Bipolar stack unit cell structure and all-solid secondary battery including the same

The tack unit cell structure addresses the challenge of volume changes in all-solid-state secondary batteries by using a bi-cell configuration with a compression pad, enhancing stability and cycle performance.

JP2024045773A5Inactive Publication Date: 2024-10-31SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024026466
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-20
Filing Date
2024-02-26
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing all-solid-state secondary batteries face challenges in designing a structure that can absorb volume changes caused by lithium deposition reactions in the negative electrode, leading to potential instability and increased costs due to the use of expensive materials like SUS for current collectors.

Method used

A tack unit cell structure is introduced, comprising a bi-cell configuration with a compression pad between negative electrode current collectors, allowing for the absorption of volume changes and stabilizing the cell by incorporating a compression pad made of elastic materials like polyurethane, which can absorb the volume fluctuations of the negative electrode.

Benefits of technology

The tack unit cell structure effectively stabilizes the battery by absorbing volume changes, ensuring a stable lifespan and enabling flexible capacity and voltage design through a bipolar structure, while reducing the risk of short circuits and improving cycle characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a bipolar stack unit cell structure and an all-solid secondary battery including the same.SOLUTION: A bipolar stack unit cell structure includes a bi-cell in which a first anode current collector, a first anode active material layer, a first electrolyte layer, a first cathode active material layer, a cathode current collector, a second cathode active material layer, a second electrolyte layer, a second anode active material layer and a second anode current collector are sequentially arranged, where multiple such bi-cells are stacked, and a compression pad is included between the first anode current collector and the second anode current collector of adjacent bi-cells. The bipolar stack unit cell structure absorbs a volume change of an anode, and reduces a volume change of the entire cell to obtain a stable lifespan, and the capacity and voltage can be freely designed by bipolar connection of the unit cells.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention ,vinegar The present invention relates to a tacked unit cell structure and an all-solid-state secondary battery including the same. [Background technology]

[0002] In recent years, due to industrial demand, there has been active development of batteries with high energy density and safety. For example, lithium-ion batteries are being used not only in the fields of information-related devices and communication devices, but also in the automotive field. In the automotive field, safety is particularly important because it is related to life.

[0003] Currently available lithium-ion batteries use electrolytes containing flammable organic solvents, which may lead to overheating and fire if a short circuit occurs. In response to this, all-solid-state secondary batteries that use solid electrolytes instead of electrolytes have been proposed.

[0004] Since the all-solid-state secondary battery does not use a flammable organic solvent, the possibility of fire or explosion can be significantly reduced even if a short circuit occurs, and therefore the all-solid-state secondary battery can be significantly safer than a lithium-ion battery that uses an electrolyte.

[0005] In addition, one of the features of the all-solid-state secondary battery is that, unlike general lithium-ion batteries, a bipolar structure can be easily constructed, which has the advantage of reducing the number of parts, allowing the easy flow of a large current, and enabling the development of a cell with high voltage, high output, and high energy density. However, it is difficult to design a structure that can absorb the volume change caused by the lithium deposition reaction used in the negative electrode of the all-solid-state secondary battery. Summary of the Invention [Problem to be solved by the invention]

[0006] The problem to be solved by the present invention is to provide a battery that can absorb the volume change of the negative electrode. Rus The objective of the present invention is to provide a tack unit cell structure.

[0007] Another problem to be solved by the present invention is Note The present invention provides an all-solid-state secondary battery including a tacked unit cell structure. [Means for solving the problem]

[0008] According to one aspect, the battery includes a bi-cell in which a first negative electrode current collector, a first negative electrode active material layer, a first electrolyte layer, a first positive electrode active material layer, a positive electrode current collector, a second positive electrode active material layer, a second electrolyte layer, a second negative electrode active material layer, and a second negative electrode current collector are sequentially arranged, and a plurality of the bi-cells are stacked, and a compression pad is provided between the first negative electrode current collector and the second negative electrode current collector of adjacent bi-cells. ,vinegar A tack unit cell structure is provided.

[0009] By other aspects, Note The stack unit cell structure includes Note An all-solid-state secondary battery is provided in which a plurality of tacked unit cell structures are stacked. Effect of the Invention

[0010] According to one aspect ,vinegar The TACK unit cell structure absorbs the volume change of the negative electrode, suppresses the volume change of the entire cell, and provides a stable lifespan. By connecting the unit cells bipolarly, the capacity and voltage can be freely designed. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic cross-sectional view of a stack unit cell structure according to an exemplary embodiment; [Diagram 2] 1 is a schematic cross-sectional view of an all-solid-state secondary battery according to an illustrative embodiment; [Diagram 3]13 is a graph showing data showing the possibility of shorting in bipolar and monopolar cells without a compression pad. [Figure 4] 1 is a diagram showing data obtained by measuring, with a load cell, volume expansion during charging and volume contraction during discharging of an all-solid-state secondary battery. [Diagram 5] 1 is a diagram showing data on the volume change of an all-solid-state secondary battery during high-rate cycle evaluation, measured with a load cell. [Figure 6] 1 is a diagram showing data obtained by measuring the pressure that can be applied to the outside when a compression pad is contracted. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present inventive concept described below can be modified in various ways and can have various embodiments, but specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, it should be understood that they do not limit the present inventive concept to specific embodiments, but include all modifications, equivalents, or alternatives included in the technical scope of the present inventive concept.

[0013] The terms used below are merely used to describe certain embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In the following, the terms "include" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. The " / " used below can be interpreted as "and" or "or" depending on the situation.

[0014] In the drawings, layers and regions are shown exaggerated or reduced in thickness for clarity. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part, such as a layer, film, region, plate, etc., is said to be "on" or "above" another part, this includes not only when it is directly on top of the other part, but also when there is another part between them. Throughout the specification, terms such as first, second, etc. are used to describe various components, but the components are not limited by the terms. The terms are used only to distinguish one component from another.

[0015] The following is an example of an embodiment. Rus The tacked unit cell structure and the all-solid-state secondary battery including the same will now be described in further detail.

[0016] Conventionally, it has been difficult to design a bipolar structure capable of absorbing the volume change caused by the lithium deposition reaction used in the negative electrodes of all-solid-state secondary batteries, and the current collectors have had to use expensive stainless steel, which has also acted as a factor in increasing prices.

[0017] For existing all-solid-state secondary batteries, a structure has been proposed in which stacked cells are placed within a bipolar structure to increase the cell capacity, but no structure has been proposed for absorbing volume changes.

[0018] As a result, the present inventors have developed a method for producing a solid-state secondary battery capable of solving the above-mentioned problems. No The present invention provides a tacked unit cell structure and an all-solid-state secondary battery having the same.

[0019] [vinegar tack unit cell structure] According to one embodiment RusThe tack unit cell structure includes a bicell in which a first negative electrode current collector, a first negative electrode active material layer, a first electrolyte layer, a first positive electrode active material layer, a positive electrode current collector, a second positive electrode active material layer, a second electrolyte layer, a second negative electrode active material layer, and a second negative electrode current collector are sequentially arranged, and a plurality of the bicells are stacked, and a compression pad is provided between the first negative electrode current collector and the second negative electrode current collector of adjacent bicells.

[0020] One Example No The bicell that forms the tack unit cell structure has a C-type bicell structure with one positive electrode layer on each side and two single-plate negative electrode layers symmetrically. When multiple bicells are stacked, a compression pad is installed between adjacent bicells. ,vinegar The volume change of the negative electrode layer can be accommodated within the tack unit cell structure. Note The tack unit cell structure has an advantage that it can suppress the volume change of the entire cell by incorporating a compression pad that can absorb the volume change of the negative electrode, thereby obtaining a stable lifespan, and that it can have both a stack and bipolar structure at the same time, allowing the capacity and voltage to be freely designed.

[0021] FIG. 1 is a block diagram of an exemplary embodiment of the present invention. Rus FIG. 2 is a schematic cross-sectional view of a tack unit cell structure.

[0022] As shown in Figure 1 ,vinegar The tack unit cell structure 1 has a structure in which a plurality of bicells 100 are stacked, and each bicell 100 has a structure in which a first negative electrode current collector 10, a first negative electrode active material layer 20, a first electrolyte layer 30, a first positive electrode active material layer 40, a positive electrode current collector 50, a second positive electrode active material layer 40', a second electrolyte layer 30', a second negative electrode active material layer 20', and a second negative electrode current collector 10' are sequentially arranged. .vinegar The tack unit cell structure 1 includes a plurality of bi-cells 100 stacked together, and includes a compression pad 60 between the first negative electrode current collector 10 and the second negative electrode current collector 10 ′ of adjacent bi-cells 100 .

[0023] As shown in Figure 1 ,vinegarA first bipolar plate 70 and a second bipolar plate 70' may be further included on the first negative electrode current collector 10 and the second negative electrode current collector 10' located at both ends of the tack unit cell structure 1, respectively. In this case, compression pads 60 may be further disposed between the first negative electrode current collector 10 and the first bipolar plate 70 located at the ends, and between the second negative electrode current collector 10' and the second bipolar plate 70' located at the ends.

[0024] [Compression pad] Between the first negative electrode current collector 10 and the second negative electrode current collector 10′ of the adjacent bicell 100 ,vinegar The compression pads 60 arranged between the first negative electrode current collector 10 and the first bipolar plate 70, and between the second negative electrode current collector 10' and the second bipolar plate 70' at both ends of the tack unit cell structure 1, may be sheet-shaped and made of an elastic material.

[0025] The elastic material may include, but is not limited to, one or more selected from the group consisting of polyurethane, natural rubber, spandex, butyl rubber (IIR), fluoroelastomer, elastomer, ethylene-propylene rubber (EPR), styrene-butadiene rubber (SBR), chloroprene, elastin, rubber epichlorohydrin, nylon, terpene, isoprene rubber, polybutadiene, nitrile rubber, thermoplastic elastomer, silicone rubber, ethylene-propylene-diene rubber (EPDM), ethylene vinyl acetate (EVA), halogenated butyl rubber, neoprene, and copolymers thereof, and any material having elasticity may be used without limitation. According to one embodiment, the compression pad 60 may be made of a urethane-based material, such as polyurethane.

[0026] The compression pad 60 may be compressed so that the thickness when placed is 40 to 90% of the initial thickness before pressure is applied. Specifically, for example, the thickness when placed of the compression pad 60 may be compressed so that the thickness is 50 to 85%, more specifically, 60 to 80%, or 65 to 75% of the initial thickness before pressure is applied. Within this range, the volume change of the negative electrode can be effectively absorbed, and the all-solid-state battery can be smoothly charged and discharged.

[0027] The thickness of the compression pad 60 can be determined to be in the range of 200 to 500% of the thickness of the lithium deposit layer of the negative electrode formed during charging of the all-solid-state secondary battery. In the all-solid-state secondary battery, the thickness of the lithium deposit layer of the negative electrode is determined in proportion to the current density of the positive electrode, that is, the thickness of the lithium deposit layer of the negative electrode is determined by the amount of lithium moving from the positive electrode to the negative electrode, thereby causing a volume change of the negative electrode. Therefore, the thickness of the compression pad can be determined so as to absorb such a volume change of the negative electrode. Therefore, by setting the thickness of the compression pad 60 to be in the range of 200 to 500% of the thickness of the lithium deposit layer of the negative electrode formed during charging of the all-solid-state secondary battery, the volume change of the negative electrode can be effectively absorbed. For example, the thickness of the compression pad 60 is in the range of 250 to 450% of the thickness of the lithium deposit layer of the negative electrode formed during charging of the all-solid-state secondary battery, specifically, for example, in the range of 300 to 400%.

[0028] The thickness of the compression pad 60 can be set, for example, in the range of 50 μm to 300 μm, and can be selectively set, for example, to 100 μm to 150 μm, 200 μm to 300 μm, or 50 μm to 100 μm, depending on the case.

[0029] In this way, by installing the compression pad 60 between the negative electrode current collectors, the volume change caused by the lithium deposition reaction used in the negative electrodes can be absorbed, thereby suppressing the volume change of the entire cell and achieving a stable lifespan.

[0030] [Positive electrode layer] In the C-type bicell, the positive electrode layer includes a positive electrode current collector 50, and a first positive electrode active material layer 40 and a second positive electrode active material layer 40' disposed on either side of the positive electrode current collector 50.

[0031] [Cathode active material layer: Cathode active material] The first and second positive electrode active material layers 40, 40' include, for example, a positive electrode active material and a solid electrolyte. The solid electrolyte included in the first and second positive electrode active material layers 40, 40' may be similar to or different from the solid electrolyte included in the first and second electrolyte layers 30, 30'. For details about the solid electrolyte, please refer to the first and second electrolyte layers 30, 30'.

[0032] The positive electrode active material is a positive electrode active material that can reversibly absorb and desorb lithium ions. The positive electrode active material is, for example, lithium transition metal oxides such as lithium cobalt oxide (LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM), lithium manganese oxide, lithium iron phosphate oxide, nickel sulfide, copper sulfide, lithium sulfide, iron oxide, or vanadium oxide, but is not necessarily limited thereto, and any material that is used as a positive electrode active material in the technical field can be used. The positive electrode active material may be used alone or in a mixture of two or more kinds.

[0033] The lithium transition metal oxide is, for example, Li a A 1-b B b D2 (wherein, in the formula, 0.90≦a≦1 and 0≦b≦0.5); Li a E 1-b B b O 2-c D c (wherein, 0.90≦a≦1, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B b O 4-c D c(wherein 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b B c O 2-α F' α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b B c O 2-α F'2 (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B c O 2-α F α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F'2 (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G d O2 (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d G eO2 (wherein, in the formula, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O2 (wherein, in the formula, 0.90≦a≦1 and 0.001≦b≦0.1); Li a CoG b O2 (wherein, in the formula, 0.90≦a≦1 and 0.001≦b≦0.1); Li a MnG b O2 (wherein, in the formula, 0.90≦a≦1 and 0.001≦b≦0.1); Li a Mn2G b O4 (wherein 0.90≦a≦1 and 0.001≦b≦0.1 in the above formula); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f)A compound represented by any one of the chemical formulas Fe2(PO4)3(0≦f≦2);LiFePO4. In such a compound, A is Ni, Co, Mn or a combination thereof, B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof, D is O, F, S, P or a combination thereof, E is Co, Mn or a combination thereof, F' is F, S, P or a combination thereof, G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof, Q is Ti, Mo, Mn or a combination thereof, I is Cr, V, Fe, Sc, Y or a combination thereof, and J is V, Cr, Mn, Co, Ni, Cu or a combination thereof. A compound having a coating layer added to the surface of such a compound can also be used, and a mixture of the above-mentioned compound and a compound having a coating layer added can also be used. The coating layer added to the surface of such a compound includes, for example, a coating element compound such as an oxide or hydroxide of the coating element, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element. The compound forming such a coating layer is amorphous or crystalline. The coating element contained in the coating layer is Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method of forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method is, for example, a spray coating method, a dipping method, etc. The specific coating method is a content that is widely understood by those skilled in the art, so a detailed description will be omitted.

[0034] The positive electrode active material includes, for example, a lithium salt of a transition metal oxide having a layered rock salt type structure among the above-described lithium transition metal oxides. The "layered rock salt type structure" is, for example, a structure in which oxygen atom layers and metal atom layers are alternately and regularly arranged in the <111> direction of a cubic rock salt type structure, whereby each atom layer forms a two-dimensional plane. The "cubic rock salt type structure" represents a sodium chloride type (NaCl type) structure which is a kind of crystal structure. Specifically, it represents a structure in which face-centered cubic lattices (fcc) formed by cations and anions, respectively, are arranged so as to be shifted from each other by about 1 / 2 of the ridge of the unit lattice. Such a lithium transition metal oxide having a layered rock salt type structure is, for example, LiNi x Co y Al z O2 (NCA) or LiNi x Co y Mn z O2 (NCM) (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1), etc., which are ternary lithium transition metal oxides. When the positive electrode active material contains a ternary lithium transition metal oxide having a layered rock salt type structure, the energy density and thermal stability of the all-solid-state secondary battery 2 are further improved.

[0035] As described above, the positive electrode active material may be covered with a coating layer. The coating layer may be any one as long as it is known as a coating layer for a positive electrode active material of an all-solid-state secondary battery. The coating layer is, for example, Li2O-ZrO2 (LZO).

[0036] When the positive electrode active material is a ternary lithium transition metal oxide such as NCA or NCM and contains nickel (Ni), the capacity density of the all-solid-state secondary battery 2 can be increased, and metal elution of the positive electrode active material can be reduced in the charged state. As a result, the cycle characteristics of the all-solid-state secondary battery 2 in the charged state are improved.

[0037] The shape of the positive electrode active material is, for example, a particulate shape such as a perfect sphere or an oval sphere. The particle size of the positive electrode active material is not particularly limited, and is within the range applicable to the positive electrode active material of a conventional all-solid-state secondary battery. The content of the positive electrode active material in the positive electrode layer 10 is also not particularly limited, and is within the range applicable to the positive electrode layer of a conventional all-solid-state secondary battery.

[0038] [Cathode active material layer: solid electrolyte] The first and second positive electrode active material layers 40, 40' may include, for example, a solid electrolyte. The solid electrolyte included in the first and second positive electrode active material layers 40, 40' may be the same as or different from the solid electrolyte included in the first and second electrolyte layers 30, 30'. For details regarding the solid electrolyte, please refer to the first and second electrolyte layers 30, 30'.

[0039] The solid electrolyte contained in the first and second positive electrode active material layers 40, 40' may have a smaller average particle size D50 than the solid electrolyte contained in the first and second electrolyte layers 30, 30'. For example, the average particle size D50 of the solid electrolyte contained in the first and second positive electrode active material layers 40, 40' may be 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or 20% or less of the average particle size D50 of the solid electrolyte contained in the first and second electrolyte layers 30, 30'.

[0040] The average particle size D50 is, for example, the median particle size D50. The median particle size D50 is, for example, the particle size corresponding to 50% cumulative volume calculated from the particle side having a small particle size in the particle size distribution measured by a laser diffraction method.

[0041] [Positive electrode active material layer: binder] The first and second positive electrode active material layers 40, 40′ may contain a binder, such as, but not limited to, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, or the like, and any binder known in the art may be used.

[0042] [Positive electrode active material layer: conductive material] The first and second positive electrode active material layers 40, 40' may contain a conductive material, such as, but not limited to, graphite, carbon black, acetylene black, ketjen black, carbon fiber, metal powder, etc., and any material used as a conductive material in the art is acceptable.

[0043] [Positive electrode active material layer: other additives] The first and second positive electrode active material layers 40, 40′ may further include additives such as a filler, a coating agent, a dispersant, and an ion conductive auxiliary in addition to the above-mentioned positive electrode active material, solid electrolyte, binder, and conductive material.

[0044] The first and second positive electrode active material layers 40, 40′ may contain, as a filler, a coating agent, a dispersant, an ion-conductive auxiliary, and the like, any known material generally used in electrodes of all-solid-state secondary batteries.

[0045] [Positive electrode layer: positive electrode current collector] The positive electrode current collector 50 may be, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector 50 may be omitted. The thickness of the positive electrode current collector 50 is, for example, 1 μm to 100 μm, 1 μm to 50 μm, 5 μm to 25 μm, or 10 μm to 20 μm.

[0046] [Electrolyte layer] 1, a first electrolyte layer 30 and a second electrolyte layer 30' are disposed on the first positive electrode active material layer 40 and the second positive electrode active material layer 40', respectively. The first electrolyte layer 30 and the second electrolyte layer 30' are also solid electrolyte layers.

[0047] [Solid electrolyte layer: solid electrolyte] The solid electrolyte may be, for example, a sulfide-based solid electrolyte. Examples of the sulfide-based solid electrolyte include Li2S-P2S5, Li2S-P2S5-LiX (X is a halogen element), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (m, n are positive numbers, and Z is one of Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p, q are positive numbers, and M is one of P, Si, Ge, B, Al, Ga, or In), Li 7-x P.S. 6-x Cl x (0≦x≦2), Li 7-x P.S. 6-x Br x (0≦x≦2) and Li 7-x P.S. 6-x I x (0≦x≦2). The sulfide-based solid electrolyte is prepared by processing starting materials such as Li2S and P2S5 by melt quenching or mechanical milling. After such processing, heat treatment can be performed. The solid electrolyte is amorphous, crystalline, or a mixture of these. The solid electrolyte may be, for example, one of the above-mentioned sulfide-based solid electrolyte materials that contains at least sulfur (S), phosphorus (P), and lithium (Li) as constituent elements. For example, the solid electrolyte may be a material containing Li2S-P2S5. When a sulfide-based solid electrolyte material containing Li2S-P2S5 is used as the sulfide-based solid electrolyte material that forms the solid electrolyte, the mixed molar ratio of Li2S and P2S5 is, for example, in the range of Li2S:P2S5=50:50 to 90:10.

[0048] The sulfide-based solid electrolyte may include, for example, an Argyrodite-type solid electrolyte represented by the following chemical formula 1:

[0049] [Chemical formula 1] Li + 12-n-x A n+ X 2- 6-x Y - x

[0050] In the above formula 1, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb, or Ta, X is S, Se, or Te, and Y is Cl, Br, I, F, CN, OCN, SCN, or N3, where 1≦n≦5 and 0≦x≦2. The sulfide-based solid electrolyte is, for example, Li 7-x P.S. 6-x Cl x (0≦x≦2), Li 7-x P.S. 6-x Br x (0≦x≦2) and Li 7-x P.S. 6-x I x (0≦x≦2). The sulfide-based solid electrolyte may be, for example, an argyrodite-type compound containing one or more selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.

[0051] The density of the argyrodite-type solid electrolyte is 1.5 to 2.0 g / cc. When the argyrodite-type solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery is reduced, and the penetration of the solid electrolyte layer by Li can be effectively suppressed.

[0052] [Solid electrolyte layer: binder] The solid electrolyte layer may include, for example, a binder. The binder included in the solid electrolyte layer may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder used as a binder in the relevant technical field may be used. The binder of the solid electrolyte layer may be the same as or different from the binder included in the first and second positive electrode active material layers 40, 40' and the first and second negative electrode active material layers 20, 20'. The binder may be omitted.

[0053] The content of the binder in the solid electrolyte layer is 0 to 10 wt%, 0 to 5 wt%, 0 to 3 wt%, 0 to 1 wt%, 0 to 0.5 wt%, or 0 to 0.1 wt% based on the total weight of the solid electrolyte layer.

[0054] [Negative electrode layer] As shown in FIG. 1, a first negative electrode active material layer 20 and a second negative electrode active material layer 20' are disposed on a first electrolyte layer 30 and a second electrolyte layer 30', respectively.

[0055] [Negative electrode active material layer: negative electrode active material] The first and second negative electrode active material layers 20, 20' contain, for example, a negative electrode active material and a binder.

[0056] The negative electrode active material contained in the first and second negative electrode active material layers 20, 20' has, for example, a particle form. The average particle size of the negative electrode active material having the particle form is, for example, 4 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, or 900 nm or less. The average particle size of the negative electrode active material having the particle form is, for example, 10 nm to 4 μm or less, 10 nm to 3 μm or less, 10 nm to 2 μm or less, 10 nm to 1 μm or less, or 10 nm to 900 nm or less. When the negative electrode active material has an average particle size in such a range, reversible absorption and / or release of lithium during charging and discharging can be further facilitated. The average particle size of the negative electrode active material is, for example, a median diameter D50 measured using a laser type particle size distribution meter.

[0057] The negative electrode active material included in the first and second negative electrode active material layers 20 and 20' includes, for example, at least one selected from a carbon-based negative electrode active material, a metal negative electrode active material, and a semi-metal negative electrode active material.

[0058] The carbon-based negative electrode active material is particularly amorphous carbon. The amorphous carbon may be, for example, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, etc., but is not necessarily limited thereto, and may be any material that is classified as amorphous carbon in the art. The amorphous carbon is carbon that has no crystallinity or has very low crystallinity, and is classified as crystalline carbon or graphite-based carbon.

[0059] The metal negative electrode active material or metalloid negative electrode active material includes, but is not necessarily limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn), and any metal negative electrode active material or metalloid negative electrode active material that forms an alloy or compound with lithium in the art can be used. For example, nickel (Ni) is not a metal negative electrode active material because it does not form an alloy with lithium.

[0060] The first and second negative electrode active material layers 20, 20' may include one of such negative electrode active materials or a mixture of a plurality of different negative electrode active materials. For example, the first and second negative electrode active material layers 20, 20' may include only amorphous carbon or may include one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the first and second negative electrode active material layers 20, 20' may include a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture of amorphous carbon and gold or the like is, for example, 10:1 to 1:2, 5:1 to 1:1, or 4:1 to 2:1 by weight, but is not necessarily limited to such ranges and is selected depending on the required characteristics of the all-solid-state secondary battery 2. When the negative electrode active material has such a composition, the cycle characteristics of the all-solid-state secondary battery 2 are further improved.

[0061] The negative electrode active material included in the first and second negative electrode active material layers 20, 20' includes, for example, a mixture of first particles made of amorphous carbon and second particles made of a metal or a metalloid. The metal or metalloid includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the metalloid is a semiconductor. The content of the second particles is 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt%, based on the total weight of the mixture. When the second particles have a content in such a range, for example, the cycle characteristics of the all-solid-state secondary battery 2 are further improved.

[0062] [Negative electrode active material layer: binder] The binder contained in the first and second negative electrode active material layers 20, 20' may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used as a binder in the art may be used. The binder may be composed of a single binder or a plurality of different binders.

[0063] Since the first and second negative electrode active material layers 20, 20' contain a binder, the first and second negative electrode active material layers 20, 20' are stabilized on the first and second negative electrode current collectors 10, 10', respectively. In addition, cracks in the first and second negative electrode active material layers 20, 20' are suppressed despite volume changes and / or relative position changes of the first and second negative electrode active material layers 20, 20' during charge and discharge. For example, when the first and second negative electrode active material layers 20, 20' do not contain a binder, the first and second negative electrode active material layers 20, 20' can be easily separated from the first and second negative electrode current collectors 10, 10'. When the first and second negative electrode active material layers 20, 20' are detached from the first and second negative electrode current collectors 10, 10', the first and second negative electrode current collectors 10, 10' come into contact with the solid electrolyte layers 30, 30' at the exposed portions of the first and second negative electrode current collectors 10, 10', increasing the possibility of short circuiting. The first and second negative electrode active material layers 20, 20' are produced, for example, by applying a slurry in which materials constituting the first and second negative electrode active material layers 20, 20' are dispersed onto the first and second negative electrode current collectors 10, 10', respectively, and drying the slurry. By including a binder in the first and second negative electrode active material layers 20, 20', it is possible to stably disperse the negative electrode active material in the slurry. For example, when the slurry is applied onto the first and second negative electrode current collectors 10, 10' by a screen printing method, clogging of the screen (for example, clogging due to agglomerates of the negative electrode active material) can be suppressed.

[0064] [Negative electrode active material layer: other additives] The first and second negative electrode active material layers 20, 20' may further include additives used in the conventional all-solid-state secondary battery 2, such as a filler, a coating agent, a dispersant, an ion-conductive auxiliary, and the like.

[0065] [Negative electrode layer: negative electrode active material layer] The thickness of the first and second negative electrode active material layers 20, 20' is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the first and second positive electrode active material layers 40, 40'. The thickness of the first and second negative electrode active material layers 20, 20' is, for example, 1 μm to 20 μm, 2 μm to 10 μm, or 3 μm to 7 μm. If the thickness of the first and second negative electrode active material layers 20, 20' is excessively thin, lithium dendrites formed between the first and second negative electrode active material layers 20, 20' and the first and second negative electrode current collectors 10, 10' collapse the first and second negative electrode active material layers 20, 20', making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 2. If the thicknesses of the first and second negative electrode active material layers 20, 20' are excessively thick, the energy density of the all-solid-state secondary battery 2 decreases, and the internal resistance of the all-solid-state secondary battery 2 due to the first and second negative electrode active material layers 20, 20' increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 2.

[0066] If the thickness of the first and second negative electrode active material layers 20, 20' is reduced, the charge capacity of the first and second negative electrode active material layers 20, 20' is also reduced. The charge capacity of the first and second negative electrode active material layers 20, 20' is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, 5% or less, or 2% or less than the charge capacity of the first and second positive electrode active material layers 40, 40'. The charge capacity of the first and second negative electrode active material layers 20, 20' is, for example, 0.1% to 50%, 0.1% to 40%, 0.1% to 30%, 0.1% to 20%, 0.1% to 10%, 0.1% to 5%, or 0.1% to 2% compared to the charge capacity of the first and second positive electrode active material layers 40, 40'. If the charge capacity of the first and second negative electrode active material layers 20, 20' is excessively low, the thickness of the first and second negative electrode active material layers 20, 20' becomes very thin, and thus, in a repeated charge / discharge process, lithium dendrites formed between the first and second negative electrode active material layers 20, 20' and the first and second negative electrode current collectors 10, 10' collapse the first and second negative electrode active material layers 20, 20', making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 2. If the charge capacity of the first and second negative electrode active material layers 20, 20' is excessively high, the energy density of the all-solid-state secondary battery 2 decreases, and the internal resistance of the all-solid-state secondary battery 2 due to the first and second negative electrode active material layers 20, 20' increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 2.

[0067] The charge capacity of the first and second positive electrode active material layers 40, 40' is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the first and second positive electrode active material layers 40, 40'. When a plurality of types of positive electrode active materials are used, the charge capacity density x mass value is calculated for each positive electrode active material, and the sum of these values ​​is the charge capacity of the first and second positive electrode active material layers 40, 40'. The charge capacity of the first and second negative electrode active material layers 20, 20' is also calculated by the same method. That is, the charge capacity of the first and second negative electrode active material layers 20, 20' is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the first and second negative electrode active material layers 20, 20'. When a plurality of negative electrode active materials are used, the charge capacity density x mass value is calculated for each negative electrode active material, and the sum of the values ​​is the charge capacity of the first and second negative electrode active material layers 20, 20'. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is a capacity estimated using an all-solid-state half-cell using lithium metal as a counter electrode. By measuring the charge capacity using the all-solid-state half-cell, the charge capacity of the first and second positive electrode active material layers 40, 40' and the first and second negative electrode active material layers 20, 20' is directly measured. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the first and second positive electrode active material layers 40, 40' and the first and second negative electrode active material layers 20, 20' may be the initial charge capacity measured during one cycle of charging.

[0068] [Negative electrode layer: 4th negative electrode active material layer] Although not shown ,vinegarThe tack unit cell structure 1 further includes a fourth negative electrode active material layer disposed, upon charging, in one or more of, for example, i) between the first negative electrode current collector 10 and the first negative electrode active material layer 20, ii) between the first negative electrode active material layer 20 and the first electrolyte layer 30, iii) between the second electrolyte layer 30' and the second negative electrode active material layer 20', and iv) between the second negative electrode active material layer 20' and the second negative electrode current collector 10'. The fourth negative electrode active material layer is a metal layer containing lithium or a lithium alloy. The metal layer contains lithium or a lithium alloy. Therefore, since the fourth negative electrode active material layer is a metal layer containing lithium, it acts, for example, as a lithium reservoir. The lithium alloy may be, for example, Li-Al alloy, Li-Sn alloy, Li-In alloy, Li-Ag alloy, Li-Au alloy, Li-Zn alloy, Li-Ge alloy, Li-Si alloy, etc., but is not limited thereto, and may be any alloy used as a lithium alloy in the art. The fourth negative electrode active material layer may be made of one of such alloys, or of lithium, or may be made of a plurality of alloys.

[0069] The thickness of the fourth negative electrode active material layer is not particularly limited, and may be, for example, 1 μm to 1000 μm, 1 μm to 500 μm, 1 μm to 200 μm, 1 μm to 150 μm, 1 μm to 100 μm, or 1 μm to 50 μm. If the thickness of the fourth negative electrode active material layer is too thin, it is difficult for the fourth negative electrode active material layer to function as a lithium storage. If the thickness of the fourth negative electrode active material layer is too thick, ,vinegar This may result in an increase in the mass and volume of the tacked unit cell structure 1, which may in turn result in a decrease in cycle characteristics. The fourth negative electrode active material layer may be, for example, a metal foil having a thickness in such a range.

[0070] vinegarIn the tack unit cell structure 1, the fourth negative electrode active material layer is, for example, disposed between the first and second negative electrode current collectors 10, 10' and the first and second negative electrode active material layers 20, 20' before assembling the all-solid-state secondary battery 2, or is deposited between the first and second negative electrode current collectors 10, 10' and the first and second negative electrode active material layers 20, 20' by charging after assembling the all-solid-state secondary battery 2. When the fourth negative electrode active material layer is disposed between the first and second negative electrode current collectors 10, 10' and the first and second negative electrode active material layers 20, 20' before assembling the all-solid-state secondary battery 2, the fourth negative electrode active material layer is a metal layer containing lithium, so it acts as a lithium reservoir. For example, a lithium foil is disposed between the first and second negative electrode current collectors 10, 10' and the first and second negative electrode active material layers 20, 20' before assembling the all-solid-state secondary battery 2. This further improves the cycle characteristics of the all-solid-state secondary battery 2 including the fourth negative electrode active material layer. When the fourth negative electrode active material layer is precipitated by charging after the all-solid-state secondary battery 2 is assembled, the all-solid-state secondary battery 2 does not include the fourth negative electrode active material layer when assembled, so the energy density of the all-solid-state secondary battery 2 increases. For example, when charging the all-solid-state secondary battery 2, the first and second negative electrode current collectors 10, 10' are charged beyond their charge capacity. That is, the first and second negative electrode current collectors 10, 10' are overcharged. At the beginning of charging, lithium is absorbed into the first and second negative electrode current collectors 10, 10'. The negative electrode active material contained in the first and second negative electrode current collectors 10, 10' forms an alloy or compound with the lithium ions that have moved from the first and second positive electrode active material layers 40, 40'. If the first and second negative electrode active material layers 20, 20' are charged beyond their capacity, for example, lithium is deposited on the back surface of the first and second negative electrode active material layers 20, 20', i.e., between the first and second negative electrode current collectors 10, 10' and the first and second negative electrode active material layers 20, 20', and a metal layer corresponding to the fourth negative electrode active material layer is formed by the deposited lithium. The fourth negative electrode active material layer is a metal layer mainly composed of lithium (i.e., metallic lithium). Such a result can be obtained, for example, by the negative electrode active material contained in the first and second negative electrode active material layers 20, 20' being composed of a material that forms an alloy or compound with lithium.During discharge, lithium in the first and second negative electrode active material layers 20, 20' and the fourth negative electrode active material layer, i.e., the metal layer, is ionized and moves toward the first and second positive electrode active material layers 40, 40'. Therefore, in the all-solid-state secondary battery 2, lithium can be used as the negative electrode active material. In addition, since the first and second negative electrode active material layers 20, 20' cover the fourth negative electrode active material layer, they act as a protective layer for the fourth negative electrode active material layer, i.e., the metal layer, and also act to suppress the precipitation growth of lithium dendrites. Therefore, short-circuiting and capacity reduction of the all-solid-state secondary battery 2 are suppressed, and as a result, the cycle characteristics of the all-solid-state secondary battery 2 are improved. Furthermore, when the fourth negative electrode active material layer is disposed by charging after assembly of the all-solid-state secondary battery 2, the first and second negative electrode current collectors 10, 10', the first and second negative electrode active material layers 20, 20', and the regions therebetween are Li-free regions that do not contain lithium (Li), for example, in the initial state or post-discharge state of the all-solid-state secondary battery.

[0071] [Negative electrode layer: negative electrode current collector] The first and second negative electrode current collectors 10, 10' are made of a material that does not react with lithium, i.e., does not form any alloy or compound. The materials constituting the first and second negative electrode current collectors 10, 10' are, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co) and nickel (Ni), but are not necessarily limited thereto, and any material that is used as an electrode current collector in the relevant technical field is possible. The first and second negative electrode current collectors 10, 10' are made of one of the above-mentioned metals, or an alloy of two or more metals, or a coating material. The first and second negative electrode current collectors 10, 10' are, for example, in the form of a plate or foil.

[0072] vinegarThe tack unit cell structure 1 may further include, for example, a thin film containing an element capable of forming an alloy with lithium on the first and second negative electrode current collectors 10, 10'. The thin film is disposed between the first and second negative electrode current collectors 10, 10' and the first and second negative electrode active material layers 20, 20'. The thin film may include, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium may be, for example, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., but is not necessarily limited thereto, and may be any element capable of forming an alloy with lithium in the art. The thin film may be composed of one of these metals, or may be composed of an alloy of multiple metals. By disposing the thin film on the first and second negative electrode current collectors 10, 10', for example, the deposition form of the fourth negative electrode active material layer deposited between the thin film and the first and second negative electrode active material layers 20, 20' is further flattened, and the cycle characteristics of the all-solid-state secondary battery 2 are further improved.

[0073] The thickness of the thin film is, for example, 1 nm to 800 nm, 10 nm to 700 nm, 50 nm to 600 nm, or 100 nm to 500 nm. If the thickness of the thin film is less than 1 nm, the function of the thin film is difficult to be exerted. If the thickness of the thin film is excessively thick, the thin film itself absorbs lithium, the amount of lithium precipitated in the negative electrode decreases, the energy density of the all-solid-state secondary battery decreases, and the cycle characteristics of the all-solid-state secondary battery 2 decrease. The thin film is disposed on the first and second negative electrode current collectors 10, 10' by, for example, a vacuum deposition method, a sputtering method, a plating method, or the like, but is not necessarily limited to such a method, and any method that can form a thin film in the technical field is possible.

[0074] [All-solid-state secondary battery] FIG. 2 is a schematic cross-sectional view of an all-solid-state secondary battery according to an illustrative embodiment.

[0075] As shown in FIG. 2, the all-solid-state secondary battery 2 has a Note Stack unit cell structure 1, front Note A plurality of stacked unit cell structures 1 are connected in a bipolar manner. .vinegar The bipolar plates 70, 70' are disposed between the stacked unit cell structures 1. The all-solid-state secondary battery 2 has a front Note By connecting the tack unit cell structures 1 bipolarly, a desired voltage design is possible, and by incorporating the compression pad 60, the volume change of the entire cell can be suppressed.

[0076] Before Lamination Note The stack unit cell structure 1 may further include a positive terminal 80 and a negative terminal 90 at both ends thereof. ,vinegar The compression pads 60 of the tack unit cell structure 1 may be in direct contact.

[0077] Alternatively, a third positive electrode active material layer, a third electrolyte layer, a third negative electrode active material layer, a third negative electrode current collector, and a compression pad may be further disposed in this order from the positive electrode terminal 80 between the positive electrode terminal 80 and the first negative electrode current collector or the second negative electrode current collector adjacent thereto, so that the third positive electrode active material layer is in direct contact with the positive electrode terminal 80 and the compression pad 60 is in direct contact with the negative electrode terminal 90.

[0078] The present invention will be described in more detail through the following examples and comparative examples, although the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0079] Example 1: Bipolar all-solid-state secondary battery with compression pads (Production of negative electrode layer) A 10 μm thick Ni foil was prepared as a negative electrode current collector, and carbon black (CB) with a primary particle size of about 30 nm and silver (Ag) particles with an average particle size of about 60 nm were prepared as a negative electrode active material.

[0080] 4 g of mixed powder obtained by mixing carbon black (CB) and silver (Ag) particles at a weight ratio of 3:1 was placed in a container, and 4 g of NMP solution containing 7 wt% of PVDF binder (#9300 manufactured by Kureha Corporation) was added thereto to prepare a mixed solution. Next, the mixed solution was stirred while adding NMP little by little to the mixed solution to prepare a slurry. The produced slurry was applied to a SUS sheet using a bar coater and dried in air at 80°C for 10 minutes. The laminate obtained thereby was vacuum dried at 40°C for 10 hours. The dried laminate was roll-pressed at a pressure of 300 MPa for 10 ms to flatten the surface of the negative electrode active material layer of the laminate. The negative electrode layer was produced by the above process. The thickness of the negative electrode active material layer contained in the negative electrode layer was about 7 μm.

[0081] (Production of the positive electrode layer) The positive electrode active material was LiNi coated with Li2O-ZrO2 (LZO). 0.8 Co 0.15 Mn 0.05 O2 (NCM) was prepared. The LZO-coated positive electrode active material was prepared by the method disclosed in Korean Patent Publication No. 10-2016-0064942. As the solid electrolyte, Li6PS5Cl (D50=0.5 μm, crystalline), which is an argyrodite-type crystal, was prepared. As the binder, polytetrafluoroethylene (PTFE) binder (Teflon binder manufactured by DuPont) was prepared. As the conductive agent, carbon nanofiber (CNF) was prepared. Such materials were mixed with xylene solvent in a weight ratio of positive electrode active material: solid electrolyte: conductive agent: binder = 84: 11.5: 3: 1.5, and the mixture was formed into a sheet, and then vacuum dried at 40 ° C for 8 hours to produce a positive electrode sheet. Two positive electrode sheets were pressed onto both sides of a positive electrode current collector made of 18 μm thick carbon-coated aluminum foil to produce a positive electrode layer. The thickness of the positive electrode layer was about 105 μm.

[0082] (Manufacturing of solid electrolyte layer) A mixture was prepared by adding 1.5 parts by weight of an acrylic binder to 98.5 parts by weight of the solid electrolyte, Li6PS5Cl, a solid electrolyte with argyrodite crystals (D50=3.0μm, crystalline). Octyl acetate was added to the prepared mixture while stirring to produce a slurry. The produced slurry was applied to a nonwoven fabric using a bar coater and dried in air at 80°C for 10 minutes to obtain a laminate. The obtained laminate was vacuum dried at 80°C for 6 hours. A solid electrolyte layer was produced by the above process.

[0083] (vinegar (Fabrication of tack unit cell structure) Referring to Fig. 1, a C-type bicell was fabricated by contacting both sides of a positive electrode layer with solid electrolyte layers, and arranging a negative electrode layer so that a negative electrode active material layer was in contact with the solid electrolyte layer, and applying pressure. Next, five bicells were stacked, and a polyurethane compression pad (Poron Microcellular #6040, manufactured by Rogers) with a thickness of 200 μm was placed between the negative electrode collectors of adjacent bicells. The positive electrode collectors of each bicell were welded to the outermost bipolar plate 1, and the negative electrode collectors of the bicells were welded to the bipolar plate 2. ,vinegar A tuck unit cell structure was fabricated.

[0084] (Manufacturing all-solid-state secondary batteries) Referring to FIG. Tas The stacked unit cell structures were sequentially stacked on the outer case of the all-solid-state battery to manufacture an all-solid-state secondary battery.

[0085] Comparative Example 1: Bipolar all-solid-state secondary battery without compression pad A bipolar all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that the compression pad between the negative electrode current collectors of the adjacent bicells was omitted.

[0086] Comparative Example 2: Monopolar all-solid-state secondary battery without compression pad The positive electrode layer was a positive electrode sheet formed on only one surface of the positive electrode current collector used in Example 1, and the negative electrode layer and solid electrolyte layer were the same as those in Example 1.

[0087] The negative electrode layer, the solid electrolyte layer, and the positive electrode layer were sequentially arranged to prepare a laminate. The prepared laminate was subjected to a plate pressure treatment at a pressure of 500 MPa for 1 minute to prepare a unit cell of a negative electrode / solid electrolyte membrane / positive electrode, and a monopolar all-solid-state secondary battery without a compression pad was manufactured.

[0088] Evaluation example 1: Charge / discharge test The charge / discharge characteristics of the all-solid-state secondary batteries produced in Example 1 and Comparative Examples 1 and 2 were evaluated by the following charge / discharge test. The charge / discharge test was performed by placing the all-solid-state secondary batteries in a thermostatic chamber at 45°C.

[0089] First, the all-solid-state secondary batteries of Example 1 and Comparative Examples 1 and 2 were charged at a constant current of 0.1 C until the voltage reached 4.25 V, and then were charged at a constant voltage of 0.05 C. After the cells that had been charged were allowed to rest for about 10 minutes, they were discharged at a constant current of 0.1 C until the voltage reached 2.5 V.

[0090] A graph of voltage over time for the all-solid-state secondary batteries of Comparative Examples 1 and 2 is shown in Figure 3. Here, the voltage refers to the voltage of the bipolar cell of Comparative Example 1 and the monopolar cell of Comparative Example 2. As shown in Figure 3, it can be seen that the bipolar all-solid-state secondary battery without a compression pad and the monopolar all-solid-state secondary battery without a compression pad cannot accommodate the volume expansion of the cell during charging, and are highly likely to cause a short circuit.

[0091] In contrast, the voltage and pressure over time of the all-solid-state secondary battery of Example 1 are shown in Figure 4. Here, the voltage refers to the voltage of the bipolar cell, and the pressure refers to the force applied to the outer wall when the volume of the cell expands. As shown in Figure 4, the bipolar all-solid-state secondary battery of Example 1, in which a compression pad is installed between the negative electrode current collectors, can be normally charged and discharged without causing a short circuit even when the volume expands during charging.

[0092] Further charge / discharge experiments were carried out on the all-solid-state secondary battery of Example 1 as described below, and the results are shown in FIG.

[0093] The cells were charged at a constant current of 0.33 C until the voltage reached 4.25 V, and then charged at a constant voltage of 0.05 C. After a rest period of about 10 minutes, the cells that had been charged were repeatedly discharged at a constant current of 0.33 C until the voltage reached 2.5 V, 10 times, and the voltage and pressure were evaluated over time.

[0094] As shown in FIG. 5, the bipolar all-solid-state secondary battery of Example 1 in which a compression pad is installed between the negative electrode current collectors repeats volume expansion and contraction during the cycle, and no short circuit occurs.

[0095] Evaluation example 2: Compressive stress evaluation In order to evaluate the compressive stress according to the installation form of the compression pad used in the all-solid-state secondary battery prepared in Example 1, the compressive stress against the compressive strain was evaluated using a Pellet Density Measuring Instrument (PDMI), and the results are shown in FIG. 6.

[0096] As shown in FIG. 6, the compression pad can apply pressure to the outside by contracting, and the pressure can be adjusted within an appropriate pressure range even if the thickness changes through the initial thickness setting of the compression pad.

[0097] Although an embodiment has been described above with reference to the drawings and embodiments, it is merely an example, and a person skilled in the art will understand that various modifications and equivalent embodiments are possible therefrom. Therefore, the scope of protection of the present invention should be determined by the claims. [Industrial Applicability]

[0098] The present invention is applicable to, for example, technical fields related to all-solid-state secondary batteries. [Explanation of symbols]

[0099] 1 stack Unit Cell Structure 2 All-solid-state secondary battery 10 First negative electrode current collector 10' 2nd negative electrode current collector 20 First negative electrode active material layer 20' Second negative electrode active material layer 30 1st electrolyte layer 30' 2nd electrolyte layer 40 First positive electrode active material layer 40' Second positive electrode active material layer 50 Positive electrode current collector 60 Compression Pads 70 First Bipolar Plate 70' 2nd Bipolar Plate 80 Positive terminal 90 Negative terminal 100 Buysell

Claims

1. a bicell in which a first negative electrode current collector, a first negative electrode active material layer, a first electrolyte layer, a first positive electrode active material layer, a positive electrode current collector, a second positive electrode active material layer, a second electrolyte layer, a second negative electrode active material layer, and a second negative electrode current collector are sequentially arranged; A cell structure comprising a plurality of the bicells stacked together, the cell structure including a compression pad between the first negative electrode current collector and the second negative electrode current collector of adjacent bicells.

2. The cell structure further includes a first plate and a second plate on the first negative electrode current collector and the second negative electrode current collector, respectively, at both ends of the cell structure, 2. The cell structure of claim 1, further comprising a compression pad disposed between the first terminal negative current collector and the first plate, and between the second terminal negative current collector and the second plate.

3. The cell structure of claim 1 , wherein the compression pad is made of a resilient material.

4. 4. The cell structure of claim 3, wherein the elastic material comprises at least one selected from the group consisting of polyurethane, natural rubber, butyl rubber (IIR), fluoroelastomer, ethylene propylene rubber (EPR), styrene butadiene rubber (SBR), chloroprene rubber, epichlorohydrin rubber, nylon, terpene polymer, isoprene rubber, polybutadiene, nitrile rubber, thermoplastic elastomer, silicone rubber, ethylene propylene diene rubber (EPDM), ethylene vinyl acetate (EVA), halogenated butyl rubber, and neoprene.

5. 2. The cell structure of claim 1, wherein the compression pad is compressed to have a thickness that is 40 to 90% of its initial thickness before pressure is applied when the compression pad is disposed between the first and second negative electrode current collectors of adjacent bicells.

6. 2. The cell structure according to claim 1, wherein the thickness of the compression pad is set to a range of 200 to 500% of the thickness of a lithium deposition layer of the negative electrode formed during charging of the all-solid-state secondary battery when the compression pad is disposed between the first negative electrode current collector and the second negative electrode current collector of an adjacent bicell.

7. The cell structure of claim 1 , wherein the first electrolyte layer and the second electrolyte layer comprise a solid electrolyte.

8. The solid electrolyte is a sulfide-based solid electrolyte, and the sulfide-based solid electrolyte is Li 2 S-P 2 S 5 , Li 2 S-P 2 S 5 -LiX (X is a halogen element), Li 2 S-P 2 S 5 -Li 2 O., Li 2 S-P 2 S 5 -Li 2 O-LiI, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 - LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S-B 2 S 3 , Li 2 S-P 2 S 5 -Z m S n (m and n are positive numbers, and Z is one of Ge, Zn, or Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 P.O. 4 , Li 2 S-SiS 2 -Li p M.O. q (p, q are positive numbers, and M is one of P, Si, Ge, B, Al, Ga, or In), Li 7-x P.S. 6-x C x (0≦x≦2), Li 7-x P.S. 6-x B x (0≦x≦2) and Li 7-x P.S. 6-x I x 8. The cell structure according to claim 7, wherein x is one or more selected from (0≦x≦2).

9. The solid electrolyte is Li 6 P.S. 5 Cl, Li 6 P.S. 5 Br and Li 6 P.S. 5 8. The cell structure according to claim 7, wherein the sulfide-based solid electrolyte is an argyrodite-type sulfide-based solid electrolyte containing one or more selected from I.

10. The cell structure of claim 1 , wherein the first and second negative electrode active material layers each include a negative electrode active material and a binder, the negative electrode active material having a particulate form, and an average particle size of the negative electrode active material being 4 μm or less.

11. 11. The cell structure of claim 10, wherein the negative electrode active material comprises at least one selected from the group consisting of a carbon-based negative electrode active material, a metal negative electrode active material, and a semi-metal negative electrode active material, and the carbon-based negative electrode active material comprises amorphous carbon.

12. 12. The cell structure of claim 11, wherein the metallic or semi-metallic anode active material comprises one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn).

13. 11. The cell structure of claim 10, wherein the negative electrode active material comprises a mixture of first particles made of amorphous carbon and second particles made of a metal or semi-metal, and a content of the second particles is 8 to 60 wt % based on a total weight of the mixture.

14. 2. The cell structure of claim 1, further comprising a fourth negative electrode active material layer disposed in one or more of: i) between the first negative electrode current collector and the first negative electrode active material layer, ii) between the first negative electrode active material layer and the first electrolyte layer, iii) between the second electrolyte layer and the second negative electrode active material layer, and iv) between the second negative electrode active material layer and the second negative electrode current collector, wherein the fourth negative electrode active material layer is a metal layer containing lithium or a lithium alloy.

15. An all-solid-state secondary battery comprising the cell structure according to claim 1 , wherein a plurality of the cell structures are stacked.

16. The stacked cell structure further includes a positive electrode terminal and a negative electrode terminal at both ends thereof, 16. The all-solid-state secondary battery according to claim 15, further comprising a third positive electrode active material layer, a third electrolyte layer, a third negative electrode active material layer, a third negative electrode current collector, and a compression pad disposed between the positive electrode terminal and the first negative electrode current collector or the second negative electrode current collector adjacent thereto, in that order from the positive electrode terminal.