METHOD FOR PRODUCING A SILICON COMPONENT
Patent Information
- Application Number
- DE602023000969
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-11
- Filing Date
- 2023-02-10
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2043-02-10
AI Technical Summary
The existing manufacturing process for silicon watch components, such as hairsprings and balance wheels, faces issues with deformation and irreversibility during thermal oxidation, leading to damage and unusability, and previous solutions like using a support plate are cumbersome and time-consuming.
A process involving a silicon-on-insulator substrate with a silicon dioxide intermediate layer, where a detachment groove is engraved in the second silicon layer to create a blind portion that links with the first layer, allowing partial removal of the intermediate layer without complete detachment, maintaining structural integrity and enabling orientation-independent processing.
This method prevents deformation during subsequent treatments, allows for easier detachment of silicon parts, and simplifies the separation process, maintaining the structural integrity of the components and facilitating their use in various applications.
Description
Technical field of the invention
[0001] The present invention relates to the manufacture of silicon parts, in particular watch components such as balance springs, anchors, escape wheels, toothed wheels, plates, hands, balance wheels. State of the art
[0002] Silicon watch components are typically manufactured using a silicon-on-insulator (SOI) substrate, also called a wafer. Such a substrate comprises a first layer of silicon in which the components are to be formed, a second layer of silicon used to stiffen the substrate, and, between these two layers of silicon, an intermediate layer of silicon dioxide serving as a stop layer for the etching operations of the first layer.
[0003] According to a known method, the first layer of silicon is etched in order to form the parts to be manufactured on the one hand and a groove surrounding said parts on the other hand. A wafer delimited by the groove and carrying the etched parts is then detached from the substrate to be generally subjected to oxidation and deoxidation operations aimed at improving the surface condition of the parts, adjusting their stiffness, and / or increasing their mechanical resistance, before they are finally detached from the wafer.
[0004] This process poses several problems. When heated to high temperatures, particularly in a thermal oxidation furnace, the wafer tends to bend under its own weight. This deformation can damage components or even detach, rendering them unusable for their intended purpose. Furthermore, the wafer's deformation is permanent and irreversible, which also precludes its use in other equipment, such as balance spring stiffness measuring equipment.
[0005] We already know, for example from application EP 3 543 795, a manufacturing method in which the wafer is supported by a support plate and turned over between each oxidation-deoxidation operation, so as to prevent or at least limit the effects of deformation of the wafer and therefore of the components.
[0006] But mounting the plate on the support plate, as well as the successive turning operations, are long and tedious.
[0007] From JP 2017 044533, a method is also known in which the second layer of an SOI type substrate is etched opposite a component formed in the first layer so as to retain a support section. Summary of the invention
[0008] The present invention aims to propose a manufacturing method making it possible to overcome the aforementioned drawbacks of the prior art.
[0009] According to the invention, this object is achieved by the subject matter of the independent claims. The more specific aspects of the present invention are described in the dependent claims as well as in the description.
[0010] More specifically, this goal is achieved with a method of manufacturing at least one silicon part, in which a) a substrate is provided comprising the superposition, in a transverse direction, of at least a first layer of silicon of thickness e1, an intermediate layer of silicon dioxide, and a second layer of silicon of thickness e2, the intermediate layer thus being interposed between the first and second layers; then, in this order or another: b) the first layer is etched to form the at least one part therein, c) in the second layer, at least one detachment groove is etched to delimit within said second layer at least one portion to be detached covering or intended to cover said at least one part, at least one portion called the blind portion of the detachment groove being etched so that a part of the second layer, forming a bond, is retained in line with said portion, d) the intermediate layer is partially removed by eliminating the silicon dioxide in line with said at least one portion to be detached or the anticipated location of said portion to be detached; and finally e) the at least one portion to be detached is mechanically separated from the rest of the substrate by breaking the bond.
[0011] The method according to the invention thus comprises the production of a detachment groove in the second layer of the substrate, to allow the detachment of a portion of this second layer and thus the release of at least one useful portion of the first layer, located opposite said portion to be detached, and carrying one or more parts.
[0012] The modified substrate obtained at the end of steps a) to e) comprises at least one reinforced part or frame, formed by the superposition of a part of the first layer and a residual portion of the second layer, linked by a part of the intermediate layer.
[0013] To ensure the preservation of such a frame, step d) is stopped after complete removal of the intermediate layer at the level of the portion(s) to be detached but before removal of the entire intermediate layer.
[0014] The modified substrate obtained by the method of the invention can thus be subjected to the same subsequent treatments as the wafer of the prior art. But its frame gives it sufficient rigidity so that it does not deform, or to a lesser extent, during these operations.
[0015] The preservation, according to the invention, of at least one link at the right of the detachment groove makes it possible to separate the steps of partial removal of the intermediate layer and effective detachment of the part to be detached. The operation of removing the silicon dioxide can thus be carried out whatever the orientation of the substrate, without risking shock between the parts and the portion to be detached. The link also makes it optional to hold the portion to be detached, for example by vacuum or electrostatic means, which makes it possible to simplify the machine used for separation.
[0016] In the present application, a link is therefore a part of the second layer delimited between the bottom of the detachment groove, etched in the second layer, and the interface plane between said second layer and the intermediate layer. A link typically forms a strip, a ribbon, a membrane extending in the plane of the substrate and whose thickness, constant or variable, is strictly less than the total thickness of said second layer.
[0017] In the following, each area of the first layer comprising one or more parts and released after detachment of a portion to be detached is called a useful portion.
[0018] A group of parts is also referred to as a set of parts facing the same portion to be detached.
[0019] A substrate is generally used for the manufacture of a plurality of parts, identical or different.
[0020] According to one example, a plurality of parts are etched in the first layer, and at least one detachment groove in the second layer defines a portion to be detached covering or intended to cover said plurality of parts.
[0021] According to one example, the detachment groove delimits, alone or in conjunction with an edge of the substrate, a closed contour.
[0022] Each portion to be detached is generally a solid portion, i.e. not engraved inside the closed contour that it delimits (alone or with the edge of the substrate).
[0023] According to one example, the detachment groove runs along the edge of the substrate, at a variable or constant distance from it, typically greater than 5 mm.
[0024] In this case in particular, at least part of the frame borders the edge of the substrate.
[0025] Advantageously, step d) may be stopped so that a width of the intermediate layer portion between the first layer and the residual portion of the second layer remains at least locally, preferably at all points, greater than 1 mm. In this way, the width remains sufficient to maintain adhesion between the two layers.
[0026] According to one example, a width of the detachment groove, measured orthogonally to the transverse direction, is less than or equal to 500 microns and advantageously greater than 50 microns.
[0027] According to one example, during step e), the part to be detached is pushed by means of at least one tool introduced through a groove etched in the first layer in step b).
[0028] Advantageously, the thickness of a link is less than the width of the detachment groove.
[0029] According to one example, the thickness of a link, measured in the transverse direction, is at least 2 microns, and preferably less than 50 microns.
[0030] The thickness of a link can be constant along the entire length of the link.
[0031] In some embodiments, however, the thickness of a link may also not be constant along its length.
[0032] According to one example, the detachment groove is etched so that a link is retained at the right of said groove over its entire length. The detachment groove is then blind over its entire length. In other words, the detachment groove extends over a thickness of the second layer strictly less than e2 over its entire length.
[0033] According to another example, the detachment groove further comprises at least one through portion on which it crosses the entire thickness e2 of the second layer.
[0034] According to one example, the detachment groove comprises an alternation of through portions on which it crosses the entire thickness e2 of the second layer and blind portions. In particular, at the end of steps b), c) and d), the portion to be detached can be linked to the residual portion of the second layer by a plurality of connecting elements spaced from one another, preferably regularly distributed over the entire length of the detachment groove.
[0035] According to an example, steps b), c), d) are carried out in this order.
[0036] In another example, steps c), b), d) are performed in this order.
[0037] In both cases, the part(s) to be manufactured are formed in the first layer and then the detachment groove(s) are etched, or vice versa, and only then is the intermediate layer partially removed. In such configurations, in step d), the intermediate layer is partially removed over an area covering the entire portion to be detached from the second layer, delimited by the groove previously made in step c).
[0038] According to yet another exemplary embodiment, steps b), d), c) are carried out in this order.
[0039] In this case, the part(s) to be manufactured are first formed in the first layer, then the intermediate layer is partially removed over at least a first area located at the planned location of the portion to be detached, before etching the detachment groove. Over its entire length, the detachment groove is then formed at the right of an area of the intermediate layer on which the silicon dioxide has already been removed.
[0040] Other more specific examples of the method according to the invention are further described below: In step d), the partial removal of the intermediate layer may be carried out by chemical etching. In the case of chemical etching, step d) may use at least one stripping agent, generally in the vapor phase, configured to gradually corrode the silicon dioxide of the intermediate layer, without attacking the silicon of the first and second layers. The etching may advantageously be hydrofluoric acid vapor etching. In order to avoid or limit condensation phenomena which could hinder the chemical etching, the substrate may be heated during step d). The removal of the intermediate layer may be carried out by chemical etching in step d), and the stripping agent may be directed towards the first layer of the substrate during said etching. In step d), the substrate detachment groove may be at least partially, preferably totally, protected against etching.More generally, during step d), the second layer and / or an edge of the substrate may be at least partially covered with protection against chemical etching, so as to delay the removal of silicon dioxide from the intermediate layer under the residual portion of the second layer. For example, in a step d0) prior to step d), a layer of protective material, for example a layer of resin resistant to chemical etching, may be deposited on the second layer and / or on the edge of the substrate, and / or a cover, for example in the form of a cover plate, may be fixed on the substrate to protect the second layer and / or its edge. At the end of step d), the remaining portion of intermediate layer is either continuous or non-continuous but present in several places distributed regularly or not.A plurality of detachment grooves may be etched in step c), with each portion to be detached delimited by a groove covering or intended to cover one or more parts formed in the first layer. At least one portion to be detached may cover a plurality of parts formed in the first layer. A single portion to be detached may cover at least half, preferably all, of the parts formed in the substrate. The residual portion may form a frame at the periphery of the substrate, said frame extending continuously over at least 30% of the periphery of the substrate, preferably over at least 50% of the periphery of the substrate. The portion to be detached may cover at least 30% of the surface of the substrate, preferably at least 50% of the surface of the substrate.When forming each part in the first layer, at least one primary groove is generally etched, which corresponds to an external edge of said part with the exception of an unetched portion or attachment (kept to ensure the connection between the part and the rest of the first layer) and where appropriate at least one internal primary groove of profile corresponding to an internal edge of said part. In step b), at least one peripheral groove may further be etched around said at least one primary groove, the at least one primary groove and the peripheral groove delimiting a clearance space of said part at the end of step d). The clearance space allows, at the end of the process, to move the part to more easily break the attachment and thus detach the part. The etching of step b) and / or step c) may be a deep reactive ion etching.the etching of step b) and / or c) may be carried out through a photosensitive resin mask. step b) may comprise at least the following sub-steps: b1) covering the first layer with a (primary) layer of photosensitive resin, b2) by photolithography, forming in said primary resin layer at least one (primary) opening corresponding to an outline of at least one part, b3) etching the first layer over its entire thickness under said at least one (primary) opening to form the part. Step b) may comprise, after step b3), a step b4) during which the primary resin layer is removed, in particular by oxygen plasma cleaning.step c) may comprise at least the following sub-steps: c1) covering the second layer with a (secondary) layer of photosensitive resin, c2) by photolithography, forming in said secondary layer of resin at least one (secondary) opening corresponding to the profile of the detachment groove, c3) etching the second layer under said at least one (secondary) opening. Step c) may comprise, after step c3), a step c4) during which the secondary layer of resin is removed, in particular by oxygen plasma cleaning. The method may comprise, prior to steps b) and / or c), a step a', respectively a", in which the substrate is oxidized, for example by growing a layer of silicon dioxide on the surface of the substrate. In this case, the layer is etched in the openings of the resin, in particular by plasma etching, in a step b2', respectively c2', prior to step b3, respectively c3.In an embodiment in which step d) is carried out prior to step c), the method may in particular comprise, after step d) and before step c), a step a") of oxidation of the substrate, in particular by growth, on the substrate, of a layer of silicon dioxide intended to form a stop layer for etching the detachment groove. Such a protective layer may in particular have a thickness of less than 2 microns. The method may comprise, after step b), preferably after steps a), b), c) and d), even more preferably after step e), at least one step f) of oxidation, or oxidation and deoxidation of the substrate, aimed in particular at smoothing and / or adjusting the dimensions of each part.The method may comprise, after steps a) to d), preferably after step e) and optionally after step f), at least one step g) of oxidation, or oxidation and deoxidation of the modified substrate, in order to adjust the stiffness or the dimensions of each part. The method may comprise, after steps a) to d), preferably after step e) and in particular after step f) and / or g), a step h) of oxidation of the modified substrate, for the purposes of thermocompensation or mechanical reinforcement of each part. The method may comprise, after step e), preferably after steps g) and / or h), a step i) of detachment of each part, in particular by breaking the attachment holding it to the substrate (and in particular to the rest of the first layer). Brief description of the drawings
[0041] The features and advantages of the present invention will appear in more detail in the context of the following description given by way of illustration and not limitation with reference to the attached drawings: THE Figures 1A to 1S schematically illustrate the steps of the method according to an embodiment of the invention corresponding to the sequence of steps of the figure 8 . There figure 2 is a top view of a substrate after steps a), b) and c) of the method, showing the first layer of the substrate (and the detachment groove in dotted lines). figure 3 is a detailed view of zone III identified on the figure 2 . There Figure 4A illustrates a pattern of an etching mask of a constant depth detachment groove. The Figure 4B illustrates a pattern of an etching mask of a detachment groove formed by alternating portions of different depths. The Figure 5illustrates a substrate provided with a detachment groove comprising at least one blind portion and a through portion, The figure 6 illustrates a substrate after steps b), c) and d), in a case where the edge of the substrate has not been protected against chemical etching. figure 7 is a top view of a substrate obtained according to an alternative embodiment of the method, in which several detachment grooves are etched in step c). The figure 8 is a diagram illustrating the succession of steps of the process according to the first mode of implementation. The figure 9 is a diagram illustrating the sequence of steps of the process according to a second mode of implementation. The figure 10 is a diagram illustrating the sequence of steps of the process according to a third mode of implementation. The Figures 11A to 11Q schematically illustrate the steps of the method according to the third embodiment of the invention corresponding to the sequence of steps of the figure 10 . Detailed description
[0042] The attached figures illustrate different modes of implementation of the method according to the invention for the manufacture of parts such as escape wheels. Any other type of silicon part, in particular balance springs, anchors, toothed wheels, plates, hands, balance wheels, may of course be produced in a similar manner. The sequence of steps according to the modes of implementation described in detail below is not limiting of the invention, and certain steps may be interchanged and / or repeated without departing from the scope of the invention.
[0043] A first embodiment of the present invention will be described below with reference to the Figures 1A to 1S .
[0044] The sequence of steps according to this first mode of implementation is illustrated by the figure 8 , on which the optional steps are indicated in dotted lines.
[0045] In a first main step (a) of the process, illustrated by the Figure 1A , a silicon-on-insulator (SOI) substrate 1000 is provided, which comprises a first silicon layer 10 in which the part(s) are to be formed, a second silicon layer 20 forming a stiffening layer of the substrate and an intermediate layer 30 of silicon dioxide (SiO 2 , also commonly called silicon oxide) interposed between the first and second layers 10, 20 in a transverse direction Z of the substrate 1000.
[0046] The silicon of the first and / or second layers 10, 20 may be polycrystalline but is preferably monocrystalline.
[0047] It can be undoped or doped, for example doped with phosphorus. Doped silicon, being electrically conductive, is more dimensionally stable and has better mechanical strength.
[0048] Preferably, the silicon of the first and / or second layers 10, 20 is of {1,1,1} orientation.
[0049] It advantageously has a resistivity less than or equal to 0.1 Ω.cm, for example a resistivity equal to 0.05 Ω.cm.
[0050] The thickness e1 of the first silicon layer 10 depends on the desired thickness of the parts to be manufactured. It is typically between 50 microns and 500 microns.
[0051] The thickness e2 of the second layer 20 is for example between 300 microns and 800 microns.
[0052] The intermediate layer 30 forms a bonding layer between the first and second layers 10, 20, and can also serve as a barrier layer during deep reactive ion etching (DRIE) operations which will be described in more detail below. The thickness e3 of the intermediate layer is for example between 0.5 microns and 3 microns.
[0053] In an optional step (a') illustrated in the Figure 1B , a layer of silicon dioxide 40 can be grown on the surface of the substrate 1000.
[0054] This step is advantageously implemented when the thickness to be etched is significant. DRIE etching is typically performed through a photosensitive resin mask, which will be described later in the process. The photosensitive resin is "consumed" during the process and may sometimes not be sufficient when the etching depth is significant. The addition of a silicon dioxide mask provides better selectivity compared to the resin layer and allows for deeper DRIE etching.
[0055] In a second main step (c) of the method, a detachment groove is etched in the second layer 20 to delimit within this layer 20 a portion to be detached intended to cover the parts which will then be formed in the first layer 10.
[0056] For example, a predicted location of the parts to be formed in the first layer can be defined in advance. Based on this predicted location of the parts, a location of the detachment groove or grooves is defined such that each detachment groove circumscribes at least one part and preferably a group of parts. The detachment grooves are advantageously provided so that all the parts etched in the first layer are covered by a portion to be detached.
[0057] The location of the detachment groove can also be chosen to define a space in the substrate in which one or more parts can be etched as needed. The substrate can thus be "prepared" in advance, and used for the manufacture of different parts and / or distributed indifferently within said space.
[0058] According to an advantageous arrangement illustrated by the figure 2in particular, the groove 200 alone delimits a closed contour, for example by circumscribing the parts 110 as closely as possible and / or by running along the edge 1000a of the substrate, in particular at a constant distance from the latter. As an alternative, the groove 200 could also delimit a closed space with a portion of the edge 1000a of the substrate 1000.
[0059] Advantageously, at least a part of the residual portion 22 of the second layer 20, located on the periphery of the portion to be detached 21, borders the edge 1000a of the substrate 1000.
[0060] To make the detachment groove 200 and as illustrated in the Figures 1C to 1E , an etching mask 62 is first produced on the second layer 20 of the substrate 1000.
[0061] In a first sub-step c1), a layer of photosensitive resin 60 is deposited on the second layer 20 of the substrate 1000 ( Figure 1C ).
[0062] In a second sub-step c2), at least one secondary opening 61 corresponding to the desired profile of the detachment groove 200 is formed by photolithography in the resin layer 60.
[0063] For this, the secondary resin 60 is exposed using a light source 81, through a photomask 80 representing the desired detachment groove pattern ( Figure 1D ).
[0064] Finally, a part of the resin 60, corresponding to the portion that one wishes to see attacked during the subsequent operation of engraving the groove, is eliminated by means of a solvent, forming the opening 61 ( Figure 1E ). In the case of a positive resin as illustrated, it is the portion of the resin exposed to the light source 81 which is removed. In the case of a negative resin, the unexposed portion is eliminated.
[0065] In the case where the substrate 1000 has been previously covered with a layer of silicon dioxide 40 according to the optional step described previously in connection with the Figure 1B , the silicon dioxide layer 40 is also etched under the secondary opening 61 of the resin, in particular by plasma etching (step c2', Figure 1F ).
[0066] As illustrated in the Figure 1G , the detachment groove 200 is then formed in the second layer 20 through the etching mask 62 thus produced (third sub-step c3).
[0067] For this, the silicon of the second layer 20, which is no longer protected by the resin 60 or by the silicon dioxide 40, is etched by deep reactive ion etching, in the transverse direction Z, perpendicular to the general plane of the substrate 1000.
[0068] The width L2 of the groove 200 corresponds substantially to the width of the opening 61 of the resin mask 62, but the sides of the groove 200 may be slightly inclined. A width L2 of the detachment groove 200, measured orthogonally to the transverse direction Z, is for example less than or equal to 500 microns and preferably greater than 50 microns.
[0069] This width L2 can be constant or variable, along the detachment groove 200, as will be described in more detail below.
[0070] According to the invention, over at least part of its length, the detachment groove 200 extends over a depth e of the second layer 20 less than the thickness e2. In other words, the groove 200 is etched to retain, at the level of the or each so-called blind portion 220, a part of the second layer 20 forming a link 222. The bottom of each blind portion 220 of the groove 200 is therefore constituted by such a link 222.
[0071] At all points, the link 222 has a thickness e' substantially smaller than the thickness e2 of the second layer, facilitating its subsequent breaking for the separation of the portion to be detached 21.
[0072] The thickness e', measured in the transverse direction Z, is typically greater than or equal to 2 microns and preferably less than 50 microns.
[0073] According to an exemplary embodiment, the detachment groove 200 may be etched so that a continuous link 222 is maintained over the entire length of the groove 200, as in the illustrated example. In a case where the detachment groove 200 alone delimits a closed contour, then the link 222 also delimits a closed contour.
[0074] The depth of the groove 200 can be either constant or variable along the length of the groove so that the transverse thickness e' of the link 222 is also variable.
[0075] More particularly, the detachment groove 200 may also comprise through portions 224 on which it crosses the entire thickness e2 of the second layer 20, as illustrated in the Figure 5 .
[0076] For example, the detachment groove 200 may comprise an alternation of through portions 224 and blind portions 220.
[0077] In this case also, the depth of the groove 200 can be either constant or variable on the same blind portion 220 or on different blind portions of the groove.
[0078] To obtain a variable depth of the detachment groove 200 (whether or not it comprises through portions 224), it is possible to modulate the width L2 of said groove along its length. The depth of the DRIE type engraving is in fact dependent on the engraving width.
[0079] There Figure 4Aillustrates a groove 61 of an etching mask 62 intended for producing a detachment groove 200 of constant depth e, over its entire length. The width L3 of the groove 61 of the mask is constant.
[0080] There Figure 4B illustrates on the contrary a groove 61 of an etching mask 62 intended for the production of a detachment groove 200 comprising portions of different depths. The groove 61 of the mask is formed of an alternation of primary sections 64 of constant width L4 and secondary sections 65 of width greater than L4, and in particular of progressively increasing then decreasing width on each secondary section 65 with a maximum width L5 on each secondary section 65. The detachment groove 200 etched through such a mask 62 will comprise portions of depth e, at the level of the primary sections 64, and sections of greater depth, greater than e, at the level of the secondary sections 65.
[0081] For example, the detachment groove 200 may comprise blind portions 220, having a first depth e, at the level of the primary sections 64 of the mask, and through portions 224 at the level of the secondary sections 65 of the mask 62 (said portions 224 extending over all or part of said secondary sections 65).
[0082] A detachment groove 200 provided with through portions 224 has the advantage of being more easily detachable, the links 222, less rigid, being easier to break.
[0083] The process continues with the removal of the secondary layer of resin 60, in particular by oxygen plasma cleaning ( Figure 1H ).
[0084] Then, in a third main step (b) of the method, the parts are formed in the first layer 10 of the substrate 1000.
[0085] For this, as illustrated by the Figures 1I to 1K, an etching mask 72 of the parts is produced on this first layer 10: In a first sub-step b1), a layer of photosensitive resin 70 is deposited on the first layer 10. Then, in a second sub-step b2), primary openings 71 corresponding to the contours of the parts to be manufactured (with the exception of a portion of its external contour intended to form an attachment of the part holding it to the rest of the substrate) are formed in this layer of resin, by photolithography (step b2). In a similar manner to the implementation described in connection with the Figure 1B , the resin 70 is for this purpose exposed, through a photomask 82 representing the desired patterns, using a light source 81 ( Figure 1I ). Then the resin 70 is removed locally using a solvent to form the openings 71 of the mask ( Figure 1J ).
[0086] In the case where the substrate 1000 is covered with a layer of silicon dioxide 40, this layer 40 is also etched under the openings 71 of the resin 70, in particular by plasma etching ( Figure 1K ).
[0087] Finally, as illustrated on the Figure 1L , the parts to be manufactured 110 are cut from a useful portion 11 of the first layer 10 located opposite the portion to be detached 21.
[0088] The silicon of the first layer 10 is etched by deep reactive ion etching (DRIE), through the openings 71 of the mask 72, in a direction perpendicular to the general plane of the substrate. The first layer 10 is etched over its entire thickness e1, the intermediate layer 30 forming a stop layer for the DRIE etching.
[0089] The grooves 100 thus produced can have different widths L1 or preferably a constant width, for example of the order of 50 to 100 microns to ensure better verticality of the engraving sides.
[0090] As illustrated by the figure 3 , for each part, at least one external primary groove 120 is typically engraved, corresponding to the external edge of said part 110, with the exception of an unetched portion called attachment 122 ensuring the connection between the part and the rest of the first layer 10, and where appropriate one or more internal primary grooves 130 corresponding to the internal edges of the part.
[0091] According to an advantageous arrangement, at least one peripheral primary groove 140 is further engraved around the external 120 and internal 130 primary grooves of each part 110, the function of which will be described in more detail below.
[0092] Once the parts have been etched, the resin layer 70 is removed, in particular by oxygen plasma cleaning ( Figure 1M ).
[0093] Optionally, the method may then comprise at least one step f) of oxidation, or oxidation then deoxidation of the substrate 1000 (step not illustrated). This step is carried out in the humid atmosphere of a thermal oxidation furnace heated to a temperature generally around 1000°C. During the oxidation, a layer of silicon dioxide is formed over the entire external surface of the substrate 1000, consuming a portion of the silicon of the first and second layers. By removing a thickness of silicon dioxide by wet etching or in the vapor phase during the deoxidation, the surface defects are eliminated and the surface of the parts to be manufactured is smoothed. This step f) may also make it possible to adjust the dimensions of each part, by measuring a dimension to be adjusted on the part. In this case, the thickness of silicon dioxide to be formed during the oxidation is calculated to adjust the measured dimension to the desired value.If the calculated thickness requires too long an oxidation time, several successive oxidation and then deoxidation operations can be carried out until the desired dimension is reached.
[0094] In a fourth main step (d) of the process, illustrated by the Figures 1N to 1P , the intermediate layer 30 is then partially removed at the level of the portion to be detached 21.
[0095] The removal of silicon dioxide is carried out, for example, by chemical etching, and in particular by chemical etching using a vapor-phase etching agent, which penetrates at least through the grooves previously made in the first layer.
[0096] This step is typically performed using a machine as illustrated in the Figure 1N including a closed enclosure 91, formed of a base 911 and a cover 912, defining a cavity in which the substrate 1000 can be housed, and housing chemical etching means 92, and means 93 for holding the substrate inside said enclosure 91.
[0097] The chemical etching means 92 comprise, in the example, a heated hydrofluoric acid bath, arranged in the base 911 of the enclosure 91, and releasing hydrofluoric acid vapor.
[0098] In the enclosure 91, the substrate 1000 is held horizontally, above the hydrofluoric acid bath, with, in the preferred example illustrated, its first layer 10 oriented downwards and towards the acid bath 92.
[0099] Alternatively, the substrate 1000 could be arranged with its first layer 10 facing upwards, but in this case it would be necessary to ensure that the vapor can reach said first layer 10, for example by maintaining sufficient space above said first layer 10.
[0100] The holding means 93 comprise, in the example, a horizontal support formed on the cover 912 making it possible to support the substrate 100, from below, at its periphery. As an alternative or in addition, the holding means 93 could also comprise electrostatic holding means and / or any other suitable holding means.
[0101] The machine 90 further advantageously comprises means for heating the substrate to avoid condensation phenomena which could block the primary grooves 100 and hinder the proper progress of the etching by slowing down or stopping the hydrofluoric acid vapor.
[0102] These heating means may for example take the form of a heating plate 95 arranged substantially horizontally in the upper part of the enclosure, the substrate 1000 thus being able to be arranged directly against the lower surface of said plate 95, or against the surface of the cover 912 integrating or supporting said plate 95 as in the Figure 1N .
[0103] To prevent the penetration of the stripping agent through the groove 200 (if the latter comprises through portions) and / or through the free edge of the intermediate layer 30, and thus delay the removal of the silicon dioxide under the residual portion 22, it may also be advantageous to place a protection on the second layer 20 and / or on the edge 1000a of the substrate (at least opposite the free edge of the intermediate layer 30). The protection may for example be a layer of resin resistant to the stripping agent of the chemical etching, and / or a cover such as a cover plate, where appropriate provided with a rim intended to cooperate with the edge of the substrate.
[0104] In the example, the upper portion of the cover 912 also forms a protection for the second layer 20 of the substrate, protecting the detachment groove 200 from hydrofluoric acid vapors.
[0105] Similarly, the side wall of the cover 912, in contact with the edge 1000a of the substrate 1000, also forms a lateral protection against the etching agent of the chemical etching.
[0106] The steam thus penetrates exclusively through the primary grooves 100 of the first layer 10 to gradually nibble away at the silicon dioxide without however attacking the silicon of the first and second layers 10, 20.
[0107] THE Figures 1O and 1P illustrate the progressive elimination of silicon dioxide from the intermediate layer 30, below then on either side of each primary groove 100 of the first layer 10.
[0108] Between two opposite etching flanks of the first layer 10, the flanks of the intermediate layer 30 gradually move closer together ( Figure 1O ) until they rejoin once all the silicon dioxide has been removed ( Figure 1P). By opposite etching flanks, we mean here etching flanks separated by a continuous portion of silicon of the first layer 10 and aligned in a direction substantially orthogonal to the tangent to one of the flanks. If necessary and to accelerate the process, additional etchings or parts can be added in the first layer 10 opposite the portion to be detached in order to reduce the distance between two etching flanks.
[0109] The etching is stopped when the intermediate layer 30 is completely removed opposite the portion to be detached 21 but before the entire intermediate layer 30 is completely removed. In other words, the etching is stopped so that a portion of the intermediate layer 30 is retained opposite the residual portion 22 of the second layer 20.
[0110] Advantageously, the chemical etching is stopped so that the portion of intermediate layer 30 between the first layer 10 and the residual portion 22 retains at least locally a width greater than or equal to 1 mm, which width is thus sufficient to ensure adhesion between the residual portion 22 and the first layer 10.
[0111] The portion of intermediate layer 30 preserved between the first layer 10 and the residual portion 22 of the second layer 20 is either continuous or non-continuous but present in several places, preferably distributed over the entire said residual portion 22.
[0112] According to the invention, the parts 110 formed in the first layer 10 are intended to be released by detachment of the portion to be detached 21 delimited by the detachment groove 200.
[0113] During detachment, and thanks to the preservation of a part of the intermediate layer 30, a frame 50 is formed around the useful portion 11 of the first layer carrying the parts 110, said frame 50 being formed by the superposition of a part of the first layer 10 and at least one so-called residual part 22 of the second layer 20, linked by a part of the intermediate layer 30.
[0114] There figure 6 illustrates a substrate 1000 of the same type as that described previously, at the end of steps b), c) and d), but without protection of the edge 1000a of the substrate (a space being kept between the side wall of the enclosure and the edge 1000a of the substrate). In the example illustrated, the detachment groove being blind over its entire length, the protection or not of the second layer 20 of the substrate and of the groove 200 does not make any difference to the progress of the chemical etching operation.
[0115] In a fifth main step (e) of the process, illustrated by the Figures 1Q and 1R , the portion to be detached 21 is mechanically separated from the rest of the substrate 1000 by breaking the bond.
[0116] As illustrated by the figures, the part to be detached 21 is pushed, for example, by means of at least one tool 84 introduced through a groove 100 etched in the first layer 10 in step b).
[0117] Advantageously, the process can continue, at the end of this step e), with one or more operations (step g) of oxidation, or of oxidation and deoxidation, with a view to adjusting the stiffness or the dimensions of each part and / or with a step h) of oxidation of the modified substrate, for the purposes of thermocompensation or mechanical reinforcement of each part.
[0118] The modified substrate 1000`, illustrated in the Figure 1S, reinforced by its peripheral frame 50, does not deform or deforms little during these subsequent treatments or when it is transported between these treatments.
[0119] The method can finally end with a step i) of detaching each part from the modified substrate 1000', by breaking its attachment 122, facilitated by the clearance space provided between the part and the corresponding peripheral groove 140.
[0120] The example described above is not, however, exhaustive and many variations could be considered.
[0121] Thus, according to an implementation method of which an example is illustrated on the figure 7 , several detachment grooves 201, 202 can be formed in the second layer 20, each delimiting on its own or in combination with the edge 1000a of the substrate 1000 a portion to be detached 211, 212 covering one or more parts, preferably several parts.
[0122] According to one example, the first layer 10 then remains in one piece at the end of the separation step e), and the frame obtained is a frame reinforced between the different useful portions 111, 112 of the first layer 10, as in the figure 7 .
[0123] According to another embodiment, during step b), at least one additional detachment groove, opening at its two ends onto the edge 1000a of the substrate, can also be made in the first layer 10, so that the first layer 10 is divided into two or more pieces during the removal step d) or separation step e).
[0124] These last two embodiments can also be combined.
[0125] There figure 9illustrates a sequence of steps according to a second embodiment of the invention. The steps as such are similar to those described previously but in this case, the parts are etched first in the first layer of the substrate (step b), then the detachment groove(s) is / are etched in the second layer. Then the intermediate layer is partially removed (step d) and then the portion to be detached is detached (step e).
[0126] In particular, the steps described above with reference respectively to the Figures 1A, 1B , 1I to 1M , 1à 1H , 1N to 1S can be done in this order.
[0127] Optional steps a'), f), g), h), i) are applicable to this embodiment as well.
[0128] There figure 10illustrates a sequence of steps according to a third embodiment of the invention. The steps as such are similar to those described previously but in this case, the parts are etched first in the first layer of the substrate (step b), the intermediate layer is partially removed (step d). Then finally the detachment groove(s) is / are etched in the second layer and the portion to be detached is detached (step e). In other words, after forming the parts, the silicon dioxide is partially removed from the intermediate layer on at least a first area located opposite the expected location of the portion to be detached, before proceeding with the etching of the detachment groove. The detachment groove is therefore etched opposite an area on which the intermediate layer has already been removed.
[0129] According to this third embodiment, more precisely, a silicon-on-insulator (SOI) type substrate 1000 is first provided, of the same type as that illustrated in the Figure 1A (step a), Figure 11A ).
[0130] In an optional step a') illustrated in the Figure 11B , a layer of silicon dioxide 40 can be grown on the surface of the substrate 1000.
[0131] In a second main step (b) of the method, the parts 110 are formed in the first layer 10 of the substrate 1000.
[0132] For this, as illustrated by the Figures 11C to 11E , an etching mask 72 of the parts 110 is produced on the first layer 10, by depositing a layer of photosensitive resin 70 on the first layer 10 ( Figure 1C) then by forming in this layer of resin 70 primary openings 71 corresponding to the contours of the parts to be manufactured 110 (with the exception of a portion of its external contour intended to form a link between the part holding it to the rest of the substrate), by photolithography through a photomask 82 ( Figure 11C ).
[0133] In the case where the substrate is covered with a layer of silicon dioxide 40, as in the figures, this layer is etched under the openings 71 of the resin 70, in particular by plasma etching ( Figure 11E ).
[0134] Finally, as illustrated on the Figure 11F , the parts to be manufactured 110 are cut from the first layer 10, in particular by DRIE engraving.
[0135] The grooves 100 thus produced extend over the entire thickness e1 of the first layer 10, the intermediate layer 30 forming a stop layer for the DRIE etching.
[0136] Optionally, the method may then comprise at least one step f) of oxidation, or oxidation then deoxidation of the substrate 1000 (step not illustrated).
[0137] According to this embodiment, the parts 110 thus formed will be released by removal of the intermediate layer 30 on a sacrificial zone 32 (see Figure 11G ) facing them, then detachment of a portion to be detached 21 from the second layer 20 covering the parts 110 and itself covered by said sacrificial zone 32, as described below.
[0138] A frame 50 is thus kept around a useful portion of the first layer carrying the parts 110.
[0139] In a third main step (d) of the process illustrated by the figures 11H to 11J , the intermediate layer 30 is therefore partially removed from an area covering the parts formed in step b).
[0140] The area 32 - called the sacrificial area of the intermediate layer 30 - on which the silicon dioxide is removed, is an area for which a closed contour can be defined in a plane parallel to the main plane of the substrate 1000 and intersecting the intermediate layer 30.
[0141] Once step d) is completed, the sacrificial zone 32, delimited by its closed contour, is completely empty.
[0142] The contour of the sacrificial zone 32, projected transversely, circumscribes at least one part 110, preferably a plurality of parts 110, in particular as in the example illustrated all of the parts 110 formed in the first layer 10.
[0143] The predicted location 2000 of the detachment groove 200, which will determine the portion to be detached 21 and the residual portion 22 of the second layer 20, can at this stage be known, and step d) can in particular be carried out so that the sacrificial zone 32 covers said predicted location 2000.
[0144] According to another example, the location of the detachment groove may be determined after step d), depending on the location of the sacrificial zone 32 formed in this step.
[0145] The removal of silicon dioxide can be carried out by chemical etching, and in particular by chemical etching using a vapor phase etching agent, in a machine 90 of the same type as that described previously with reference to Figures 1N to 1P .
[0146] THE figures 11H to 11Jillustrate the progressive elimination of silicon dioxide from the intermediate layer 30, below then on either side of each primary groove 100 of the first layer 10.
[0147] In a fourth main step (c) of the method, a detachment groove 200 is etched in the second layer 20 to delimit within this layer at least one portion to be detached 21 covering the parts formed in the first layer 10 in the transverse direction Z and covered by the sacrificial zone 32 of the intermediate layer 30 in the same transverse direction Z.
[0148] In an optional step a") prior, illustrated on the Figure 11K, a protective layer of silicon dioxide 42 is grown over the entire substrate 1000, in particular with a thickness of less than 2 micrometers. The thickness of this protective layer 42 must be sufficiently small to cover the surfaces of the first and second layers 10, 20 delimiting the sacrificial zone 32 without refilling said zone 32. Locally, this layer 42 can be superimposed on the layer 40 remaining on the surface of the substrate at the end of step c) of partial elimination of the intermediate layer 30 (as illustrated in the Figure 1K For example).
[0149] This protective layer 42 is intended to serve as a stop layer for the etching of the detachment groove 200 according to the description which follows.
[0150] As illustrated next on the figures 11L to 11N , an etching mask 62 of the detachment groove 200 is first produced on the second layer 20 of the substrate 1000.
[0151] For this, a layer of photosensitive resin 60 is deposited on the second layer 20 ( Figure 11L ).
[0152] Then a secondary opening 61 corresponding to the desired profile of the detachment groove 200 is formed by photolithography in the resin layer 60 ( Figures 11L and 11M ), using a photomask 80 representing the desired detachment groove pattern 200 ( Figure 11L ).
[0153] Finally, a part of the resin 60, corresponding to the portion that we wish to see attacked during the subsequent operation of engraving the groove 200, is eliminated by means of a solvent, forming the opening 61 ( figure 11M ).
[0154] In the case where the substrate 1000 has been previously covered with a protective layer of silicon dioxide 42 according to the optional step described previously in connection with the Figure 11K, the protective layer 42 is also etched under the secondary opening 61 of the resin, in particular by plasma etching ( Figure 11N ). Layer 40 from step a') ( Figure 1B ) and remaining on the surface of the second layer 20 is, where appropriate, also etched.
[0155] As illustrated in the Figure 11O , the detachment groove 200 is then formed in the second layer 20 through the etching mask 62 thus produced, so as to delimit, within the second layer 20, the portion to be detached 21 covering the parts 110 previously formed in the first layer 10.
[0156] During DRIE etching, the protective layer 42 deposited as described with reference to the Figure 11K forms a stop layer at the right of the through portions 224 of the detachment groove 200.
[0157] This protective layer 42 may be omitted in cases where the groove is blind along its entire length, as illustrated in the figure 12 In the case of a detachment groove that is at least partially through, and in the absence of a protective layer 42, the etching of said groove would affect the first layer 10.
[0158] The process continues with the removal of the secondary resin layer 60, as well as possibly the protective layer 42 of silicon dioxide, and the remainder of the layer 40 ( Figure 11P ).
[0159] In a new step e) of the method, the portion to be detached 21 is mechanically separated from the rest of the substrate 1000 by breaking the connecting element(s) 222, as illustrated in particular in the Figure 11Q .
[0160] To do this, for example, the part to be detached 21 is pushed by means of at least one tool introduced through a groove 100 etched in the first layer 10 in step b).
[0161] The part of the first layer 10, uncovered by the removal of said portion 21, and carrying the parts 110, is called the useful portion 11 of the first layer. It is reinforced, at its periphery, by the frame 50.
[0162] Advantageously, the process can continue, at the end of this step, with one or more operations (step g) of oxidation and deoxidation in order to adjust the stiffness or the dimensions of each part and / or with a step h) of oxidation of the modified substrate, for the purposes of thermocompensation or mechanical reinforcement of each part.
[0163] The method can finally end with a step i) of detaching each part from the modified substrate, by breaking its attachment 122, facilitated by the clearance space provided between the part 110 and the corresponding peripheral groove 140.
Claims
1. Method for manufacturing at least one part in silicon wherein a) a substrate (1000) is provided comprising the superposition, in a transverse direction (Z), of at least a first layer (10) of silicon of thickness e1, an intermediate layer (30) of silicon dioxide, and a second layer (20) of silicon of thickness e2, the intermediate layer (30) thus being interposed between the first and second layers (10, 20); then, in this order or another: b) the first layer (10) is etched to form the at least one part (110), c) at least one detachment groove (200) is etched in the second layer (20) to delimit within said second layer (20) at least one portion to be detached (21) covering or intended to cover said at least one part (110), at least one so-called blind portion (220) of the detachment groove (200) being etched in such a way that a part (222) of the second layer (20), forming a connection, is retained in line with said portion (220), and d) the intermediate layer (30) is partially removed by eliminating the silicon dioxide in line with the said at least one portion to be detached (21) or the intended location of the said portion to be detached (21); and finally e) the at least one portion to be detached (21) is mechanically separated from the rest of the substrate by breaking the connection (222).
2. Method according to claim 1, wherein in step e), the part (21) to be detached is pushed by means of at least one tool (84) inserted through a groove (100) etched in the first layer (10) in step b).
3. Method according to claim 1 or 2, wherein the thickness (e') of a connection (222), measured in the transverse direction (Z), is at least 2 microns.
4. Method according to any one of the claims 1 to 3, wherein the detachment groove (200), alone or together with an edge of the substrate (1000a), defines a closed contour.
5. Method according to any one of the claims 1 to 4, wherein the detachment groove (200) has a depth which varies along its length.
6. Method according to any one of the claims 1 to 5, wherein the detachment groove (200) further comprises at least one through portion (224) over which it passes through the entire thickness e2 of the second layer (20).
7. Method according to claim 6, wherein the detachment groove (200) comprises an alternation of through portions (224) on which it passes through the entire thickness e2 of the second layer (20) and blind portions (220).
8. Method according to any one of the claims 1 to 5, wherein the detachment groove (200) is engraved in such a way that a part (222) of the second layer (20), forming a connection, is retained in line with the said groove (200) over its entire length.
9. Method according to any one of the claims 1 to 8, wherein a plurality of parts (110) is etched in the first layer (10), and at least one detachment groove (200) delimits a portion to be detached (21) covering or intended to cover said plurality of parts (110).
10. Method according to any one of the claims 1 to 9, wherein the steps b), c), d) are carried out in this order.
11. Method according to any one of the claims 1 to 9, wherein the steps c), b), d) are carried out in this order.
12. Method according to any one of the claims 1 to 9, wherein the steps b), d), c) are carried out in this order.
13. Method according to any one of the claims 1 to 12, wherein in step d), part of the intermediate layer (30) is kept opposite at least one residual portion (22) of the second layer (20) located outside a portion to be detached (21) or a planned location of such a portion to be detached (21).
14. Method according to any one of the claims 1 to 13, wherein a width of the detachment groove (200), measured orthogonally to the transverse direction (Z), is less than or equal to 500 microns.