Method for regenerating lithium precursor and system for regenerating lithium precursor
The dry rotary heating reactor process efficiently recovers lithium precursors from lithium secondary batteries with high purity and selectivity, addressing inefficiencies in existing recycling methods by separating lithium from transition metals without wet processes.
Patent Information
- Application Number
- JP2024111045
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2018-11-07
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-09-16
AI Technical Summary
Existing methods for recycling lithium secondary battery active materials are inefficient and lack high selectivity and low cost, particularly in the recovery of valuable metals like nickel, cobalt, and manganese.
A dry rotary heating reactor process is used to recover lithium precursors by reacting electrode active material mixtures at controlled temperatures and rotation speeds, forming pre-precursor mixtures that are then hydrated to separate lithium precursors from transition metals, eliminating the need for wet processes and additional steps.
The process achieves high-purity lithium precursor recovery with improved selectivity and yield, reducing environmental impact and operational costs by avoiding wet processes and by-product formation.
Smart Images

Figure 2024133679000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method and system for regenerating a lithium precursor, and more particularly to a method and system for regenerating a lithium precursor from a lithium secondary battery. [Background technology]
[0002] Secondary batteries are capable of repeated charging and discharging, and have been widely used in portable electronic communication devices such as camcorders, mobile phones, and laptops with the development of the information and communication and display industries. Examples of secondary batteries include lithium secondary batteries, nickel-cadmium batteries, and nickel-metal hydride batteries. Among them, lithium secondary batteries have been actively developed and applied due to their high operating voltage and energy density per unit weight, as well as their advantages of fast charging and lightweight design.
[0003] A lithium secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator, and an electrolyte impregnated in the electrode assembly. The lithium secondary battery may further include, for example, a pouch-shaped exterior material that accommodates the electrode assembly and the electrolyte.
[0004] The positive electrode active material of the lithium secondary battery can be a lithium metal oxide, which can further contain a transition metal such as nickel, cobalt, or manganese.
[0005] Since the positive electrode active material uses the aforementioned expensive valuable metals, the production of the positive electrode material accounts for more than 20% of the production cost. In addition, with the recent increase in interest in environmental protection, research into methods for recycling positive electrode active materials is progressing.
[0006] For example, research has been conducted into methods of recovering valuable metals by leaching waste cathode active materials in a strong acid such as sulfuric acid. However, this wet process requires a water washing step, which can be disadvantageous in terms of regeneration selectivity and regeneration time.
[0007] For example, Korean Patent Publication No. 10-0709268 discloses an apparatus and method for recycling waste manganese batteries and alkaline batteries, but does not provide a satisfactory method for recovering valuable metals with high selectivity and low cost. Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a method for recovering active metals of lithium secondary batteries with high efficiency and high purity.
[0009] An object of the present invention is to provide a system for recovering active metals of lithium secondary batteries with high efficiency and high purity. [Means for solving the problem]
[0010] In a method for regenerating a lithium precursor according to an embodiment of the present invention, an electrode active material mixture obtained from a lithium secondary battery is prepared, the electrode active material mixture is reacted in a dry rotary heating reactor to form a pre-precursor mixture, and a lithium precursor is selectively recovered from the pre-precursor mixture.
[0011] In an exemplary embodiment, the pre-precursor mixture may be formed by rotating the dry rotary heater reactor about the longitudinal axis while moving the electrode active material mixture in the longitudinal direction of the dry rotary heater reactor.
[0012] In an exemplary embodiment, the dry rotary heater reactor can rotate at 5 to 200 rpm on the longitudinal axis of the dry rotary heater reactor.
[0013] In an exemplary embodiment, the pre-precursor mixture may be formed by reacting the electrode active material mixture at 250 to 600°C.
[0014] In an exemplary embodiment, the pre-precursor mixture may be formed by contacting the electrode active material mixture with a reducing reactant gas.
[0015] In an exemplary embodiment, the reducing reactant gas may be supplied from the rear end of the dry rotary heating reactor in the length direction, and may form a counterflow to the electrode active material mixture supplied from the front end of the dry rotary heating reactor in the length direction.
[0016] In an exemplary embodiment, the reducing reactant gas may be introduced along with the electrode active material mixture at the front end of the dry rotary heater reactor.
[0017] In an exemplary embodiment, the pre-precursor mixture can include pre-lithium precursor particles and transition metal-containing particles.
[0018] In an exemplary embodiment, the lithium precursor can be recovered by collecting the reserve lithium precursor particles prior to the transition metal-containing particles.
[0019] In an exemplary embodiment, the reserve lithium precursor particles can include lithium hydroxide, lithium oxide, and lithium carbonate.
[0020] In an exemplary embodiment, the lithium precursor can be recovered by hydrating the preliminary lithium precursor particles to lithium oxide.
[0021] In an exemplary embodiment, the reserve lithium precursor can be hydrated and the lithium precursor can be collected prior to the transition metal-containing particles.
[0022] In an exemplary embodiment, the transition metal precursor can be recovered by treating the transition metal-containing particles with an acid solution.
[0023] In an exemplary embodiment, the dry rotary heater reactor may be an indirectly heated rotary kiln.
[0024] In an exemplary embodiment, a lithium precursor regeneration system may include an electrode active material mixture supply unit, a dry rotary heating reactor that reacts the electrode active material mixture supplied from the electrode active material mixture supply unit with a reducing gas, and a lithium precursor recovery unit that collects a lithium precursor from a reactant of the electrode active material mixture produced in the dry rotary heating reactor.
[0025] In an exemplary embodiment, the lithium precursor regeneration system may further include a supply channel connected to at least one of the front end and the rear end in the longitudinal direction of the dry rotary heating reactor to supply the reducing gas.
[0026] In an exemplary embodiment, the lithium precursor regeneration system may further include a transition metal precursor recovery unit that collects the transition metal precursor from the electrode active material mixture reactants. [Effects of the Invention]
[0027] According to the above-described exemplary embodiment, a lithium precursor can be recovered from an electrode active material mixture through a dry-based process using a dry rotary heating reactor, thereby obtaining a high-purity lithium precursor without additional processes that would be required in a wet-based process.
[0028] In addition, by adjusting the rotation speed, reaction temperature, and longitudinal movement distance of the reactants of the dry rotary heating reactor, the reaction time, residence time, and reaction degree of the electrode active material mixture and the reducing reactant gas can be easily controlled, thereby further improving the selectivity and efficiency of the lithium precursor regeneration process.
[0029] In addition, by using a dry rotary indirectly heated reactor, the reactor body can be indirectly heated without generating combustion products by using a jacket or an electric furnace within the indirectly heated reactor, thereby preventing contamination of the pre-precursor mixture with combustion products and enabling the production of a high-purity lithium precursor without an additional process. [Brief explanation of the drawings]
[0030] [Figure 1] FIG. 1 is a process flow diagram illustrating a method for regenerating a lithium precursor according to an exemplary embodiment. DETAILED DESCRIPTION OF THE INVENTION
[0031] An embodiment of the present invention provides a method for recovering active metals from lithium secondary batteries in high purity and high yield through a dry-based process utilizing a dry rotary kiln.
[0032] Hereinafter, embodiments of the present invention will be described in more detail with reference to the drawings. However, these embodiments are merely illustrative of the present invention and are not intended to limit the present invention.
[0033] As used herein, the term "precursor" is used to refer collectively to a compound containing a specific metal to provide the specific metal contained in the electrode active material.
[0034] 1 is a schematic flow chart illustrating a method for recovering active metals from a lithium secondary battery according to an exemplary embodiment. For convenience of explanation, FIG. 1 also illustrates a schematic diagram of a dry rotary heating reactor along with the process flow.
[0035] 1, the electrode active material mixture 50 can be prepared from a lithium secondary battery (e.g., step S10). According to an exemplary embodiment, the electrode active material mixture 50 can be prepared from an electrode obtained from a lithium secondary battery. For example, the electrode active material mixture 50 can be prepared from a lithium-containing compound obtained from a lithium secondary battery.
[0036] The term "electrode active material mixture" used in the present application may refer to raw materials that are introduced into a dry rotary heating reactor described below after the positive and negative electrode current collectors have been substantially removed from the electrodes recovered from the lithium secondary battery.
[0037] The electrode active material mixture 50 may be a mixture of materials obtained from a lithium secondary battery, including a positive electrode active material mixture obtained from a lithium secondary battery. Preferably, the electrode active material mixture 50 may be a positive electrode active material mixture. Hereinafter, a case where the electrode active material mixture 50 is a positive electrode active material mixture will be described in detail. However, this is merely an example and is not limited thereto.
[0038] The lithium secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, and the positive electrode and the negative electrode may include a positive electrode active material layer and a negative electrode active material layer coated on the entire positive electrode current collector and the negative electrode current collector, respectively.
[0039] For example, the positive electrode active material contained in the positive electrode active material layer may include an oxide containing lithium and a transition metal.
[0040] In some embodiments, the positive electrode active material may include a compound represented by Formula 1:
[0041] [ka]
[0042] In Chemical Formula 1, M1, M2, and M3 may be a transition metal selected from Ni, Co, Mn, Na, Mg, Ca, Ti, V, Cr, Cu, Zn, Ge, Sr, Ag, Ba, Zr, Nb, Mo, Al, Ga, or B. <x≦1.1、2≦y≦2.02、0<a<1、0<b<1、0<c<1、0<a+b+c≦1であってもよい。
[0043] In some embodiments, the positive electrode active material may be an NCM-based lithium oxide containing nickel, cobalt, and manganese. The NCM-based lithium oxide as the positive electrode active material may be prepared by reacting a lithium precursor and an NCM precursor (e.g., an NCM oxide) with each other, for example, by coprecipitation.
[0044] However, the embodiments of the present invention can be applied not only to the electrode material containing the NCM-based lithium oxide but also to all lithium-containing electrode materials.
[0045] The lithium precursor may include lithium hydroxide (LiOH), lithium oxide (LiO2), or lithium carbonate (Li2CO3). Lithium hydroxide may be advantageous as a lithium precursor in terms of the charge / discharge characteristics, life characteristics, and high-temperature stability of a lithium secondary battery. For example, lithium carbonate may cause a deposition reaction on the separator, reducing life stability.
[0046] As a result, according to an embodiment of the present invention, a method for regenerating lithium hydroxide as a lithium precursor with high selectivity can be provided.
[0047] For example, the positive electrode can be separated and recovered from the lithium secondary battery. The positive electrode includes a positive electrode current collector (e.g., aluminum (Al)) and a positive electrode active material layer. The positive electrode active material layer may include a conductive material and a binder in addition to the positive electrode active material.
[0048] The conductive material may include, for example, a carbon-based material such as graphite, carbon black, graphene, carbon nanotubes, etc. The binder may include, for example, a resin material such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, etc.
[0049] A positive electrode active material mixture can be prepared from the recovered positive electrode. In some embodiments, the positive electrode active material mixture can be produced in powder form by a physical method such as a grinding process. The positive electrode active material mixture can include a lithium-transition metal oxide powder, such as an NCM-based lithium oxide powder (e.g., Li(NCM)O).
[0050] The term “positive electrode active material mixture” as used herein may refer to raw materials that are introduced into a dry rotary heating reactor described below after the positive electrode current collector has been substantially removed from the recovered positive electrode.
[0051] In one embodiment, the positive electrode active material mixture may include positive electrode active material particles such as the NCM-based lithium oxide. In one embodiment, the positive electrode active material mixture may also include a portion of a component derived from the binder or the conductive material. In one embodiment, the positive electrode active material mixture may be substantially composed of the positive electrode active material particles.
[0052] In some embodiments, the positive electrode active material mixture may have an average particle size (D50) of 5 to 100 μm, which allows the lithium-transition metal oxide, such as Li(NCM)O, to be easily separated from the positive electrode current collector, conductive material, and binder contained in the positive electrode active material mixture.
[0053] In some embodiments, the cathode active material mixture may be heat-treated before being introduced into a dry rotary heater reactor, which will be described later. The heat treatment may remove or reduce impurities, such as the conductive material and binder, contained in the cathode active material mixture, allowing the lithium-transition metal oxide to be introduced into the dry rotary heater reactor with high purity.
[0054] The temperature of the heat treatment may be, for example, about 100 to 500° C., preferably about 350 to 450° C. Within this range, the impurities are substantially removed, and decomposition and damage to the lithium-transition metal oxide can be prevented.
[0055] In some embodiments, the positive electrode active material mixture can be obtained by immersing the recovered positive electrode in an organic solvent, for example, by immersing the recovered positive electrode in an organic solvent to separate and remove the positive electrode current collector, and then selectively extracting the positive electrode active material by centrifugation.
[0056] By the above-described process, substantially all components of the positive electrode aggregate, such as aluminum, are completely separated and removed, and a positive electrode active material mixture can be obtained in which the content of carbonaceous components derived from the conductive material and binder is removed or reduced.
[0057] The process for obtaining the positive electrode active material mixture has been described above in detail. As described above, the electrode active material mixture 50 includes the positive electrode active material mixture described above, and may further include a negative electrode active material mixture, etc., in addition to the positive electrode active material mixture described above.
[0058] For example, in step S20, the electrode active material mixture 50 can be reacted in a dry rotary heating reactor 100 to form a pre-precursor mixture 60.
[0059] 1, the dry rotary heater reactor 100 can be divided into a reactor body 150, a reactor front end 130, and a reactor rear end 170. The reactor body 150 can include a heating section 104 such as a heater or an electric furnace.
[0060] The electrode active material mixture 50 can be supplied to the reactor front end 130 through the electrode active material mixture supply unit 110. The electrode active material mixture 50 can move to the reactor body 150 through the reactor front end 110.
[0061] A reactant gas for converting the electrode active material mixture 50 into a pre-precursor may be supplied into the reactor body 150 via a first supply passage 102a connected to the reactor front end 130 or a second supply passage 102b connected to the reactor rear end 170. According to an exemplary embodiment, the reactant gas may include a reducing gas, such as hydrogen (H). The reactant gas contacts the electrode active material mixture 50 to reduce the electrode active material mixture 50 into a pre-precursor mixture 60.
[0062] When the reactant gas is supplied to the reactor body 150 through the second supply passage 102b connected to the rear end 170 of the dry rotary heating reactor 100, the reactant gas may come into contact with the electrode active material mixture 50 injected into the electrode active material mixture supply unit 110 connected to the front end 130 of the dry rotary heating reactor 100, thereby forming a counter flow of the electrode active material mixture 50 and the reactant gas. The counter flow allows unreacted electrode active material mixture 50 to come into contact with the high-purity reactant gas, thereby improving the reaction conversion rate.
[0063] When the reactant gas is supplied to the reactor body 150 through the first supply flow path 102a connected to the front end 130 of the dry rotary heating reactor 100, it comes into contact with the electrode active material mixture 50 injected into the electrode active material mixture supply unit 110 connected to the front end 130 of the dry rotary heating reactor 100, forming a co-flow of the electrode active material mixture 50 and the reactant gas. The co-flow increases the contact time between the electrode active material mixture 50 and the reactant gas, thereby improving the selectivity and efficiency of the reduction reaction between the electrode active material mixture 50 and the reactant gas. In addition, contact between the highly concentrated electrode active material mixture 50 and the reactant gas increases the initial reduction reaction rate, and the electrode active material mixture 50 and the reactant gas quickly pass through the dry rotary heating reactor 100, thereby shortening the overall process time.
[0064] In some embodiments, the electrode active material mixture 50 can be reduced by the hydrogen-containing reactant gas to form a pre-precursor mixture 60. For example, the pre-precursor mixture 60 can include pre-lithium precursor particles 70 including a lithium oxide (e.g., LiO) and transition metal-containing particles 80 including a transition metal or transition metal oxide. For example, the reduction reaction can produce Ni, Co, Mn, NiO, CoO, and MnO along with the lithium oxide.
[0065] The reactor body 150 may include a heating unit 104. The heating unit 104 may be at least one selected from the group consisting of a heater, a burner, a jacket, and an electric furnace. Preferably, the heating unit may be a jacket or an electric furnace. The heating unit 104 is located within the reactor body 150 and may be a separate component or may be integrated with the reactor body 150.
[0066] The heating unit 104 can heat the reactor body 150 to a temperature of about 250 to 600°C, preferably 350 to 450°C. Within this temperature range, a reduction reaction can occur. Within this reaction temperature range, the reduction reaction between the electrode active material mixture 50 and the reaction gas can be promoted. If the temperature of the reactor body 150 is below 350°C, the reduction reaction may not proceed sufficiently. If the temperature exceeds 450°C, an excessive amount of unnecessary heat may be supplied without promoting the reduction reaction, which may reduce the economic efficiency of the reduction process.
[0067] The dry rotary heating reactor may be an indirect firing rotary kiln. The indirect heating rotary reactor may increase the temperature of the reactor body 150 using a jacket or an electric furnace. The indirect heating rotary kiln indirectly heats the reactor body 150 through heat conduction using a jacket or an electric furnace. Since the indirect heating rotary kiln indirectly heats the reactor body 150, no combustion products are generated during the process of increasing the temperature of the reactor body 150, preventing contamination of the pre-precursor mixture by combustion products. The indirect heating rotary kiln may easily produce a high-purity lithium precursor without requiring an additional process for removing combustion products.
[0068] 1, the dry rotary heating reactor 100 may rotate about a longitudinal axis (X) of the dry rotary heating reactor 100, which is the direction in which the electrode active material mixture 50 moves. For example, the reactor body 150 of the dry rotary heating reactor 100 may rotate about the longitudinal axis (X) of the dry rotary heating reactor 100. Rotation of the dry rotary heating reactor 100 about the longitudinal axis (X) may increase contact between the electrode active material mixture 50 and the reactant gas, thereby accelerating the reduction reaction. In addition, aggregation between the electrode active material mixture 50 and the pre-precursor mixture 60 formed by the reduction reaction of the reactant gas may be prevented.
[0069] The dry rotary heating reactor 100 may rotate at 5 to 200 rpm about the longitudinal axis (X) along which the electrode active material mixture 50 moves. This rotation speed range effectively prevents aggregation between the electrode active material mixture 50 and the pre-precursor mixture 60 formed by the reduction reaction of the reactant gas, and also prevents the pre-precursor mixture 60 from depositing on the inner surface of the reactor body 150 of the dry rotary heating reactor 100. If the rotation speed of the dry rotary heating reactor 100 is less than 5 rpm, the contact rate between the electrode active material mixture 50 and the reactant gas may decrease, resulting in insufficient reaction. If the rotation speed of the dry rotary heating reactor 100 exceeds 200 rpm, centrifugal force may cause the reactants to deposit on the inner surface of the reactor body 150, and the movement speed of the electrode active material mixture 50 may increase, resulting in the discharge of unreacted electrode active material mixture 50 in which the reduction reaction has not progressed.
[0070] 1, the length of the reactor body 150 can be adjusted to control the distance that the electrode active material mixture 50 moves within the reactor body 150. This allows the residence time of the electrode active material mixture 50 and the reactant gases within the reactor body 150 and the total reaction time to be controlled.
[0071] The length of the reactor body 150 may be 1 to 60 m. If the length of the reactor body 150 is less than 1 m, the reduction reaction between the electrode active material mixture 50 and the reactant gas may not proceed sufficiently. If the length of the reactor body 150 is more than 60 m, the pre-precursor mixture 60 formed after the reaction has already completed may remain excessively within the reactor body 150, reducing process efficiency. In addition, agglomeration of the pre-precursor mixture 60 may occur as the pre-precursor mixture 60 moves within the reactor body 150.
[0072] Within the reactor body 150, a pre-precursor mixture 60 may be formed that includes preliminary lithium precursor particles 70 and transition metal-containing particles 80 (e.g., the transition metal or transition metal oxide). The preliminary lithium precursor particles 70 may include, for example, lithium hydroxide, lithium oxide, and / or lithium carbonate.
[0073] Referring to FIG. 1, a pre-precursor mixture 60 including preliminary lithium precursor particles 70 and transition metal-containing particles 80 can be collected via an outlet 106 connected to the rear end 170 of the reactor.
[0074] The pre-precursor mixture 60 collected through the outlet 106 is injected into the hydration reaction section 210. In the hydration reaction section 210, a hydration reaction between the pre-precursor mixture 60 and water may occur (e.g., step S30).
[0075] According to an exemplary embodiment, the preliminary lithium precursor particles 70 are hydrated with water in the hydration reaction unit 210 to recover lithium hydrate (e.g., LiOH) as a lithium precursor. The hydration reaction can produce a crystallized lithium precursor.
[0076] The lithium precursor formed in the hydration reaction unit 210 can be recovered in the lithium precursor recovery unit 230 (for example, step S40).
[0077] Since the transition metal-containing particles 80, including nickel, cobalt, or manganese, are relatively heavier than the lithium precursor particles, the lithium precursor particles can be collected first. Because the lithium precursor particles are collected first, the lithium precursor particles can be separated without a separate separation process. This improves the efficiency, productivity, and selectivity of the lithium precursor in the lithium precursor regeneration process.
[0078] In a comparative example, a wet process such as a strong acid leaching process can be used to recover lithium or transition metals from a lithium secondary battery. However, the wet process has limitations in selectively separating lithium. In addition, a water washing process is required to remove solution residues, and the production of by-products such as hydrates due to contact with the solution can increase.
[0079] In contrast, according to embodiments of the present invention, pre-precursor mixture 60 is collected through a dry process that eliminates the use of solutions, and the lithium precursor is isolated through a hydration reaction that eliminates the use of strong acids, thereby reducing by-products, increasing yield, and eliminating the need for wastewater treatment, enabling an environmentally friendly process design.
[0080] Furthermore, since the lithium precursor particles can be selectively recovered by the hydration reaction section 210 before the transition metal-containing particles 80, the selectivity, yield, and purity of the lithium precursor can be further improved.
[0081] In addition, the dry rotary heating reactor 100 can adjust or accelerate the reaction rate between the electrode active material mixture 50 and the reactant gas by adjusting the rotation speed of the reactor, the length of the reactor body 150, the temperature inside the reactor body, etc., and can further improve the selectivity, yield, and purity of the lithium precursor.
[0082] In some embodiments, after recovering the lithium precursor from the hydration reaction section 210, the transition metal-containing particles 80 can be collected in the transition metal precursor recovery section 250. The transition metal precursor can be obtained from the transition metal-containing particles 80 collected from the transition metal precursor recovery section 250 (e.g., step S50).
[0083] For example, the preliminary lithium precursor particles 70 can be collected through the outlet 106, and then the transition metal-containing particles 80 can be recovered through the hydration reaction section 210. The transition metal-containing particles 80 can then be treated with an acid solution to form precursors of the respective transition metals in the form of acid salts.
[0084] In one embodiment, sulfuric acid can be used as the acid solution, in which case NiSO4, MnSO4, and CoSO4 can be recovered as the transition metal precursors, respectively.
[0085] As described above, after the lithium precursor is collected through the dry process and hydration reaction, the transition metal precursor is selectively extracted using an acid solution, thereby improving the purity and selectivity of each metal precursor and reducing the load of the wet process, thereby reducing the increase in wastewater and by-products.
Claims
1. Providing an electrode active material mixture collected from a lithium secondary battery; reducing the electrode active material mixture in a dry rotary heater reactor to form a pre-precursor mixture; and selectively recovering the lithium precursor from said pre-precursor mixture.
2. 2. The method of claim 1, wherein the step of forming the preliminary precursor mixture comprises rotating the dry rotary heater reactor on the longitudinal axis while moving the electrode active material mixture along the longitudinal axis of the dry rotary heater reactor.
3. 3. The method for regenerating lithium precursor according to claim 2, wherein the step of forming the pre-precursor mixture comprises rotating the dry rotary heater reactor about the longitudinal axis at 5 to 200 rpm.
4. 2. The method for regenerating a lithium precursor according to claim 1, wherein the reaction temperature in forming the pre-precursor mixture is 250-600° C.
5. 2. The method of claim 1, wherein the step of forming the pre-precursor mixture comprises contacting the electrode active material mixture with a reducing reactant gas.
6. 6. The method for regenerating a lithium precursor according to claim 5, wherein the reducing reaction gas is supplied from the rear end of the dry rotary heating reactor in the length direction, and forms a counterflow with respect to the electrode active material mixture supplied to the front end of the dry rotary heating reactor in the length direction.
7. 6. The method for regenerating a lithium precursor according to claim 5, wherein the reducing reactant gas is introduced together with the electrode active material mixture at the front end in the length direction of the dry rotary heating reactor.
8. 2. The method of claim 1, wherein the preliminary precursor mixture comprises preliminary lithium precursor particles and transition metal-containing particles.
9. 9. The method for regenerating a lithium precursor according to claim 8, wherein said spare lithium precursor particles comprise lithium hydroxide, lithium oxide and lithium carbonate.
10. 9. The method for regenerating a lithium precursor according to claim 8, wherein the step of recovering the lithium precursor further comprises the step of hydrating the reserve lithium precursor particles to produce a lithium precursor.
11. 11. The method for regenerating a lithium precursor according to claim 10, wherein the step of hydrating the reserve lithium precursor comprises collecting the lithium precursor particles prior to the transition metal-containing particles.
12. 9. The method for regenerating a lithium precursor according to claim 8, further comprising treating the transition metal-containing particles with an acid solution to recover a transition metal precursor.
13. The method for recovering active metals from lithium secondary batteries according to claim 1 , wherein the dry rotary heating reactor is an indirect heating rotary furnace.
14. An electrode active material mixture supply unit; a dry rotary heating reactor for reacting the electrode active material mixture supplied from the electrode active material mixture supply unit with a reducing gas; and a lithium precursor recovery section for collecting a lithium precursor from the electrode active material mixture reactant produced in the dry rotary heater reactor.
15. 15. The lithium precursor regeneration system according to claim 14, further comprising a supply channel connected to at least one of the front end or the rear end in the length direction of the dry rotary heating reactor to supply the reducing gas.
16. The system for regenerating a lithium precursor according to claim 14, further comprising a transition metal precursor recovery section for collecting a transition metal precursor from the electrode active material mixture reactants.
Citation Information
Patent Citations
Method for recovering lithium
JP2011094227A
System for collecting raw material powder
JP2013036717A
Method for recovering valuables from used lithium ion batteries
JP2018120716A
A Method Of Manufacturing A Lithium Carbonate With High Purity By Recycling A Lithium From A Anode Material Of Used Lithium Ion Secondary Battery
KR101682217B1
Method for crushing cell
US6524737B1