrodes. However, hydrometallurgical processes present significant risks linked to the use of concentrated acid mixtures, in particular due to the release of NOx, and to the subsequent treatment of aqueous effluents, which, in addition, generates additional costs in terms of industrial safety that can jeopardize the economic balance of such processes.

[0011] To overcome the disadvantages of the pyrometallurgical and hydrometallurgical processes just mentioned, new platinum recovery processes have recently been proposed.

[0012] For example, US 2009 / 0049954 A1 proposes a process in which the AME is cooled to -75°C and then pulverized into a powder. The resulting paste is then subjected to a leaching step, at 200°C, in an acidic medium, for example in aqua regia or concentrated hydrochloric acid with hydrogen peroxide. The platinum contained in the leachate is recovered by electrolytic deposition and / or chemical reduction. This process requires not only a cryogenic step, which makes the process complicated to industrialize, but also concentrated acid solutions at high temperatures, which requires special precautions for the treatment of effluents.

[0013] In document US 2008 / 0064771 A1, a catalyst-coated membrane is subjected to supercritical water treatment at 382°C and 240 bars for 7 hours. At the end of the treatment, a greenish solution comprising a black sediment (composed of carbon and platinum) is obtained. The fluorinated part (membrane and ionomer dispersed in the catalytic layer) is separated from the solid residue by filtration. This process requires other additional steps to be able to separate the platinum from the carbon and purify it.

[0014] Another solution is to dissolve the platinum particles with an alcoholic solution. For example, US 2007 / 0292745 A1 describes a method for recycling PEMFC fuel cell membrane / electrode assemblies. The MEA is brought into contact with an alcohol having an alkyl chain ranging from C1 to C8, which leads to the separation of the membrane from the anodic and cathodic layers. The dispersion of the ionomer film takes place by heating the solvent to a temperature ranging, for example, from 50°C to 180°C. The ionomer particles are then separated from the platinum particles, for example by filtering the solution and then carrying out, on the filtrate, a combustion of the carbon or by dissolution in an acidic medium, optionally, at temperature and pressure.

[0015] In WO 2016 / 156815 A1, the AME is immersed in a solution comprising a C 1-8 aliphatic diol comprising at least one CH 2 OH group, such as ethylene glycol. The solution can be heated to a temperature of 230°C. A subsequent filtration or centrifugation step separates the solvent and ionomers from the catalytic components.

[0016] However, these different processes require the use of alcohols which are flammable and volatile, in the presence of platinum nanoparticles, under the mentioned treatment conditions (temperature >100°C). These solutions therefore generate flammability risks. The implementation of these processes at high temperature increases the risk of explosion and therefore requires special precautions, which represents an additional economic cost. In addition, these processes are energy-intensive since they involve high pressure and temperature and / or a combustion step.

[0017] In document EP 3 263 744 A1, the process for recycling membrane / electrode assemblies from PEMFC fuel cells uses an electrolysis step. For this, the Pt / C catalytic layer with the ionomer is immersed in an electrolytic solution formed from a mixture of ionic liquids. The platinum is extracted by electro-dissolution of the platinum, and the dissolved platinum is recovered by electrodeposition on a counter-electrode. This type of process requires the electrode of the MEA to be placed on an electrical conductor, which complicates the process and increases its costs. In such a process, the conditions for electrodeposition are sensitive to concentration fluctuations, and the treatment conditions inevitably generate the degradation of the ionic liquids during electrolysis. It is therefore necessary to treat / change the ionic liquid solution regularly.Furthermore, this solution is only applicable for an electrically conductive support. However, in the case of MEAs where the membrane is coated with a catalyst (CCM for "Catalyst Coated Membrane"), the active layer is deposited directly on the membrane, a significant quantity of nanoparticles is therefore supported by the polymer membrane which is electrically insulating. This process cannot therefore be used for such materials. Document US 2010 / 206134 provides an example of the use of ionic liquids to recover metals from a catalytic support. STATEMENT OF THE INVENTION

[0018] An aim of the present invention is to propose a recycling method which overcomes the drawbacks of the prior art and, in particular, to propose a method which makes it possible to directly extract nanoparticles contained in an electrically insulating support whilst avoiding problems linked to solvents (inflammability in particular) and / or their degradation over time.

[0019] For this, the present invention proposes a method for recovering platinoid particles contained in an electrically insulating support, the method comprising an extraction step during which the electrically insulating support is immersed in an ionic liquid solution comprising a first ionic liquid, so as to extract the platinoid particles from the electrically insulating support.

[0020] Platinoid particles are particles made of an element from the MGP group (or PGM for "Platinum Group Metals"), i.e. an element that can be chosen from platinum, palladium, rhodium, ruthenium, iridium, osmium, rhenium or one of their alloys.

[0021] The invention fundamentally differs from the prior art by the separation of the platinoid nanoparticles from the electrically insulating support in an ionic liquid solution.

[0022] The anion of the first ionic liquid is chosen from halides, amines, dicyanamides and anions having a sulfur ligand such as thiocyanates. These anions have a stabilizing effect on the platinoid particles and promote their dispersion in solution.

[0023] The cation of the first ionic liquid is chosen from imidazolium, pyrrolidinium, ammonium, piperidinium, sulfonium and phosphonium. These anions promote the swelling of polymer materials, in particular ionomers, containing platinoid particles and therefore the extraction of the latter.

[0024] The process does not involve any electrochemical steps (i.e., there is no electrodissolution or electrodeposition). The invention can be used for many electrically insulating substrates. The ionic liquid solution allows the particles to be extracted from their support by simply immersing the support. In addition to being able to recover the particles directly in metallic form, the support, free of particles, can be recycled.

[0025] Advantageously, the electrically insulating support is made of a polymer material.

[0026] Advantageously, the electrically insulating support is a proton exchange membrane.

[0027] Advantageously, the particles are nanoparticles having a largest dimension less than 1µm.

[0028] Advantageously, the step of extracting the platinoid particles is carried out with stirring.

[0029] Advantageously, the extraction step is carried out at a temperature ranging from 20°C to 180°C, preferably from 60 to 150°C, for example 80°C.

[0030] Advantageously, the duration of the extraction step ranges from 2 minutes to 2 days, preferably from 2 hours to 18 hours, for example 6 hours.

[0031] Advantageously, the ionic liquid solution comprises a second ionic liquid.

[0032] Advantageously, the ionic liquid solution comprises from 55% to 100% molar of the first ionic liquid and from 0% to 45% of the second ionic liquid.

[0033] The process has many advantages: avoid high temperature and / or high pressure treatments, optimize industrial safety and environmental safety conditions because the process does not generate toxic gases, such as NOx, and does not use highly concentrated acid (aqua regia or pirhana mixture), do not use organic solvents that are dangerous for humans and the environment, limit the risks of flammability and explosion, recover both the nanoparticles and the support, do not require dissolving and then reducing the platinoid, be economical since the ionic liquid solution is not degraded and can be reused, be easy to implement, for any type of support.

[0034] The invention also relates to a method for recovering platinoid particles contained in membrane electrode assemblies of a fuel cell, such as a PEMFC proton exchange membrane fuel cell, preferably used or discarded, this method comprising the following successive steps: (a) a step of separating the membrane electrode assemblies and the bipolar plates of the fuel cell, (b) a step of separating the membrane and the electrodes of each membrane electrode assembly separated in step (a), and (c) a step of recovering the platinoid particles contained in the membrane by implementing the recovery method described above.

[0035] Other characteristics and advantages of the invention will emerge from the additional description which follows.

[0036] It goes without saying that this additional description is given only as an illustration of the subject of the invention and must in no case be interpreted as a limitation of this subject. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The present invention will be better understood by reading the description of exemplary embodiments given purely for informational purposes and in no way limiting, with reference to the appended drawings in which: There figure 1 represents, schematically, and in section, a membrane electrode assembly according to a particular embodiment of the invention, The figure 2 is a photograph obtained by transmission electron microscopy of the catalytic powder used for the manufacture of an electrode, according to a particular embodiment of the invention, The Figures 3A and 3Bare images obtained by transmission electron microscopy, at different scales, of the ionic liquid solution at the end of the extraction process, according to a particular embodiment of the invention.

[0038] The different parts represented in the figures are not necessarily on a uniform scale, to make the figures more readable.

[0039] The different possibilities (variants and embodiments) must be understood as not being mutually exclusive and can be combined with each other. DETAILED DESCRIPTION OF SPECIFIC EMBODIMENTS

[0040] Subsequently, even if the description refers to a membrane of a fuel cell, and in particular to a membrane of a low-temperature fuel cell (PEMFC, DMFC), the invention can be transposed to any other membrane, and, more generally, to any other electrically insulating support supporting metallic particles, and in particular particles of the platinoid type (i.e. particles of ruthenium, rhodium, palladium, osmium, iridium, rhenium and platinum, alone or in a mixture, or in one of their alloys). By way of illustration and non-limiting example, the support may be a ceramic, for example from a catalytic converter.

[0041] Although this is in no way limiting, the invention particularly finds applications in the field of recycling membrane / electrode assemblies (MEA).

[0042] There figure 1represents a membrane electrode assembly 100 (MEA or AME for “Membrane Electrode Assembly”) of a fuel cell. The AME 100, also called the cell core, comprises a membrane 110 covered on both sides by a catalytic layer 120a, 120b (or CL for “catalyst layer”). Each catalytic layer 120a, 120b is itself covered by a microporous layer 130a, 130b (or MPL for “Microporous Layer”). Finally, each microporous layer is covered by a gas diffusion layer 140a, 140b (or GDL for “gas diffusion layer”).

[0043] The membrane 110 is an electrolytic membrane allowing the selective passage of protons between the electrodes (anode and cathode). The membrane 110 comprises, for example, a perfluorosulfonated ionomer (PFSA), such as Nafion ® marketed by the company Dupont.

[0044] The catalytic layers 120a, 120b are also called active layers or electrodes. Each catalytic layer 120a, 120b comprises a carbon support 121, catalytic particles 122, and optionally an ionomer 123.

[0045] The carbon 121 support is, for example, in the form of aggregates.

[0046] The catalytic particles 122 are supported by the carbon support 121.

[0047] Particles are defined as elements of shape, for example, spherical, elongated, or ovoid. They can have a larger dimension, for example the diameter in the case of spherical particles, ranging from 2nm to 5µm. This size can be determined by photon correlation spectroscopy.

[0048] The particles 122 are advantageously nanoparticles to accelerate the hydrogen dissociation reactions at the anode and the oxygen reduction reactions at the cathode. They have a larger dimension ranging from 1nm to 1µm, and preferably from 1nm to 50nm, and even more preferably from 2nm to 5nm.

[0049] The catalytic particles 122 are made of platinoid. The platinoid element is chosen from platinum, iridium, palladium, ruthenium and osmium, alone or in a mixture, or one of their alloys. The alloy may contain several (two or three for example) of the aforementioned atomic elements. For example, it is an alloy of platinum and palladium. According to another alternative, it may contain one or more of the aforementioned atomic elements in association with one or more metallic elements other than platinoids, in particular with one or more other transition metals. For example, it is an alloy of platinum and cobalt.

[0050] The catalytic layer 120a, 120b may further comprise an ionomer 123, i.e. a polymer having an ionized group allowing charge transport. Advantageously, it is identical to that constituting the membrane. According to an alternative embodiment, it is different from that constituting the membrane.

[0051] The AME 100 can be manufactured by forming the catalytic layer 120a, 120b on the membrane 110 (CCM for “Catalyst Coated Membrane”) or by forming the catalytic layer 120a, 120b on the gas diffusion layer 140a, 140b (CCB for “Catalyst Coated Backing”).

[0052] To extract the particles 122 from their support, here the membrane 110, the membrane 110 is first separated from the other elements of the AME 100, and in particular from the gas diffusion layers 140a, 140b, and the microporous layers 130a, 130b.

[0053] The catalytic layers 120a, 120b can remain integral with the membrane 110. It is also possible to separate the membrane 110 from one or both catalytic layers 120a, 120b.

[0054] In a first alternative, this separation step can be carried out by immersing the AME 100 in a 50 / 50 water / ethanol solution by volume so as to cause swelling of the membrane 110 and to break the bonds between the active layer 120a, 120b and the membrane 110. At the end of this step, catalytic particles 122 remain supported by the membrane 110. The membrane 110 is then immersed in the ionic liquid solution to extract the catalytic particles 122.

[0055] According to a second alternative, the AME 100 is immersed in the ionic liquid solution, which makes it possible, in one step, to separate the membrane 110 from the other constituents of the AME 100 and simultaneously to extract the particles 122 supported by the membrane 110. Advantageously, this alternative also makes it possible to extract the platinoid particles contained in the catalytic layers when the latter are immersed in the ionic liquid solution.

[0056] By immersion is meant that it is at least partially immersed and preferably completely immersed in the ionic liquid solution.

[0057] The immersion of the membrane 110 in the solution generates the extraction of the particles 122 from their support and their suspension in metallic form in the ionic liquid solution.

[0058] The particle extraction step 122 is carried out without an electrochemical step, that is to say without imposing current (or voltage) in the sample.

[0059] The support containing the particles 122 to be extracted can be attached to another element or float in the solution.

[0060] The ionic liquid solution makes it possible to swell the membrane 110 to facilitate the extraction of the particles 122, and to stabilize the particles 122 while preventing their dissolution.

[0061] The ionic liquid solution comprises an ionic liquid or a mixture of ionic liquids. Ionic liquids are non-volatile, non-flammable solvents that are chemically stable at temperatures above 200°C. An ionic liquid is a combination of at least one cation and one anion that generates a liquid with a melting point below or close to 100°C.

[0062] The solution contains at least one ionic liquid known as a stabilizing (or complexing) liquid. A stabilizing ionic liquid is an ionic liquid that promotes the complexation of platinum nanoparticles and has a complexing power that allows the stabilization of the nanoparticles in solution in the form of a suspension.

[0063] When the solution contains an additional ionic liquid, it is advantageously a solvent ionic liquid. A solvent ionic liquid is an ionic liquid that does not allow the dissolution of platinum and has little or no complexing power on platinum.

[0064] The first ionic liquid (stabilizing ionic liquid) is formed by a first organic cation and a first inorganic anion.

[0065] The second ionic liquid (solvent ionic liquid) is formed by a second organic cation and a second inorganic anion.

[0066] The cation of the first ionic liquid and the cation of the second ionic liquid are advantageously chosen from the cations of the family: imidazolium, pyrrolidinium, ammonium, piperidinium, sulfonium and phosphonium.

[0067] Advantageously, the first and second organic cations may be chosen from the group consisting of a tetraalkylammonium, a N,N- dialkylimidazolium, a N,N -dialkylpyrrolidinium, a tetraalkylphosphonium, a trialkylsulfonium and a N,N -dialkylpiperidinium.

[0068] Preferably, it is a phosphonium cation. This cation is stable and promotes swelling of the ionomer, which facilitates the extraction of the platinoid particles from their support.

[0069] More advantageously, a cation having C2-C14 alkyl or fluoroalkyl chains will be chosen, typically the cation [P66614] +< (trihexyltetradecylphosphonium).

[0070] Preferably, the cation of the first ionic liquid and the second ionic liquid are the same to increase the solubility of the second ionic liquid in the first ionic liquid.

[0071] The anion of the first ionic liquid is a complexing / stabilizing or coordinating anion chosen, for example, from the family of halide (Cl -< , Br -< , I -< ), the family of amines, for example dicyanamides N(CN) 2 -< noted DCA -< and / or an anion possessing a sulfur ligand such as thiocyanates SCN -< .

[0072] The anion of the second solvent ionic liquid is either organic or inorganic. It has no or very little complexing affinity. Advantageously, anions will be used which make it possible to obtain a low viscosity, a low melting temperature (liquid at room temperature) and / or good solubility with the first ionic liquid. The anion of the second ionic liquid is, for example, chosen from the anions bis(trifluoromethanesulfonyl)imide (CF 3 SO 2 ) 2 N -< denoted TFSI -< , bis(fluorosulfonyl)imide (FSO 2 ) 2 N -< denoted FSI -< , trifluoromethanesulfonate or triflate CF 3 SO 3 -< , tris(pentafluoroethyl)trifluorophosphate denoted FAP -< and bis(oxalato)borate denoted BOB -< . Advantageously, the TFSI anion will be chosen.

[0073] More advantageously, the mixture of ionic liquids is liquid at room temperature.

[0074] For example, we will choose a mixture comprising [P66614][CI] as the first ionic liquid and [P66614][TFSI] as the second ionic liquid.

[0075] In an advantageous variant of the invention, the solution may comprise: from 50 mol% to 100 mol%, and preferably from 55 mol% to 100 mol%, of the first ionic liquid, and from 0 mol% to 50 mol%, and preferably from 0% to 45 mol%, of the second ionic liquid.

[0076] The molar concentration of the first ionic liquid ranges, for example, from 2mol / L to 6mol / L.

[0077] The molar concentration of the second ionic liquid ranges, for example, from 0mol / L to 4mol / L.

[0078] The ionic liquid solution may, optionally, further comprise an anhydrous drying agent or an agent promoting the transport of matter.

[0079] The anhydrous drying agent is, for example, selected from MgSO 4 , Na 2 SO 4 , CaCl 2 , CaSO 4 , K 2 CO 3 , NaOH, KOH, and CaO.

[0080] The agent promoting the transport properties can be a salt or the association of a third ionic liquid.

[0081] The ionic liquid solution is preferably stirred during the extraction step to promote extraction kinetics.

[0082] After suspending the particles 122, the membrane 110 is extracted from the bath and the particles 122 can be separated from the solution by conventional liquid / solid separation techniques such as, for example, centrifugation, ultrafiltration (membrane techniques), or filtration. The ionic liquid solution is reusable to carry out a new treatment cycle.

[0083] The extraction process described above is particularly interesting for recycling fuel cells, particularly of the PEMFC type. The process for recycling such cells includes a step during which the bipolar plates are separated from the different AMEs, for example by a manual operation. The AME is then recovered according to the process described above. The bipolar plates can also be advantageously recovered. Illustrative and non-limiting examples of an embodiment:

[0084] In this example, a CCM type AME 100 is recycled, i.e. manufactured using a process during which the catalyst is deposited on the membrane 110 (“Catalyst Coated Membrane”). figure 2 is a photograph obtained using a transmission electron microscope (TEM) of the catalyst deposited on a pristine electrode (or virgin electrode corresponding to the new electrode).

[0085] First, the proton exchange membrane and the catalytic layer are separated from the microporous layer.

[0086] The recycling process is carried out on a sample with a surface area of ​​1cm 2< .

[0087] The composition of the sample is listed in the following Table I: Pt Nation C Loading in Pt Size of NPs 34% 26% 40% 0.19 mg Pt / cm 2< 3,0 ± 0,6

[0088] The sample is composed of platinum, carbon black and ionomer.

[0089] The sample is placed in a pillbox containing 1 mL of ionic liquid solution of trihexyltetradecylphosphonium chloride (P66614Cl). The sample is immersed in the ionic liquid at a temperature of 80°C with stirring at 400 rpm for 6 hours. The stirrer is at a distance from the sample.

[0090] Over time, the ionic liquid solution darkens until it reaches a black color, characterizing the suspension of the platinum nanoparticles.

[0091] After treatment, the sample is removed from the ionic liquid. TEM analysis of the ionic liquid solution indicates the presence of platinum nanoparticles (Figures 5A and 5B) which are in dispersed form.

[0092] No decomposition of the ionic liquid is observed by NMR after treatment. By separating the particles from the liquid phase, the ionic liquid solution can be reused for a new cycle.

Claims

1. A method for recovering platinoid particles (122) contained in an electrically insulating support (110), the method comprising an extraction step during which the electrically insulating support (110) containing the platinoid particles (122) is immersed in an ionic liquid solution comprising a first ionic liquid, characterised in that - the anion of the first ionic liquid is selected from halides, amines, dicyanamides and the anions having a sulphur ligand such as thiocyanates, and - the cation of the first ionic liquid is selected from imidazolium, pyrrolidinium, ammonium, piperidinium, sulfonium and phosphonium, whereby the platinoid particles (122) of the electrically insulating support (110) are extracted from the electrically insulating support (110).

2. The method according to claim 1, wherein the electrically insulating support (110) is made of a polymer material.

3. The method according to claim 2, wherein the electrically insulating support (110) is a proton exchange membrane.

4. The method according to any one of the preceding claims, characterised in that the particles (122) are nanoparticles having a largest dimension of less than 1 µm.

5. The method according to any one of the preceding claims, wherein the step of extracting the platinoid particles (122) is carried out with stirring.

6. The method according to any one of the preceding claims, wherein the extraction step is carried out at a temperature ranging from 20°C to 180°C, preferably from 60 to 150°C, for example 80°C.

7. The method according to any one of the preceding claims, wherein the duration of the extraction step ranges from 2 minutes to 2 days, preferably from 2 h to 18 h, for example 6 h.

8. The method according to any one of the preceding claims s, wherein the ionic liquid solution comprises a second ionic liquid.

9. The method according to claim 8, wherein the ionic liquid solution comprises from 55 mole % to 100 mole % of the first ionic liquid and from 0 mole % to 45 mole % of the second ionic liquid.

10. The method according to any one of the preceding claims, characterised in that the cation of the first ionic liquid is a phosphonium.

11. The method according to any one of claims 1 to 9, characterised in that the cation of the first ionic liquid is a tetraalkylammonium, an N,N-dialkylimidazolium, an N,N-dialkylpyrrolidinium, a tetraalkylphosphonium, a trialkylsulfonium or an N,N-dialkylpiperidinium.

12. The method according to any one of the preceding claims, characterised in that the first ionic liquid is [P66614][CI].

13. The method according to any one of the preceding claims, characterised in that the cation of the second ionic liquid is selected from the imidazolium, pyrrolidinium, ammonium, piperidinium, sulfonium and phosphonium cations and in that the anion of the second ionic liquid is selected from the bis(trifluoromethanesulfonyl)imide (CF3SO2)2N-, bis(fluorosulfonyl)imide (FSO2)2N-, trifluoromethanesulfonate, tris(pentafluoroethyl)trifluorophosphate and bis(oxalato)borate anions.

14. The method according to claim 12, characterised in that the second ionic liquid is [P66614][TFSI].

15. The method for recovering platinoid particles (122) contained in membrane electrode assemblies (100) of a fuel cell, such as a proton exchange membrane fuel cell PEMFC, preferably used or discarded, this method comprising the following successive steps: (a) a step of separating the membrane electrode assemblies (100) and the bipolar plates of the fuel cell, (b) a step of separating the membrane (110) and the electrodes (120a, 120b) of each membrane electrode assembly (110) separated in step (a), and (c) a step of recovering the platinoid particles (122) contained in the membrane (110) by implementing the recovery method according to any one of claims 1 to 14.