Method for early detecting deterioration of concrete

The method uses minimum principal strain patterns in digital images to quickly and accurately identify early signs of concrete deterioration, facilitating timely maintenance and extending the life of concrete structures.

JP2024133850APending Publication Date: 2024-10-03TAIHEIYO CEMENT CORP

Patent Information

Application Number
JP2023043844
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for detecting concrete deterioration are either too complex, require extensive time, or fail to accurately identify early signs of cracking before they become visible, making it difficult to implement effective preventive measures.

Method used

A method utilizing the distribution of minimum principal strain in digital images, acquired through image acquisition, strain manifestation treatment, and digital image correlation, to detect early signs of concrete deterioration by identifying specific patterns associated with alkali-silica reaction, delayed ettringite formation, freeze-thaw, drying shrinkage, and reinforcing bar corrosion.

Benefits of technology

Enables rapid and clear detection of potential cracking areas, allowing for timely intervention and maintenance to extend the life of concrete structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133850000001_ABST
    Figure 2024133850000001_ABST
Patent Text Reader

Abstract

To provide a method enabling early, quick and clear detection of a concentration area of strain that may lead to a future crack in a concrete structure.SOLUTION: Deterioration of concrete is early detected using an image of distribution of minimum principal strains obtained through steps (A) to (D): (A) a first image acquisition step for acquiring a digital image of an image acquisition target surface for acquiring a digital image of the concrete; (B) a strain manifestation processing step for subjecting the image acquisition target surface to any processing of heating, drying and cooling to make strains manifest; (C) a second image acquisition step for again acquiring a digital image of the image acquisition target surface after the treatment; (D) a minimum principal strain distribution acquisition step for calculating strains using a digital image correlation method based on the digital images before and after the, and obtaining distribution of change in minimum principal strains based on the calculated strains.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for early detection of concrete deterioration by analyzing digital images of a concrete surface. [Background technology]

[0002] In the past, the Ministry of Land, Infrastructure, Transport and Tourism compiled "Past research examples on the lifespan of reinforced concrete structures (concrete)," which "estimated the physical lifespan of reinforced concrete buildings to be 117 years" (Iizuka Yutaka, 1979, Building Maintenance and Management, Kajima Institute Publishing). In addition, in terms of "the number of years that reinforced concrete members will continue to function," it was stated that "the useful life of a general building (including a residence) is 120 years, with an extension of 150 years due to exterior finishing" (Taxation Bureau, Ministry of Finance, 1951, Method of Calculating the Useful Life of Fixed Assets), and concrete was thought to have a durability of over 100 years (Non-Patent Document 1). However, research into the durability of concrete to date has revealed that factors such as alkali-silica reaction, delayed formation of ettringite, freezing and thawing, drying shrinkage, and corrosion of reinforcing bars are responsible for concrete deterioration, and that concrete deterioration occurs when deterioration factors such as carbon dioxide and salt penetrate into cracks caused by these factors.

[0003] Among these causes of concrete deterioration, alkali-silica reaction occurs when silica in reactive aggregate reacts with alkali metal ions in concrete in a high pH environment to produce alkali silica gel. This gel then absorbs water and expands, causing cracks.

[0004] Delayed formation of ettringite may occur in a concentrated form several years after steam curing of concrete, and this ettringite causes the concrete to expand and collapse.

[0005] In addition, freeze-thaw is a phenomenon in which water in concrete repeatedly freezes and thaws over many years, causing cracks to form due to the volume expansion of the frozen water.

[0006] Drying shrinkage is a phenomenon in which moisture in concrete evaporates as it dries, causing the concrete to shrink and generate tensile stress, resulting in cracks.

[0007] Furthermore, corrosion of reinforcing bars is a phenomenon in which the passive film on the surface of reinforcing bars is damaged by neutralization or salt damage, causing the reinforcing bars to rust, expand, and crack.

[0008] In these types of concrete deterioration, by the time cracks become apparent and can be seen, the deterioration has often progressed too far. Therefore, in order to prevent concrete cracking, it is necessary to detect the signs of cracking before they become apparent and to deal with the deterioration of concrete according to the type of crack. However, because concrete surfaces are subject to scratches, dirt, moisture, and the like, it is difficult to detect early signs of cracks using visual crack detection methods.

[0009] Therefore, several methods have been proposed to detect the deterioration of concrete. For example, The method for inspecting cracks in concrete structures described in Patent Document 1 involves sequentially laminating a primer layer, a sheet layer for preventing spalling, and a topcoat layer on the base that constitutes the concrete structure, and then sequentially laminating on the topcoat layer a high-elasticity coating layer containing a fluorescent dye that glows in response to excitation light and a low-elasticity coating layer containing a blocking agent that blocks the transmission of the excitation light, and after the concrete structure has begun to be used, irradiating the structure with excitation light to detect cracks that have developed in the base due to deterioration over time.

[0010] In addition, the concrete deterioration factor detection method described in Patent Document 2 involves imaging the concrete surface to obtain a visible light image, irradiating the concrete surface with infrared light and inputting the reflected light from the concrete surface into a spectroscope via a scanning device, detecting absorbance based on the light intensity of a specific wavelength to detect a specific deterioration factor using the spectroscope, converting the absorbance into a concentration of the deterioration factor and quantizing the concentration, and based on the quantized value, expressing the concentration in shades or colors corresponding to the concrete surface to be measured to obtain a deterioration factor image, and combining the deterioration factor image with the visible light image.

[0011] Moreover, the concrete deterioration detection method described in Patent Document 3 is a method in which digital images are acquired over time and strain distribution is obtained using a digital image correlation method.

[0012] Furthermore, the method for early detection of concrete deterioration described in Patent Document 4 is a method for detecting concrete deterioration using the pattern that appears in an image of the distribution of maximum principal strain obtained through a specific process. Incidentally, Figure 1 shows the distribution of maximum principal strain of a flat plate specimen due to alkali-silica reaction (ASR), delayed ettringite formation (DEF), drying shrinkage, and corrosion of rebar.

[0013] However, the method described in Patent Document 1 is merely a method for detecting cracks after they have occurred, and further requires sequentially laminating an undercoat layer, an anti-peeling sheet layer, and a topcoat layer, and then sequentially laminating a high-elasticity coating layer and a low-elasticity coating layer, making the work complicated.

[0014] Furthermore, the method described in Patent Document 2 requires not only obtaining a visible light image of the concrete surface, but also irradiating the concrete surface with infrared light, inputting the reflected light from the concrete surface into a spectroscope, and detecting absorbance based on the light intensity of specific wavelengths to detect deterioration factors, which is also a complicated process.

[0015] Furthermore, the method described in Patent Document 3 requires measuring the change in strain over time multiple times over a long period of time, which requires time and effort to detect deterioration.

[0016] Furthermore, although the method described in Patent Document 4 is useful for flat plate specimens, when the maximum principal strain is used to detect deterioration of a concrete structure, the deterioration may not be clearly detected (FIGS. 5 and 6). [Prior art documents] [Non-patent literature]

[0017] [Non-Patent Document 1] Concrete Medical Center, "Four issues affecting the lifespan of condominiums and checkpoints for judging their lifespan," Internet<URL:https: / / concrete-mc.jp / mansion-lifespan> [Patent documents]

[0018] [Patent Document 1] JP 2014-85200 A [Patent Document 2] JP 2007-85850 A [Patent Document 3] JP 2018-155023 A [Patent Document 4] JP 2020-153784 A Summary of the Invention [Problem to be solved by the invention]

[0019] Therefore, the present invention is a further development of the method for early detection of concrete deterioration described in Patent Document 4, and aims to provide a method that can quickly, early and clearly detect areas of concentrated strain that may lead to cracks in future, even in concrete structures. [Means for solving the problem]

[0020] The inventors have investigated detection methods that meet the above-mentioned objectives, and have found that the above-mentioned objectives can be achieved by using the pattern that appears in the image of the distribution of minimum principal strains, and have thus completed the present invention. Specifically, the present invention is a method for early detection of deterioration of concrete, which comprises the following components:

[0021] [1] A method for early detection of concrete deterioration, which detects deterioration of concrete using an image of the distribution of minimum principal strain obtained through the following steps (A) to (D). (A) a first image acquisition step of acquiring a digital image on an image acquisition target surface for acquiring a digital image of concrete; (B) a distortion manifestation treatment step of subjecting the image acquisition surface to any one of heating, drying, and cooling treatment to manifest distortion; (C) a second image acquisition step of acquiring a digital image of the image acquisition target surface again after performing the treatment. (D) A minimum principal strain distribution acquisition step of calculating strain using a digital image correlation method based on the digital images before and after the treatment, and obtaining a distribution of changes in minimum principal strain based on the strain. [2] The method for early detection of concrete deterioration described in [1] above, wherein a pattern appearing in the image of the distribution of minimum principal strain is used to detect deterioration of concrete based on the following criteria (a) to (e). (a) The areas where a tortoiseshell pattern appears are detected as an alkali-silica reaction. (b) Areas where a uniform pattern appears overall are detected as delayed formation of ettringite. (c) Areas where a spotted pattern appears are detected as freezing and thawing. (d) Linear patterns appearing in areas where there are no reinforcing bars, or linear patterns appearing diagonally to structural components such as columns or beams, are detected as drying shrinkage. (e) Where a linear pattern appears directly above the reinforcing bar, this is detected as corrosion of the reinforcing bar. [3] The method for early detection of concrete deterioration described in [2] above, further comprising detecting deterioration of concrete based on the distribution of positive and negative strain in addition to the pattern. [4] A method for early detection of concrete deterioration as described in [1] above, in which areas where negative (shrinkage) lines appear in the image of the distribution of minimum principal strain are detected as areas where cracks may occur. [5] A method for early detection of concrete deterioration described in [4], comprising using the pattern and distribution of negative strain to detect concrete deterioration based on the following criteria (f) to (j). (f) In areas where a tortoiseshell pattern appears, where the lines of the tortoiseshell pattern show larger negative (shrinkage) strain, and where the substrate (area other than the pattern) also shows overall negative (shrinkage) strain, this is detected as an alkali silica reaction. (g) Areas where a uniform pattern appears overall and the paste or mortar portion shows negative (shrinkage) strain overall are detected as delayed formation of ettringite. (h) Areas where a spotted pattern appears and the spots show large negative (shrinkage) strain are detected as freezing and thawing. (i) A linear pattern appears in an area where there is no reinforcing bar, or a linear pattern appears diagonally on a structural member such as a column or beam, and the line portion of the pattern shows negative (shrinkage) strain and the substrate portion shows negative (shrinkage) strain overall. This is detected as drying shrinkage. (j) When a linear pattern appears directly above a reinforcing bar and the lines of the pattern indicate negative (shrinkage) strain, this is detected as corrosion of the reinforcing bar. [6] The method for early detection of deterioration of concrete according to [1] or [4], wherein the concrete is a concrete structure. [7] The method for early detection of concrete deterioration according to [1] or [4], wherein the heating treatment is performed at 40 to 80°C for 5 to 120 minutes. Effect of the Invention

[0022] The method for early detection of concrete deterioration of the present invention can detect concrete deterioration early, quickly, and clearly. [Brief description of the drawings]

[0023] [Figure 1] FIG. 13 shows the distribution of maximum principal strains of plate specimens due to ASR, DEF, drying shrinkage, and corrosion of rebar. [Diagram 2] This is a photograph showing the concrete image capture surface to which anchor plugs (circles) have been attached to secure a digital image capture scanner and to capture a digital image imprinted with a random pattern (black and white dots). [Diagram 3] 1 is a photograph showing an example of a line sensor scanner used as a scanner for acquiring digital images. [Figure 4] Shown here are a method of heating the surface to be imaged so that it is surrounded by heat (left photo), and a method of heating with gaps above and below (right photo). [Diagram 5] The maximum principal strain distribution (upper photo) and minimum principal strain distribution (lower photo) are shown on the surface (same for top and bottom) of a concrete structure for which images were captured. [Figure 6] This figure shows the maximum principal strain distribution of a flat plate test specimen and a concrete structure (actual structure) (photo on the left), and the minimum principal strain distribution of a flat plate test specimen and a concrete structure (photo on the right). The upper photo shows the strain distribution of the flat plate test specimen, and the lower photo shows the strain distribution of the concrete structure. [Figure 7] FIG. 1 is a diagram showing calculation formulas for maximum principal strain ε1 and minimum principal strain ε2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] As described above, the method for early detection of concrete deterioration of the present invention is a method for early detection of concrete deterioration using an image of the distribution of minimum principal strains obtained through (A) the first image acquisition step, (B) the strain elicitation treatment step, (C) the second image acquisition step, and (D) the minimum principal strain distribution acquisition step. The present invention will be described in detail below.

[0025] (A) A first image acquisition step and (C) a second image acquisition step. Both processes are processes for acquiring digital images of the concrete surface before (first image acquisition process) and after (second image acquisition process) performing any one of the treatments of heating, drying, and cooling the concrete surface on the image acquisition target surface for acquiring a digital image of the concrete surface. Since the operations of these processes are the same, both processes will be explained together below.

[0026] First, in order to obtain a good digital image, it is preferable to polish the concrete surface to be imaged. In addition, the image is preferably taken after the concrete has hardened but before cracks become visible, because the accumulated strain is released when cracks occur.

[0027] Here, if moisture is present on the capture surface when a digital image is captured, the color contrast may be reduced and color unevenness may occur, which may reduce the correlation between the images captured before and after any of the heating, drying, and cooling processes. To avoid this reduction in correlation, before capturing an image, a process is performed in which the moisture on the image capture surface of the concrete is removed by absorbing it into a cloth or the like, or the surface is air-dried until all moisture is removed. This process is an optional process that is performed when moisture is present on the image capture surface.

[0028] Next, as shown in Figure 2, anchor plugs (circles) for fixing the digital image acquisition scanner are placed on the concrete surface, and a random pattern (black and white dots) is marked on the concrete surface to prepare for the first image acquisition. Note that the preparation for the first image acquisition step does not necessarily have to be performed immediately before the image acquisition. After the above preparations are completed, a digital image scanner is placed in contact with the concrete surface to be imaged to capture an image. There are no particular limitations on the type of scanner, but a line sensor scanner is preferred because it does not require adjustments for illumination or lens aberration and can capture fine images. Here, an example of a line sensor scanner is shown in Figure 3.

[0029] The concrete that is the subject of the present invention is not particularly limited, and examples thereof include ordinary concrete, watertight concrete, hot weather concrete, cold weather concrete, mass concrete, flowable concrete, high flowability concrete, high strength concrete, low heat concrete, expansive concrete, prestressed concrete, low shrinkage concrete, fiber reinforced concrete, lightweight concrete, and polymer concrete. The concrete targeted by the present invention is preferably a concrete structure in which early detection of concrete deterioration has been difficult using conventional methods, and among concrete structures, mass concrete and reinforced concrete are more preferred.

[0030] (B) Strain manifestation treatment process This process is a process of making the strain apparent by subjecting the image acquisition surface to any one of heating, drying, and cooling treatments. By performing a treatment such as heating for a short period of time without acquiring images over a long period of time, a change in length due to temperature strain occurs, making it possible to clarify the strain distribution. Heating treatment can be done, for example, by surrounding the surface to be imaged (left photo) and by heating at regular intervals above and below (right photo) as shown in Figure 4. When heating at regular intervals above and below, it is advisable to heat in a direction perpendicular to the expected cracks in order to make the distortion more apparent. To prevent the manifestation of distortion and deterioration of the concrete, the heating treatment is preferably performed at 40 to 80°C for 5 to 120 minutes. If the heating is performed at 40 to 80°C for 5 to 120 minutes, distortion will become apparent. The heating temperature is more preferably 50 to 70°C, and even more preferably 60 to 70°C, and the heating time is more preferably 10 to 100 minutes, and even more preferably 20 to 80 minutes. Examples of the heating device include a sheet heater, a jet heater, a burner, a halogen heater, and sunlight.

[0031] The drying treatment may involve applying hot air using an electric fan, compressed air, a jet heater, a burner, etc., or heating the surface with a halogen heater, sunlight, etc. The drying temperature is not particularly limited, but in consideration of the drying speed, the concrete surface temperature is preferably 30° C. or higher, more preferably 40° C. or higher. In order to prevent deterioration of the concrete, the concrete surface temperature is preferably 80° C. or lower, more preferably 60° C. or lower. The lower limit of the drying time depends on the drying method, but is preferably 10 minutes, more preferably 1 hour, and even more preferably 3 hours so that the strain distribution becomes clearer. The upper limit of the drying time is preferably 1 week, more preferably 3 days, and even more preferably 1 day in order to ensure the rapidity of the detection method and to prevent deterioration of the concrete.

[0032] Other drying methods include immersion in an organic solvent such as alcohol or acetone, spraying the organic solvent, etc., and dehydrating (absorbing) the water in the concrete. The dehydration time is preferably 30 minutes or more. After immersion in the organic solvent, condensation may occur, so it is recommended to quickly remove the organic solvent by wiping it off, or to leave it to stand under dry conditions. The strain distribution will be more obvious if the concrete surface is soaked, sprayed, or covered with a wet cloth before drying, and then dried after the concrete surface has absorbed enough water. This water absorption time is preferably 30 minutes or more.

[0033] The cooling treatment may be, for example, blowing cold air onto the concrete surface using a cold air generator or spraying with a cooling spray. The concrete surface may also be cooled by covering it with a cold insulation material or cold water. In order to increase the cooling efficiency and reduce the variation in cooling, it is better to cover the heat transfer plate of metal or the like installed on the concrete surface with a cold insulation material. The cooling temperature is preferably at least 20°C lower, more preferably at least 40°C lower, than the original surface temperature of the concrete in order to make the strain distribution clearer. The lower limit of the cooling temperature is preferably minus 10°C, more preferably 0°C, in terms of the surface temperature of the concrete in order to prevent deterioration of the concrete. Alternatively, the surface temperature of the concrete may be increased by heating to obtain a first image, and then cooled before obtaining a second image. The cooling time is preferably 10 minutes or more, more preferably 30 minutes or more, and even more preferably 1 hour or more in order to sufficiently cool the concrete surface. The upper limit of the cooling time is preferably within 1 day, more preferably within 6 hours, and even more preferably within 3 hours in order to increase the efficiency of strain manifestation and prevent deterioration of the concrete. After heating using the above-mentioned heating method, the material may be exposed to the air and cooled to the air temperature.

[0034] (D) Minimum principal strain distribution acquisition process The step involves calculating strain using a digital image correlation method based on digital images taken before and after the treatment, and obtaining a distribution of minimum principal strains based on the strain. The digital image correlation method is a method for calculating the amount of movement on the concrete surface based on the distribution of brightness values ​​of digital images acquired before and after the treatment, and converting the amount of movement into minimum principal strain.

[0035] Specifically, the strain is calculated through the following calculation process. (i) In the pre-treatment digital image, a distribution of brightness values ​​within a subset centered on an arbitrary position is determined. (ii) A subset of the pre-treatment digital image having a brightness value distribution that is most highly correlated with the brightness value distribution of the post-treatment digital image is searched for, its center point is taken as the position after the point of interest has been displaced, the amount of displacement from the point of interest to the center point is calculated, and the amount of displacement is further converted into a minimum principal strain. For example, if a concentrated area of ​​minimum principal strain distribution (where the minimum principal strain is -200μ or less) is confirmed compared to the substrate area (where the minimum principal strain is 0μ or more), it will be detected as a crack (including cracks that may occur in the future). The correlation between the subsets before and after the treatment is expressed using the correlation coefficient R in the following formula (1). TIFF2024133850000002.tif51151In reality, the subset before treatment is set to a rectangle, but since the digital image after treatment itself is deformed, the subset may not be rectangular. In this case, to correct this, the following formula (2) is used for the coordinates (x, y) and (x*, y*) before and after treatment, assuming that the displacement gradient is constant within the subset. The above calculations can be performed using commercially available image analysis software (for example, Digital:Correlated Solutions).

[0036] For comparison, the maximum and minimum strain distributions on the same image acquisition target surface are shown in Figure 5. Also, for comparison, the maximum principal strain distributions (left photo) of the flat plate specimen and the concrete structure (actual structure) and the minimum principal strain distributions (right photo) of the flat plate specimen and the concrete structure are shown in Figure 6. Furthermore, the formulas for calculating the maximum principal strain and the minimum principal strain are shown in FIG.

[0037] Furthermore, the method for early detection of concrete deterioration of the present invention is a method for detecting areas where a minus (shrinkage) line appears in the minimum principal strain distribution image as areas where cracks may occur. Specifically, the criteria used in the present invention for detecting the causes of deterioration of concrete are described below. (a) The area where the tortoiseshell pattern appears is detected as an alkali silica reaction. In addition, the lines of the pattern show a larger negative (shrinkage) strain, and the matrix (area other than the pattern) also shows an overall negative (shrinkage) strain, which is detected as an alkali silica reaction. (b) In the area where a uniform pattern appears overall, the area where the paste or mortar part shows negative (shrinkage) strain overall is detected as delayed formation of ettringite. Also, the area where aggregate is located on the surface shows a low strain value, but the other paste or mortar parts show negative (shrinkage) strain overall. (c) Areas where a spotted pattern appears and where the spots show a large negative (shrinkage) strain are detected as freezing and thawing. Areas other than the spots show positive (expansion) or negative (shrinkage) strain depending on the concrete mix conditions and installation conditions, so they cannot be used to detect deterioration. (d) A linear pattern appears in a place where there is no reinforcing bar, or a linear pattern appears diagonally on a member such as a column or beam of a structure, and the line part of the pattern shows a negative (shrinkage) strain, while the substrate part shows a negative (shrinkage) strain as a whole. This is detected as drying shrinkage. Note that the places in a structure where there is no reinforcing bar can be confirmed in advance using existing methods such as drawings and electromagnetic radar. Furthermore, the diagonal pattern on members such as columns or beams does not limit the angle of each member. Also, the lines of the pattern indicate positive (expansion) strain, while the substrate generally indicates negative (contraction) strain. (e) When a linear pattern appears directly above a rebar (the rebar cover), and the lines in the pattern indicate negative (shrinkage) strain, this is detected as corrosion of the rebar. The position of the rebar can be confirmed in advance using existing methods such as drawings of the structure or electromagnetic radar. The lines in the pattern indicate positive (expansion) strain, and the strain in other areas will be positive (expansion) or negative (shrinkage) depending on the concrete mix conditions and installation conditions. In addition, when detecting various causes of deterioration, deterioration phenomena can be detected more efficiently by selecting the image acquisition locations and specific examples shown in Table 1 as the targets for acquiring digital images of concrete.

[0038] [Table 1]

[0039] As described above, the method for early detection of concrete deterioration of the present invention can detect various causes of concrete deterioration early, quickly, and clearly, allowing measures to be taken against deterioration at an early stage, thereby contributing to the maintenance and extension of the life of concrete. EXAMPLES

[0040] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. 1. Image acquisition target The subject of the image acquisition was a prestressed concrete bridge pier (3m wide, 1m deep) that was completed several decades ago.

[0041] 2.Preprocessing of the image acquisition target surface In order to perform analysis using the digital image correlation method, a random pattern (black and white dots) was applied to the surface of the pier using a commercially available spray paint (product name: Lacquer Spray, manufactured by Monotaro Co., Ltd.) as shown in Figure 2.

[0042] 3. Digital Image Acquisition Using a digital image acquisition scanner (line sensor type full-field strain measurement device, resolution: 1200 dpi, device name: strain measurement scanner FS-2, manufactured by Newly) shown in Figure 3, the surface of the pier with the random pattern within the square frame was scanned to acquire a digital image (first image acquisition process). After that, the surface of the structure was heat-treated at 60°C for 30 minutes at an outside temperature of 4°C, and a digital image was acquired again (second image acquisition process). Here, the random pattern was a mottled pattern painted with black and white spray paint to vary the brightness value of the surface to be measured.

[0043] 4. Calculation of maximum principal strain The acquired digital images were analyzed using image analysis software Digital (Correlated Solutions), and the distribution of minimum principal strains (shrinkage strain and compression strain) on the surface of the pier was calculated using the digital image correlation method. Specifically, the distribution of minimum principal strains was obtained through the following calculation processes (i) and (ii). (i) In digital images of the surface of the structure before and after heating, the distribution of brightness values ​​within a subset centered on an arbitrary position was determined. (ii) A subset of digital images having the brightness value distribution most highly correlated with the brightness value distribution of the digital image of the surface of the structure after heating was searched for, and the center point of the subset was taken as the position after the focus point had moved (displaced), and the distance (displacement) moved from the focus point to the center point was calculated, and the distance moved was further converted into the minimum principal strain. The correlation coefficient R in the above formula (1) was used for the correlation between subsets in the digital image of the surface of the structure. Furthermore, the above formula (2) was used for the coordinates (x, y) and (x*, y*). The distribution of the minimum principal strain obtained is shown in Figs. 5 and 6. Figure 5 shows a 210 mm x 375 mm image of the structure (bridge pier). As can be seen from Figure 5, the linear objects do not appear in the image using the maximum principal strain, but they appear clearly in the image using the minimum principal strain, and the strain concentration areas (places where cracks will occur or are expected to occur) can be recognized, so that the present invention makes it possible to detect deterioration of concrete structures at an early stage.

Claims

1. A method for early detection of concrete deterioration, comprising the steps of: detecting deterioration of concrete using an image of the distribution of minimum principal strain obtained through the steps (A) to (D) below. (A) a first image acquisition step of acquiring a digital image of an image acquisition target surface for acquiring a digital image of concrete; (B) a distortion manifestation treatment step of subjecting the image acquisition surface to any one of heating, drying, and cooling treatment to manifest distortion; (C) a second image acquisition step of acquiring a digital image of the image acquisition target surface again after the treatment is performed. (D) A minimum principal strain distribution acquisition step of calculating strain using a digital image correlation method based on the digital images before and after the treatment, and obtaining a distribution of changes in minimum principal strain based on the strain.

2. 2. The method for early detection of concrete deterioration according to claim 1, further comprising detecting deterioration of concrete based on the following criteria (a) to (e) using a pattern appearing in the image of the distribution of minimum principal strain: (a) The areas where a tortoiseshell pattern appears are detected as an alkali silica reaction. (b) Areas where a uniform pattern appears overall are detected as delayed formation of ettringite. (c) Areas where a spotted pattern appears are detected as freezing and thawing. (d) Where linear patterns appear in areas where reinforcing bars are not present, or where linear patterns appear diagonally relative to components such as columns or beams of a structure, these are detected as drying shrinkage. (e) Where a linear pattern appears directly above a reinforcing bar, this is detected as corrosion of the reinforcing bar.

3. 3. The method for early detection of deterioration of concrete according to claim 2, further comprising detecting deterioration of concrete based on a distribution of positive and negative strains in addition to the pattern.

4. 2. The method for early detection of concrete deterioration according to claim 1, wherein a portion where a minus (shrinkage) line appears in the image of the distribution of minimum principal strain is detected as a portion where cracks may occur.

5. 5. The method for early detection of concrete deterioration according to claim 4, further comprising detecting deterioration of concrete based on the following criteria (f) to (j) using the pattern and the distribution of negative strain: (f) Areas where a tortoiseshell pattern appears, where the lines of the tortoiseshell pattern show larger negative (shrinkage) strain, and where the substrate area (area other than the pattern) also shows overall negative (shrinkage) strain, are detected as having an alkali silica reaction. (g) A portion where a uniform pattern appears overall and the portion made of paste or mortar shows negative (shrinkage) strain overall is detected as delayed formation of ettringite. (h) Areas where a spotted pattern appears and the spots show large negative (shrinkage) strain are detected as freezing and thawing. (i) A linear pattern appears in an area where there is no reinforcing bar, or a linear pattern appears diagonally relative to a structural member such as a column or beam, and the line portion of the pattern shows negative (shrinkage) strain and the substrate portion shows negative (shrinkage) strain overall. This is detected as drying shrinkage. (j) When a linear pattern appears directly above a reinforcing bar and the lines of the pattern indicate negative (shrinkage) strain, this is detected as corrosion of the reinforcing bar.

6. 5. The method for early detection of deterioration of concrete according to claim 1, wherein the concrete is a concrete structure.

7. 5. The method for early detection of deterioration of concrete according to claim 1 or 4, wherein the heat treatment is performed at 40 to 80° C. for 5 to 120 minutes.

Citation Information

Patent Citations

  • Deterioration factor detecting method and device of concrete

    JP2007085850A

  • Crack inspection method for concrete structure and concrete structure

    JP2014085200A

  • Prediction method of crack occurrence timing, and early detection method of alkali-silica reaction

    JP2018155023A

  • Method for detecting deterioration of concrete at early stage

    JP2020153784A

Cited By

  • Online dryness and drying stage detection and identification method and system for spraying production line

    CN119713822A