Resin composition, resin molded product, and method for producing the same

JP2022164711A5Inactive Publication Date: 2024-12-05SEKISUI TECH MOLDING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022129648
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-06-23
Filing Date
2022-08-16
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing resin moldings face a trade-off between electromagnetic wave shielding properties and moldability due to increased conductivity from high filler content, leading to reduced fluidity in the molding process.

Method used

A resin composition comprising a thermoplastic resin, graphite, and two types of carbon black with specific BET surface areas and content ratios, optimized to enhance both electromagnetic wave shielding and moldability.

Benefits of technology

The composition achieves electromagnetic wave shielding of 20 dB or more across various frequencies and thermal conductivity of 1 W/(m·K) or more, while maintaining excellent moldability and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000028_0000
    Figure 00000028_0000
  • Figure 00000028_0001
    Figure 00000028_0001
  • Figure 00000028_0002
    Figure 00000028_0002
Patent Text Reader

Abstract

Provided is a resin composition that has excellent electromagnetic wave shielding properties. The present invention relates to a thermoplastic resin (A), a graphite (B), and two or more types of carbon black (C), wherein the carbon black (C) has a BET specific surface area of ​​600 m 2 / g or more and the first carbon black (C-1) with a BET specific surface area of ​​600m 2 and a second carbon black (C-2) having a molecular weight of less than 1000 kJ / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, a resin molded body using the resin composition, and a method for manufacturing the resin molded body.

Background Art

[0002] Conventionally, for the housings of communication devices used indoors and outdoors, electronic devices such as security cameras or smart meters, multi-information displays such as car navigation systems and smart meters, heat dissipation chassis of in-vehicle cameras, LED heat dissipation heat sinks, heat dissipation plates for SoC, or GDC, etc., metal plates, resin molded bodies having heat conductivity, etc. have been used. Here, SoC refers to "System-on-a-chip", and GDC refers to "Graphics Display Controller".

[0003] Patent Document 1 below discloses a molded product obtained by molding a resin compound containing a thermoplastic resin, graphite, and carbon black. In Patent Document 1, it is described that it is preferable to contain 20 to 80% by weight of graphite with respect to the entire resin compound. Also, it is described that it is preferable to contain 1 to 30% by weight of carbon black with respect to the entire resin compound.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] In recent years, with the increase in the speed of CPUs, there has been a demand for resin molded bodies having higher electromagnetic wave shielding properties than before.

[0006] However, in the production of a resin molded body such as that of Patent Document 1, when increasing the filling amount of a conductive filler such as carbon black to enhance conductivity, on the other hand, there is a problem that the fluidity in the molding process such as injection molding during production decreases, and ultimately the moldability decreases.

[0007] An object of the present invention is to provide a resin composition excellent in electromagnetic shielding properties, a resin molded body using the resin composition, and a method for producing the resin molded body.

Means for Solving the Problems

[0008] The resin composition according to the first invention of the present application contains a thermoplastic resin (A), graphite (B), and two or more types of carbon black (C), and the carbon black (C) has a BET specific surface area of 600 m 2 / g or more of the first carbon black (C-1) and a BET specific surface area of less than 600 m 2 / g of the second carbon black (C-2).

[0009] In a specific aspect of the resin composition according to the first invention of the present application, with respect to 100 parts by weight of the thermoplastic resin (A), the content of the first carbon black (C-1) is 5 parts by weight or more and 50 parts by weight or less, the content of the second carbon black (C-2) is 5 parts by weight or more and 50 parts by weight or less, and the total content of the carbon black (C) is 15 parts by weight or more and 90 parts by weight or less.

[0010] In another specific aspect of the resin composition according to the first invention of the present application, the DBP oil absorption amount of the first carbon black (C-1) is 250 ml / 100 g or more, and the DBP oil absorption amount of the second carbon black (C-2) is less than 250 ml / 100 g.

[0011] In still another specific aspect of the resin composition according to the first invention of the present application, the ash content of the carbon black (C) is 1% or less.

[0012] In yet another specific aspect of the resin composition according to the first invention of the present application, the graphite (B) is plate graphite.

[0013] In yet another specific aspect of the resin composition according to the first invention of this application, the volume-average particle size of the graphite (B) is 5 μm or more and 500 μm or less.

[0014] In yet another specific aspect of the resin composition according to the first invention of this application, the content of graphite (B) is 50 parts by weight or more and 300 parts by weight or less per 100 parts by weight of thermoplastic resin (A).

[0015] In yet another specific aspect of the resin composition according to the first invention of the present application, the thermoplastic resin (A) is at least one of olefin resins and nylon resins.

[0016] In yet another specific aspect of the resin composition relating to the first invention of this application, the volume resistivity is 1.0 × 10 5 It is less than or equal to Ω·cm.

[0017] The resin composition according to the second invention of this application is a resin composition comprising a thermoplastic resin (A), graphite (B), and carbon black (D), and is obtained by filling a mold with the molten resin composition in a direction perpendicular to the thickness direction of the resin molded body, and when a resin molded body of 100 mm in length × 100 mm in width × 2 mm in thickness is obtained, the resin molded body is measured by the Hahn Echo method at 125°C using pulsed NMR. 1 When the free induction damping curve of spin-spin relaxation of H is separated by the least squares method into three curves originating from the S component, M component, and L component in order of increasing relaxation time, the relaxation time of the L component is 1.3 msec or less.

[0018] In a specific aspect of the resin composition according to the second invention of this application, the ratio of component L to the sum of component S, component M, and component L (component L / (component S + component M + component L)) is 10% or less.

[0019] In other specific aspects of the resin composition according to the second invention of this application, the ratio of component L to the sum of component S, component M, and component L (component L / (component S + component M + component L)) is 4% or more.

[0020] In yet another specific aspect of the resin composition according to the second invention of this application, the graphite (B) is plate graphite.

[0021] In yet another specific aspect of the resin composition according to the second invention of this application, the thermoplastic resin (A) includes an olefin resin.

[0022] Hereinafter, the first and second inventions of this application may be collectively referred to as the present invention.

[0023] In yet another specific aspect of the resin composition according to the present invention, when the molten resin composition is filled into a mold from a direction perpendicular to the thickness direction of the resulting resin molded body, and a resin molded body measuring 100 mm in length, 100 mm in width, and 2 mm in thickness is obtained, the electromagnetic shielding effect of the resin molded body at any of the frequencies of 3 GHz, 25 GHz, 50 GHz, and 75 GHz is 20 dB or more.

[0024] In yet another specific aspect of the resin composition according to the present invention, when the molten resin composition is filled into a mold from a direction perpendicular to the thickness direction of the resin molded body to obtain a resin molded body measuring 100 mm in length, 100 mm in width, and 2 mm in thickness, the in-plane thermal conductivity of the resin molded body is 1 W / (m·K) or more.

[0025] The resin molded article according to the present invention is a molded article of a resin composition constructed in accordance with the present invention.

[0026] In a particular aspect of the resin molded article according to the present invention, the resin molded article contains fibers.

[0027] In other specific aspects of the resin molded article according to the present invention, the volume resistivity is 1.0 × 10⁻⁶ 5 It is less than or equal to Ω·cm.

[0028] A method for producing a resin molded article according to the present invention comprises the steps of: mixing a resin composition configured according to the present invention with a composite (E) containing a thermoplastic resin and fibers to obtain a mixture; and molding the mixture to obtain a resin molded article. [Effects of the Invention]

[0029] According to the present invention, it is possible to provide a resin composition that exhibits excellent electromagnetic wave shielding properties, a resin molded article using the resin composition, and a method for manufacturing the resin molded article. [Brief explanation of the drawing]

[0030] [Figure 1] Figure 1 is a schematic perspective view showing the heat dissipation chassis. [Figure 2] Figure 2 is a schematic perspective view showing the heat dissipation enclosure. [Figure 3] Figure 3 is a schematic perspective view showing the shape of the heatsink. [Modes for carrying out the invention]

[0031] The details of the present invention will be described below.

[0032] [Resin composition of the first invention] The resin composition of the first invention of this application comprises a thermoplastic resin (A), graphite (B), and two or more types of carbon black (C). The carbon black (C) has a BET specific surface area of ​​600 m². 2 First carbon black (C-1) with a concentration of 600m² or more, and a BET specific surface area of ​​600m² 2 It contains less than 1g of secondary carbon black (C-2).

[0033] The BET specific surface area can be measured from the nitrogen adsorption isotherm in accordance with the BET method. For example, the Anton Paar "NOVAtouchLX2" measuring device can be used.

[0034] Since the resin composition of the first invention contains a thermoplastic resin (A), graphite (B), and two or more specific carbon blacks (C), it is excellent in both electromagnetic wave shielding properties and moldability.

[0035] Conventionally, when manufacturing a resin molded body, increasing the filling amount of a conductive filler such as carbon black to enhance conductivity has a problem that, on the other hand, the fluidity in the molding process such as injection molding during manufacturing decreases, and ultimately the moldability decreases.

[0036] The inventors of the present invention focused on the BET specific surface areas of the first carbon black (C-1) and the second carbon black (C-2) in a resin composition containing a thermoplastic resin (A), graphite (B), and two or more carbon blacks (C). In particular, the inventors of the present invention found that by using carbon black (C) containing a first carbon black (C-1) having a BET specific surface area of 600 m 2 / g or more and a second carbon black (C-2) having a BET specific surface area of less than 600 m 2 / g, it is possible to enhance both the electromagnetic wave shielding properties and the moldability of the resin composition.

[0037] Hereinafter, each component of the resin composition will be described in detail.

[0038] (Thermoplastic resin (A)) The thermoplastic resin is not particularly limited, and known thermoplastic resins can be used. Specific examples of the thermoplastic resin include polyolefin, polystyrene, polyacrylate, polymethacrylate, polyacrylonitrile, polyester, polyamide, polyurethane, polyethersulfone, polyetherketone, polyimide, polydimethylsiloxane, polycarbonate, or a copolymer containing at least two of these. These thermoplastic resins may be used alone or in combination of a plurality. Note that the thermoplastic resin is preferably a resin having a high elastic modulus. Polyolefin (olefin resin) and polyamide (nylon resin) are more preferable because they are inexpensive and easy to mold under heating.

[0039] The polyolefin is not particularly limited, and known polyolefins can be used. Specific examples of polyolefins include polyethylene, which is an ethylene homopolymer; polyethylene-α-olefin copolymers; ethylene-(meth)acrylic acid copolymers; ethylene-(meth)acrylic acid ester copolymers; and polyethylene-vinyl acetate copolymers. Alternatively, the polyolefin may be polypropylene, which is a propylene homopolymer; polypropylene, which is a propylene-α-olefin copolymer; polybutene, which is a butene homopolymer; or a homopolymer or copolymer of conjugated dienes such as butadiene and isoprene. These polyolefins may be used individually or in combination. From the viewpoint of further improving heat resistance and elastic modulus, polypropylene is preferred as the polyolefin.

[0040] Furthermore, it is preferable that the polyolefin (olefin resin) contains an ethylene component. The ethylene component content is preferably 5% to 40% by mass. When the ethylene component content is within the above range, the impact resistance and heat resistance of the resin molded article can be further enhanced.

[0041] The MFR of thermoplastic resins, measured in accordance with JIS K7210, is preferably 10 g / 10 min or more, more preferably 30 g / 10 min or more, preferably 200 g / 10 min or less, and more preferably 150 g / 10 min or less. When the MFR is within the above range, the fluidity of the thermoplastic resin can be further improved.

[0042] The content of thermoplastic resin in the resin composition is preferably 20% by weight or more, more preferably 25% by weight or more, preferably 65% ​​by weight or less, and more preferably 60% by weight or less. When the content of thermoplastic resin is within the above range, the moldability of the resin composition can be further improved.

[0043] (Graphite (B)) The graphite is not particularly limited, but plate graphite is preferred. The plate graphite is not particularly limited as long as it is plate graphite, but for example, graphite, flake graphite, or graphene can be used. From the viewpoint of further improving thermal conductivity and flame retardancy, graphite or flake graphite is preferred. These may be used alone or in combination. In the first invention, for example, flake graphite can be used as plate graphite. From the viewpoint of further improving flame retardancy, expanded graphite may also be used.

[0044] Thinned graphite is obtained by exfoliating the original graphite and refers to a stack of graphene sheets that is thinner than the original graphite. The exfoliation process for producing thinned graphite is not particularly limited and may be performed using either a mechanical exfoliation method using a supercritical fluid or a chemical exfoliation method using an acid. The number of stacks of graphene sheets in thinned graphite should be less than that of the original graphite, but it is preferably 1000 layers or less, more preferably 500 layers or less, and even more preferably 200 layers or less.

[0045] In the first invention, the volume average particle diameter of the plate-shaped graphite is preferably 5 μm or more, more preferably 30 μm or more, even more preferably 60 μm or more, preferably 500 μm or less, more preferably 350 μm or less, and even more preferably 300 μm or less. When the volume average particle diameter of the plate-shaped graphite is above the lower limit, the electromagnetic wave shielding and heat dissipation properties can be further improved. On the other hand, when the volume average particle diameter of the plate-shaped graphite is below the upper limit, the impact resistance of the resin molded article can be further improved. Furthermore, as long as the volume average particle diameter of the plate-shaped graphite contained in the resin composition of the first invention is within the above range, two or more types of graphite particles with different particle sizes may be used in combination.

[0046] In the first invention, the volume-average particle diameter refers to the value calculated using the laser diffraction method with a laser diffraction / scattering particle size distribution analyzer in accordance with JIS Z 8825:2013, based on the volume-referenced distribution.

[0047] For example, plate-shaped graphite is placed in a soapy water solution (containing 0.01% neutral detergent) to a concentration of 2% by weight, and ultrasonic waves are irradiated for 1 minute at an output of 300W using an ultrasonic homogenizer to obtain a suspension. Next, the volume particle size distribution of the plate-shaped graphite is measured using a laser diffraction / scattering particle size analyzer (manufactured by Nikkiso Co., Ltd., product name "Microtrac MT3300"). The cumulative value of 50% of this volume particle size distribution can be calculated as the volume average particle size of the plate-shaped graphite.

[0048] The content of plate-shaped graphite is preferably 50 parts by weight or more, more preferably 70 parts by weight or more, even more preferably 100 parts by weight or more, preferably 300 parts by weight or less, more preferably 250 parts by weight or less, and even more preferably 200 parts by weight or less, per 100 parts by weight of thermoplastic resin. When the content of plate-shaped graphite is above the lower limit, electromagnetic wave shielding and heat dissipation can be further enhanced. Also, if the content of plate-shaped graphite is too high, the surface area of ​​the interface that becomes the starting point of fracture increases, so when the content of plate-shaped graphite is below the upper limit, impact resistance can be further enhanced.

[0049] The aspect ratio of the plate-shaped graphite is preferably 5 or more, more preferably 21 or more, preferably less than 2000, more preferably less than 1000, and even more preferably less than 100. When the aspect ratio of the plate-shaped graphite is equal to or greater than the lower limit, the heat dissipation in the planar direction can be further improved. Also, when the aspect ratio of the plate-shaped graphite is less than the upper limit, the graphite particles themselves are less likely to bend in the thermoplastic resin, for example, during injection molding. Therefore, the electromagnetic wave shielding performance can be further improved. In this specification, the aspect ratio refers to the ratio of the maximum dimension of the plate-shaped graphite in the lamination plane direction to the thickness of the plate-shaped graphite.

[0050] The thickness of the plate-like graphite can be measured, for example, using a transmission electron microscope (TEM) or a scanning electron microscope (SEM). From the viewpoint of making observation easier, it is desirable to heat a test piece cut from the resin composition or resin molded body to 600°C to remove the resin and then observe it with a transmission electron microscope (TEM) or a scanning electron microscope (SEM). The test piece may be cut along the direction along the main surface of the resin molded body, or along a direction perpendicular to the main surface of the resin molded body, as long as the thickness of the plate-like graphite can be measured after removing the resin.

[0051] (Carbon Black (C)) First-grade carbon black (C-1); As the first carbon black, for example, oil furnace black such as Ketjenblack, acetylene black, channel black, and thermal black can be used. Among these, oil furnace black is preferred from the viewpoint of further improving the conductivity of the resulting resin molded article. The ash content of the carbon black is preferably 1% or less. The carbon black may also contain metal impurities such as Fe and Ni.

[0052] The BET specific surface area of ​​the first carbon black is 600 m². 2 / g or more, preferably 700m 2 / g or more, more preferably 800m 2 The value is 1 / g or more. If the BET specific surface area of ​​the first carbon black is greater than or equal to the above lower limit, the conductivity can be further improved. The upper limit of the BET specific surface area of ​​the first carbon black is, for example, 1800m 2 It can be expressed as / g, preferably 1600m 2 / g or less, more preferably 1200m 2 It is less than / g.

[0053] The DBP oil absorption amount of the first carbon black is not particularly limited, but is preferably 250 ml / 100g or more, more preferably 270 ml / 100g or more, and even more preferably 300 ml / 100g or more. When the DBP oil absorption amount of the first carbon black is above the lower limit, the conductivity can be further enhanced. The upper limit of the DBP oil absorption amount of the first carbon black can be, for example, 600 ml / 100g.

[0054] In this specification, the DBP oil absorption amount of carbon black can be obtained by calculating the DBP drop amount at 70% of the maximum torque in accordance with JIS K 6217-4. The DBP oil absorption amount can be measured, for example, using an absorption amount meter (manufactured by Asahi Research Institute, model number "S-500").

[0055] The primary particle size of the first carbon black is not particularly limited, but is preferably 15 nm or larger, more preferably 20 nm or larger, more preferably 60 nm or smaller, and more preferably 50 nm or smaller. When the primary particle size of the first carbon black is within the above range, even higher conductivity can be obtained with an even lower concentration of the first carbon black.

[0056] In this specification, the primary particle size of carbon black is the average primary particle size determined, for example, using image data of carbon black obtained by a transmission electron microscope. As a transmission electron microscope, for example, a JEOL Ltd. product name "JEM-2200FS" can be used.

[0057] The content of the first carbon black is preferably 5 parts by weight or more, more preferably 10 parts by weight or more, preferably 50 parts by weight or less, and more preferably 40 parts by weight or less, per 100 parts by weight of thermoplastic resin. When the content of the first carbon black is above the lower limit, the conductivity can be further enhanced. Furthermore, when the content of the first carbon black is below the upper limit, the fluidity during molding can be further improved, and the moldability can be further enhanced.

[0058] Secondary carbon black (C-2); As the second carbon black, for example, oil furnace black such as Ketjenblack, acetylene black, channel black, and thermal black can be used. Among these, oil furnace black is preferred from the viewpoint of further improving the conductivity of the resulting resin molded article. In particular, it is more preferable that both the first and second carbon blacks are oil furnace black. The ash content of the carbon black is preferably 1% or less. The carbon black may also contain metal impurities such as Fe and Ni.

[0059] The BET specific surface area of ​​the second carbon black is 600 m². 2 Less than 400mg / g, preferably 400mg 2 Less than / g, more preferably 300m 2 It is less than or equal to / g. When the BET specific surface area of ​​the second carbon black is less than or equal to the above upper limit, the fluidity during molding can be further improved, and the moldability can be further enhanced. The lower limit of the BET specific surface area of ​​the second carbon black is, for example, 30m 2 It can be expressed as / g, preferably 100m 2 / g or more, comfortable 150m 2 It is 1 / g or more.

[0060] The DBP oil absorption amount of the second carbon black is not particularly limited, but is preferably less than 250 ml / 100g, and more preferably 200 ml / 100g or less. When the DBP oil absorption amount of the second carbon black is less than or equal to the above upper limit, the fluidity during molding can be further improved, and the moldability can be further enhanced. The lower limit of the DBP oil absorption amount of the second carbon black can be, for example, 30 ml / 100g.

[0061] The primary particle size of the second carbon black is preferably 5 nm or larger, more preferably 10 nm or larger, even more preferably 15 nm or larger, preferably 80 nm or smaller, more preferably 70 nm or smaller, even more preferably 60 nm or smaller, and particularly preferably 50 nm or smaller. When the primary particle size of the second carbon black is within the above range, even higher conductivity can be obtained with an even lower concentration of the second carbon black.

[0062] The content of the second carbon black is preferably 5 parts by weight or more, more preferably 10 parts by weight or more, preferably 50 parts by weight or less, and more preferably 40 parts by weight or less, per 100 parts by weight of thermoplastic resin. When the content of the second carbon black is above the lower limit, the fluidity during molding can be further improved, and the moldability can be further enhanced. Also, when the content of the second carbon black is below the upper limit, the conductivity can be further enhanced.

[0063] The ratio of the first carbon black to the second carbon black, (C-1) / (C-2), is preferably 0.01 or more, more preferably 0.1 or more, even more preferably 0.5 or more, preferably 10 or less, even more preferably 5 or less, and still more preferably 2 or less, in terms of weight ratio. When (C-1) / (C-2) is above the lower limit, the conductivity can be further enhanced. Also, when (C-1) / (C-2) is below the upper limit, the fluidity during molding can be further improved, and the moldability can be further enhanced.

[0064] The total carbon black content is preferably 15 parts by weight or more, more preferably 25 parts by weight or more, preferably 90 parts by weight or less, and more preferably 70 parts by weight or less, per 100 parts by weight of thermoplastic resin. When the total carbon black content is above the lower limit, the conductivity can be further enhanced. Furthermore, when the total carbon black content is below the upper limit, the fluidity during molding can be further improved, and the moldability can be further enhanced.

[0065] Furthermore, the carbon black may also contain other carbon blacks besides the first and second carbon blacks. The other carbon blacks can be those described in the sections on the first and second carbon blacks.

[0066] (Other additives) The resin composition of the first invention may contain various other additives as optional components, as long as they do not impair the effects of the first invention. Examples of additives include antioxidants such as phenolic, phosphorus-based, amine-based, and sulfur-based agents; ultraviolet absorbers such as benzotriazole-based and hydroxyphenyltriazine-based agents; metal damage inhibitors; various fillers; antistatic agents; stabilizers; and pigments. These may be used individually or in combination.

[0067] (Method for manufacturing resin compositions) The resin composition described above consists of a thermoplastic resin (A), graphite (B), and a resin with a BET specific surface area of ​​600 m². 2 First carbon black (C-1) with a concentration of 600m² or more, and a BET specific surface area of ​​600m² 2 It can be obtained by melt-mixing a second carbon black (C-2) in a quantity of less than 1g, along with other additives as needed.

[0068] The method of melt-kneading is not particularly limited, but examples include kneading under heating using a kneading device such as a twin-screw kneader like a Plastmill, a single-screw extruder, a twin-screw extruder, a Banbury mixer, a roll, or a pressurized kneader. Among these, the method of melt-kneading using an extruder is preferred. The form of the resin composition of the first invention is not particularly limited, but for example, it can be in the form of pellets.

[0069] When forming pellets, their shape is not particularly limited, but examples include spherical, cylindrical, and prismatic shapes. Among these, cylindrical is preferred from the viewpoint of pellet shape stability. Furthermore, in the case of cylindrical pellets, for example, the diameter is preferably 0.5 mm or more, more preferably 1 mm or more, preferably 5 mm or less, and more preferably 3 mm or less. The length is preferably 1 mm or more, more preferably 3 mm or more, preferably 10 mm or less, and more preferably 7 mm or less. The size of the pellets can be measured by randomly taking 100 pellets from the sample and using calipers.

[0070] Furthermore, for resin compositions other than cylindrical pellets, the diameter (pellet diameter) is preferably 1 mm or more, more preferably 5 mm or more, preferably 15 mm or less, and more preferably 10 mm or less. The pellet diameter can be determined by randomly selecting 100 pellets from the sample and measuring the diameter at the longest point using calipers.

[0071] The resin composition of the first invention preferably has a volume resistivity of 1.0 × 10 5 Ω·cm or less, more preferably 1.0 × 10⁻⁶ 2 It is less than or equal to Ω·cm. The lower limit of the volume resistivity is not particularly limited, but for example, 1.0 × 10⁻⁶ -4 The value is Ω·cm. Furthermore, the volume resistivity can be calculated by measuring the resistance value using a low-resistivity resistivity meter and using the resistivity correction coefficient and the thickness of the resin composition. For example, it can be measured at room temperature in air using a four-probe resistivity measuring device (Loresta AX MCP-T370, manufactured by Mitsubishi Chemical Analytec Co., Ltd.).

[0072] [Second Invention] The resin composition of the second invention of this application comprises a thermoplastic resin (A), graphite (B), and carbon black (D). Furthermore, the resin composition of the second invention has a relaxation time of 1.3 msec or less for the L component when measured using pulsed NMR.

[0073] The pulsed NMR measurement described above can be performed, for example, as follows: 700 mg of a sample of the resin molded body obtained under the molding conditions below is placed in a 10 mm diameter glass sample tube (BRUKER, part number 1824511, 10 mm diameter, 180 mm length, flat bottom). Next, the sample tube is placed in a pulsed NMR spectrometer (BRUKER "the minispe mq20") and held at 125°C for 10 minutes. Afterward, the Hahn Echo method is performed at 125°C, and the results are obtained. 1 The free induction damping curve of spin-spin relaxation of H is separated into three waveforms, each originating from the S component, M component, and L component, in order of increasing relaxation time, using the least squares method.

[0074] <Molding conditions> The molten resin composition of the second invention is filled into a mold from a direction perpendicular to the thickness direction of the resin molded body to obtain a resin molded body measuring 100 mm in length, 100 mm in width, and 2 mm in thickness. A sample of the resin molded body is obtained by cutting the flat sheet of the obtained resin molded body into 5 mm squares.

[0075] Waveform separation is performed by fitting using an exponential type. The fitting is performed using BRUKER's analysis software "TD-NMRA (Version 4.3 Rev 0.8)" according to the product manual.

[0076] The following formula is used for fitting.

[0077] Y = A1 × exp(-1 ÷ w1 × (t ÷ T2A)) w1 ) + B1 × exp(-1 ÷ w2 × (t ÷ T2B) w2 ) + C1 × exp(-1 ÷ w3 × (t ÷ T2C) w3 )

[0078] Here, w1 to w3 are Weibull coefficients, where w1, w2, and w3 take a value of 1. A1 is the ratio of the S component, B1 is the ratio of the M component, and C1 is the ratio of the L component. T2A represents the relaxation time of the S component, T2B represents the relaxation time of the M component, and T2C represents the relaxation time of the L component. t is time.

[0079] Furthermore, the following settings are required for the Hahn Echo method. Scans: 16 times Recycle Deray: 1 sec First 90-180 Pluse Separation:0.0082msec Final Plus Separation: 5msec Number of Points for Fitting:100

[0080] The above measurement conditions are just an example. It is desirable to set the Final Pulse Separation so that the intensity of the normalized relaxation curve is 0.02 msec or less, and to set the Recycle Deray to a value five times the longitudinal relaxation time T1.

[0081] Generally, when measured by pulsed NMR, 1 The free induction decay curve for spin-spin relaxation of H is obtained. The obtained free induction decay curve can be waveform-separated into three curves originating from the S component, M component, and L component, in order of increasing relaxation time. In other words, the measured free induction decay curve is a superposition of the free induction decay curves originating from the three components, S component, M component, and L component. This method of separating and analyzing into three components using pulsed NMR is well known, and an example of literature describing this method is Japanese Patent Application Publication No. 2018-2983.

[0082] The S component represents a component with a short relaxation time in pulsed NMR measurements, indicating low molecular mobility and a rigid structure. Conversely, the L component represents a component with a long relaxation time in pulsed NMR measurements, indicating high molecular mobility and a flexible structure. The M component has a relaxation time in pulsed NMR measurements between that of the S and L components, and therefore its molecular mobility is also between that of the S and L components.

[0083] The resin composition of the second invention can improve long-term heat resistance by having a relaxation time of component L of 1.3 msec or less. The relaxation time of component L is preferably 1.2 msec or less, and more preferably 1.0 msec or less. The lower limit of the relaxation time of component L is not particularly limited, but can be, for example, 0.5 msec.

[0084] Furthermore, in the resin composition of the second invention, the ratio of component L to the sum of components S, M, and L (component L / (component S + component M + component L)) is preferably 4% or more, more preferably 5% or more, more preferably 10% or less, and more preferably 9% or less. When the ratio (component L / (component S + component M + component L)) is within the above range, the long-term heat resistance can be further improved.

[0085] Furthermore, the relaxation time and component ratio of component L in the resin composition of the second invention can be set to the above-mentioned range by adjusting the type and content ratio of each component constituting the resin composition. Component L, which is a soft component with high molecular mobility, can be controlled by the affinity between the resin composition and the filler, and the dispersibility of the fillers that inhibit molecular mobility. Therefore, the relaxation time of component L can be further shortened by including two or more types of carbon black (D) in the resin composition, or by manufacturing it using the dry blending method described later.

[0086] The following provides a detailed explanation of each component of the resin composition.

[0087] (Thermoplastic resin (A)) The thermoplastic resin is not particularly limited, and any known thermoplastic resin can be used. Specific examples of thermoplastic resins include polyolefins, polystyrenes, polyacrylates, polymethacrylates, polyacrylonitriles, polyesters, polyamides, polyurethanes, polyethersulfones, polyetherketones, polyimides, polydimethylsiloxanes, polycarbonates, or copolymers containing at least two of these. These thermoplastic resins may be used individually or in combination. It is preferable that the thermoplastic resin has a high modulus of elasticity. Polyolefins (olefin-based resins) and polyamides (nylon-based resins) are more preferable, and polyolefins are even more preferable, due to their low cost and ease of molding under heat.

[0088] The polyolefin is not particularly limited, and known polyolefins can be used. Specific examples of polyolefins include polyethylene, which is an ethylene homopolymer; polyethylene-α-olefin copolymers; ethylene-(meth)acrylic acid copolymers; ethylene-(meth)acrylic acid ester copolymers; and polyethylene-vinyl acetate copolymers. Alternatively, the polyolefin may be polypropylene, which is a propylene homopolymer; polypropylene, which is a propylene-α-olefin copolymer; polybutene, which is a butene homopolymer; or a homopolymer or copolymer of conjugated dienes such as butadiene and isoprene. These polyolefins may be used individually or in combination. From the viewpoint of further improving heat resistance and elastic modulus, polypropylene is preferred as the polyolefin.

[0089] Furthermore, it is preferable that the polyolefin (olefin resin) contains an ethylene component. The ethylene component content is preferably 5% to 40% by mass. When the ethylene component content is within the above range, the impact resistance and heat resistance of the resin molded article can be further enhanced.

[0090] The MFR of thermoplastic resins, measured in accordance with JIS K7210, is preferably 10 g / 10 min or more, more preferably 30 g / 10 min or more, preferably 200 g / 10 min or less, and more preferably 150 g / 10 min or less. When the MFR is within the above range, the fluidity of the thermoplastic resin can be further improved.

[0091] The content of thermoplastic resin in the resin composition is preferably 20% by weight or more, more preferably 25% by weight or more, preferably 65% ​​by weight or less, and more preferably 60% by weight or less. When the content of thermoplastic resin is within the above range, the moldability of the resin composition can be further improved.

[0092] (Graphite (B)) The graphite is not particularly limited, but plate graphite is preferred. The plate graphite is not particularly limited as long as it is plate graphite, but for example, graphite, flake graphite, or graphene can be used. From the viewpoint of further improving thermal conductivity and flame retardancy, graphite or flake graphite is preferred. These may be used alone or in combination. In the second invention, for example, flake graphite can be used as plate graphite. From the viewpoint of further improving flame retardancy, expanded graphite may also be used.

[0093] Thinned graphite is obtained by exfoliating the original graphite and refers to a stack of graphene sheets that is thinner than the original graphite. The exfoliation process for producing thinned graphite is not particularly limited and may be performed using either a mechanical exfoliation method using a supercritical fluid or a chemical exfoliation method using an acid. The number of stacks of graphene sheets in thinned graphite should be less than that of the original graphite, but it is preferably 1000 layers or less, more preferably 500 layers or less, and even more preferably 200 layers or less.

[0094] In the second invention, the volume-average particle diameter of the plate-shaped graphite is preferably 5 μm or more, more preferably 30 μm or more, even more preferably 60 μm or more, preferably 500 μm or less, more preferably 350 μm or less, and even more preferably 300 μm or less. When the volume-average particle diameter of the plate-shaped graphite is above the lower limit, the electromagnetic wave shielding and heat dissipation properties can be further improved. On the other hand, when the volume-average particle diameter of the plate-shaped graphite is below the upper limit, the impact resistance of the resin molded article can be further improved. Furthermore, as long as the volume-average particle diameter of the plate-shaped graphite contained in the resin composition of the second invention is within the above range, two or more types of graphite particles with different particle sizes may be used in combination.

[0095] In the second invention, the volume-average particle diameter refers to the value calculated using the laser diffraction method with a laser diffraction / scattering particle size distribution analyzer in accordance with JIS Z 8825:2013, based on the volume-referenced distribution.

[0096] For example, plate-shaped graphite is placed in a soapy water solution (containing 0.01% neutral detergent) to a concentration of 2% by weight, and ultrasonic waves are irradiated for 1 minute at an output of 300W using an ultrasonic homogenizer to obtain a suspension. Next, the volume particle size distribution of the plate-shaped graphite is measured using a laser diffraction / scattering particle size analyzer (manufactured by Nikkiso Co., Ltd., product name "Microtrac MT3300"). The cumulative value of 50% of this volume particle size distribution can be calculated as the volume average particle size of the plate-shaped graphite.

[0097] The content of plate-shaped graphite is preferably 50 parts by weight or more, more preferably 70 parts by weight or more, even more preferably 100 parts by weight or more, preferably 300 parts by weight or less, more preferably 250 parts by weight or less, and even more preferably 200 parts by weight or less, per 100 parts by weight of thermoplastic resin. When the content of plate-shaped graphite is above the lower limit, electromagnetic wave shielding and heat dissipation can be further enhanced. Also, if the content of plate-shaped graphite is too high, the surface area of ​​the interface that becomes the starting point of fracture increases, so when the content of plate-shaped graphite is below the upper limit, impact resistance can be further enhanced.

[0098] The aspect ratio of the plate-shaped graphite is preferably 5 or more, more preferably 21 or more, preferably less than 2000, more preferably less than 1000, and even more preferably less than 100. When the aspect ratio of the plate-shaped graphite is equal to or greater than the lower limit, the heat dissipation in the planar direction can be further improved. Also, when the aspect ratio of the plate-shaped graphite is less than the upper limit, the graphite particles themselves are less likely to bend in the thermoplastic resin, for example, during injection molding. Therefore, the electromagnetic wave shielding performance can be further improved. In this specification, the aspect ratio refers to the ratio of the maximum dimension of the plate-shaped graphite in the lamination plane direction to the thickness of the plate-shaped graphite.

[0099] The thickness of the plate-like graphite can be measured, for example, using a transmission electron microscope (TEM) or a scanning electron microscope (SEM). From the viewpoint of making observation easier, it is desirable to heat a test piece cut from the resin composition or resin molded body to 600°C to remove the resin and then observe it with a transmission electron microscope (TEM) or a scanning electron microscope (SEM). The test piece may be cut along the direction along the main surface of the resin molded body, or along a direction perpendicular to the main surface of the resin molded body, as long as the thickness of the plate-like graphite can be measured after removing the resin.

[0100] (Carbon Black (D)) As carbon black, for example, oil furnace black such as Ketjenblack, acetylene black, channel black, and thermal black can be used. Among these, oil furnace black is preferred from the viewpoint of further improving the conductivity of the resulting resin molded product. The ash content of the carbon black is preferably 1% or less. Furthermore, the carbon black may contain metal impurities such as Fe and Ni.

[0101] The BET specific surface area of ​​carbon black is preferably 30 m². 2 / g or more, comfortably 50m 2 / g or more, preferably 2000m 2 / g or less, more preferably 1500m 2It is less than / g. If the BET specific surface area of ​​carbon black is within the above range, conductivity can be further improved.

[0102] The BET specific surface area can be measured from the nitrogen adsorption isotherm in accordance with the BET method. For example, the Anton Paar "NOVAtouchLX2" measuring device can be used.

[0103] The amount of DBP absorbed by carbon black is not particularly limited, but is preferably 50 ml / 100g or more, more preferably 100 ml / 100g or more, preferably 450 ml / 100g or less, and more preferably 400 ml / 100g or less. When the amount of DBP absorbed by carbon black is within the above range, conductivity can be further improved.

[0104] In this specification, the DBP oil absorption amount of carbon black can be obtained by calculating the DBP drop amount at 70% of the maximum torque in accordance with JIS K 6217-4. The DBP oil absorption amount can be measured, for example, using an absorption amount meter (manufactured by Asahi Research Institute, model number "S-500").

[0105] The primary particle size of the carbon black is not particularly limited, but is preferably 30 nm or larger, more preferably 35 nm or larger, more preferably 50 nm or smaller, and more preferably 45 nm or smaller. When the primary particle size of the carbon black is within the above range, even higher conductivity can be obtained with an even lower concentration of carbon black.

[0106] In this specification, the primary particle size of carbon black is the average primary particle size determined, for example, using image data of carbon black obtained by a transmission electron microscope. As a transmission electron microscope, for example, a JEOL Ltd. product name "JEM-2200FS" can be used.

[0107] The carbon black content is preferably 3 parts by weight or more, more preferably 5 parts by weight or more, preferably 200 parts by weight or less, and more preferably 150 parts by weight or less, per 100 parts by weight of thermoplastic resin. When the carbon black content is within the above range, conductivity and long-term heat resistance can be further improved.

[0108] Furthermore, two or more types of carbon black may be used. For example, the first carbon black (C-1) and the second carbon black (C-2) of the first invention may be used as carbon black. The preferred range of their content and content ratio is the same as that of the resin composition of the first invention. In this case, the relaxation time of the L component in pulsed NMR measurement can be further shortened.

[0109] (Other additives) The resin composition of the second invention may contain various other additives as optional components, to the extent that they do not impair the effects of the second invention. Examples of additives include antioxidants such as phenolic, phosphorus-based, amine-based, and sulfur-based agents; ultraviolet absorbers such as benzotriazole-based and hydroxyphenyltriazine-based agents; metal damage inhibitors; various fillers; antistatic agents; stabilizers; and pigments. These may be used individually or in combination.

[0110] (Method for manufacturing resin compositions) The resin composition described above can be obtained by first melt-kneading a thermoplastic resin (A), graphite (B), carbon black (D), and other additives as needed.

[0111] The method of melt-kneading is not particularly limited, but examples include kneading under heating using a kneading device such as a twin-screw kneader like a Plastmill, a single-screw extruder, a twin-screw extruder, a Banbury mixer, a roll, or a pressurized kneader. Among these, the method of melt-kneading using an extruder is preferred. The form of the resin composition of the second invention is not particularly limited, but for example, it can be in the form of pellets.

[0112] The resin composition of the second invention preferably has a volume resistivity of 1.0 × 10 5 Ω·cm or less, more preferably 1.0 × 10⁻⁶ 2 It is less than or equal to Ω·cm. The lower limit of the volume resistivity is not particularly limited, but for example, 1.0 × 10⁻⁶ -4 The value is Ω·cm. Furthermore, the volume resistivity can be calculated by measuring the resistance value using a low-resistivity resistivity meter and using the resistivity correction coefficient and the thickness of the resin composition. For example, it can be measured at room temperature in air using a four-probe resistivity measuring device (Loresta AX MCP-T370, manufactured by Mitsubishi Chemical Analytec Co., Ltd.).

[0113] Hereinafter, the first invention and the second invention may be collectively referred to as the present invention. The first invention and the second invention may be implemented individually, or they may be implemented in combination.

[0114] The resin composition of the present invention, when used to obtain a resin molded article under the following conditions, exhibits an electromagnetic shielding effect of 20 dB or more, more preferably 20 dB or more, and even more preferably 41 dB or more, at any of the frequencies of 3 GHz, 25 GHz, 50 GHz, and 75 GHz. The upper limit of the electromagnetic shielding effect of the above-mentioned resin molded article is not particularly limited, but can be, for example, 80 dB.

[0115] <Molding conditions> A molten resin composition is filled into a mold from a direction perpendicular to the thickness direction of the resin molded body to obtain a resin molded body measuring 100 mm in length, 100 mm in width, and 2 mm in thickness.

[0116] The resin composition of the present invention, when used to obtain a molded resin article under the following conditions, has an in-plane thermal conductivity of preferably 1 W / (m·K) or more, more preferably 3 W / (m·K) or more, and even more preferably 5 W / (m·K) or more. The upper limit of the in-plane thermal conductivity of the molded resin article can be, for example, 50 W / (m·K).

[0117] <Molding conditions> A molten resin composition is filled into a mold from a direction perpendicular to the thickness direction of the resin molded body to obtain a resin molded body measuring 100 mm in length, 100 mm in width, and 2 mm in thickness.

[0118] [Method for manufacturing resin molded products] The resin molded article according to the present invention is a molded article of the resin composition according to the present invention described above. Therefore, the resin molded article of the present invention can be obtained by molding the resin composition described above.

[0119] The molding method is not particularly limited, but examples include press working, extrusion, extrusion lamination, or injection molding. Among these, it is preferable to mold the mixture by injection molding. In this case, the mechanical strength of the resulting resin molded article can be further increased.

[0120] In the present invention, a resin molded article may be obtained by mixing the resin composition according to the present invention described above with a composite (E) containing a thermoplastic resin and fibers to obtain a mixture, and then molding the mixture.

[0121] In the second invention, it is desirable that the mixture of the above-described resin composition and the composite (E) be used as the resin composition of the second invention. Therefore, when performing measurements in pulsed NMR, it is also desirable to use the mixture of the above-described resin composition and the composite for measurement. By using such a mixture, the relaxation time of the L component in pulsed NMR measurements can be further shortened.

[0122] When obtaining the mixture, it is preferable to mix the resin composition and composite (E) by dry blending. In this case, a resin molded article with even greater mechanical strength can be obtained.

[0123] In this specification, dry blending refers to mixing without melting or adding solvents. The method of dry blending is not particularly limited and can be performed, for example, by simply mixing the resin composition and the composite (E) by hand. Alternatively, mixing may be done using a small tumbler or the like.

[0124] The thermoplastic resin included in composite (E) can be any of the thermoplastic resins described in the section on resin compositions above. While it is preferable that the thermoplastic resin included in composite (E) be the same as the thermoplastic resin included in the resin composition, it may also be a different resin.

[0125] The fibers may be inorganic fibers or organic fibers. Alternatively, inorganic and organic fibers may be used in combination.

[0126] Examples of fibers that can be used include metal fibers, carbon fibers, cellulose fibers, aramid fibers, or glass fibers. These may be used individually or in combination.

[0127] While not particularly limited, carbon fibers such as PAN-based or pitch-based carbon fibers can be used.

[0128] The fibers are preferably oriented within the thermoplastic resin, and more preferably uniaxially oriented. Such a composite (E) can be produced by aligning the fibers and bringing them into contact with molten thermoplastic resin. In particular, when produced by the plutonation method, a composite (E) in which the thermoplastic resin is impregnated into the fibers can be obtained. The form of the composite (E) is not particularly limited, but for example, it can be in the form of pellets.

[0129] The length of the fibers is not particularly limited, but is preferably 3 mm or more, more preferably 5 mm or more, more preferably 20 mm or less, and more preferably 15 mm or less. When the fiber length is within the above range, the mechanical strength of the resulting resin molded article can be further increased.

[0130] Furthermore, the fiber diameter is preferably 5 μm or more, more preferably 10 μm or more, more preferably 50 μm or less, and more preferably 30 μm or less. When the fiber diameter is within the above range, the mechanical strength of the resulting resin molded article can be further increased.

[0131] The fiber length and fiber diameter can be determined by taking the average of 100 measurements, for example, using a transmission electron microscope (TEM) or scanning electron microscope (SEM). From the viewpoint of making observation easier, it is desirable to heat a test piece cut from the composite (E) or resin molded body to 600°C to remove the resin and then observe it with a transmission electron microscope (TEM) or scanning electron microscope (SEM).

[0132] The fiber content is not particularly limited, but it is preferably 50 parts by weight or more and 200 parts by weight or less per 100 parts by weight of thermoplastic resin contained in the composite (E). When the fiber content is within the above range, the mechanical strength of the resulting resin molded article can be further increased.

[0133] [Resin molded product] The resin molded article of the present invention can be obtained by the resin molded article manufacturing method described above. Since the resin composition of the present invention is used in the resin molded article manufacturing method described above, it has excellent conductivity and, consequently, excellent electromagnetic wave shielding properties.

[0134] The resin molded article of the present invention preferably has a volume resistivity of 1.0 × 10⁻⁶. 5 Ω·cm or less, more preferably 1.0 × 10⁻⁶ 3 It is less than or equal to Ω·cm. In this case, the electromagnetic shielding properties of the resin molded body can be further enhanced. The lower limit of the volume resistivity is not particularly limited, but for example, 1.0 × 10 -4 It can be expressed as Ω·cm.

[0135] Furthermore, the volume resistivity can be calculated by measuring the resistance value using a low-resistivity resistivity meter and then using the resistivity correction coefficient and the thickness of the resin molded body. For example, it can be measured at room temperature in air using a four-probe resistivity measuring device (Loresta AX MCP-T370, manufactured by Mitsubishi Chemical Analytec Co., Ltd.).

[0136] The resin molded article of the present invention has an electromagnetic shielding effect at a frequency of 3 GHz, preferably 20 dB or more, more preferably 25 dB or more, and even more preferably 30 dB or more. The upper limit of the electromagnetic shielding effect is not particularly limited, but for example, it is 80 dB.

[0137] The electromagnetic shielding effect (electromagnetic shielding performance) at a frequency of 3 GHz can be measured, for example, using the Dual-Focus Flat Cavity (DFFC) method.

[0138] In the present invention, the in-plane thermal conductivity of the main surface of the resin molded article is preferably 2 W / (m·K) or more, more preferably 5 W / (m·K) or more, and even more preferably 10 W / (m·K) or more. In this case, the heat dissipation performance of the resin molded article can be further improved. Furthermore, the upper limit of the in-plane thermal conductivity is not particularly limited, but for example, it can be 50 W / (m·K).

[0139] The main surface may be a flat surface or a curved surface. In this invention, the main surface refers to the surface with the largest area among multiple surfaces on the outer surface of the resin molded article, and which is a continuous surface.

[0140] The thermal conductivity in the in-plane direction can be calculated using the following equation (1).

[0141] Thermal conductivity (W / (m·K)) = Specific gravity (g / cm³) 3 ) × Specific heat (J / g·K) × Thermal diffusivity (mm 2 / s)…Formula (1)

[0142] Thermal diffusivity can be measured, for example, using a Xenon Flash Laser Analyzer LFA467 HyperFlash manufactured by Netch Japan Co., Ltd.

[0143] Because the resin molded articles of the present invention have excellent electromagnetic shielding properties, they can be suitably used as housings for communication equipment requiring electromagnetic shielding, as well as for electronic devices such as smart meters and in-vehicle ECUs.

[0144] The resin molded article of the present invention may be in the shape of a heat dissipation chassis, a heat dissipation housing, or a heat sink. Specific examples of heat dissipation chassis, heat dissipation housings, and heat sink shapes will be described below with reference to Figures 1 to 3.

[0145] Figure 1 is a schematic perspective view of a heat dissipation chassis. When a resin molded body is the heat dissipation chassis, the part indicated by arrow A in Figure 1 is the main surface.

[0146] Figure 2 is a schematic perspective view of a heat dissipation enclosure. When the heat dissipation enclosure is a resin molded body, the part indicated by arrow B in Figure 2 is the main surface. Note that, as shown in Figures 1 and 2, the main surface may have irregularities.

[0147] Figure 3 is a schematic perspective view of a heat sink shape. When a resin molded body is in the shape of a heat sink, the part indicated by arrow C in Figure 3 is the main surface. Specifically, the main surface on one side of the bottom plate and the surface of the fin are the main surfaces. In this way, there may be multiple main surfaces.

[0148] Furthermore, circuits may be formed on the surface of such a resin molded body.

[0149] The effects of the present invention will be clarified below by giving specific examples and comparative examples of the present invention. However, the present invention is not limited to the following examples.

[0150] (Example 1) A resin composition was obtained by melt-kneading 100 parts by weight of polypropylene (PP) as a thermoplastic resin, 150 parts by weight of flake-shaped graphite particles as plate-shaped graphite particles, 20 parts by weight of oil furnace black as a first carbon black, and 20 parts by weight of oil furnace black as a second carbon black, at 200°C using a Laboplast Mill (manufactured by Toyo Seiki Co., Ltd., product number "R100"). The obtained resin composition was injection-molded at a resin composition temperature of 230°C and a mold temperature of 40°C to obtain a resin molded body measuring 300 mm in length, 300 mm in width, and 2 mm in thickness. The polypropylene used was "BC08F" (MFR: 70 g / 10 min (230°C)) manufactured by Nippon Polypropylene Co., Ltd. The flake-shaped graphite particles used were "CPB-100B" (volume average particle diameter: 80 μm) manufactured by Chuetsu Graphite Industry Co., Ltd. The first carbon black oil furnace black is Lion Corporation's "EC300J" (BET specific surface area: 800m²). 2 The carbon black used was a carbon black with a DBP oil absorption capacity of 365 ml / 100 g and a primary particle size of 40 nm. The second carbon black oil furnace black was Cabot's "VulcanXC72" (BET specific surface area: 254 m²). 2 ( / g, DBP oil absorption: 174 ml / 100 g, primary particle size: 30 nm) was used.

[0151] The MFR of the thermoplastic resins in the examples and comparative examples was measured in accordance with JIS K7210. The volume-average particle size of graphite was calculated using the laser diffraction method with a laser diffraction / scattering particle size distribution analyzer (Nikkiso Co., Ltd., product name "Microtrac MT3300") in accordance with JIS Z 8825:2013, based on the volume-based distribution. The BET specific surface area of ​​the first and second carbon blacks was measured from the nitrogen adsorption isotherm in accordance with the BET method. The measuring device used was Anton Paar, product number "NOVAtouch LX2". The DBP oil absorption amount of the first and second carbon blacks was measured using an absorption meter (Asahi Soken Co., Ltd., product number "S-500"), and the DBP drop amount was calculated at 70% of the maximum torque in accordance with JIS K 6217-4. The primary particle sizes of the first and second carbon blacks were determined from the average value of 1000 carbon black particles in image data obtained using a transmission electron microscope (JEOL Ltd., product name "JEM-2200FS").

[0152] (Example 2) The first carbon black used is oil furnace black, manufactured by Lion Corporation, product name "Lionite CB" (BET specific surface area: 1052 m²). 2 A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the values ​​were changed to ( / g, DBP oil absorption: 280 ml / 100g, primary particle size: 41 nm).

[0153] (Example 3) The first carbon black used is oil furnace black from Cabot, product name "BlackPearls2000" (BET specific surface area: 1475 m²). 2 A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the values ​​were changed to ( / g, DBP oil absorption: 330 ml / 100 g, primary particle size: 15 nm).

[0154] (Example 4) As a second carbon black, we used oil furnace black manufactured by Asahi Carbon Co., Ltd., product name "F-200GS" (BET specific surface area: 55m²). 2A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the ratio ( / g, DBP oil absorption: 55 ml / 100 g, primary particle size: 38 nm) was changed.

[0155] (Example 5) A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the flake-shaped graphite particles, which were plate-shaped graphite particles, were changed to "CPB-300" (volume-average particle size: 300 μm), manufactured by Chuetsu Graphite Industry Co., Ltd.

[0156] (Example 6) A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the flake-shaped graphite particles, which were plate-shaped graphite particles, were changed to "F#2" (volume-average particle size: 140 μm), manufactured by Nippon Graphite Industries Co., Ltd.

[0157] (Example 7) A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the polypropylene (PP) used as the thermoplastic resin was changed to "SA06GA" (MFR: 60g / 10min (230℃)) manufactured by Nippon Polypropylene Co., Ltd.

[0158] (Example 8) A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the thermoplastic resin was changed to Toray Industries' Nylon 6, trade name "CM1007" (MFR: 62g / 10min (260℃)), the melt mixing temperature was set to 230℃, and the injection molding temperature was set to 260℃.

[0159] (Example 9) Manufacturing of resin composition (A-1); 100 parts by weight of polypropylene (PP) as a thermoplastic resin, 160 parts by weight of flake graphite as plate-like graphite, 20 parts by weight of oil furnace black as a first carbon black, and 20 parts by weight of oil furnace black as a second carbon black were used. These were melt-kneaded at 200°C using a laboplast mill (manufactured by Toyo Seiki Co., Ltd., model number "R100") to obtain resin composition (A-1).

[0160] The obtained resin composition (A-1) was in pellet form, with a pellet diameter of 3 mm. The pellet diameter was determined by randomly selecting 100 pellets from the sample and measuring the diameter at the longest point using calipers. For the polypropylene, we used "MA04A" (MFR: 40 g / 10 min (230°C)) manufactured by Nippon Polypropylene Co., Ltd. For the flaky graphite, we used "CPB-300" (average particle size: 300 μm, aspect ratio: 10) manufactured by Chuetsu Graphite Industry Co., Ltd. For the first carbon black oil furnace black, we used "EC300J" (BET specific surface area: 800 m²) manufactured by Lion Corporation. 2 The carbon black used was a carbon black with a DBP oil absorption capacity of 365 ml / 100 g and a primary particle size of 40 nm. The second carbon black oil furnace black was Cabot's "VulcanXC72" (BET specific surface area: 254 m²). 2 ( / g, DBP oil absorption: 174 ml / 100 g, primary particle size: 30 nm) was used.

[0161] Manufacturing of resin composition (B-1); A resin composition (B-1) was obtained using 60 parts by weight of polypropylene (PP) as a thermoplastic resin and 40 parts by weight of glass fibers with a length of 7 mm, following the pultrusion method. The obtained resin composition (B-1) was in pellet form, with a pellet diameter of 7 mm. The polypropylene used was "MA04A" (MFR: 40 g / 10 min (230℃)) manufactured by Nippon Polypropylene Co., Ltd. The roving fiber (glass fiber) used was "TUFROV4520" (fiber diameter: 16 μm) manufactured by Nippon Electric Glass Co., Ltd.

[0162] The obtained resin composition (A-1) and resin composition (B-1) were dry-blended in a ratio of 85:15 using a small tumbler at a rotation speed of 30 rpm for 5 minutes to obtain a resin composition. The resin molded article was obtained in the same manner as in Example 1 in other respects.

[0163] (Comparative Example 1) A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the content of plate-shaped graphite particles was changed to 200 parts by weight and the first and second carbon blacks were not used.

[0164] (Comparative Example 2) A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the content of the first carbon black was changed to 40 parts by weight and the second carbon black was not used.

[0165] (Comparative Example 3) A resin composition and a resin molded article were obtained in the same manner as in Example 1, except that the content of the second carbon black was changed to 40 parts by weight and the first carbon black was not used.

[0166] [evaluation] <Volume resistivity> The volume resistivity of the resin molded articles obtained in Examples 1-9 and Comparative Examples 1-3 was measured using a four-probe resistivity measuring device (Mitsubishi Chemical Analytec Co., Ltd., part number "Loresta AX MCP-T370").

[0167] <Electromagnetic shielding effect (dB) at a frequency of 3GHz> The electromagnetic shielding effect (electromagnetic shielding performance, unit: dB) at a frequency of 3 GHz of the resin molded articles obtained in Examples 1-9 and Comparative Examples 1-3 was measured using a dual-focus flat cavity (DFFC) (manufactured by Sanken Corporation) jig for measuring shielding characteristics. Specifically, electromagnetic waves were radiated from the transmitting focal point, and the intensity of the electromagnetic waves focused at the receiving focal point was measured as the received voltage. The received voltage V0 with no sample inserted and the received voltage V with a sample inserted were measured, and the electromagnetic shielding effect was calculated according to the following equation (2).

[0168] Electromagnetic shielding effect = 20 × log 10 (V0 / V)…Equation (2)

[0169] The measurement frequency range was 1 GHz to 15 GHz, and the measuring instrument used was an Agilent Technologies "Component Analyzer N4375D". The sample dimensions of the resin molded body were 300 mm x 20 mm x 2.0 mm.

[0170] <Spiral flow length> The fluidity of the resin compositions obtained in Examples 1-9 and Comparative Examples 1-3 was evaluated as spiral flow length. Specifically, the flow length was measured when injection molding was performed using a resin flow length measuring mold with an Archimedes spiral channel measuring 20 mm in width and 2 mm in thickness, at a cylinder temperature of 230°C, a mold temperature of 40°C, and an injection pressure of 150 MPa.

[0171] The results are shown in Tables 1 and 2 below.

[0172] [Table 1]

[0173] [Table 2]

[0174] Tables 1 and 2 show that Examples 1-9 exhibited excellent electromagnetic shielding and moldability. On the other hand, Comparative Examples 1 and 3 did not exhibit sufficient electromagnetic shielding, and Comparative Example 2 did not exhibit sufficient moldability.

[0175] (Example 10) Instead of the first and second carbon blacks, use oil furnace black as the carbon black (Lion Corporation product name "Lionite CB", BET specific surface area: 1052 m²). 2 (1 / g, DBP oil absorption: 280 ml / 100 g, primary particle size: 41 nm) 40 parts by weight were used. The resin composition was obtained in the same manner as in Example 9 in other respects.

[0176] (Example 11) A resin composition was obtained by melt-kneading 100 parts by weight of polypropylene (PP) as a thermoplastic resin, 160 parts by weight of flake graphite as plate-shaped graphite particles, and 40 parts by weight of oil furnace black as carbon black at 200°C using a Laboplast Mill (manufactured by Toyo Seiki Co., Ltd., product number "R100"). The polypropylene used was "MA04A" (MFR: 40g / 10min (230°C)) manufactured by Nippon Polypropylene Co., Ltd. The flake graphite used was "CPB-300" (average particle size: 300μm, aspect ratio: 10) manufactured by Chuetsu Graphite Industry Co., Ltd. The oil furnace black used was "Lionite CB" (BET specific surface area: 1052m²) manufactured by Lion Corporation. 2 (The following parameters were used: / g, DBP oil absorption rate: 280 ml / 100g, primary particle size: 41 nm).

[0177] (Example 12) Manufacturing of resin composition (A-2); 100 parts by weight of polypropylene (PP) as a thermoplastic resin, 70 parts by weight of flake graphite as plate-like graphite, and 30 parts by weight of oil furnace black as carbon black were used. These were melt-kneaded at 200°C using a laboplast mill (manufactured by Toyo Seiki Co., Ltd., model number "R100") to obtain resin composition (A-2).

[0178] The obtained resin composition (A-2) was in pellet form, with a pellet diameter of 3 mm. The pellet diameter was determined by randomly selecting 100 pellets from the sample and measuring the diameter at the longest point using calipers. For the polypropylene, we used "MA04A" (MFR: 40 g / 10 min (230°C)) manufactured by Nippon Polypropylene Co., Ltd. For the flaky graphite, we used "CPB-300" (average particle size: 300 μm, aspect ratio: 10) manufactured by Chuetsu Graphite Industry Co., Ltd. For the oil furnace black, we used "F-200GS" (BET specific surface area: 55 m²) manufactured by Asahi Carbon Co., Ltd. 2 ( / g, DBP oil absorption: 55 ml / 100 g, primary particle size: 38 nm) was used.

[0179] The obtained resin composition (A-2) and the same resin composition (B-1) as in Example 9 were dry-blended in a ratio of 70:30 using a small tumbler at a rotation speed of 30 rpm for 5 minutes to obtain a resin composition.

[0180] [evaluation] (Pulsed NMR) The resin compositions obtained in Examples 4, 9-12 and Comparative Example 1 were subjected to Hahn Echo spectroscopy at 125°C using pulsed NMR, and the results were obtained 1 The free induction damping curve of H's spin-spin relaxation was separated into three waveforms, each originating from the S, M, and L components, in order of increasing relaxation time, using the least squares method. The relaxation time of the L component and the ratio of the L component to the sum of the S, M, and L components (L component / (S component + M component + L component)) were then calculated and evaluated according to the following evaluation criteria.

[0181] <Evaluation Criteria> Relaxation time of the L component; 〇…1.3msec or less ×...Exceeding 1.3 msec

[0182] Ratio (L component / (S component + M component + L component)) (1); ○...10% or less ×...over 10%

[0183] Ratio (L component / (S component + M component + L component)) (2); ○...4% or more ×...less than 4%

[0184] The measurement using the Hahn Echo method with pulsed NMR described above was performed using the following method.

[0185] The resin compositions obtained in Examples 4, 9-12 and Comparative Example 1 were injection molded to obtain resin molded bodies measuring 100 mm in length, 100 mm in width, and 2 mm in thickness. Furthermore, samples of the resin molded bodies were obtained by cutting the resulting flat sheets into 5 mm squares. The injection molding was performed under the following conditions: resin temperature 230°C, mold temperature 50°C, and injection speed 30 mm / s.

[0186] 700 mg of the obtained resin molded sample was introduced into a 10 mm diameter glass sample tube (BRUKER, part number 1824511, 10 mm diameter, 180 mm length, flat bottom). The sample tube was then placed in a pulsed NMR spectrometer (BRUKER "the minispe mq20") and held at 125°C for 10 minutes. After that, the Hahn Echo method was performed at 125°C, and the results were obtained. 1 The free induction damping curve of spin-spin relaxation of H was separated into three waveforms, each originating from the S, M, and L components, in order of increasing relaxation time, using the least squares method.

[0187] Waveform separation was performed using an exponential type and fitting. The fitting was performed using BRUKER's analysis software "TD-NMRA (Version 4.3 Rev 0.8)" according to the product manual.

[0188] The following formula was used for fitting.

[0189] Y = A1 × exp(-1 ÷ w1 × (t ÷ T2A)) w1 ) + B1 × exp(-1 ÷ w2 × (t ÷ T2B) w2 ) + C1 × exp(-1 ÷ w3 × (t ÷ T2C) w3 )

[0190] Here, w1 to w3 are Weibull coefficients, with w1, w2, and w3 taking a value of 1. A1 is the ratio of the S component, B1 is the ratio of the M component, and C1 is the ratio of the L component. T2A is the relaxation time of the S component, T2B is the relaxation time of the M component, and T2C is the relaxation time of the L component. t is time.

[0191] Furthermore, the following settings were made in the Hahn Echo method.

[0192] Scans: 16 times Recycle Deray: 1 sec First 90-180 Pluse Separation:0.0082msec Final Plus Separation: 5msec Number of Points for Fitting:100

[0193] Electromagnetic shielding properties; The resin compositions obtained in Examples 4, 9-12 and Comparative Example 1 were injection molded to obtain resin molded bodies measuring 100 mm in length, 100 mm in width, and 2 mm in thickness, which were used as measurement samples. The injection molding was performed under the following conditions: resin temperature 230°C, mold temperature 50°C, and injection speed 30 mm / s.

[0194] The electromagnetic shielding effect (electromagnetic shielding performance, unit: dB) of the obtained resin molded body at a frequency of 3 GHz was measured using a dual-focus flat cavity (DFFC) fixture (manufactured by Sanken Corporation) for measuring shielding characteristics. Specifically, electromagnetic waves were radiated from the transmitting focal point, and the intensity of the electromagnetic waves focused at the receiving focal point was measured as the received voltage. The received voltage V0 with no sample inserted and the received voltage V with the sample inserted were measured, and the electromagnetic shielding effect was calculated according to the following equation (2).

[0195] Electromagnetic shielding effect = 20 × log 10 (V0 / V)…Equation (2)

[0196] The measurement frequency range was 1 GHz to 15 GHz, and the measuring instrument used was an Agilent Technologies "Component Analyzer N4375D". The sample dimensions of the resin molded body were 100 mm x 100 mm x 2 mm.

[0197] Thermal conductivity; The resin compositions obtained in Examples 4, 9-12 and Comparative Example 1 were injection molded to obtain resin molded bodies measuring 100 mm in length, 100 mm in width, and 2 mm in thickness, which were used as measurement samples. The injection molding was performed under the following conditions: resin temperature 230°C, mold temperature 50°C, and injection speed 30 mm / s.

[0198] The thermal conductivity (in-plane and thickness-direction thermal conductivity) of the obtained measurement samples was measured using a Xenon Flash Laser Analyzer LFA467 HyperFlash manufactured by Netch Japan Co., Ltd. Specifically, the measurement sample was placed in the holder in an orientation that allowed for measurement of thermal conductivity, the thermal diffusivity at 30°C was measured, and the thermal conductivity was calculated according to the following equation (1).

[0199] Thermal conductivity (W / (m·K)) = Specific gravity (g / cm³) 3 ) × Specific heat (J / g·K) × Thermal diffusivity (mm 2 / s)…Formula (1)

[0200] long-term heat resistance; The resin compositions obtained in Examples 4, 9-12 and Comparative Example 1 were injection molded to obtain dumbbell-shaped test specimens in accordance with ISO 527. The injection molding was performed under the following conditions: resin temperature 230°C, mold temperature 50°C, and injection speed 30 mm / s.

[0201] The obtained test specimens were exposed to constant temperature baths at 23°C and 125°C for 3000 hours each. The specimen left at 23°C was used as the sample before heat degradation, and the specimen left at 125°C was used as the sample after heat degradation. Tensile tests were performed in accordance with ISO 527, and the tensile strength was measured. Long-term heat resistance was calculated according to the following formula (2).

[0202] Long-term heat resistance (%) = Tensile strength after heat degradation (MPa) / Tensile strength before heat degradation (MPa) ... Equation (2)

[0203] The results are shown in Table 3 below.

[0204] [Table 3]

Claims

1. A thermoplastic resin (A), graphite (B), and two or more types of carbon black (C), The carbon black (C) has a BET specific surface area of ​​600 m 2 / g or more, and a first carbon black (C-1) having a BET specific surface area of ​​600 m 2 and a second carbon black (C-2) having a molecular weight of less than 1.0 / g.

2. Relative to 100 parts by weight of the thermoplastic resin (A), The content of the first carbon black (C-1) is 5 parts by weight or more and 50 parts by weight or less, The content of the second carbon black (C-2) is 5 parts by weight or more and 50 parts by weight or less, The resin composition according to claim 1, wherein the total content of the carbon black (C) is 15 parts by weight or more and 90 parts by weight or less.

3. The first carbon black (C-1) has a DBP oil absorption of 250 ml / 100 g or more, The resin composition according to claim 1 or 2, wherein the second carbon black (C-2) has a DBP oil absorption of less than 250 ml / 100 g.

4. The resin composition according to claim 1, wherein the first carbon black (C-1) has a BET specific surface area of ​​1200 m 2 / g or less.

5. The resin composition according to claim 1, wherein the second carbon black (C-2) has a BET specific surface area of ​​55 m 2 / g or more.

6. The resin composition according to any one of claims 1 to 5, wherein the ash content of the carbon black (C) is 1% or less.

7. The resin composition according to any one of claims 1 to 6, wherein the graphite (B) is platelet graphite.

8. Volume resistivity is 1.0×10 5The resin composition according to any one of claims 1 to 7, having a viscosity of Ω·cm or less.

9. A resin composition comprising a thermoplastic resin (A), graphite (B), and carbon black (D), The resin composition in a molten state is filled into a mold from a direction perpendicular to the thickness direction of the resin molded product to be obtained, and a resin molded product having a length of 100 mm, a width of 100 mm, and a thickness of 2 mm is obtained. The resin molded body is measured by the Hahn Echo method at 125° C. using pulse NMR. 1 A resin composition, wherein when a free induction decay curve of spin-spin relaxation of H is separated into three curves derived from three components, S component, M component, and L component, in order of shortest relaxation time by the least squares method, the relaxation time of the L component is 1.3 msec or less.

10. The resin composition according to claim 9, wherein a ratio of the L component to the total of the S component, the M component, and the L component (L component / (S component+M component+L component)) is 10% or less.

11. The resin composition according to claim 9 or 10, wherein a ratio of the L component to the total of the S component, the M component, and the L component (L component / (S component+M component+L component)) is 4% or more.

12. The resin composition according to any one of claims 9 to 11, wherein the graphite (B) is platelet graphite.

13. The resin composition in a molten state is filled into a mold from a direction perpendicular to the thickness direction of the resin molded product to be obtained, and a resin molded product having a length of 100 mm, a width of 100 mm, and a thickness of 2 mm is obtained. The resin composition according to any one of claims 1 to 12, wherein the electromagnetic wave shielding effect of the resin molding at any one of frequencies of 3 GHz, 25 GHz, 50 GHz, and 75 GHz is 20 dB or more.

14. The resin composition in a molten state is filled into a mold from a direction perpendicular to the thickness direction of the resin molded product to be obtained, and a resin molded product having a length of 100 mm, a width of 100 mm, and a thickness of 2 mm is obtained. The resin composition according to any one of claims 1 to 13, wherein the thermal conductivity in an in-plane direction of the resin molding is 1 W / (m · K) or more.

15. A resin molded article, which is a molded article of the resin composition according to any one of claims 1 to 14.

16. Volume resistivity is 1.0×10 5 The resin molded article according to claim 15, having a resistivity of Ω·cm or less.

17. A step of mixing the resin composition according to any one of claims 1 to 14 with a composite (E) containing a thermoplastic resin and fibers to obtain a mixture; A step of obtaining a resin molded body by molding the mixture; A method for producing a resin molded body comprising the steps of: