No details

GB202414938D0Pending Publication Date: 2024-11-27YUKING TECHNOLOGIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
GB2024014938
Authority / Receiving Office
GB · GB
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2023-06-30
Publication Date
2024-11-27

AI Technical Summary

Technical Problem

The amount of traditional dispersed dyes added during the dyeing process is high, resulting in serious pollution of printing and dyeing wastewater, poor stability, and difficult to preserve for a long time.

Method used

Polyether modified polymer A and polyamide polymer B are combined to prepare water-soluble dispersants, which improve the wetting and protection of the dispersed dye by controlling the proportion of functional chain segments, and improve the grinding efficiency and slurry stability.

Benefits of technology

It significantly improves the grinding efficiency and slurry stability of the dispersed dye, reduces the organic content of the printing and dyeing wastewater, extends the storage time of the dye, and optimizes the application performance of the dye.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A water-soluble dispersant, a preparation method therefor, and the use thereof. The water-soluble dispersant comprises a polyether modified polymer A and a polyamide high-molecular polymer B. Raw materials for preparing the polyether modified polymer A comprise a vinyl benzene monomer, a vinyl sulfonic acid monomer and an active macromonomer polyether. The polyamide high-molecular polymer B comprises a homopolymer of vinyl pyrrolidone and / or a copolymer of vinyl pyrrolidone. The water-soluble dispersant improves the wetting and protective effects of a dispersant on disperse dye particles, and therefore the grinding efficiency of disperse dye, the proportion of dye particles in slurry, and the stability of slurry are all improved.
Need to check novelty before this filing date? Find Prior Art

Description

A water-soluble dispersant and its preparation method and application Technical Field

[0001] The embodiments of the present application relate to the technical field of color paste additives, such as a water-soluble dispersant and its preparation method and application. Background Art

[0002] Disperse dyes are a class of dyes with relatively small molecules and no water-soluble groups. They offer a comprehensive color spectrum, resulting in vibrant colors and excellent performance across various performance attributes. Therefore, they are widely used in dyeing various synthetic fibers, acetate fibers, and blended fabrics. Dispersants are required to evenly disperse the dye in the dye solution, enabling them to dye fibers like polyester.

[0003] With the rapid development of my country's industrial printing and dyeing industry, wastewater discharge and pollution levels have increased significantly. The diversification of printing and dyeing products has also made the composition of printing and dyeing wastewater more complex and more difficult to treat. Traditional disperse dyes incorporate large amounts of lignin salts, naphthalenesulfonates, and other dispersing agents during dispersion. This not only results in slow grinding efficiency during the production process, but also the dispersant dosage, which ranges from 70% to 150% of the dye, results in a high concentration of organic matter in the printing and dyeing wastewater, making the treatment process cumbersome and complex, and posing a significant environmental risk. Furthermore, liquid disperse dye slurries have a short stability period and are difficult to store long-term, requiring spray drying to create commercially available dyes to extend their shelf life.

[0004] CN114644762A discloses a kind of multiple modified lignin dye dispersant and preparation method thereof, with industrial alkali lignin as raw material, under alkaline conditions, with sulfonating agent 1, sulfonating agent 2 as sulfonating agent system, introduce sulfonic acid group simultaneously at different sites, can greatly improve the content of hydrophilic group sulfonic acid group.Then selectively add blocking agent, reduce residual hydroxyl content, while improving molecular weight.This multiple modified lignin sulfonate can be applied to dye dispersant, the disperse dye system with good dispersibility and excellent high temperature stability that can be obtained without grinding, and it has extremely low staining property, has lower reduction rate to azo dyes, can significantly improve dye uptake simultaneously, can greatly reduce the production cost of printing and dyeing industry.But the dispersant of this application adds ratio higher when being used for disperse dye, and color paste particle size is still larger.

[0005] Therefore, it is desirable in the art to develop a water-soluble dispersant for dye dispersion.

[0006] Summary of the Invention

[0007] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0008] The present invention provides a water-soluble dispersant, a preparation method, and an application thereof. The water-soluble dispersant provided herein improves the wetting and protective effects of the dispersant on disperse dye particles, thereby improving the grinding efficiency of disperse dyes, the proportion of dye particles in the slurry, and the slurry stability.

[0009] In a first aspect, an embodiment of the present application provides a water-soluble dispersant, wherein the water-soluble dispersant includes a polyether-modified polymer A and a polyamide-based polymer B;

[0010] The raw materials for preparing the polyether-modified polymer A include vinylbenzene monomers, vinyl sulfonic acid monomers and active macromonomer polyether;

[0011] The polyamide-based high molecular polymer B includes a homopolymer of vinyl pyrrolidone and / or a copolymer of vinyl pyrrolidone.

[0012] The present application obtains a water-soluble dispersant by compounding a polyether-modified polymer A and a polyamide-type high molecular polymer B, wherein the polyether-modified polymer A is a comb-shaped polymer obtained by bulk free radical polymerization by self-made active macromonomer polyether, self-made vinyl sulfonic acid monomer, and vinylbenzene monomer under the initiation of a peroxide initiator; the active macromonomer polyether provides a hydrophilic segment of the polymer side chain, the alkyl ester chain and the sulfonic acid functional group contained in the vinyl sulfonic acid monomer give the polymer the wetting and electrostatic repulsion effect on the dye particles, the conjugated effect of the benzene ring of the vinylbenzene monomer improves the affinity of the polymer anchor group for the disperse dye group, and the application performance of the polymer for disperse dyes is regulated by controlling the ratio of the corresponding monomers of each functional segment of the polymer. The composite system of polyether-modified polymer A and polar polyamide-type high molecular polymer B makes the types of functional groups of the water-soluble dispersant system more diversified, improves the wetting and protective effect of the dispersant on the disperse dye particles, and improves the grinding efficiency of the disperse dye, the proportion of dye particles in the slurry, and the slurry stability.

[0013] Preferably, the active macromonomer polyether is prepared by the following preparation method:

[0014] Adding polyetheramine and allyl succinic anhydride into the reactor, raising the temperature and keeping the temperature until no water is distilled out during the reaction, thereby obtaining the active macromonomer polyether.

[0015] Preferably, the polyetheramine is a monoprimary amino polyether in which the terminal hydroxyl group is converted into an amine by using a monoalcohol as an initiator to initiate the self-polymerization of ethylene oxide or the copolymerization of ethylene oxide and propylene oxide.

[0016] Preferably, the weight average molecular weight of the polyetheramine is 500 to 2500 g / mol, for example, 500 g / mol, 800 g / mol, 1000 g / mol, 1300 g / mol, 1500 g / mol, 1800 g / mol, 2000 g / mol, 2300 g / mol or 2500 g / mol.

[0017] Preferably, the polyetheramine includes any one of JEFFAMINE M-2070, JEFFAMINE M-1000 or JEFFAMINE M-600, or a combination of at least two thereof.

[0018] Preferably, the molar ratio of the polyetheramine to allylsuccinic anhydride is (0.5-1.5):1, such as 0.5:1, 1:1 or 1.5:1, and preferably 1:1.

[0019] Preferably, the temperature is raised to 120-160°C, such as 120°C, 130°C, 140°C, 150°C or 160°C.

[0020] Preferably, the insulation time is 2 to 6 hours, such as 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.

[0021] Preferably, the preparation process of the reactive macromonomer polyether is carried out under the protection of an inert gas.

[0022] Preferably, the reactive macromonomer polyether has a structure as shown in the following formula I:

[0023] wherein R1 is hydrogen or methyl, R2 is methyl, ethyl, propyl or butyl, m is an integer from 10 to 60, such as 10, 15, 20, 25, 30, 35, 40, 45, 50, 55 or 60, and n is an integer from 0 to 15, such as 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15.

[0024] Preferably, the vinyl sulfonic acid monomer is prepared by the following preparation method:

[0025] Adding hydroxylated acrylic acid monomer and alkyl sultone into a reactor, mixing and reacting until the residual amount of alkyl sultone is less than 0.5%, thereby obtaining the vinyl sulfonic acid monomer.

[0026] In the present application, vinyl sulfonic acid monomers are obtained by ring-opening esterification of acrylic acid monomers with alkyl sultones.

[0027] Preferably, the hydroxylated acrylic monomer includes any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, hydroxypentyl acrylate or hydroxypentyl methacrylate, or a combination of at least two thereof.

[0028] Preferably, the alkyl sultone includes any one of 1,3-propane sultone, 1-methyl-1,3-propane sultone, 2-methyl-1,3-propane sultone, 3-methyl-1,3-propane sultone, 1,4-butane sultone, 1-methyl-1,4-butane sultone, 2-methyl-1,4-butane sultone, 3-methyl-1,4-butane sultone or 4-methyl-1,4-butane sultone, or a combination of at least two thereof.

[0029] Preferably, the molar ratio of the hydroxylated acrylic monomer to the alkyl sultone is 1:1.

[0030] Preferably, the reaction system further includes an acid catalyst.

[0031] Preferably, the acid catalyst comprises any one of p-toluenesulfonic acid, sulfuric acid, propionic acid or hydrochloric acid, or a combination of at least two thereof.

[0032] Preferably, the amount of the acid catalyst added is 0.5% to 3% of the sum of the weight of the hydroxylated acrylic monomer and the alkyl sultone, for example, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%.

[0033] Preferably, the mixing temperature is 60-90°C, such as 60°C, 70°C, 80°C or 90°C.

[0034] Preferably, the reaction time is 5 to 20 hours, for example, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours or 20 hours, etc.

[0035] Preferably, the preparation process of the vinyl sulfonic acid monomer is carried out under the protection of an inert gas.

[0036] Preferably, the residual amount of alkyl sultone is tested by gas chromatography, and the sample is gasified and then detected by flame ionization detector, and the amount is quantified by corrected area normalization method.

[0037] Preferably, the vinylbenzene monomer includes any one of styrene, β-methylstyrene, allylbenzene, 3-methylstyrene, 2-methylstyrene or 2-isopropenyltoluene, or a combination of at least two thereof.

[0038] Preferably, the mass ratio of the vinylbenzene monomer, the vinyl sulfonic acid monomer and the reactive macromonomer polyether is (3-10):(10-20):(20-50), for example, 3:10:20, 10:20:50, 3:20:20 or 10:10:20.

[0039] Preferably, the raw materials for preparing the polyether-modified polymer A also include an initiator.

[0040] Preferably, the initiator comprises any one or a combination of at least two of benzoyl peroxide, tert-butyl benzoyl peroxide, methyl ethyl ketone peroxide, dicumyl peroxide, di-tert-butyl peroxide or 2,2-bis(tert-butyl peroxide)butane.

[0041] Preferably, the raw materials for preparing the polyether-modified polymer A include the following components in parts by weight:

[0042] Preferably, the raw materials for preparing the polyether-modified polymer A are calculated by weight, and the amount of the vinylbenzene monomer used can be 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 20 parts.

[0043] Preferably, the raw materials for preparing the polyether-modified polymer A are calculated in parts by weight, and the amount of the vinyl sulfonic acid monomer used can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts or 40 parts, etc.

[0044] Preferably, the amount of the active macromonomer polyether used in the preparation of the polyether-modified polymer A can be 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 95 parts or 100 parts, etc., based on parts by weight.

[0045] Preferably, the amount of the initiator used in the preparation of the polyether-modified polymer A can be 0.5 parts, 1 part or 1.5 parts by weight.

[0046] Preferably, the weight average molecular weight of the polyether-modified polymer A is 50,000 to 200,000 g / mol, for example, 50,000 g / mol, 80,000 g / mol, 100,000 g / mol, 130,000 g / mol, 150,000 g / mol, 180,000 g / mol or 200,000 g / mol, and preferably 50,000 to 100,000 g / mol.

[0047] Preferably, the weight average molecular weight of the polyamide polymer B is 2000-100000 g / mol, for example, 2000 g / mol, 5000 g / mol, 8000 g / mol, 10000 g / mol, 30000 g / mol, 50000 g / mol, 80000 g / mol or 100000 g / mol, etc., preferably 10000-50000 g / mol.

[0048] Preferably, the copolymer of vinyl pyrrolidone comprises a copolymer of vinyl pyrrolidone and vinyl acetate.

[0049] Preferably, the polyamide polymer B includes any one of PVPK25, PVPK30, PVPK35 or copovidone VA64, or a combination of at least two thereof.

[0050] Preferably, the mass ratio of the polyether modified polymer A to the polyamide polymer B is (60-160):(40-70), for example, 60:40, 60:60, 60:70, 100:40, 100:60, 100:70, 160:40, 160:60 or 160:70.

[0051] Preferably, the water-soluble dispersant further includes deionized water and a pH regulator.

[0052] Preferably, the pH adjuster includes any one of sodium hydroxide, potassium hydroxide, monoethanolamine, diethanolamine or triethanolamine, or a combination of at least two thereof.

[0053] Preferably, the raw materials for preparing the water-soluble dispersant include the following components in parts by weight:

[0054] Polyether modified polymer A 60-160 parts

[0055] Polyamide polymer B 40-70 parts

[0056] 100-200 parts deionized water

[0057] The pH adjuster adjusts the pH of the system to 7 to 10 (eg, 7, 8, 9, or 10).

[0058] Preferably, the raw materials for preparing the water-soluble dispersant are calculated in parts by weight, and the amount of polyether-modified polymer A used can be 60 parts, 70 parts, 80 parts, 90 parts, 100 parts, 110 parts, 120 parts, 130 parts, 140 parts, 150 parts or 160 parts, etc.

[0059] Preferably, the amount of the polyamide polymer B used in the preparation of the water-soluble dispersant can be 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts or 70 parts by weight.

[0060] Preferably, the raw materials for preparing the water-soluble dispersant are calculated by weight, and the amount of deionized water used can be 100 parts, 110 parts, 120 parts, 130 parts, 140 parts, 150 parts, 160 parts, 170 parts, 180 parts, 190 parts or 200 parts.

[0061] In a second aspect, the present invention provides a method for preparing the water-soluble dispersant according to the first aspect, the method comprising the following steps:

[0062] (1) adding a formulated amount of active macromonomer polyether into a reactor, raising the temperature, then adding a vinylbenzene monomer, a vinyl sulfonic acid monomer, and an optional initiator, and maintaining the temperature for reaction to obtain the polyether-modified polymer A;

[0063] (2) Cooling the polyether-modified polymer A obtained in step (1), then adding optional deionized water and polyamide polymer B, and then adding an optional pH regulator, stirring to obtain the water-soluble dispersant.

[0064] Preferably, the heating in step (1) is to 100-150°C, for example, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C.

[0065] Preferably, when adding the vinylbenzene monomer, the vinyl sulfonic acid monomer, and the optional initiator in step (1), these three raw materials are first prepared into a mixed solution and then added dropwise, and the dropping time is controlled to be 5 to 15 hours, for example, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours or 15 hours, etc.

[0066] Preferably, the temperature of the insulation reaction in step (1) is 100-150°C, for example, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, and the insulation reaction time is 1-3 hours, for example, 1 hour, 2 hours or 3 hours.

[0067] Preferably, both step (1) and step (2) are carried out under the protection of an inert gas.

[0068] Preferably, the cooling in step (2) is cooling to 50-60°C, such as 50°C, 55°C or 60°C.

[0069] In a third aspect, an embodiment of the present application provides a use of the water-soluble dispersant as described in the first aspect in dye dispersion.

[0070] Compared with the related art, the embodiments of the present application have at least the following beneficial effects:

[0071] In the embodiments of the present application, vinylbenzene monomers, vinyl sulfonic acid monomers and active macromonomer polyethers are polymerized by bulk free radical polymerization to obtain polyether-modified polymer A, and the polyether-modified polymer A and polyamide-type high molecular polymer B are compounded to obtain a water-soluble dispersant. The types of functional groups in the water-soluble dispersant system are more diversified, which improves the wetting and protective effects of the dispersant on the disperse dye particles, thereby improving the grinding efficiency of the disperse dye, the proportion of dye particles in the slurry, and the stability of the slurry.

[0072] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION

[0073] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.

[0074] Preparation Example 1

[0075] In this preparation example, a reactive macromonomer polyether is provided, and the preparation method comprises the following steps:

[0076] 200 g of polyetheramine JEFFAMINE M-2070 and 14 g of allyl succinic anhydride were added to a reaction flask protected by N2, and the temperature was raised to 130°C and kept warm for 4 hours until anhydrous water was distilled off during the reaction to obtain the active macromonomer polyether, which was recorded as a1.

[0077] Preparation Example 2

[0078] In this preparation example, a reactive macromonomer polyether is provided, and the preparation method comprises the following steps:

[0079] 200 g of polyetheramine JEFFAMINE M-1000 and 28 g of allyl succinic anhydride were added to a reaction flask protected by N2, and the temperature was raised to 140°C and kept warm for 3 hours until anhydrous water was distilled off during the reaction to obtain the active macromonomer polyether, which was recorded as a2.

[0080] Preparation Example 3

[0081] In this preparation example, a reactive macromonomer polyether is provided, and the preparation method comprises the following steps:

[0082] To a nitrogen-protected reaction flask, 180 g of polyetheramine JEFFAMINE M-600 and 42 g of allyl succinic anhydride were added, and the temperature was raised to 160° C. and kept warm for 2.5 hours until anhydrous water was distilled off during the reaction to prepare a reactive macromonomer polyether, designated as a3.

[0083] Preparation Example 4

[0084] In this preparation example, a vinyl sulfonic acid monomer is provided, and the preparation method includes the following steps:

[0085] 50 g of hydroxyethyl acrylate and 52.6 g of 1,3-propane sultone were added to a reaction flask protected by N2, and stirred at 60°C. Then, 0.6 g of p-toluenesulfonic acid was added and stirred for 5 hours until the residual amount of 1,3-propane sultone was 0.2%, thereby obtaining the vinyl sulfonic acid monomer, which was recorded as b1.

[0086] Preparation Example 5

[0087] In this preparation example, a vinyl sulfonic acid monomer is provided, and the preparation method includes the following steps:

[0088] 50 g of hydroxypropyl acrylate and 52.3 g of 1,4-butane sultone were added to a reaction flask protected by N2, and stirred evenly at 80°C. Then, 1 g of propionic acid was added and stirred for 12 hours until the residual amount of 1,4-butane sultone was 0.3%, thereby obtaining the vinyl sulfonic acid monomer, which was recorded as b2.

[0089] Preparation Example 6

[0090] In this preparation example, a vinyl sulfonic acid monomer is provided, and the preparation method includes the following steps:

[0091] 50 g of hydroxyethyl methacrylate and 46.9 g of 1,3-propane sultone were added to a reaction flask protected by N2, and stirred at 90°C. Then, 2.9 g of hydrochloric acid was added and stirred for 5 hours until the residual amount of 1,3-propane sultone was 0.4%, thereby obtaining the vinyl sulfonic acid monomer, which was recorded as b3.

[0092] Comparative Preparation Example 1

[0093] The only difference between this comparative preparation example and preparation example 1 is that allyl succinic anhydride is replaced by an equimolar amount of maleic anhydride, and the obtained polyether is recorded as D-a1.

[0094] Example 1

[0095] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:

[0096] (1) Add 40 parts by weight of the active macromonomer polyether a1 into a reaction flask protected by N2, stir and heat to 105°C; uniformly add dropwise a mixture of 20 parts of styrene, 30 parts of the vinyl sulfonic acid monomer b1, and 0.5 parts of benzoyl peroxide, and complete the addition within 5 hours. After the addition is complete, keep the mixture at 110°C for 1.5 hours to obtain a polyether-modified polymer A;

[0097] (2) 80 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, cooled to 60°C, and then 200 parts of deionized water and 70 parts of PVPK30 were added. Potassium hydroxide was then added to adjust the pH value of the system to 7.5, and the mixture was stirred evenly to obtain the water-soluble dispersant.

[0098] Example 2

[0099] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:

[0100] (1) Add 60 parts by weight of the active macromonomer polyether a2 into a reaction flask protected by N2, stir and heat to 115°C; uniformly dropwise add a mixture of 6 parts of styrene, 20 parts of the vinyl sulfonic acid monomer b2, and 0.6 parts of tert-butyl benzoyl peroxide, and complete the addition over 15 hours. After the addition is complete, keep the mixture at 115°C for 2 hours to obtain a polyether-modified polymer A;

[0101] (2) 60 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, cooled to 60°C, and then 100 parts of deionized water and 40 parts of PVPK35 were added. Then, sodium hydroxide was added to adjust the pH value of the system to 10, and the mixture was stirred evenly to obtain the water-soluble dispersant.

[0102] Example 3

[0103] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:

[0104] (1) Add 100 parts by weight of the active macromonomer polyether a3 to a reaction flask protected by N2, stir and heat to 140°C; uniformly dropwise add a mixture of 14 parts of 3-methylstyrene, 40 parts of the vinyl sulfonic acid monomer b3, and 1.5 parts of methyl ethyl ketone peroxide, and complete the addition within 12 hours. After the addition is complete, heat and react at 140°C for 2.5 hours to obtain a polyether-modified polymer A;

[0105] (2) 160 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, and the mixture was cooled to 60°C. 150 parts of deionized water and 50 parts of copolyvidone VA64 were then added, followed by potassium hydroxide to adjust the pH value of the system to 8.0, and the mixture was stirred evenly to obtain the water-soluble dispersant.

[0106] Example 4

[0107] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:

[0108] (1) Add 80 parts by weight of the active macromonomer polyether a1 into a reaction flask protected by N2, stir and heat to 150°C; uniformly dropwise add a mixture of 8 parts of 2-methylstyrene, 25 parts of the vinyl sulfonic acid monomer b2, and 1.3 parts of methyl ethyl ketone peroxide, and complete the addition over 11 hours. After the addition is complete, heat at 150°C for 3 hours to obtain a polyether-modified polymer A;

[0109] (2) 110 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, cooled to 60°C, and then 160 parts of deionized water and 60 parts of PVPK35 were added. Potassium hydroxide was then added to adjust the pH value of the system to 9, and the mixture was stirred evenly to obtain the water-soluble dispersant.

[0110] Example 5

[0111] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:

[0112] (1) Add 70 parts by weight of active macromonomer polyether a2 into a reaction flask protected by N2, stir and heat to 140°C; uniformly dropwise add a mixture of 12 parts of allylbenzene, 35 parts of vinyl sulfonic acid monomer b1, and 1.2 parts of dicumyl peroxide, and complete the addition within 10 hours. After the addition is complete, heat at 140°C for 1 hour to obtain a polyether-modified polymer A;

[0113] (2) 110 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, cooled to 60°C, and then 180 parts of deionized water and 50 parts of PVPK30 were added. Then, sodium hydroxide was added to adjust the pH value of the system to 7.5, and stirred evenly to obtain the water-soluble dispersant.

[0114] Example 6

[0115] In this embodiment, a water-soluble dispersant is provided, and the preparation method includes the following steps:

[0116] (1) Add 50 parts by weight of the active macromonomer polyether a3 into a reaction flask protected by N2, stir and heat to 125°C; uniformly dropwise add a mixture of 18 parts of styrene, 28 parts of the vinyl sulfonic acid monomer b2, and 0.7 parts of di-tert-butyl peroxide, and complete the addition over 8 hours. After the addition is complete, keep the mixture at 125°C for 1.5 hours to obtain a polyether-modified polymer A;

[0117] (2) 90 parts by weight of the polyether-modified polymer A obtained in step (1) were added to a reaction flask protected by N2, cooled to 60°C, and then 120 parts of deionized water and 40 parts of PVPK25 were added. Then, sodium hydroxide was added to adjust the pH value of the system to 8.5, and the mixture was stirred evenly to obtain the water-soluble dispersant.

[0118] Example 7

[0119] The only difference between this embodiment and embodiment 1 is that the weight portion of the reactive macromonomer polyether a1 in step (1) is 30 parts.

[0120] Example 8

[0121] The only difference between this embodiment and embodiment 3 is that the weight portion of the reactive macromonomer polyether a1 in step (1) is 110 parts.

[0122] Comparative Example 1

[0123] The only difference between this comparative example and Example 1 is that the active macromonomer polyether a1 in step (1) is replaced by allyl polyether APEG2000 in equal parts by weight.

[0124] Comparative Example 2

[0125] The only difference between this comparative example and Example 1 is that the vinyl sulfonic acid monomer b1 in step (1) is replaced by an equal weight portion of vinyl sulfonic acid.

[0126] Comparative Example 3

[0127] The only difference between this comparative example and Example 1 is that the vinylbenzene monomer (styrene) in step (1) is replaced by an equal weight portion of sodium p-styrenesulfonate.

[0128] Comparative Example 4

[0129] The only difference between this comparative example and Example 1 is that the polyamide polymer B (PVPK30) in step (2) is replaced by PVPK12 in equal parts by weight.

[0130] Comparative Example 5

[0131] The only difference between this comparative example and Example 1 is that the active macromonomer polyether a1 in step (1) is replaced by the polyether D-a1 prepared in Comparative Preparation Example 1 in equal parts by weight.

[0132] Comparative Example 6

[0133] A commercially available dispersant is MF.

[0134] Test Case

[0135] Using the laboratory sand mill method, according to the total amount of slurry formula of 200g, dispersant, water, and disperse dye (disperse blue 79 dye) are added in proportion; after stirring evenly, 400g of zirconium beads with a particle size of 0.8-1mm are added and sealed in a glass jar, shaken for 12 hours, and filtered to obtain the color paste.

[0136] The specific formula of the color paste prepared in this application is shown in Table 1:

[0137] Table 1

[0138] Performance Testing

[0139] (1) Viscosity: measured using NDJ-1B rotational viscometer, Shanghai Changji Geological Instrument Co., Ltd.; “-” indicates that the viscosity is too high to be measured;

[0140] (2) Particle size: Measured using BT-90 laser particle size analyzer, Dandong Better Instrument Co., Ltd.; “\” represents precipitation or lack of fluidity and cannot be measured;

[0141] (3) Storage stability: Store at 55°C for 7 days, observe the color paste state, and re-measure the particle size and viscosity;

[0142] (4) Centrifugal sedimentation rate (%): After centrifuging the dye paste at 4000 rpm for 20 minutes, wash with anhydrous ethanol, dry at 90°C to constant weight, and accurately weigh the sedimentation weight; Sedimentation rate = sedimentation weight ÷ (dye content in the paste × sample volume) × 100%; where "+" indicates no fluidity and cannot be tested.

[0143] The specific test results are shown in Table 2:

[0144] Table 2

[0145] As can be seen from Table 2, the water-soluble dispersant obtained by compounding the polyether-modified polymer A and the polyamide polymer B in the present application has a good dispersing effect on the dye paste (particle size D50 (initial): 189-234 nm) under the premise of a small amount, and the viscosity of the paste can also meet the requirements (viscosity (initial): 98-125 mPa·s), the centrifugal sedimentation rate is low (0.6%-2.3%), and the paste has good stability (stored at 55°C for 7 days, the viscosity and particle size of the paste do not change much), the storage period is long, and it is superior to commercially available dispersants.

[0146] From the comparison between Test Example 7 and Test Example 1, it can be seen that if the amount of active macromonomer polyether added is too small, the viscosity, particle size and centrifugal sedimentation rate of the dye paste will increase significantly, and the stability will deteriorate; from the comparison between Test Example 8 and Test Example 3, it can be seen that if the amount of active macromonomer polyether added is too much, the viscosity, particle size and centrifugal sedimentation rate of the dye paste will increase significantly.

[0147] From the comparison of comparative test examples 1-5 with test example 1, it can be seen that if any one of the raw materials for preparing polyether-modified polymer A (vinylbenzene monomer, vinyl sulfonic acid monomer and active macromonomer polyether) is replaced by other components, or if the polyamide polymer B is replaced by other components, the viscosity, particle size and centrifugal sedimentation rate of the dye paste will be significantly increased.

[0148] The applicant declares that this application uses the above-mentioned embodiments to illustrate the water-soluble dispersant of this application, its preparation method, and application, but this application is not limited to the above-mentioned embodiments, that is, it does not mean that this application must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvements to this application, equivalent replacement of various raw materials of the product of this application, addition of auxiliary ingredients, selection of specific methods, etc., all fall within the scope of protection and disclosure of this application.

Claims

1. A water-soluble dispersant comprising a polyether-modified polymer A and a polyamide-based high molecular polymer B; The raw materials for preparing the polyether-modified polymer A include vinylbenzene monomers, vinyl sulfonic acid monomers and active macromonomer polyether; The polyamide-based high molecular polymer B includes a homopolymer of vinyl pyrrolidone and / or a copolymer of vinyl pyrrolidone.

2. The water-soluble dispersant according to claim 1, in, The active macromonomer polyether is prepared by the following preparation method: Add polyetheramine and allyl succinic anhydride into the reactor, raise the temperature, and keep the temperature until anhydrous water is distilled out during the reaction to obtain the active macromonomer polyether.

3. The water-soluble dispersant according to claim 2, in, The polyetheramine is a monoprimary amino polyether in which the terminal hydroxyl group is converted into an amine by using a monoalcohol as an initiator to initiate the self-polymerization of ethylene oxide or the copolymerization of ethylene oxide and propylene oxide.

4. The water-soluble dispersant according to claim 2 or 3, in, The weight average molecular weight of the polyetheramine is 500 to 2500 g / mol.

5. A water-soluble dispersant according to any one of claims 2 to 4, in, The polyetheramine includes any one of JEFFAMINE M-2070, JEFFAMINE M-1000 or JEFFAMINE M-600 or a combination of at least two thereof; Preferably, the molar ratio of the polyetheramine to allyl succinic anhydride is (0.5-1.5):1, preferably 1:1; Preferably, the heating is to 120-160°C; Preferably, the insulation time is 2 to 6 hours; Preferably, the preparation process of the reactive macromonomer polyether is carried out under the protection of an inert gas.

6. A water-soluble dispersant according to any one of claims 1 to 5, in, The active macromonomer polyether has a structure as shown in the following formula I: Among them, R 1 is hydrogen or methyl, R 2 is methyl, ethyl, propyl or butyl, m is an integer of 10 to 60, and n is an integer of 0 to 15.

7. A water-soluble dispersant according to any one of claims 1 to 6, in, The vinyl sulfonic acid monomer is prepared by the following preparation method: Adding hydroxylated acrylic acid monomer and alkyl sultone into a reactor, mixing and reacting until the residual amount of alkyl sultone is less than 0.5%, thereby obtaining the vinyl sulfonic acid monomer; Preferably, the hydroxylated acrylic monomer comprises any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, hydroxypentyl acrylate or hydroxypentyl methacrylate, or a combination of at least two thereof; Preferably, the alkyl sultone includes any one of 1,3-propane sultone, 1-methyl-1,3-propane sultone, 2-methyl-1,3-propane sultone, 3-methyl-1,3-propane sultone, 1,4-butane sultone, 1-methyl-1,4-butane sultone, 2-methyl-1,4-butane sultone, 3-methyl-1,4-butane sultone or 4-methyl-1,4-butane sultone, or a combination of at least two thereof; Preferably, the molar ratio of the hydroxylated acrylic monomer to the alkyl sultone is 1:

1.

8. The water-soluble dispersant according to claim 7, in, The reaction system also includes an acid catalyst; Preferably, the acid catalyst comprises any one or a combination of at least two of p-toluenesulfonic acid, sulfuric acid, propionic acid or hydrochloric acid; Preferably, the amount of the acid catalyst added is 0.5% to 3% of the sum of the weight parts of the hydroxylated acrylic monomer and the alkyl sultone; Preferably, the mixing temperature is 60 to 90°C; Preferably, the reaction time is 5 to 20 hours; Preferably, the preparation process of the vinyl sulfonic acid monomer is carried out under the protection of an inert gas.

9. A water-soluble dispersant according to any one of claims 1 to 8, in, The vinylbenzene monomer includes any one or a combination of at least two of styrene, β-methylstyrene, allylbenzene, 3-methylstyrene, 2-methylstyrene or 2-isopropenyltoluene; Preferably, the mass ratio of the vinylbenzene monomer, the vinyl sulfonic acid monomer and the active macromonomer polyether is (3-10):(10-20):(20-50); Preferably, the raw materials for preparing the polyether-modified polymer A also include an initiator.

10. The water-soluble dispersant according to any one of claims 1 to 9, in, The weight average molecular weight of the polyether modified polymer A is 50000 to 200000 g / mol, preferably 50000 to 100000 g / mol; Preferably, the weight average molecular weight of the polyamide polymer B is 2000 to 100000 g / mol, preferably 10000 to 50000 g / mol; Preferably, the polyamide polymer B includes any one of PVPK25, PVPK30, PVPK35 or copolyvidone VA64, or a combination of at least two thereof; Preferably, the mass ratio of the polyether modified polymer A to the polyamide polymer B is (60-160):(40-70); Preferably, the water-soluble dispersant further comprises deionized water and a pH regulator; Preferably, the raw materials for preparing the water-soluble dispersant include the following components in parts by weight:

11. A method for preparing a water-soluble dispersant as claimed in any one of claims 1 to 10, wherein The following steps are involved: (1) adding a formulated amount of active macromonomer polyether into a reactor, raising the temperature, then adding vinylbenzene monomer, vinyl sulfonic acid monomer, and an optional initiator, and reacting at the same temperature to obtain the polyether-modified polymer A; (2) Cooling the polyether-modified polymer A obtained in step (1), then adding optional deionized water and polyamide polymer B, and then adding an optional pH adjuster, stirring, to obtain the water-soluble dispersant.

12. The preparation method according to claim 11, in, The heating in step (1) is to heat the mixture to 100-150°C.

13. The preparation method according to claim 11 or 12, in, The temperature of the insulation reaction in step (1) is 100-150° C., and the insulation reaction time is 1-3 hours.

14. The preparation method according to any one of claims 11 to 13, in, Step (1) and step (2) are both carried out under the protection of an inert gas; Preferably, the cooling in step (2) is cooling to 50-60°C.

15. Use of the water-soluble dispersant according to any one of claims 1 to 10 in dye dispersion.