Method for manufacturing laminate for battery, and device for manufacturing laminate for battery

By incorporating an insulating layer with ion conductivity and a porous structure, the misalignment of electrodes in battery laminate manufacturing is reduced, enhancing the efficiency and quality of the production process.

JP2024134197APending Publication Date: 2024-10-03RICOH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023044385
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing battery laminate manufacturing techniques face issues with misalignment of electrodes due to the flexibility of film separators, leading to potential displacement and inefficiencies in the manufacturing process.

Method used

The use of an insulating layer with ion conductivity, a porous structure, and a bicontinuous structure, along with a resin as a main component, to form a crosslinked structure that stabilizes the electrodes during the manufacturing process, reducing misalignment.

Benefits of technology

This approach effectively minimizes electrode misalignment, ensuring precise stacking and efficient production of high-quality battery laminates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134197000001_ABST
    Figure 2024134197000001_ABST
Patent Text Reader

Abstract

To provide a technique that can reduce displacement of laminated electrodes.SOLUTION: In a method for manufacturing a laminate for a battery according to an aspect of the present invention, an insulating layer forming unit forms at least one of an insulating layer having ion conductivity, an insulating layer having a porous structure, an insulating layer having a bicontinuous structure, an insulating layer having resin as a main component, and an insulating layer having a crosslinked structure.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for manufacturing a battery stack. [Background technology]

[0002] In recent years, the demand for secondary batteries has been increasing, and there is a demand for technology for producing highly efficient and high-quality laminates for batteries.

[0003] For example, Patent Document 1 discloses a technique for forming a battery stack by abutting electrodes against a wall of a storage container in order to eliminate the need for an alignment adjustment mechanism when inserting electrodes into a storage container. Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the technology of Patent Document 1, the butted ends are flexible, and there is a concern that the flexibility of the film separator may cause misalignment of the stacked electrodes when they are butted.

[0005] An object of the present invention is to provide a technique capable of reducing the misalignment of stacked electrodes. [Means for solving the problem]

[0006] In one embodiment of the manufacturing method for a battery laminate of the present invention, the insulating layer forming section forms at least one of an insulating layer having ionic conductivity, an insulating layer having a porous structure, an insulating layer having a co-continuous structure, an insulating layer mainly composed of a resin, and an insulating layer having a cross-linked structure. Effect of the Invention

[0007] According to the present invention, a technique capable of reducing the misalignment of stacked electrodes can be provided. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a cross-sectional view that illustrates an example of a manufacturing apparatus for a battery laminate according to the embodiment. [Diagram 2] 3 is a cross-sectional view that illustrates a first example of an insulating layer forming unit according to the embodiment. FIG. [Diagram 3] 6 is a cross-sectional view illustrating a second example of an insulating layer forming section according to the embodiment. FIG. [Figure 4] 4A and 4B are schematic diagrams showing a first example of a laminated section according to an embodiment, in which FIG. 4A is a cross-sectional view and FIG. 4B is a perspective view. [Diagram 5] 5A to 5C are top views each showing a schematic example of a shape of an alignment portion according to an embodiment. [Figure 6] 6A and 6B are schematic diagrams showing a first example of the operation of the stacking unit according to the embodiment, in which FIG. 6A is a cross-sectional view and FIG. 6B is a perspective view. [Figure 7] 7A and 7B are schematic diagrams showing a second example of a laminated section according to the embodiment, in which FIG. 7A is a cross-sectional view and FIG. 7B is a perspective view. [Figure 8] FIG. 13 is a schematic diagram showing a third example of a laminated section according to the embodiment. [Figure 9] FIG. 13 is a schematic diagram showing a fourth example of a laminated section according to the embodiment. [Figure 10] FIG. 1 is a schematic perspective view showing a first example of a battery electrode according to an embodiment of the present invention. [Figure 11] 1 is a schematic cross-sectional view showing a first example of a battery electrode according to an embodiment of the present invention. [Figure 12] FIG. 4 is a schematic perspective view showing a second example of a battery electrode according to the embodiment. [Figure 13] FIG. 4 is a schematic cross-sectional view showing a second example of a battery electrode according to the embodiment. [Figure 14] FIG. 4 is a schematic cross-sectional view showing a third example of a battery electrode according to the embodiment. [Figure 15] 15A and 15B are diagrams showing an example of a porous insulating layer according to an embodiment, in which FIG. 15A is a plan view and FIG. 15B is a cross-sectional view. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In each drawing, the same components are given the same reference numerals, and duplicated explanations will be omitted as appropriate.

[0010] In the following description, terms indicating specific directions or positions (for example, "upper", "lower", and other terms including these terms) may be used. In this specification, the up-down direction is the direction along the normal line of the surface on which the electrodes are arranged on the stage of the manufacturing apparatus for battery laminates according to the embodiment. The surface on which the electrodes are arranged on the stage is called the top surface. Viewing an object from above is called a top view. A view of an object viewed from above is called a top view. A direction perpendicular to the up-down direction is called a lateral direction. A view of an object viewed from the side is called a side view. However, these terms are only used to make the relative directions and positions in the referenced drawings easier to understand. In addition, an end view showing only a cut surface may be used as a cross-sectional view.

[0011] In each drawing, a Cartesian coordinate system having an X-axis, a Y-axis, and a Z-axis is used to express directions. The direction along the X-axis is called the X-direction, the direction along the Y-axis is called the Y-direction, and the direction along the Z-axis is called the Z-direction. The Z-direction is expressed as the up-down direction. However, these directional expressions do not limit the directions in the embodiments of the present invention.

[0012] [Embodiment] <Configuration of the Battery Laminate Manufacturing Apparatus 1000> FIG. 1 is a cross-sectional view showing an example of a battery laminate manufacturing apparatus 1000 according to an embodiment. As shown in FIG. 1, the battery laminate manufacturing apparatus 1000 has an insulating layer forming section 100, an electrode cutting section 200, and a lamination section 300. The battery laminate manufacturing apparatus 1000 forms an insulating layer on an electrode 2000 supplied through a guide member 8 by the insulating layer forming section 100. The battery laminate manufacturing apparatus 1000 cuts the electrode 2000 on which the insulating layer has been formed by the electrode cutting section 200, and laminates the electrodes cut by the electrode cutting section 200 by the lamination section 300. The battery laminate manufacturing apparatus 1000 has the insulating layer forming section 100 and the electrode cutting section 200, and therefore does not need to perform a winding operation or secure a storage space for the wound electrode after the insulating layer is formed. This makes it possible to efficiently produce high-quality batteries.

[0013] (Insulating layer forming section 100) 2 and 3 are cross-sectional views that typically show the insulating layer forming unit 100. Fig. 2 shows a first example, and Fig. 3 shows a second example. In this embodiment, the insulating layer forming unit 100 can form at least one of an insulating layer having ion conductivity, an insulating layer having a porous structure, an insulating layer having a co-continuous structure, an insulating layer mainly composed of resin, and an insulating layer having a cross-linked structure.

[0014] As shown in Figs. 2 and 3, the insulating layer forming unit 100 may have a liquid composition applying unit 100-1, an energy applying unit 100-2, a drying unit 100-3, and the like, as necessary. The liquid composition applying unit 100-1 applies a liquid composition containing a polymerizable compound and a liquid to at least a part of the electrode 2000 to form an insulating layer. The energy applying unit 100-2 applies energy to the liquid composition to polymerize the polymerizable compound to form a porous insulating layer. The drying unit 100-3 removes the solvent contained in the liquid composition.

[0015] ((Liquid composition application process section 100-1)) The liquid composition application process section 100-1 includes a liquid composition application device 1a, which is an example of a means for realizing a process of applying a liquid composition having a polymerizable compound and a liquid to at least a portion of an electrode 2000 for a battery, a liquid composition storage container 1b that stores the liquid composition, and a liquid composition supply tube 1c that supplies the liquid composition stored in the liquid composition storage container 1b to the liquid composition application device 1a.

[0016] The liquid composition storage container 1b stores the liquid composition 5, and the liquid composition application process unit 100-1 ejects the liquid composition 5 from the liquid composition application device 1a and applies the liquid composition 5 onto the electrode 2000 to form a thin film.

[0017] The liquid composition storage container 1b and the liquid composition supply tube 1c can be arbitrarily selected as long as they can stably store and supply the liquid composition 5. The material constituting the liquid composition storage container 1b and the liquid composition supply tube 1c preferably has a light blocking property in the relatively short wavelength region of ultraviolet light and visible light. This prevents the liquid composition 5 from being polymerized by external light. If necessary, as shown in FIG. 3, it is also possible to provide a plurality of liquid composition application process sections 100-1 and form other materials at desired positions.

[0018] ((Energy application process section 100-2)) As shown in Figs. 2 and 3, the energy application process unit 100-2 has an energy application device which is an example of a first irradiation means for polymerizing a polymerizable compound by applying active energy rays such as heat or light to the liquid composition. As described above, energy can be applied by either heat or light. However, it is preferable to apply energy by light from the viewpoint of energy application efficiency. High energy application efficiency allows the polymerizable compound contained in the porous insulating film forming layer to be polymerized immediately, making it possible to form a porous layer with low fluidity and high film thickness uniformity. The energy application device applies energy to the porous film forming layer formed by the liquid composition application process unit 100-1 to form a porous insulating layer.

[0019] When the energy applying device is a light irradiation device 2a, it is appropriately selected according to the absorption wavelength of the photopolymerization initiator contained in the porous film forming layer, and is not particularly limited as long as it can initiate and advance the polymerization of the compound in the liquid composition layer, and examples thereof include ultraviolet light sources such as high pressure mercury lamps, metal halide lamps, hot cathode tubes, cold cathode tubes, and LEDs. However, since light with a shorter wavelength generally tends to reach deeper parts, it is preferable to select a light source according to the thickness of the porous film to be formed.

[0020] The energy application process section 100-2 may also have a polymerization inert gas circulation device 2b. The polymerization inert gas circulation device 2b reduces the concentration of polymerization active oxygen contained in the atmosphere, and allows the polymerization reaction of the polymerizable compound near the surface of the porous film formation layer to proceed without being inhibited. The polymerization inert gas used in the polymerization inert gas circulation device 2b is not particularly limited as long as it satisfies the above-mentioned functions, and examples thereof include nitrogen, carbon dioxide, and argon. In addition, the flow rate of the polymerization inert gas is preferably less than 20% (an environment with a lower oxygen concentration than the atmosphere), more preferably 0% to 15%, and even more preferably 0% to 5% in consideration of the effective inhibition reduction effect, and the polymerization inert gas circulation device 2b is preferably provided with a temperature control means capable of adjusting the temperature in order to realize stable polymerization progress conditions.

[0021] ((Drying process section 100-3)) The drying process section 100-3 has a heating device 3a capable of heating, which is an example of a drying means. The drying process section 100-3 heats and dries the solvent remaining in the formed active material formation layer and porous film formation layer using the heating device 3a to remove it. The drying process section 100-3 may perform the solvent drying process under reduced pressure. The drying process section 100-3 may heat and dry the photopolymerization initiator remaining in the porous insulating layer using the heating device 3a to remove it. The heating device 3a is not particularly limited as long as it satisfies the above functions, and examples of the heating device include an IR heater and a hot air heater. The heating temperature and heating time can be appropriately selected depending on the boiling point of the solvent contained in the porous insulating layer and the thickness of the formed film.

[0022] (Electrode cutting section 200) 1 has a function of cutting the electrode, which is continuously transported by being unwound from a rolled state, into a desired size. For example, a cutting mechanism using a blade, a punching mechanism using a Thomson blade or Pinnacle blade (registered trademark), a laser processing device, etc. can be used as the electrode cutting unit 200. However, the electrode cutting unit 200 is not limited to these.

[0023] (Laminated portion 300) The laminated section 300 will be described with reference to Figs. 4 to 8. Fig. 4 is a schematic diagram showing a first example of the laminated section 300. Fig. 4(a) is a cross-sectional view. Fig. 4(b) is a perspective view. Fig. 5 is a top view showing a schematic example of the shape of the alignment section 7.

[0024] As shown in FIG. 4, the stacking unit 300 has a stage 14 on which electrodes are stacked, a transport unit 300-2 that transports the electrodes to the stage 14, and an alignment unit 7 that aligns the electrodes on the stacking surface 140. The "electrodes on the stacking surface 140" includes electrodes that are on the stacking surface 140 and directly disposed on the stacking surface, and electrodes that are on the stacking surface 140 and disposed on electrodes stacked on the stacking surface. The stacking unit 300 stacks a plurality of electrodes including a first electrode 4 and a second electrode 15. In the terminology of this specification, when the first electrode 4 and the second electrode 15 are not distinguished from each other, they are simply referred to as "electrodes."

[0025] In this embodiment, the end of the electrode contacts the alignment unit 7 after the electrode is separated from the transport unit 300-2. In the example shown in FIG. 4, the end 4a of the first electrode 4 and the end 15a of the second electrode 15 each contact the alignment unit 7 after being separated from the transport unit 300-2. "After being separated from the transport unit 300-2" specifically means after each of the first electrode 4 and the second electrode 15 is transported by the transport unit 300-2 and separated from the transport unit 300-2 to be placed on the stage 14. In FIG. 4(b), 8 indicates a current collector of the first electrode 4, 10 indicates a porous insulating layer, 11 indicates a current collector of the second electrode 15, and 12 indicates an active material of the second electrode 15. In this specification and the claims, the end of the electrode refers to the side surface of the electrode substrate, or a functional layer such as an electrode composite layer or an insulating layer that is laminated on the electrode substrate and adheres to the electrode substrate, which faces a surface parallel to the electrode plane, or a functional layer such as an insulating layer adhered to the side surface of the electrode substrate that faces a surface parallel to the electrode plane, i.e., the end of the electrode substrate and the functional layer adhered to the electrode substrate, and does not include, for example, the end of a bag-shaped separator that is not adhered to the electrode substrate as described in Prior Art Document 1. In this embodiment, the end of the electrode that is in close contact with the electrode base, which has a relatively high rigidity, comes into contact with the alignment portion 7, so that the occurrence of bending or folding of the electrode can be suppressed.

[0026] In this embodiment, after the electrode is separated from the transport unit 300-2, an end of the electrode comes into contact with the alignment unit 7, thereby adjusting, i.e. aligning, the position of the electrode on the stage 14. When multiple electrodes are stacked on the stage 14, the positions of each of the multiple electrodes on the stage 14 are aligned. This makes it possible to provide a technology that can reduce misalignment of the stacked electrodes.

[0027] The stacking unit 300 may have a sensor unit 300-6, a control unit 300-7, an electrode storage unit 300-1, a friction reduction unit 300-8, and the like. The sensor unit 300-6 detects that the electrodes are placed on the stage 14. The control unit 300-7 controls the operation of the alignment unit 7 based on at least one of the transport state by the transport unit 300-2 and the detection result by the sensor unit 300-6. For example, the control unit 300-7 can receive information from the transport unit 300-2 and the sensor unit 300-6 and transmit a control signal to the movable unit 7-1. The electrode storage unit 300-1 is a member that stores the electrodes cut to a stacking size. The friction reduction unit 300-8 reduces the frictional force generated between the electrodes and the electrodes after they are stacked on the stage.

[0028] ((Stage 14)) The stage 14 is a platform on which the electrodes are arranged and stacked. There are no particular limitations on the material or shape as long as the electrodes can be stacked. However, the stage 14 is preferably flat. By being flat, the stage 14 can maintain the shape of the electrodes when the electrodes are stacked by the transport unit 300-2 or when the electrodes are pressed downward by the movable unit 7-1.

[0029] The stage 14 may be movable in the vertical direction (Z direction) relative to the alignment unit 7. By being movable in the vertical direction relative to the alignment unit 7, the length of the alignment unit 7 protruding from the stage 14 can be adjusted, and the stacking conditions can be adjusted. For example, by reducing the height of the stage 14 by the thickness of the stacked electrodes every time an electrode is stacked, the electrodes can be placed on the stage 14 at a constant height by the transport unit 300-2. As a result, the electrode placement conditions can be kept constant. As a configuration for performing such an operation, for example, the stage 14 has an opening, and the alignment unit 7 is provided so as to penetrate the opening.

[0030] A plurality of stages 14 may be provided in the battery laminate manufacturing apparatus 1000. In this case, the plurality of stages 14 are preferably configured to be movable so that they can be replaced. Examples of this movement include rotational movement by an index table and translational movement by a conveyor.

[0031] ((Transport section 300-2)) The transport unit 300-2 has a function of transporting a plurality of electrodes onto the stage 14. The transport unit 300-2 can be realized by a belt conveyor, an arm equipped with a suction mechanism, or the like. The transport unit 300-2 can transport the electrodes to a predetermined position on the stage by having, for example, an arm equipped with a suction mechanism.

[0032] ((Alignment section 7)) In this embodiment, the alignment unit 7 is movable on the stage 14. When the alignment unit 7 moves on the stage 14 in any direction on the XY plane, the ends of the electrodes come into contact with the alignment unit 7. After the electrodes transported by the transport unit 300-2 are stacked on the stage 14, the alignment unit 7 comes into contact with the ends of the electrodes to align the electrodes. As long as the above function is realized, there are no limitations on the material or shape of the alignment unit 7.

[0033] 4(a) and 4(b), the alignment unit 7 includes four pillar members 71-74 on the stage 14, and driving units connected to each of the four pillar members 71-74. The four pillar members 71-74 are arranged one by one so as to be positioned around an electrode arranged on the stage 14. The driving units can move each of the four pillar members 71-74 toward and away from the center of the stage 14, i.e., move them back and forth on the XY plane, in response to a control signal from the control unit 300-7.

[0034] For example, the first electrode 4, after its end 4a is separated from the transport section 300-2, comes into contact with the alignment section 7 arranged around it and has its position adjusted, thereby being aligned within the upper surface of the stage 14 or within the upper surface of the second electrode 15. In addition, the second electrode 15, after its end 15a is separated from the transport section 300-2, comes into contact with at least two of the four pillar members 71 to 74 arranged around it and has its position adjusted, thereby being aligned within the upper surface of the first electrode 4.

[0035] Here, FIG. 5 shows the shape of one columnar member 71 of the four columnar members 71 to 74 in the alignment section 7 in a top view. As shown in FIG. 5, the shape of the alignment section 7 is preferably a shape corresponding to the contact portion of the first electrode 4 to be contacted. By having the alignment section 7 have such a shape, the pressing amount of the alignment section 7 is accurately converted to the pressing amount of the first electrode 4, and the alignment can be performed accurately. Note that, like the columnar member 71 shown in FIG. 5, the columnar members 72 to 74 are also preferably shaped to correspond to the contact portion of the first electrode 4. In addition, the contact object is not limited to the first electrode 4, but may be the second electrode 15, or may be a laminate of the first electrode 4 and the second electrode 15.

[0036] Furthermore, when stacking the electrodes, if the alignment section 7 is too high in the stacking direction, there is a concern that it may come into contact with the electrodes when stacking the electrodes. For this reason, it is preferable that the height of the alignment section 7 in the stacking direction is variable. Furthermore, when multiple electrodes are stacked to a predetermined height, it is preferable that the height of the alignment section 7 in the stacking direction is equal to or greater than the predetermined height. The height of the alignment section 7 in the stacking direction may be variable by moving the above-mentioned stage 14 in the vertical direction (Z direction) relative to the alignment section 7, or may be variable by having a movable configuration in which a part of the alignment section 7 is movable.

[0037] The alignment portion 7 may have various shapes, not limited to a columnar member. The alignment portion 7 may have a shape in which a part of it protrudes toward the electrode. The alignment portion 7 may have a columnar shape when stacked, and may be deformable so that a part of it protrudes toward the electrode at a predetermined timing. This protruding part may include a mechanism capable of pressing the stacked electrodes in the stacking direction. Such a mechanism may be a mechanism in which the protruding part moves in the stacking direction, or a mechanism in which the alignment portion 7 itself including the protruding part moves in the stacking direction.

[0038] ((Electrode storage section 300-1)) In Fig. 4, the electrode storage unit 300-1 has a function of storing electrodes cut to a stacking size. A plurality of electrode storage units 300-1 may be provided for each of a plurality of types of electrodes. Furthermore, when the first electrodes 4 and the second electrodes 15 are alternately stacked, one electrode storage unit 300-1 may be provided. When the manufacturing apparatus 1000 for a battery laminate has an electrode cutting unit 200, the electrodes cut by the electrode cutting unit 200 are stored in the electrode storage unit 300-1. The material and shape can be freely selected as long as the above function is realized.

[0039] ((Sensor unit 300-6)) The sensor unit 300-6 detects that an electrode has been placed on the stage 14. The stacking unit 300 can determine the timing for moving the alignment unit 7, etc., based on the detection result by the sensor unit 300-6. For the sensor unit 300-6, for example, a pressure sensor that detects pressure due to the weight of the electrodes stacked on the stage 14, a camera that captures images on the stage 14, etc. can be used. However, the sensor unit 300-6 is not limited to these.

[0040] ((Control unit 300-7)) The control unit 300-7 controls the operation of the alignment unit 7 based on at least one of the conveying state of the conveying unit 300-2 and the detection result of the sensor unit 300-6. For example, the control unit 300-7 inputs information from the conveying unit 300-2 and the sensor unit 300-6 and transmits a control signal to the alignment unit 7. The stacking unit 300 can control the movement operation of the alignment unit 7 by the control unit 300-7. The control signal may be an electrical signal or a physical signal.

[0041] The functions of the control unit 300-7 can be realized by one or more processing circuits. Here, the term "processing circuit" in this specification includes a processor programmed to execute each function by software, such as a processor implemented by an electronic circuit, and devices such as an ASIC (Application Specific Integrated Circuit), a DSP (Digital Signal Processor), an FPGA (Field Programmable Gate Array), and a conventional circuit module designed to execute each function described above.

[0042] For example, the control unit 300-7 moves the stage 14 or the alignment unit 7 according to the position of the transport unit 300-2 and information detected by the sensor unit 300-6 that the electrode has been placed on the stage 14. For example, the control unit 300-7 can move at least two of the four columnar members 71-74 in the alignment unit 7 to contact the ends of the electrodes before the placement of the electrodes on the stage 14 is completed.

[0043] ((Friction reduction section 300-8)) The friction reduction unit 300-8 reduces the frictional force generated between the electrodes after the electrodes are placed on the stage 14. The friction reduction unit 300-8 is, for example, a vibration mechanism that vibrates the stage 14. A piezoelectric element, a motor, or the like can be used as the vibration mechanism. Alternatively, the stage 14 may be vibrated by irradiating the stage 14 with ultrasonic waves.

[0044] For example, there is a concern that the electrodes or functional layers such as insulating layers may be damaged due to friction between the electrodes during alignment by contact between the electrode ends and the alignment unit 7. To prevent this, alignment can be performed by the alignment unit 7 while vibrating the electrodes by vibrating the stage 14.

[0045] The friction reduction unit 300-8 may be an injection mechanism that blows air between the stacked electrodes or between the stacked electrodes and the stage, in addition to the vibration mechanism. By performing alignment while blowing air between the electrodes using the injection mechanism, friction occurring between the electrodes during alignment can be reduced. When blowing air between the electrodes, if there is a difference in film thickness between the electrodes, it is preferable to blow air onto the side with the thicker film thickness. By blowing air onto the thicker side, damage such as bending of the electrode caused by blowing air can be reduced. It is also effective to change the material provided on the electrode surface to a member with low friction. For example, when a porous insulating layer is provided on the electrode, the entire porous skeleton is integrally connected, so that the surface member in which the material is less likely to slip off may be used as the friction reduction unit 300-8.

[0046] <Example of Operation of Stacking Unit 300> 6A and 6B are schematic diagrams showing an example of the operation of the stacking unit 300. Fig. 6(a) is a cross-sectional view, and Fig. 6(b) is a perspective view.

[0047] For example, the first electrodes 4 and the second electrodes 15 are alternately stacked on top of each other on a stage 14 provided in a horizontal direction (XY direction) perpendicular to the vertical direction. In this embodiment, the end 4a of the first electrode 4 and the end 15a of the second electrode 15 are brought into contact with each other and aligned by moving each of the four columnar members 71 to 74 arranged on the stage 14.

[0048] From the viewpoint of reducing damage to the electrodes, the pushing operation of the alignment unit 7 is preferably performed each time one electrode is finished being stacked on the stage 14. Moreover, from the viewpoint of increasing productivity, it is preferably performed after all of the multiple electrodes are finished being stacked on the stage 14.

[0049] 6, the ends of the four columnar members 71-74 in the alignment section 7 are in contact with each other during alignment. However, the ends of the four columnar members 71-74 may not be in contact with each other during alignment.

[0050] The timing and speed of movement of each of the four columnar members 71 to 74 can be appropriately controlled. The timing of contact between each of the four columnar members 71 to 74 and the electrode may be the same or different. Also, the speed of movement of each of the four columnar members 71 to 74 may be the same or different. From the viewpoint of productivity, it is preferable that the timing of contact between each of the four columnar members 71 to 74 and the electrode is the same, and that the speed of movement of each of the four columnar members 71 to 74 is the same. From the viewpoint of reducing damage to the electrode, it is preferable that the timing of contact between each of the four columnar members 71 to 74 and the electrode is different. Also, from the viewpoint of reducing damage to the electrode, it is preferable that the speed of movement of each of the four columnar members 71 to 74 at the time of contact is slower than the speed of movement at the start of movement. In addition, the moving speed of each of the four columnar members 71 to 74 just before contacting each other is preferably such that the electrode does not have inertia in the moving direction of each of the four columnar members 71 to 74 due to contact between the electrode and each of the four columnar members 71 to 74.

[0051] After the alignment by the alignment unit 7 is completed, each of the four columnar members 71 to 74 is separated from the electrode on which it is placed. The operation of the alignment unit 7 after the alignment is completed is preferably an operation that makes it easy to maintain the alignment state of the electrodes after the alignment is completed. For example, when each of the four columnar members 71 to 74 is separated from the electrode, each of the four columnar members 71 to 74 is vibrated by the friction reduction unit 300-8 described above. This allows each of the four columnar members 71 to 74 to be separated from the electrode while maintaining the alignment state of the electrodes.

[0052] From the viewpoint of increasing productivity, it is preferable that the timing at which each of the four columnar members 71 to 74 separates from the electrode is the same. From the viewpoint of reducing damage to the electrode and increasing productivity, it is preferable that the moving speed of each of the four columnar members 71 to 74 when separating them from the electrode is slow when each of the four columnar members 71 to 74 separates from the electrode, and is then increased.

[0053] <Another Example of the Stacked Section 300> Various modifications are possible to the laminated section 300. Below, other examples of the laminated section 300 will be described. Note that the same reference numerals are used to designate the same or substantially the same configurations as those in the examples already described, and redundant descriptions of the configurations and functions will be omitted as appropriate.

[0054] (Example 2) In the second example, the electrode can slide on stage 14 or on other electrodes stacked on stage 14, and the end of the electrode comes into contact with alignment section 7 by sliding on stage 14 or on other electrodes stacked on stage 14, which is different from the first example shown in FIGS. 4 to 6. Note that "slide" means to slide or to perform a sliding motion. "The electrode slides on stage 14" may be rephrased as "the electrode slides on stage 14."

[0055] Fig. 7 is a schematic diagram showing a second example of the stacking unit. Fig. 7(a) is a cross-sectional view, and Fig. 7(b) is a perspective view. The battery stack manufacturing apparatus according to the second example has a tilting mechanism 300-9 that tilts the stage 14. The electrodes can slide on the stage 14 due to the action of gravity caused by the tilting mechanism 300-9 tilting the stage 14.

[0056] The tilting mechanism 300-9 is a mechanism that tilts the upper surface of the stage 14 by vertically raising and lowering a part of the stage 14. However, as long as the tilting mechanism 300-9 can tilt the stage 14, it is not limited to a lifting mechanism, and a swinging mechanism or the like may be used. Further, when the stage 14 is tilted and arranged in advance, the manufacturing apparatus for the laminated body for a battery according to the second example does not necessarily have to have a tilting mechanism.

[0057] In FIG. 7, the first electrode 4 and the second electrode 15 are alternately stacked on the stage 14 arranged obliquely with respect to the horizontal direction. The first electrode 4 and the second electrode 15 are aligned by the ends 4a of the first electrode 4 and the ends 15a of the second electrode 15 each contacting the alignment portion 7 disposed on the stage 14.

[0058] In the present embodiment, assuming that the tilting angle of the stage 14 is θ, the static friction coefficient of the stage 14 is μ, and the dynamic friction coefficient of the stage is μ', the tilting angle θ of the stage 14 may satisfy either μ < tanθ or μ' < tanθ. By doing so, the electrodes stacked on the stage 14 slide on the stage 14 due to the action of gravity, so that the contact between the ends 4a and 15a and the alignment portion 7 is accurately performed, and the alignment accuracy is improved. The stage 14 may always be tilted. Further, after the lamination of the electrodes on the stage 14 is completed, the stage 14 may perform a tilting operation in response to a control signal from the control unit 300-7 based on the detection result of the sensor unit 300-6.

[0059] Further, when the electrode has a thick film portion and a thin film portion with different thicknesses, from the viewpoint of reducing damage to the electrode, it is preferable that the contact portion between the alignment portion 7 and the electrode includes the side where the thick film is located. In particular, it is preferable that any side of the current collector (lead-out wire) or the side not adjacent to the thick film portion of the current collector does not contact the alignment portion 7 during alignment.

[0060] From the viewpoint of reducing damage to the electrodes, the alignment operation by the alignment unit 7 is preferably performed each time stacking of one electrode on the stage 14 is completed. On the other hand, from the viewpoint of increasing productivity, the alignment operation is preferably performed after stacking of all of the multiple electrodes on the stage 14 is completed.

[0061] Furthermore, when alignment is performed by contacting multiple sides of the electrode with the alignment portion 7, all of the multiple sides that can be in contact may be in parallel contact with the alignment portion 7. Alternatively, some of the sides that can be in contact may be in contact with the alignment portion 7 at different times, or all of the sides that can be in contact may be in contact with the alignment portion 7 at different times. From the viewpoint of reducing damage to the electrode, it is preferable to contact the alignment portion 7 with the longer side first among the sides that can be in contact.

[0062] (Example 3) The third example differs from the first and second examples in that at least two alignment sections 7 are arranged on the stage 14, and the ends of the alignment sections 7 and the electrodes are in contact in at least two directions in a plane approximately parallel to the top surface of the stage 14.

[0063] 8 is a schematic diagram showing a third example of the stacked section 300. The alignment section 7 includes columnar members 76-78. The columnar members 76-78 are arranged on the stage 14 such that their respective longitudinal directions are approximately perpendicular to each other. The columnar members 76-78 correspond to at least two alignment sections 7.

[0064] The first electrode 4 and the second electrode 15 are alternately stacked on the stage 14 arranged at an angle to the horizontal direction. For example, when the end 4a of the first electrode 4 comes into contact with the columnar member 76, the alignment of the first electrode 4 in a direction substantially perpendicular to the longitudinal direction of the columnar member 76 is performed by moving the alignment unit in a plane substantially parallel to the upper surface of the stage 14. Then, when the end 4b of the first electrode 4 comes into contact with the columnar member 77 by the tilting mechanism, the alignment of the first electrode 4 in a direction substantially perpendicular to the longitudinal direction of the columnar member 77 is performed in a plane substantially parallel to the upper surface of the stage 14. The surface of the end 4a and the surface of the end 4b are substantially perpendicular to each other. The longitudinal direction of the columnar member 76 and the longitudinal direction of the columnar member 77 are also substantially perpendicular to each other.

[0065] The method of contacting the columnar members 76-78 with the first electrode 4 and the second electrode 15, respectively, and the operation of the alignment unit 7 after alignment is completed are almost the same as in the second example, so duplicated explanations will be omitted here. With this configuration, alignment can be performed without contacting the alignment unit with at least one side of the electrodes.

[0066] (Example 4) The fourth example differs from the first to third examples in that a part of the alignment portion 7 is deformable.

[0067] 9 is a schematic diagram showing a fourth example of the stacking unit 300. For example, a part of the alignment unit 7 is deformed from the state before the electrode is transported to the stage 14 by the transport unit 300-2. In addition, the part of the alignment unit 7 is deformed so that the cross-sectional area changes from the state before the deformation. By deforming the part of the alignment unit 7, it is possible to reduce the detachment of the electrode from the alignment unit 7 due to distortion or the like of the electrode when the electrode is stacked on the stage 14. In addition, it is possible to provide a technology that can reduce the floating of the stacked electrodes by pressing the upper surface of the stacked electrodes with the deformed part of the alignment unit 7.

[0068] For example, the alignment portion 7 includes a movable portion 7-1 and a non-movable portion 7-2. The alignment portion 7 can be deformed by the movable portion 7-1 being movable. The alignment portion 7 deforms between a state in which the movable portion 7-1 can be inserted into a positioning hole provided in the electrode and the non-movable portion 7-2 can be inserted into the positioning hole, and a state in which the movable portion 7-1 cannot be inserted into the positioning hole and the non-movable portion 7-2 can be inserted into the positioning hole. The shape and material of the alignment portion 7 are not important as long as they can achieve the above purpose.

[0069] The movable part 7-1 corresponds to a part of the alignment part 7. The movable part 7-1 has a function of reducing detachment of the electrodes from the alignment part 7 when the electrodes are stacked on the stage 14, and the shape of the movable part 7-1 is not important. The movable part 7-1 can be realized by various deformations. There is also no particular limitation on the deformation means.

[0070] The non-movable part 7-2 has a function of holding the stacked electrodes when the electrodes are stacked on the stage 14, and the shape is not important. The shape of the side surface may be a straight shape, a tapered shape, a widened shape, a zigzag shape having repeated unevenness, a wavy shape, or the like. Among these, a straight shape is preferable from the viewpoint of suppressing the occurrence of misalignment of the electrodes after stacking. Furthermore, in the case of a shape having repeated unevenness, it is preferable that one period approximately matches the period of the positive and negative electrodes of the electrodes.

[0071] In Fig. 9, alignment portion 7a1 shows a state before deformation, and alignment portion 7b1 shows a state after deformation. In the example shown in Fig. 9, movable portion 7-1 includes a plurality of claws that can be opened and closed, and a drive unit that drives the plurality of claws. Movable portion 7-1 can open and close the plurality of claws by the drive unit in response to a control signal from control unit 300-7. As shown in Fig. 9, in movable portion 7-1, the plurality of claws are in a closed state before deformation, and the plurality of claws are in an open state after deformation.

[0072] For example, the electrode is provided with a positioning hole in advance. When the multiple claws of the movable part 7-1 are closed, the movable part 7-1 can be inserted into the positioning hole of the electrode. The electrodes are stacked on the stage 14 so that the movable part 7-1 can be inserted into the positioning hole, and the electrodes are aligned after stacking. After the alignment is completed, the multiple claws of the movable part 7-1 open. The height of the multiple claws of the movable part 7-1 in the open state is adjusted in advance to a height that allows the uppermost surface of the electrodes stacked on the stage to be pressed. Therefore, by opening the multiple claws of the movable part 7-1, the multiple claws can press the uppermost surface of the stacked electrodes.

[0073] The movable part 7-1 has multiple claws that press the multiple electrodes to prevent the multiple electrodes from coming off the non-movable part 7-2, and can fix the multiple electrodes on the stage 14. When removing the multiple electrodes from the electrode storage part 300-1, the alignment part 7 closes the multiple claws of the movable part 7-1.

[0074] <Method of manufacturing battery components> The manufacturing method of the battery member according to this embodiment will be described in detail. In this embodiment, the manufacturing apparatus 1000 for the battery laminate transports and places the electrodes on the stage 14 on which the electrodes are laminated by the transport section 300-2, and aligns the electrodes by the alignment section 7 arranged on the stage 14. The end of the electrode comes into contact with the alignment section 7 after the electrode is separated from the transport section 300-2. Furthermore, the manufacturing method for the battery laminate according to this embodiment may include an insulating layer forming step and an electrode cutting step as necessary, as shown in FIG. 1.

[0075] (Transportation process) The electrode transport step is a step of transporting a first electrode and a second electrode, at least one of which is provided with an insulating layer, that form a battery stack onto a stage. There is no limitation on the method for realizing the transport step as long as it can achieve the above-mentioned contents.

[0076] (Lamination process) The stacking process is a process in which the first electrode and the second electrode, at least one of which is provided with an insulating layer, are stacked after the transporting process to form a stack for a battery. In the above process, the first electrode and the second electrode capable of electrochemically reacting with each other are alternately stacked to form a stack that functions as a battery.

[0077] (Alignment process) The alignment step is a step of adjusting and fixing the position of the electrode to be placed on the stage 14. This is achieved by bringing the end of the electrode into contact with the alignment unit 7 after the electrode is separated from the transport unit 300-2. In order to manufacture a battery stack of good quality, it is important to stack the first electrode and the second electrode as designed without any misalignment. If any misalignment occurs, it will cause problems in the characteristics of the battery stack, such as a decrease in the capacity of the battery stack.

[0078] In this embodiment, in order to reduce the misalignment, when the first electrodes and the second electrodes are alternately stacked or after stacking, the ends of the electrodes are brought into contact with the alignment unit 7 arranged on the stage 14 to perform alignment. This alignment is possible because the insulating layer is closely attached to the battery stack and integrated, which allows the battery stack and the insulating layer to be aligned simultaneously. When a film separator used in the battery stack is used, even if the ends of the film separator are brought into contact with the alignment unit, it may be difficult to perform alignment because the film separator is flexible. In addition, when the ends of the electrodes are brought into contact with the alignment unit, the electrodes can be aligned, but the film separator placed on the electrodes may slip, making it difficult to align the film separator. For this reason, the porous insulating layer used in the battery stack according to this embodiment is a member that allows accurate alignment because the electrodes and the insulating layer are integrated and slippage does not occur between the electrodes and the insulating layer.

[0079] (Cutting process) The cutting process is a process in which the electrode, which is continuously transported by a roll, is cut into a desired size.

[0080] (Insulation layer formation process) The insulating layer forming step is a step of forming an insulating layer consisting of at least one of an organic layer and an inorganic layer on a substrate, which is a first electrode. As shown in Figures 2 to 3, the porous insulating layer forming step by the insulating layer forming unit 100 includes a liquid applying step of applying a liquid composition to the first electrode to form a liquid composition layer, and may include a step of irradiating the liquid composition with active energy rays and a removal step of removing a solvent contained in the liquid composition, etc., as necessary.

[0081] (Liquid composition application step) The liquid composition application step is a step of applying a liquid composition having a polymerizable compound and a liquid to at least a part of the electrode. The applied liquid composition preferably forms a liquid composition layer, which is a liquid film of the liquid composition, on the electrode. The liquid composition is applied by a dispenser, a die coater, lift-up coating, or the like. In addition, liquid ejection methods such as spraying and inkjet printing can also be used. In particular, when inkjet printing is used, it is preferable because it is possible to form a desired pattern with a desired film thickness while minimizing waste of materials and forming an insulating layer of any shape.

[0082] (Energy application process) The energy application step is a step of irradiating the liquid composition applied in the liquid composition application step with active energy rays. In particular, the energy application step to the liquid composition that causes polymerization-induced phase separation improves the porosity of the finally produced porous resin, thereby improving the uptake of fluids such as liquids or gases in the porous resin. Specifically, the liquid composition is irradiated with active energy rays to form a porous precursor having a porous structure that is the basis for forming a porous resin with a high porosity.

[0083] The active energy ray is not particularly limited as long as it can provide the energy required for the polymerization reaction of the polymerizable compound, and examples thereof include ultraviolet rays, electron beams, α rays, β rays, γ rays, and X-rays. Among these, ultraviolet rays are preferable. In addition, when a light source with particularly high energy is used, the polymerization reaction can be promoted without using a polymerization initiator. The reason why the liquid composition forms a porous precursor by the energy application step will be described below. As described above, when a porous resin is formed by polymerization-induced phase separation, the structure and properties of the porous resin change based on the polymerization conditions. For example, when a liquid composition is irradiated with active energy rays having a high irradiation intensity to form a porous resin under conditions in which polymerization of a polymerizable compound is promoted, polymerization tends to proceed before phase separation occurs sufficiently, making it difficult to manufacture a porous resin with a high porosity. Therefore, in order to form a porous resin with a high porosity, the irradiation intensity of the irradiated active energy rays is set not to be too high. Specifically, the irradiation intensity of the active energy rays is preferably 1 W / cm2 or less, more preferably less than 300 mW / cm2, and even more preferably 100 mW / cm2 or less. However, if the irradiation intensity of the active energy rays is too low, phase separation will proceed excessively, which will easily cause variation and coarsening of the porous structure, and further, the irradiation time will be longer, which will reduce productivity, so that the irradiation intensity is preferably 10 mW / cm2 or more, and more preferably 30 mW / cm2 or more.

[0084] (drying process) The drying step is a step of removing the dispersion medium or liquid from the liquid composition. The method of removing the dispersion medium or liquid is not particularly limited, and for example, a method of removing the dispersion medium or liquid by heating can be mentioned. In this case, heating under reduced pressure is preferable because it can further promote the removal of the dispersion medium or liquid and suppress the remaining dispersion medium or liquid in the formed active material layer and porous insulating layer.

[0085] <Laminate for batteries> The laminate for a battery according to the present embodiment will be described with reference to Figs. 10 to 15. Figs. 10 to 14 are schematic perspective views showing a first example of a battery electrode according to the embodiment. Fig. 11 is a schematic cross-sectional view showing a first example of a battery electrode according to the embodiment. Fig. 12 is a schematic perspective view showing a second example of a battery electrode according to the embodiment. Fig. 13 is a schematic cross-sectional view showing a second example of a battery electrode according to the embodiment. Fig. 14 is a schematic cross-sectional view showing a third example of a battery electrode according to the embodiment. Fig. 15 is a diagram showing an example of a porous insulating layer according to the embodiment. Fig. 15(a) is a plan view, and Fig. 15(b) is a cross-sectional view. In Figs. 10 to 15, 8 indicates a current collector of the first electrode. 9 indicates an active material of the first electrode. 10 indicates a porous insulating layer. 10x indicates voids. 13 indicates an insulating layer protection layer.

[0086] The battery laminate according to this embodiment is an electrode laminate in which first and second electrodes are alternately laminated, and when the first electrode is a negative electrode, the second electrode refers to a positive electrode, and when the first electrode is a positive electrode, the second electrode refers to a negative electrode. In addition, the electrode substrates of the first and second electrodes must be removed so as not to overlap, and there is no restriction on the method of removal.

[0087] (electrode) In the case of electrodes, the negative electrode and the positive electrode are collectively referred to as electrodes, the negative electrode substrate and the positive electrode substrate are collectively referred to as electrode substrates, and the negative electrode mixture layer and the positive electrode mixture layer are collectively referred to as electrode mixture layers. In addition, if the first electrode is a negative electrode, the second electrode refers to a positive electrode, and if the first electrode is a positive electrode, the second electrode refers to a negative electrode.

[0088] (electrode base) The electrode substrate for the negative electrode and the electrode substrate for the positive electrode are not particularly limited as long as they are flat and conductive. In general, aluminum foil, copper foil, stainless steel foil, titanium foil, and etched foils obtained by etching these foils to form fine holes, which are suitable for use in secondary batteries and capacitors, which are storage elements, and especially lithium ion secondary batteries, can be used. Carbon paper used in power generation elements such as fuel cells, fibrous electrodes that are nonwoven or woven and flat, and the above-mentioned perforated electrode substrates having fine holes can also be used. In addition, in the case of solar cells, in addition to the above, a transparent semiconductor thin film such as an indium-titanium oxide or zinc oxide can be formed on a flat substrate such as glass or plastic, or a conductive electrode film can be thinly evaporated on the substrate.

[0089] (electrode mixture layer) The negative electrode mixture layer and the positive electrode mixture layer are not particularly limited and can be appropriately selected according to the purpose. For example, they contain at least an active material (negative electrode active material or positive electrode active material), and may contain, as necessary, a binder (binding agent), a thickener, a conductive agent, a dispersant, a nonaqueous electrolyte, a solid electrolyte, a gel electrolyte, or one or more monomers that become a gel electrolyte through a polymerization process. The negative electrode mixture layer and the positive electrode mixture layer are formed by dispersing a powdered active material or a catalyst composition in a liquid, applying the liquid on an electrode substrate, fixing it, and drying it. Usually, printing using a spray, a dispenser, a die coater, or a pull-up coating is used, and the layer is formed by drying after application. The negative electrode active material is not particularly limited as long as it is a material that can reversibly occlude and release alkali metal ions. Typically, a carbon material containing graphite having a graphite-type crystal structure can be used as the negative electrode active material. Examples of such carbon materials include natural graphite, spherical or fibrous artificial graphite, non-graphitizable carbon (hard carbon), and graphitizable carbon (soft carbon). Examples of materials other than carbon materials include lithium titanate. In addition, from the viewpoint of increasing the energy density of lithium ion batteries, high-capacity materials such as silicon, tin, silicon alloys, tin alloys, silicon oxide, silicon nitride, and tin oxide can also be suitably used as negative electrode active materials.

[0090] As the active material in the nickel-metal hydride battery, the hydrogen storage alloy may be exemplified by AB2-based or A2B-based hydrogen storage alloys such as Zr-Ti-Mn-Fe-Ag-V-Al-W and Ti15Zr21V15Ni29Cr5Co5Fe1Mn8. The positive electrode active material is not particularly limited as long as it is a material capable of reversibly absorbing and releasing alkali metal ions. Typically, an alkali metal-containing transition metal compound can be used as the positive electrode active material. For example, the lithium-containing transition metal compound may be a composite oxide containing lithium and at least one element selected from the group consisting of cobalt, manganese, nickel, chromium, iron, and vanadium.

[0091] Examples of the composite oxide include lithium-containing transition metal oxides such as lithium cobaltate, lithium nickelate, and lithium manganate, olivine-type lithium salts such as LiFePO4, chalcogen compounds such as titanium disulfide and molybdenum disulfide, and manganese dioxide. The lithium-containing transition metal oxide is a metal oxide containing lithium and a transition metal, or a metal oxide in which a part of the transition metal in the metal oxide is replaced by a different element. Examples of the different elements include Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, and among them, Mn, Al, Co, Ni, and Mg are preferred. The different elements may be one type or two or more types. These positive electrode active materials can be used alone or in combination of two or more types. Examples of the active materials in nickel-hydrogen batteries include nickel hydroxide. For the binder of the negative electrode or positive electrode, for example, PVDF, PTFE, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polyacrylic acid methyl ester, polyacrylic acid ethyl ester, polyacrylic acid hexyl ester, polymethacrylic acid, polymethacrylic acid methyl ester, polymethacrylic acid ethyl ester, polymethacrylic acid hexyl ester, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene butadiene rubber, carboxymethyl cellulose, etc. can be used.

[0092] In addition, a copolymer of two or more materials selected from tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene may be used. In addition, two or more materials selected from these may be mixed and used. Examples of the conductive agent contained in the electrode mixture layer include graphites such as natural graphite and artificial graphite, carbon blacks such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fibers and metal fibers, metal powders such as carbon fluoride and aluminum, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, phenylene derivatives, and organic conductive materials such as graphene derivatives are used.

[0093] In general, the active material in a fuel cell is a catalyst for a cathode electrode or an anode electrode, in which metal particles such as platinum, ruthenium, or a platinum alloy are supported on a catalyst carrier such as carbon. To support catalyst particles on the surface of a catalyst carrier, for example, the catalyst carrier is suspended in water, and a precursor of the catalyst particle (for example, chloroplatinic acid, dinitrodiamino platinum, platinic chloride, platinous chloride, bisacetylacetonato platinum, dichlorodiammine platinum, dichlorotetramine platinum, platinic sulfate chlororuthenic acid, chloroiridic acid, chlororhodium acid, ferric chloride, cobalt chloride, chromium chloride, gold chloride, silver nitrate, rhodium nitrate, palladium chloride, nickel nitrate, iron sulfate, copper chloride, or other alloy components) is added, dissolved in the suspension, and an alkali is added to generate a hydroxide of the metal and obtain a catalyst carrier supported on the surface of the catalyst carrier. Such a catalyst carrier is applied to an electrode substrate and reduced under a hydrogen atmosphere, etc., to obtain an electrode mixture layer with catalyst particles (active material) applied to the surface.

[0094] In the case of solar cells and the like, examples of the active material include tungsten oxide powder, titanium oxide powder, and oxide semiconductor layers such as SnO2, ZnO, ZrO2, Nb2O5, CeO2, SiO2, and Al2O3. The semiconductor layer supports a dye, and examples of such dyes include compounds such as ruthenium-tris type transition metal complexes, ruthenium-bis type transition metal complexes, osmium-tris type transition metal complexes, osmium-bis type transition metal complexes, ruthenium-cis-diaqua-bipyridyl complexes, phthalocyanines and porphyrins, and organic-inorganic perovskite crystals.

[0095] (insulating layer) The insulating layer is a member that separates the positive electrode and the negative electrode and ensures ionic conductivity between the positive electrode and the negative electrode. The thickness of the insulating layer formed is not particularly limited as long as the insulation between the positive electrode and the negative electrode is maintained, but is preferably 1 μm to 50 μm, and particularly preferably 5 μm to 20 μm. If the thickness is thinner than the above, it is difficult to maintain good insulation between the positive electrode and the negative electrode. Also, if the thickness is thicker than the above, it is difficult to ensure good ionic conductivity. Also, the size of the pores in the obtained insulating layer is not particularly limited as long as it has ionic conductivity, but is preferably 0.01 μm to 10 μm from the viewpoint of the permeability of the electrolyte. Also, the porosity of the porous resin is preferably 30% or more, and more preferably 50% or more. Also, by forming the insulating layer from a material having a melting point or Tg, the insulating layers located above and below the stack can be heat-bonded after stacking, and the electrode position deviation after the stack is formed can be suppressed.

[0096] (liquid composition) The liquid composition is a liquid to be applied to form an insulating layer, and contains an organic and / or inorganic compound, a solvent or a dispersion liquid, etc. The organic and / or inorganic compound, and the solvent or the dispersion liquid can be appropriately selected as necessary, so long as the organic layer and / or the inorganic layer finally formed has insulating properties.

[0097] For example, examples of inorganic materials having insulating properties include metal oxides, metal nitrides, and other metal particles. Examples of metal oxides include Al2O3 (alumina), TiO2, BaTiO3, and ZrO2. Examples of metal nitrides include aluminum nitride and silicon nitride. Examples of other metal particles include poorly soluble ion crystal particles such as aluminum fluoride, calcium fluoride, barium fluoride, and barium sulfate, or mineral resource-derived substances such as boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, and bentonite, or their artificial products. Examples of inorganic materials having insulating properties include glass ceramic powder. Examples of glass ceramic powder include crystallized glass ceramics using ZnO-MgO-Al2O3-SiO2-based crystallized glass, and non-glass ceramics using BaO-Al2O3-SiO2-based ceramic powders and Al2O3-CaO-SiO2-MgO-B2O3-based ceramic powders. Furthermore, as the solid electrolyte, a ceramic solid electrolyte such as an oxide or a sulfide can be used.

[0098] The oxides include LISICON-type oxides such as γ-Li3PO4, Li3BO4, 0.75Li4GeO4-0.25Li2ZnGeO4 solid solution, Li4SiO4-Zn2SiO4 solid solution, Li4GeO4-Li3VO4 solid solution, and NASICON-type oxides such as Li 1.3 Al 0.3 Ti 1.7 (PO4)3 or Li 17a l 0.6 Ge 0.8 Ti 0.6 (PO4)3, (Li,La)TiO3 with a perovskite structure, and La5Li3Nb2O, a garnet-type oxide 12 , Li5La3TaO 12 , or Li7La3Zr2O 12 Examples include:

[0099] Sulfides include Li4GeS4-Li3PS4 solid solution, Li4SiS4-Li3PS4 solid solution, Li3PS4-Li2S solid solution, Li2S-P2S5 solid solution, Li2S-SiS2, Li10 GeP2S 12 , Argyrodite type Li6PS5X (X = Cl, Br, I), or L7P3S 11 Examples include crystals.

[0100] (Ceramic solid electrolyte for sodium ion secondary batteries) As for oxides, NASICON type Na 1+x Zr2Si x P 3-x O 12 (0≦x≦1), or β-alumina type Na2O-11Al2O3. Sulfides include Na2S-P2S5, Na3PS4, Na3SbS4, Na2S-SiS2, or Na2S-GeS2. Selenides include Na3PSe4. These may be used as composite electrolytes with polymers. The particle size of these inorganic materials is preferably 10 μm or less, more preferably 3 μm or less.

[0101] The above inorganic material is dispersed in a liquid to obtain a liquid composition for forming an inorganic layer. The liquid is selected from liquids suitable for the inorganic material to be dispersed. When dispersing the above inorganic material in a liquid, a binder material is added. The binder material has a function of adhering between fine particles of the inorganic material so that the inorganic material is held as an insulating layer. As the binder material, an acrylic resin, a styrene butadiene resin, a polyvinylidene fluoride resin, or the like can be used. When preparing the ink for preparing the inorganic layer, the ink may be dispersed using a homogenizer. As the homogenizer, a high-speed rotation shear stirring method, a high-pressure injection dispersion method, an ultrasonic dispersion method, a medium stirring mill method, or the like can be used. When preparing the ink for preparing the inorganic layer, additives such as a dispersing agent and a surfactant may be used as necessary. As the dispersing agent and the surfactant, Megafac (DIC Corporation), Marialim (NOF Corporation), S-Ream (NOF Corporation), Solsperse (Lubrizol), Polyflow (Kyoeisha Chemical Co., Ltd.), or the like can be used. As other additives, thickening agents such as propylene glycol and carboxymethyl cellulose can be used to adjust the viscosity.

[0102] Furthermore, a resin can be used as at least one of the organic and inorganic materials having insulating properties. To form the resin, a liquid composition for preparing a resin layer is used, which is prepared by dissolving or dispersing at least one of the resin and the precursor of the resin (at least one of the resin and the precursor of the resin) in a liquid. The liquid is selected from liquids suitable for the resin to be dissolved or dispersed. Specifically, water, a hydrocarbon liquid, an alcohol liquid, a ketone liquid, an ester liquid, and an ether liquid can be used. As such a resin and a precursor of the resin, a resin or an oligomer having a structure crosslinkable by ionizing radiation or infrared rays (heat) in the molecule is preferably dissolved in a liquid. Preferred examples of such resins and precursors of said resins include low molecular weight oligomer precursors of polyimide resins, polyester resins, polyamide resins, polyolefin resins, and acrylic resins, and those modified with, for example, a hydrocarbon group having an aliphatic unsaturated bond in a portion thereof. For example, acrylic copolymers having unsaturated bonds such as allyl groups, allyloxy groups, acryloyl groups, butenyl groups, cinnamyl groups, cinnamoyl groups, crotomyl groups, cyclohexadenyl groups, isopropenyl groups, methacryloyl groups, pentenyl groups, propenyl groups, styryl groups, vinyl groups, and butadiene groups in a portion of the side chain thereof are preferred.

[0103] Furthermore, for polybutylene terephthalate, polyethylene terephthalate, polyacrylonitrile, polyvinylidene fluoride, polyether ketone, polyethylene naphthalate, polysulfone, polyimide, polyester, polypropylene, polyoxymethylene, polyamide, polyvinylpyrrolidone, and cellulose, etc., by using relatively low molecular weight dispersion precursors or cellulose nanofibers with a molecular weight of 10,000 or less and heating them with ionizing radiation or infrared rays, the insolubility and crosslinking properties after fixing can be increased.

[0104] Furthermore, these precursors may contain up to about 30 parts by weight of an azide compound in order to enhance crosslinking. For example, 3.3'-dichloro-4.4'-diazidodiphenylmethane, 4.4'-diazidodiphenyl ether, 4.4'-diazidodiphenyl disulfide, 4.4'-diazidodiphenyl sulfide, 4.4'-diazidodiphenyl sulfone, 4-azidochalcone, 4-azido-4'-hydroxychalcone, 4-azido-4'-methoxychalcone, 4-azido-4'-morpholinochalcone, 4-dimethylamino-4'-azidochalcone, 2.6-bis(4'-azidobenzal)-4-methylcyclohexanoate, 2.6-bis(4'-azidobenzal)-cyclohexanone, cinnamylidene-4-azidoacetophenone, 4-azidocinnamylideneacetophenone, 4-azido-4'-dimethylaminocinnamylideneacetophenone, cinnamylidene-4-azidocinnamylideneacetone, 2.6-bis(4'-azidocinnamylidene)-4-methylcyclohexanone, 2.6-bis(4'-azidocinnamylidene)-cyclohexanone, 1.4'-azidobenzylideneindene, 1.4'-azidobenzylideneindene 1.4'-azidobenzylidene-3-α-hydroxy-4"-azidobenzylindene, 9.4'-azidobenzylidenefluorene, 9.4'-azidocinnamylidenefluorene, 4.4'-diazidostilbene-2.2'-disulfonyl-N-(p-methoxyphenyl)amide, 4.4'-diazidostilbene-2.2'-disulfonyl-N-(p-hydroxyethylphenyl)amide, 4.4'-diazidostilbene-2.2'-disulfonyl-N-(p-hydroxy ...ethylphenyl)amide, 4.4'-diazidostilbene-2.2'-disulfonyl-N-(p-hydroxyphenyl)amide, Didostilbene-2.2'-disulfonylamide, 4.4'-diazidobenzophenone, 4.4'-diazidostilbene, 4.4'-diazidochalcone, 4.4'-diazidobenzalacetone, 6-azido-2-(4'-azidostyryl)benzimidazole, 3-azidobenzylideneaniline-N-oxyp~(4-azidobenzylideneamido)benzoic acid, 1.4-bis(3'-azidostyryl)benzene, 3.3'-diazidodiphenylsulfone, 4.4'-diazidodiphenylmethane, etc.

[0105] Among them, 2,6-bis-(4'azidobenzal)-4-methylcyclohexanone and the like can be particularly preferably used. The solvent in which these materials are dissolved is not particularly limited, but any solvent in which the above compounds can be dissolved and which has a boiling point and surface tension suitable for the subsequent coating and drying processes can be used alone or in combination.

[0106] When the resin layer formed of the resin has voids inside, it is preferable because it allows ions of electrolytes or the like to pass through and can provide a function as a separator and a function to prevent thermal runaway.

[0107] From the viewpoint of the permeability and liquid retention of the electrolyte, it is desirable to have not only ion permeability but also fine openings. It is more desirable to include a material such as a foaming agent in the resin, heat the resin after application, include a soluble salt such as an electrolyte, and after application, immerse the resin in an electrolyte solution to dissolve the salt, thereby forming openings and pores, thereby expressing ion permeability. Alternatively, a block-shaped molecular skeleton may be used to form specific phase separation or microphase separation after application, thereby forming fine openings, thereby expressing ion permeability in the same way. Alternatively, a volatile solvent may be included in the ink composition, so that solid-liquid phase separation may be caused by polymerization or the like following printing, and then fine mesh-like openings may be obtained by removing (drying) the solvent. In particular, a liquid composition that causes solid-liquid phase separation (hereinafter also referred to as "polymerization-induced phase separation") by polymerization is preferable because it can provide a porous resin structure with high ion permeability in a short time.

[0108] The resin may contain a resin and a non-aqueous electrolyte, an ionic liquid, a glyme, or an electrolyte salt as a gel electrolyte.

[0109] (Porous insulating layer) The porous insulating layer is a member that separates the positive electrode and the negative electrode and ensures ion conductivity between the positive electrode and the negative electrode, and has a co-continuous structure with a resin as a skeleton. The resin is preferably a crosslinked resin, and is a polymer of a polymerizable compound that can be polymerized by energy irradiation. Here, the "co-continuous structure" means a structure in which two or more substances each have a continuous structure and do not form an interface, and in this embodiment, it means a structure in which both the resin phase and the pore phase are three-dimensional branched network continuous phases. Such a structure can be formed, for example, by polymerizing the liquid composition described later by a polymerization-induced phase separation method.

[0110] The porous insulating layer has a bicontinuous structure with a three-dimensional branched network structure as a skeleton, which makes it possible to realize a porous insulating layer with high porosity and high strength. That is, as shown in Figures 3(a) and (b), the porous insulating layer 10 has a large number of pores 10x, and each pore 10x has connectivity with other pores 10x around it and spreads three-dimensionally.

[0111] The porous insulating layer has a co-continuous structure, and the pores are interconnected, so that the electrolyte can penetrate sufficiently and the movement of ions is not hindered. A method for confirming that the porous insulating layer has a co-continuous structure and that the pores are interconnected can be, for example, a method for observing an image of a cross section of the porous insulating layer using a scanning electron microscope (SEM) or the like to confirm that the pores are interconnected. Air permeability is one of the physical properties that can be obtained by interconnecting the pores.

[0112] (Image observation using a scanning electron microscope (SEM) and measurement of porosity) The porosity of the porous insulating layer is preferably 30% or more, more preferably 50% or more. Also, it is preferably 90% or less, more preferably 85% or less. When the porosity is 30% or more, the porous insulating layer is sufficiently permeated with liquids and gases, and functions such as substance separation and reaction field can be efficiently exhibited. When the porous insulating layer is used as an insulating layer in an electricity storage element, the permeability of the electrolyte and the permeability of ions are improved, and the reaction inside the electricity storage element proceeds efficiently. Also, when the porosity is 90% or less, the strength of the porous insulating layer is improved.

[0113] Specifically, the porosity can be determined by the following procedure. There is no particular limitation on the method for evaluating the porosity of the porous insulating layer, and the method can be appropriately selected depending on the purpose, and an example of such a method is to fill the porous insulating layer with unsaturated fatty acid (commercially available butter), apply osmium staining, cut out the internal cross-sectional structure with a focused ion beam (FIB), and measure the porosity with a scanning electron microscope (SEM).

[0114] (Air permeability) The air permeability of the porous insulating layer is preferably 1,000 sec / 100 mL or less, more preferably 500 sec / 100 mL or less, and even more preferably 300 sec / 100 mL or less. The air permeability is measured in accordance with JIS P8117, and can be measured, for example, using a Gurley densometer (manufactured by Toyo Seiki Seisakusho Co., Ltd.). As an example, it may be determined that the pores are interconnected when the air permeability is 1,000 sec / 100 mL or less.

[0115] The cross-sectional shape of the pores in the porous resin may be various shapes and sizes, such as a substantially circular shape, a substantially elliptical shape, a substantially polygonal shape, etc. Here, the size of the pores refers to the length of the longest part in the cross-sectional shape. The size of the pores can be obtained from a cross-sectional photograph taken with a scanning electron microscope (SEM).

[0116] The size of the pores in the porous resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01 μm or more and 10 μm or less from the viewpoint of liquid and gas permeability. When the pore size is 0.1 μm or more and 10 μm or less, the liquid and gas can be sufficiently infiltrated into the porous insulating layer, and functions such as material separation and reaction field can be efficiently exhibited. In addition, as described later, when the porous insulating layer is used as an insulating layer of an electric storage element, a pore size of 10 μm or less can prevent a short circuit between the positive electrode and the negative electrode caused by lithium dendrites generated inside the electric storage element, thereby improving safety.

[0117] The method for adjusting the pore size and porosity of the porous resin to fall within these ranges is not particularly limited, and examples thereof include a method of adjusting the content of the polymerizable compound in the liquid composition to fall within the above-mentioned range, a method of adjusting the content of the porogen in the liquid composition to fall within the above-mentioned range, and a method of adjusting the irradiation conditions of active energy rays.

[0118] The average thickness of the porous insulating layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1.0 μm to 50.0 μm, more preferably 5.0 μm to 20.0 μm. When the average thickness is 5.0 μm or more, short circuits due to unevenness of the active material are unlikely to occur, and when it is 20.0 μm or less, good battery characteristics can be obtained.

[0119] In this case, the thickness refers to the thickness of only the porous resin layer, and does not include the thickness of the layer including the porous resin layer and the substrate, for example, if the porous resin layer penetrates into the substrate.

[0120] (Liquid composition for forming porous insulating layer) The liquid composition for forming a porous insulating layer is a liquid applied to form a porous insulating layer, and contains a polymerizable compound and a liquid, and further contains other components such as a polymerization initiator as necessary. The liquid composition for forming a porous insulating layer forms a porous resin, and the light transmittance at a wavelength of 550 nm measured while stirring the liquid composition is 30% or more, and the increase rate of the haze value in a haze measurement element produced by polymerizing the liquid composition is 1.0% or more. The liquid composition for forming a porous insulating layer forms a porous structure. That is, a resin structure (also called a "porous resin" or "porous structure") having a porous structure with a resin skeleton is formed by polymerization and curing of the polymerizable compound in the liquid composition.

[0121] (polymerizable compound) The polymerizable compound forms a resin by polymerization, and forms a porous resin depending on the composition and characteristics of the liquid composition. The polymerizable compound is not particularly limited as long as it forms a polymer (resin) by polymerization, and a known polymerizable compound can be appropriately selected depending on the purpose, but it is preferable that the polymerizable compound has at least one radical polymerizable functional group.

[0122] Suitable examples of the polymerizable compound include radical polymerizable compounds such as monofunctional, bifunctional, trifunctional or higher functional radical polymerizable monomers and oligomers; functional monomers and oligomers having a functional group other than the polymerizable functional group. Among these, bifunctional or higher functional radical polymerizable compounds are preferred.

[0123] The polymerizable group of the polymerizable compound is preferably at least one of a (meth)acryloyl group and a vinyl group, and more preferably a (meth)acryloyl group.

[0124] The polymerizable compound is preferably polymerizable by energy irradiation, and more preferably polymerizable by heat or light.

[0125] The resin formed from the polymerizable compound is preferably a resin having a mesh-like structure formed by application of active energy rays (for example, by irradiation with light or heating), etc. Suitable examples thereof include acrylate resins, methacrylate resins, urethane acrylate resins, vinyl ester resins, unsaturated polyester resins, epoxy resins, oxetane resins, vinyl ether resins, and resins formed by ene-thiol reactions.

[0126] Among these, acrylate resins, methacrylate resins, and urethane acrylate resins, which are resins formed from polymerizable compounds having a (meth)acryloyl group, are more preferred because they can be easily used to form a structure by utilizing highly reactive radical polymerization, and from the viewpoint of productivity, vinyl ester resins, which are resins formed from polymerizable compounds having a vinyl group, are more preferred.

[0127] These may be used alone or in combination of two or more. When using two or more, the combination of polymerizable compounds is not particularly limited and can be appropriately selected according to the purpose, but for example, in order to impart flexibility, it is preferable to mix other resins with urethane acrylate resin as the main component. Note that a polymerizable compound having at least one of an acryloyl group and a methacryloyl group is referred to as a polymerizable compound having a (meth)acryloyl group.

[0128] The active energy ray is not particularly limited as long as it can provide the energy required for the polymerization reaction of the polymerizable compound in the liquid composition, and can be appropriately selected according to the purpose, and examples thereof include ultraviolet rays, electron beams, α rays, β rays, γ rays, and X-rays. Among these, ultraviolet rays are preferred. In particular, when a high-energy light source is used, the polymerization reaction can be promoted without using a polymerization initiator.

[0129] Examples of the monofunctional radical polymerizable compound include 2-(2-ethoxyethoxy)ethyl acrylate, methoxypolyethylene glycol monoacrylate, methoxypolyethylene glycol monomethacrylate, phenoxypolyethylene glycol acrylate, 2-acryloyloxyethyl succinate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, tetrahydrofurfuryl acrylate, 2-ethylhexyl carbitol acrylate, 3-methoxybutyl acrylate, benzyl acrylate, cyclohexyl acrylate, isoamyl acrylate, isobutyl acrylate, methoxytriethylene glycol acrylate, phenoxytetraethylene glycol acrylate, cetyl acrylate, isostearyl acrylate, stearyl acrylate, and styrene monomer. These may be used alone or in combination of two or more.

[0130] Examples of bifunctional radically polymerizable compounds include 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, neopentyl glycol diacrylate, EO-modified bisphenol A diacrylate, EO-modified bisphenol F diacrylate, neopentyl glycol diacrylate, tricyclodecane dimethanol diacrylate, etc. These may be used alone or in combination of two or more.

[0131] Examples of the radical polymerizable compound having three or more functionalities include trimethylolpropane triacrylate (TMPTA), trimethylolpropane trimethacrylate, EO-modified trimethylolpropane triacrylate, PO-modified trimethylolpropane triacrylate, caprolactone-modified trimethylolpropane triacrylate, HPA-modified trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate (PETTA), glycerol triacrylate, ECH-modified glycerol triacrylate, EO-modified glycerol triacrylate, PO-modified glycerol triacrylate, trimethylolpropane triacrylate, trimeth ... Examples of the acrylates include (acryloxyethyl) isocyanurate, dipentaerythritol hexaacrylate (DPHA), caprolactone-modified dipentaerythritol hexaacrylate, dipentaerythritol hydroxypentaacrylate, alkyl-modified dipentaerythritol pentaacrylate, alkyl-modified dipentaerythritol tetraacrylate, alkyl-modified dipentaerythritol triacrylate, dimethylolpropane tetraacrylate (DTMPTA), pentaerythritol ethoxy tetraacrylate, EO-modified phosphoric acid triacrylate, and 2,2,5,5-tetrahydroxymethylcyclopentanone tetraacrylate. These may be used alone or in combination of two or more.

[0132] The content of the polymerizable compound is preferably from 5.0 to 70.0% by mass, more preferably from 10.0 to 50.0% by mass, and even more preferably from 20.0 to 40.0% by mass, based on the total amount of the liquid composition.

[0133] When the content is 70.0% by mass or less, the size of the pores in the resulting porous body is not too small, such as a few nm or less, and the porous body has an appropriate porosity, which is preferable because it can suppress the tendency for liquids and gases to become less likely to penetrate. Also, when the content is 5.0% by mass or more, the three-dimensional network structure of the resin is sufficiently formed, a sufficient porous structure is obtained, and the strength of the resulting porous structure also tends to be improved, which is preferable.

[0134] (liquid) The liquid contains a porogen, and further contains other liquids other than the porogen as necessary. The porogen is a liquid that is compatible with the polymerizable compound, and becomes incompatible with the polymer (resin) (causes phase separation) in the process of polymerizing the polymerizable compound in the liquid composition. By containing a porogen in the liquid composition, a porous resin is formed when the polymerizable compound is polymerized. In addition, it is preferable that the liquid composition is capable of dissolving a compound (a polymerization initiator described later) that generates a radical or an acid by light or heat. The liquid or porogen may be used alone or in combination of two or more kinds. In this embodiment, the liquid does not have polymerizability.

[0135] The boiling point of one type of porogen alone or two or more types of porogen in combination is preferably 50°C to 250°C, more preferably 70°C to 200°C, and even more preferably 120°C to 190°C at normal pressure. By having a boiling point of 50°C or more, vaporization of the porogen at around room temperature is suppressed, making the liquid composition easy to handle and facilitating control of the porogen content in the liquid composition. In addition, by having a boiling point of 250°C or less, the time required for the process of removing the porogen after polymerization is shortened, improving the productivity of the porous resin. In addition, since the amount of porogen remaining inside the porous resin can be suppressed, the quality is improved when the porous resin is used as a functional layer such as a material separation layer that separates substances or a reaction layer as a reaction field.

[0136] Examples of the porogen include ethylene glycols such as diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisopropyl ether, and dipropylene glycol monomethyl ether; esters such as γ-butyrolactone and propylene carbonate; and amides such as N,N-dimethylacetamide. In addition, liquids with relatively large molecular weights such as methyl tetradecanoate, methyl decanoate, methyl myristate, and tetradecane can also be used. In addition, liquids such as acetone, 2-ethylhexanol, and 1-bromonaphthalene can also be used. Note that the above-mentioned liquids do not necessarily correspond to porogens.

[0137] As described above, a porogen is a liquid that is compatible with a polymerizable compound and is incompatible with (subjects to phase separation from) a polymerized product (resin) produced in the course of polymerization of the polymerizable compound in a liquid composition. In other words, whether or not a liquid corresponds to a porogen is determined by its relationship with the polymerizable compound and the polymerized product (resin formed by polymerization of the polymerizable compound).

[0138] In addition, since the liquid composition only needs to contain at least one type of porogen having the above-mentioned specific relationship with the polymerizable compound, the range of material selection when preparing the liquid composition is broadened, and the liquid composition can be easily designed. By broadening the range of material selection when preparing the liquid composition, the range of response is broadened when there are characteristics required for the liquid composition from a viewpoint other than the formation of a porous structure. For example, when the liquid composition is discharged by the inkjet method, the liquid composition is required to have discharge stability and the like from a viewpoint other than the formation of a porous structure, and the wide range of material selection makes it easy to design the liquid composition.

[0139] The content of the liquid or porogen is preferably from 30.0 to 95.0% by mass, more preferably from 50.0 to 90.0% by mass, and even more preferably from 60.0 to 80.0% by mass, based on the total amount of the liquid composition.

[0140] When the liquid or porogen content is 30.0% by mass or more, the size of the pores in the resulting porous body is not too small, such as a few nm or less, and the porous body has an appropriate porosity, which is preferable because it can suppress the tendency for liquid or gas to penetrate less easily. Also, when the liquid or porogen content is 95.0% by mass or less, the three-dimensional network structure of the resin is sufficiently formed, a porous structure is sufficiently obtained, and the strength of the resulting porous structure also tends to be improved, which is preferable.

[0141] As described above, the liquid composition is required to contain at least one type of porogen having the above-mentioned specific relationship with the polymerizable compound, and may additionally contain other liquids (liquids that are not porogens) that do not have the above-mentioned specific relationship with the polymerizable compound.

[0142] The content of other liquids is preferably 10.0% by mass or less, more preferably 5.0% by mass or less, still more preferably 1.0% by mass or less, and particularly preferably 0% by mass (not included), based on the total amount of the liquid composition.

[0143] The mass ratio of the polymerizable compound content to the porogen content in the liquid composition (polymerizable compound:porogen) is preferably from 1.0:0.4 to 1.0:19.0, more preferably from 1.0:1.0 to 1.0:9.0, and even more preferably from 1.0:1.5 to 1.0:4.0.

[0144] (Polymerization initiator) The liquid composition may contain other components such as a polymerization initiator. The polymerization initiator is a material capable of generating active species such as radicals and cations by energy such as light and heat, and initiating polymerization of a polymerizable compound. Examples of the polymerization initiator include known radical polymerization initiators, cationic polymerization initiators, and base generators. These may be used alone or in combination of two or more. Among these, a photoradical polymerization initiator is preferred.

[0145] The photoradical polymerization initiator is not particularly limited, and a known photoradical generator can be appropriately selected depending on the purpose. Examples of the photoradical polymerization initiator include Michler's ketone and benzophenone, known under the trade names Irgacure and Darocur, and acetophenone derivatives.

[0146] Specific examples of the compounds include α-hydroxy-acetophenone, α-aminoacetophenone, 4-aroyl-1,3-dioxolane, benzil ketal, 2,2-diethoxyacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, benzophenone, 2-chlorobenzophenone, pp'-dichlorobenzophenone, pp'-bisdiethylaminobenzophenone, Michler's ketone, benzil, benzoin, benzil dimethyl ketal, tetramethylthiuram monosulfide, thioxanthone, and 2-chlorothioxanthone. benzoin peroxide, di-tert-butyl peroxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, methyl benzoyl formate, benzoin isopropyl ether, benzoin methyl ether, benzoin ethyl ether, benzoin ether, benzoin isobutyl ether, benzoin n-butyl ether, benzoin Zoin n-propyl, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 1-hydroxy-cyclohexyl-phenyl-ketone, 2,2-dimethoxy-1,2-diphenylethan-1-one, bis(η5-2,4-cyclopentadiene-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-methyl-1[4-(methylthio) )phenyl]-2-morpholinopropan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Darocur 1173), bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one monoacylphosphine oxide, bisacylphosphine oxide; titanocene, fluorescene, anthraquinone, thioxanthone; xanthone, lophine dimer, trihalomethyl compounds;Examples include dihalomethyl compounds, active ester compounds, and organic boron compounds.

[0147] Furthermore, a photocrosslinking radical generator such as a bisazide compound may be simultaneously contained. When polymerization is performed by heat alone, a thermal polymerization initiator such as azobisisobutyronitrile (AIBN), which is a typical radical generator, can be used.

[0148] The content of the polymerization initiator is preferably from 0.05% by mass to 10.0% by mass, and more preferably from 0.5% by mass to 5.0% by mass, based on the total mass of the polymerizable compounds being 100.0% by mass, in terms of obtaining a sufficient curing rate.

[0149] The liquid composition may be a non-dispersed composition that does not contain a dispersion in the liquid composition, or a dispersed composition that contains a dispersion in the liquid composition, but is preferably a non-dispersed composition.

[0150] (Polymerization-induced phase separation) Porous resins are formed by polymerization-induced phase separation. Polymerization-induced phase separation refers to a state in which the polymerizable compound and porogen are compatible, but the polymer (resin) that is generated during the polymerization process of the polymerizable compound and the porogen are not compatible (phase separation occurs). Although there are other methods for obtaining porous bodies by phase separation, the polymerization-induced phase separation method can form a porous body with a network structure, which is expected to be highly resistant to chemicals and heat. In addition, compared to other methods, it has the advantage of a shorter process time and easier surface modification.

[0151] Next, a process for forming a porous resin using polymerization-induced phase separation by a liquid composition containing a polymerizable compound will be described. The polymerizable compound undergoes a polymerization reaction by light irradiation or the like to form a resin. During this process, the solubility of the porogen in the growing resin decreases, and phase separation occurs between the resin and the porogen. Finally, the resin forms a porous structure having a co-continuous structure due to the resin skeleton, with the porogen filling the pores. When this is dried, the porogen is removed, and a porous resin having a co-continuous structure of a three-dimensional network structure remains. Therefore, in order to form a porous resin with an appropriate porosity, the compatibility of the porogen with the polymerizable compound and the compatibility of the porogen with the resin formed by polymerization of the polymerizable compound are examined.

[0152] (light transmittance) The light transmittance at a wavelength of 550 nm measured while stirring the liquid composition is 30% or more. The compatibility between the porogen and the polymerizable compound can be determined by the light transmittance. When the light transmittance is 30% or more, it is determined that the liquid contains a porogen and the polymerizable compound and the porogen are in a compatible state, and when the light transmittance is less than 30%, it is determined that the polymerizable compound and the liquid are in an incompatible state.

[0153] Specifically, the light transmittance can be measured by the following method: First, the liquid composition is poured into a quartz cell, and while stirring with a stirrer at 300 rpm, the transmittance of the liquid composition at a wavelength of 550 nm (visible light) is measured under the following conditions. Quartz cell: Special microcell with screw cap (product name: M25-UV-2, manufactured by GL Sciences Inc.) ·Transmittance measurement device: Ocean Optics USB4000 Stirring speed: 300 rpm ·Measurement wavelength: 550nm Reference: Obtained by measuring the light transmittance at a wavelength of 550 nm when the quartz cell is filled with air (transmittance: 100%)

[0154] (Rate of increase in haze value) The increase rate of the haze value in a haze measuring element prepared by polymerizing the liquid composition is 1.0% or more. The compatibility of the porogen with the resin formed by polymerization of the polymerizable compound can be judged by the increase rate of the haze value.

[0155] When the increase in haze value is 1.0% or more, it is determined that the liquid contains porogen and the resin and the porogen are incompatible, and when it is less than 1.0%, it is determined that the resin and the liquid are compatible.

[0156] The haze value in the haze measuring element increases as the compatibility between the porogen and the resin formed by polymerization of the polymerizable compound decreases, and decreases as the compatibility increases. Also, the higher the haze value, the easier it is for the resin formed by polymerization of the polymerizable compound to form a porous structure.

[0157] Specifically, the rate of increase in haze value is the rate of increase in haze value before and after polymerization of a haze-measuring element having an average thickness of 100 μm produced by polymerizing the liquid composition, and can be measured by the following method.

[0158] - Fabrication of haze measurement element - First, resin particles as a gap agent are uniformly dispersed on a non-alkali glass substrate by spin coating. Then, the substrate coated with the gap agent is bonded to a non-alkali glass substrate not coated with the gap agent, with the surfaces coated with the gap agent sandwiched between them. Next, a liquid composition is filled between the bonded substrates by utilizing capillary action to prepare a "pre-UV haze measurement element". Next, the pre-UV haze measurement element is irradiated with UV light to harden the liquid composition. Finally, the periphery of the substrate is sealed with a sealant to prepare a "haze measurement element". The size of the gap agent (average particle diameter 100 μm) corresponds to the average thickness of the haze measurement element. The various conditions during preparation are shown below. Non-alkali glass substrate: Nippon Electric Glass, 40mm, t=0.7mm, OA-10G Gap agent: Sekisui Chemical Co., Ltd., resin microparticle Micropearl GS-L100, average particle size 100 μm Spin coating conditions: Dispersion drop amount 150 μL, rotation speed 1000 rpm, rotation time 30 s Filled liquid composition volume: 160μL UV irradiation conditions: UV-LED is used as the light source, light source wavelength 362Nm, irradiation intensity 30mW / cm2, irradiation time 20s Sealant: TB3035B (Three Bond)

[0159] - Haze value (cloudiness) measurement - Next, the haze value (cloudiness) is measured using the prepared haze measurement element before UV irradiation and the haze measurement element. The measured value in the haze measurement element before UV irradiation is set as a reference (haze value 0), and the increase rate of the measured value (haze value) in the haze measurement element relative to the measured value in the haze measurement element before UV irradiation is calculated.

[0160] The equipment used for the measurements is shown below. Haze measuring device: Haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.

[0161] (viscosity) From the viewpoint of workability when applying the liquid composition, the viscosity of the liquid composition at 25°C is preferably 1.0 mPa·s or more and 150.0 mPa·s or less, more preferably 1.0 mPa·s or more and 30.0 mPa·s or less, and particularly preferably 1.0 mPa·s or more and 25.0 mPa·s or less. When the viscosity of the liquid composition is 1.0 mPa·s or more and 30.0 mPa·s or less, good ejection properties can be obtained even when the liquid composition is applied to an inkjet method. Here, the viscosity can be measured using, for example, a viscometer (device name: RE-550L, manufactured by Toki Sangyo Co., Ltd.) or the like.

[0162] (Hansen Solubility Parameter (HSP)) The compatibility between the porogen and the polymerizable compound, and the compatibility between the porogen and the resin formed by polymerization of the polymerizable compound, can be predicted through Hansen Solubility Parameter (HSP).

[0163] Hansen Solubility Parameter (HSP) is a useful tool for predicting the compatibility of two substances, and is a parameter discovered by Charles M. Hansen. Hansen Solubility Parameter (HSP) is expressed by combining the following three parameters (δD, δP, and δH) derived experimentally and theoretically. The unit of Hansen Solubility Parameter (HSP) is MPa0.5 or (J / cm3)0.5. In this embodiment, (J / cm3)0.5 is used. · δD: Energy resulting from London dispersion forces. · δP: Energy resulting from dipole-dipole interactions. · δH: Energy derived from hydrogen bonding forces.

[0164] Hansen Solubility Parameter (HSP) is a vector quantity expressed as (δD, δP, δH) and is plotted in a three-dimensional space (Hansen space) with three parameters as coordinate axes. The Hansen Solubility Parameter (HSP) of commonly used substances is available from publicly known information sources such as databases, so the Hansen Solubility Parameter (HSP) of a desired substance can be obtained, for example, by referring to the database. For substances whose Hansen Solubility Parameter (HSP) is not registered in the database, the Hansen Solubility Parameter (HSP) can be calculated from the chemical structure of the substance or the Hansen Solubility Sphere method described below, for example, by using computer software such as Hansen Solubility Parameters in Practice (HSPiP). The Hansen Solubility Parameter (HSP) of a mixture containing two or more substances is calculated as the vector sum of the Hansen Solubility Parameter (HSP) of each substance multiplied by the volume ratio of each substance to the entire mixture. In this embodiment, the Hansen Solubility Parameter (HSP) of a liquid (porogen) obtained based on a known information source such as a database is referred to as the "Hansen Solubility Parameter of a liquid."

[0165] In addition, the relative energy difference (RED) based on the Hansen solubility parameters (HSP) of a solute and a solution is expressed by the following formula:

number

[0166] In the above formula, Ra indicates the interaction distance between the Hansen Solubility Parameter (HSP) of the solute and the Hansen Solubility Parameter (HSP) of the solution, and Ro indicates the interaction radius of the solute. The interaction distance (Ra) between Hansen Solubility Parameters (HSP) indicates the distance between two substances. The smaller the value, the closer the two substances are in the three-dimensional space (Hansen space), indicating a higher possibility of dissolving (being compatible) with each other.

[0167] Assuming that the Hansen Solubility Parameters (HSP) for two substances (solute A and solution B) are as follows, Ra can be calculated as follows: Highly Sensitive People A =(δD A , δP A , δH A ) Highly Sensitive People B =(δD B , δP B , δH B ) ·Ra=[4×(δD A -δD B ) 2 +(δP A -δP B ) 2 +(δH A -δH B ) 2 ] 1 / 2

[0168] Ro (the interaction radius of a solute) can be determined, for example, by the Hansen dissolved sphere method described below.

[0169] (Hansen dissolving ball method) First, prepare the substance for which Ro is to be obtained and several dozen types of evaluation liquids (liquids whose meaning is different from the above-mentioned "liquid (porogen)") whose Hansen solubility parameters (HSP) are known, and perform a compatibility test of the target substance with each evaluation liquid. In the compatibility test, the Hansen solubility parameters (HSP) of the evaluation liquids that showed compatibility and the Hansen solubility parameters (HSP) of the evaluation liquids that showed no compatibility are plotted on the Hansen space. Based on the plotted Hansen solubility parameters (HSP) of each evaluation liquid, create a virtual sphere (Hansen sphere) in the Hansen space that includes the Hansen solubility parameters (HSP) of the evaluation liquids that showed compatibility and does not include the Hansen solubility parameters (HSP) of the evaluation liquids that showed no compatibility. The radius of the Hansen sphere is the interaction radius R0 of the substance, and the center is the Hansen solubility parameter (HSP) of the substance. The evaluation criteria (criteria for determining whether or not compatibility exists) between the substance for which the interaction radius R0 and the Hansen solubility parameter (HSP) are to be calculated and the liquid for evaluation whose Hansen solubility parameter (HSP) is known are set by the evaluator himself / herself. The evaluation criteria in this embodiment will be described later.

[0170] -Hansen Solubility Parameter (HSP) and Interaction Radius of Polymerizable Compounds- The Hansen solubility parameter (HSP) of the polymerizable compound in this embodiment and the interaction radius of the polymerizable compound are determined by the Hansen dissolved ball method. As described above, the evaluation criteria for compatibility in the Hansen dissolved ball method are set by the evaluator himself, so the Hansen solubility parameter (HSP) of the polymerizable compound in this embodiment obtained by the following criteria is represented as the "Hansen solubility parameter C of the polymerizable compound", and the interaction radius of the polymerizable compound is represented as the "interaction radius D of the polymerizable compound". In other words, the "Hansen solubility parameter C of the polymerizable compound" and the "interaction radius D of the polymerizable compound" are obtained based on the Hansen solubility parameter of the liquid, which is obtained based on a publicly known information source such as a database, and are obtained based on the Hansen dissolved ball method including the evaluation criteria for compatibility set by the evaluator himself.

[0171] The Hansen solubility parameter C and the interaction radius D of the polymerizable compound are determined by evaluating the compatibility of the polymerizable compound with the evaluation liquid in accordance with the following [1-1] and the above-mentioned method for measuring light transmittance (based on "the light transmittance at a wavelength of 550 nm of the transmittance measurement composition, which is measured while stirring the transmittance measurement composition containing the polymerizable compound and the evaluation liquid").

[0172] [1-1] Preparation of composition for transmittance measurement First, prepare a polymerizable compound for which the Hansen Solubility Parameter (HSP) is to be calculated and several dozen types of evaluation liquids with known Hansen Solubility Parameter (HSP), and mix the polymerizable compound, each evaluation liquid, and polymerization initiator in the ratio shown below to prepare a composition for transmittance measurement. As several dozen types of evaluation liquids with known Hansen Solubility Parameter (HSP), the following 21 types of evaluation liquids are used.

[0173] ~Composition ratio for transmittance measurement~ Polymerizable compound for which Hansen Solubility Parameter (HSP) is to be calculated: 28.0% by mass Liquid for evaluation with known Hansen Solubility Parameters (HSP): 70.0% by mass Polymerization initiator (Irgacure 819, manufactured by BASF): 2.0% by mass

[0174] ~Evaluation liquid group (21 types)~ Ethanol, 2-propanol, mesitylene, dipropylene glycol monomethyl ether, N-methyl 2-pyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether, propylene carbonate, ethyl acetate, tetrahydrofuran, acetone, n-tetradecane, ethylene glycol, diethylene glycol monobutyl ether, diethylene glycol butyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone, 2-ethylhexanol, diisobutyl ketone, benzyl alcohol, 1-bromonaphthalene

[0175] -Hansen solubility parameter (HSP) and interaction radius of resin formed by polymerization of polymerizable compounds- The Hansen solubility parameter (HSP) of the resin formed by polymerization of the polymerizable compound and the interaction radius of the resin formed by polymerization of the polymerizable compound are determined by the Hansen solubility parameter (HSP) of the resin formed by polymerization of the polymerizable compound in this embodiment obtained by the following criteria is represented as "Hansen solubility parameter A of the resin", and the interaction radius of the resin formed by polymerization of the polymerizable compound is represented as "interaction radius B of the resin". In other words, "Hansen solubility parameter A of the resin" and "interaction radius B of the resin" are obtained based on the Hansen solubility parameter of the liquid, which is obtained based on a publicly known information source such as a database, and are obtained based on the Hansen solubility parameter of the resin including the evaluation criteria of compatibility set by the evaluator himself.

[0176] The Hansen solubility parameter A of the resin and the interaction radius B of the resin are determined by evaluating the compatibility of the resin with the evaluation liquid in accordance with the following [2-1] and the above-mentioned method for measuring the rate of increase in haze value (evaluation based on "the rate of increase in haze value (cloudiness) in a haze measurement element prepared using a haze measurement composition containing a polymerizable compound and an evaluation liquid").

[0177] [2-1] Preparation of composition for haze measurement First, prepare a precursor (polymerizable compound) of the resin for which the Hansen Solubility Parameter (HSP) is to be calculated, and several dozen types of evaluation liquids with known Hansen Solubility Parameter (HSP), and mix the polymerizable compound, each evaluation liquid, and polymerization initiator in the ratio shown below to prepare a composition for haze measurement. As several dozen types of evaluation liquids with known Hansen Solubility Parameter (HSP), the following 21 types of evaluation liquids are used.

[0178] ~Composition ratio for haze measurement~ Precursor of the resin for which you want to calculate the Hansen Solubility Parameter (HSP) (polymerizable compound): 28.0% by mass Liquid for evaluation with known Hansen Solubility Parameters (HSP): 70.0% by mass Polymerization initiator (Irgacure 819, manufactured by BASF): 2.0% by mass

[0179] ~Evaluation liquid group (21 types)~ Ethanol, 2-propanol, mesitylene, dipropylene glycol monomethyl ether, N-methyl 2-pyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether, propylene carbonate, ethyl acetate, tetrahydrofuran, acetone, n-tetradecane, ethylene glycol, diethylene glycol monobutyl ether, diethylene glycol butyl ether acetate, methyl ethyl ketone, methyl isobutyl ketone, 2-ethylhexanol, diisobutyl ketone, benzyl alcohol, 1-bromonaphthalene

[0180] -Relative Energy Difference (RED) based on Hansen Solubility Parameters (HSP) of resin and liquid (porogen)- As described above, the relative energy difference (RED) calculated based on the Hansen solubility parameter A of the resin formed by polymerization of the polymerizable compound, which is determined based on the rate of increase in the haze value (cloudiness) in a haze measurement element prepared using a composition for haze measurement containing a polymerizable compound and an evaluation liquid, the interaction radius B of the resin, and the Hansen solubility parameter of the porogen according to the following formula 1 is preferably 1.00 or more, more preferably 1.10 or more, even more preferably 1.20 or more, and particularly preferably 1.30 or more.

number

[0181] When the relative energy difference (RED) based on the Hansen solubility parameter (HSP) between the resin and the porogen is 1.00 or more, the resin and the porogen formed by polymerization of the polymerizable compound in the liquid composition are more likely to undergo phase separation, which is preferable because it makes it easier to form a porous resin.

[0182] -Relative Energy Difference (RED) based on Hansen Solubility Parameters (HSP) of polymerizable compounds and liquids (porogens)- As described above, the relative energy difference (RED) calculated based on the Hansen solubility parameter C of the polymerizable compound, which is determined based on the light transmittance at a wavelength of 550 nm of the transmittance measurement composition containing the polymerizable compound and the evaluation liquid, measured while stirring the transmittance measurement composition containing the polymerizable compound and the evaluation liquid, the interaction radius D of the polymerizable compound, which is determined based on the compatibility between the polymerizable compound and the evaluation liquid, and the Hansen solubility parameter of the liquid, based on the following formula 2, is preferably 1.05 or less, more preferably 0.90 or less, even more preferably 0.80 or less, and particularly preferably 0.70 or less.

number

[0183] When the relative energy difference (RED) based on the Hansen solubility parameter (HSP) between the polymerizable compound and the porogen is 1.05 or less, the polymerizable compound and the porogen are more likely to exhibit compatibility, and as the RED approaches 0, the compatibility becomes more pronounced. Therefore, when the relative energy difference (RED) is 1.05 or less, a liquid composition exhibiting high dissolution stability such that the polymerizable compound does not precipitate over time after dissolving the polymerizable compound in the porogen can be obtained. Since the polymerizable compound has high solubility in the porogen, the ejection stability of the liquid composition can be maintained, and the liquid composition of this embodiment can be suitably applied to a method of ejecting the liquid composition, such as an inkjet method. In addition, when the relative energy difference (RED) is 1.05 or less, separation between the polymerizable compound and the porogen is suppressed in the state of the liquid composition before the start of the polymerization reaction, and the formation of an irregular or non-uniform porous resin is suppressed.

[0184] (Method of producing liquid composition) The method for producing the liquid composition is not particularly limited and can be appropriately selected depending on the purpose. However, it is preferable to produce the liquid composition through a step of dissolving a polymerization initiator in a polymerizable compound, a step of further dissolving a porogen and other components, and a step of stirring to obtain a homogeneous solution.

[0185] <Insulating protective layer> The insulating protective layer improves the strength of the electrode end portion during lamination, and by providing it around the electrode active material as shown in Figures 1 to 3, it is possible to flatten the surface on which the insulating layer is formed and form an insulating layer having a uniform thickness on the upper portion. There is no limitation on the material as long as it has insulating properties, and it can be provided at any desired location on the electrode.

[0186] <Experimental section> The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0187] (Preparation of negative electrode) For forming the negative electrode composite layer, 97.0% by mass of graphite, 1.0% by mass of thickener (carboxymethyl cellulose), 2.0% by mass of polymer (styrene butadiene rubber), and 100.0% by mass of water as a solvent were mixed to prepare a negative electrode paint. This negative electrode paint was applied to both sides of the copper foil substrate and dried to obtain a negative electrode with a negative electrode composite layer weight of 9.0 mg / cm2 on one side. Next, the electrode was pressed with a roll press machine so that the deposition density of the electrode was 1.6 g / cm3, and the negative electrode to be used was obtained. At this time, the total film thickness of the negative electrode was 112.0 um. Finally, the negative electrode was punched out using a die punching machine (punching area: 60.0 mm × 30.0 mm) as shown in Figure 10.

[0188] (Preparation of positive electrode) A positive electrode paint was prepared by dispersing 92.0% by mass of lithium nickel oxide (NCA) as a positive electrode active material, 3.0% by mass of acetylene black as a conductive material, and 5.0% by mass of polyvinylidene fluoride (PVDF) as a binder in N-methylpyrrolidone (NMP). This positive electrode paint was applied to both sides of an aluminum foil substrate and then dried to obtain a positive electrode with a positive electrode composite layer weight of 15.0 mg / cm2 on one side. Next, the electrode was pressed with a roll press machine so that the volume density of the electrode was 2.8 g / cm3, and the positive electrode to be used was obtained. The total thickness of the positive electrode at this time was 132.0 um. Finally, the positive electrode was punched out using a die punching machine (punching area: 60.0 mm x 30.0 mm) as shown in FIG. 10.

[0189] Example 1 - Preparation of insulating layer-forming liquid composition - An insulating layer-forming liquid composition was prepared by mixing the materials in the ratios shown below: 29.0 mass% of tricyclodecane dimethanol diacrylate (manufactured by Daicel Allnex Corporation) as a polymerizable compound, 70.0 mass% of dipropylene glycol monomethyl ether (manufactured by Kanto Chemical Industry Co., Ltd.) as a solvent (porogen), and 1.0 mass% of Irgacure 184 (manufactured by BASF) as a polymerization initiator were mixed to obtain an insulating layer-forming liquid composition.

[0190] - Formation of insulating layer - The liquid composition for forming the insulating layer was filled into a die coat printing device. The amount of liquid composition discharged was controlled for the positive electrode punched out with a die, and an insulating layer was formed on both sides of the positive electrode composite layer so as to have a film thickness of 20.0 um on the active material. Immediately thereafter, the coating area was irradiated with UV light (light source: UV-LED (manufactured by Phoseon, product name: FJ800), wavelength: 365 nm, irradiation intensity: 30 mW / cm2, irradiation time: 20 s) in an N2 atmosphere to cure. Next, the cured product was heated at 120°C for 1 minute using a hot air drying oven to remove the solvent, and a positive electrode with an insulating layer was obtained.

[0191] evaluation: Using the prepared electrodes, a laminate was prepared according to the following procedure. Examples 1 to 4: As shown in FIG. 4, three sets of positive and negative electrodes were placed on the stage 14 . Comparative Example 1: As shown in Fig. 1, three sets of positive and negative electrodes were placed on stage 14 with a film separator larger than the positive and negative electrodes sandwiched between them. After placement, the ends of the electrodes were brought into contact with alignment unit 7 provided on stage 14 as shown in Fig. 5, and alignment was performed.

[0192] A pressure of 500 kPa was applied from above and below the obtained laminate, and the resistance value between the positive electrode and the negative electrode was measured to evaluate the presence or absence of lamination misalignment according to the following criteria. 〇: Resistance value is greater than 20MΩ ×: Resistance value 20MΩ or less The results are shown in Table 1.

[0193] Example 2 In Example 1, an insulating layer was formed on the negative electrode in the same manner as in the positive electrode. Thereafter, Evaluation 1 was carried out in the same manner as in Example 1. Table 1 shows the results.

[0194] Example 3 In Example 1, the formation of the insulating layer-forming liquid composition was changed to the procedure shown below, and an insulating layer was formed on both the positive and negative electrodes, and a positive electrode with an insulating layer was obtained in the same manner as in Example 1. Thereafter, Evaluation 1 was carried out in the same manner as in Example 1. The results are shown in Table 1.

[0195] -Formation of insulating layer-forming liquid composition in Example 3- The materials were mixed in the ratio shown below to prepare an insulating layer forming liquid composition. 29.0 mass% of EBECRYL8402 (manufactured by Daicel Allnex Corporation) was used as a polymerizable compound, 70.0 mass% of diisobutyl ketone (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as a solvent (porogen), and 1.0 mass% of Irgacure184 (manufactured by BASF) was used as a polymerization initiator to obtain an insulating layer forming liquid composition. After lamination, the laminate was heated and pressed at 120°C for 1 hour while being held at 0.2 MPa, and it was confirmed that the electrodes could be bonded to each other.

[0196] Example 4 A positive electrode with an insulating layer was obtained in the same manner as in Example 1, except that the preparation of the insulating layer-forming liquid composition was changed to the procedure shown below. Thereafter, Evaluation 1 was carried out in the same manner as in Example 1. The results are shown in Table 1.

[0197] -Formation of insulating layer-forming liquid composition in Example 4- A pre-dispersion was prepared by mixing 40.0 mass% of α-alumina (primary particle size (D50) 0.5 μm, specific surface area 7.8 g / m2) as an inorganic solid, 58.0 mass% of a mixed solution of dimethyl sulfoxide and ethylene glycol (DMSO-EG), and 2.0 mass% of Marialim HKM-150A (manufactured by NOF Corp.) as a dispersant. This pre-dispersion was placed in a container together with zirconia beads (Φ2 mm), and a dispersion treatment was performed at 1500 rpm for 3 minutes using a frozen nano-pulverizer NP-100 (manufactured by Thinky Corp.) to obtain a dispersion. The zirconia beads were removed from the obtained dispersion using a 25 μm mesh filter to prepare an insulating layer-forming liquid composition.

[0198] Comparative Example 1 In Example 1, the insulating layer was not formed, but a film separator was used as the insulating layer instead. Except for this, Evaluation 1 was carried out in the same manner as in Example 1. Table 1 shows the results. [Table 1]

[0199] By using an electrode-integrated insulating layer, it was shown that electrode alignment was possible by contacting the electrode end with a jig installed on the stage, indicating that the effect can be obtained regardless of the material of the insulating layer.

[0200] Although the preferred embodiments have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.

[0201] The present embodiment is applicable to power storage elements such as secondary batteries, capacitors, and lithium ion secondary batteries, and is particularly suitable for lithium ion secondary batteries.

[0202] For example, aspects of the present invention are as follows. <1> The insulating layer forming section is a method for manufacturing a laminate for a battery, which forms at least one of an insulating layer having ionic conductivity, an insulating layer having a porous structure, an insulating layer having a co-continuous structure, an insulating layer mainly composed of a resin, and an insulating layer having a cross-linked structure. <2> A method for manufacturing a battery stack using a manufacturing apparatus for a battery stack, the manufacturing apparatus for a battery stack transports electrodes to a stacking surface of a stage on which electrodes are stacked using a conveying unit, and aligns the electrodes on the stacking surface using an alignment unit, at least a portion of the alignment unit is positioned to be located on the stacking surface, and the alignment unit is capable of contacting an end of the electrode transported to the stacking surface by the conveying unit. <3> the alignment unit is movable on the stage, and the end of the electrode comes into contact with the alignment unit as the alignment unit moves on the stage; <2> 2. A method for producing the laminate for a battery according to claim 1 . <4> The electrode is slidable on the stage or on another electrode arranged on the stage, and an end of the electrode comes into contact with the alignment unit by sliding the electrode on the stage or on another electrode arranged on the stage. <2> or the above <3> 2. A method for producing the laminate for a battery according to claim 1 . <5> the battery stack manufacturing apparatus detects, by a sensor unit, that the electrodes have been stacked on the stage; <2> From the above <4> The present invention relates to a method for producing the laminate for a battery according to any one of the above. <6> The battery laminate manufacturing apparatus controls the operation of the alignment unit based on at least one of a conveying state of the conveying unit and a detection result of the sensor unit by a control unit. <5> 2. A method for producing the laminate for a battery according to claim 1 . <7> the battery stack manufacturing apparatus includes a friction reduction unit that reduces frictional force generated between the electrodes and the stage after the electrodes are stacked on the stage; <2> From the above <6> The present invention relates to a method for producing the laminate for a battery according to any one of the above. <8> The battery laminate manufacturing apparatus includes an insulating layer forming unit that forms an insulating layer. <2> From the above <7> The present invention relates to a method for producing the laminate for a battery according to any one of the above. <9> The battery laminate manufacturing apparatus includes an insulating layer forming unit that forms an insulating layer, and an electrode cutting unit that cuts the electrode on which the insulating layer has been formed by the insulating layer forming unit. <2> From the above <8> The present invention relates to a method for producing the laminate for a battery according to any one of the above. <10> The present invention relates to an apparatus for manufacturing a stacked body for a battery, the apparatus comprising: a stage on which electrodes are stacked; a transport unit that transports the electrodes to a stacking surface of the stage; and an alignment unit that aligns the electrodes on the stacking surface, wherein at least a portion of the alignment unit is positioned so as to be located on the stacking surface, the alignment unit is capable of contacting an end of the electrode transported to the stacking surface by the transport unit, the alignment unit is movable on the stage, and the end of the electrode comes into contact with the alignment unit as the alignment unit moves on the stage. <11> The electrode is slidable on the stage or on another electrode stacked on the stage, and an end of the electrode comes into contact with the alignment section by the electrode sliding on the stage or on another electrode stacked on the stage. <10> 2 is a manufacturing apparatus for the battery laminate described in 1. <12> a tilting mechanism for tilting the stage, the electrode sliding on the stage due to the action of gravity caused by the tilting mechanism; <10> or the above <11> It is a manufacturing apparatus as described in the above. <13> a sensor unit for detecting that the electrode is placed on the stage, <10> From the above <12> 1 is a manufacturing apparatus for a battery laminate according to any one of the above items. <14> a control unit that controls an operation of the alignment unit based on at least one of a conveying state of the conveying unit and a detection result of the sensor unit, <13> 2 is a manufacturing apparatus for the battery laminate described in 1. <15> The electrode is laminated on the stage, and the friction reducing portion reduces a frictional force generated between the electrode and the stage. <10> From the above <14> 1 is a manufacturing apparatus for a battery laminate according to any one of the above items. <16> The insulating layer forming portion is provided. <10> From the above <15> 2 is a manufacturing apparatus for the battery laminate described in 1. <17> an insulating layer forming section; and an electrode cutting section that cuts the electrode on which an insulating layer has been formed by the insulating layer forming section. <10> From the above <16> 1 is a manufacturing apparatus for a battery laminate according to any one of the above items. [Explanation of symbols]

[0203] 100 Insulating layer forming section 100-1 Liquid composition application process section 100-2 Energy application process section 100-3 Drying process department 200 Electrode cutting section 300 Laminated section 300-1 Electrode storage section 300-2 Conveyor section 300-6 Sensor section 300-7 Control section 300-8 Friction reduction part 300-9 Tilt mechanism 1a Liquid composition application device 1b Liquid composition container 1c Liquid composition supply tube 2a Light irradiation device 2b Polymerization inert gas circulation device 3a Heating device 4 First electrode 4a, 4b ends 5 Liquid composition 7, 7a1, 7b1 Alignment section 71~78 Column members 7-1 Moving parts 7-2 Non-moving parts 8 Guide member 10a First thickness region 10b Second thickness region 11 Second electrode 14 Stages 140 Laminated surface 15 Second electrode 15a end 16 Positioning hole 17 Aperture 1000 Battery laminate manufacturing equipment 2000 electrodes θ Tilt angle [Prior art documents] [Patent documents]

[0204] [Patent Document 1] International Publication No. 2017 / 073677

Claims

1. A method for manufacturing a laminate for a battery, wherein the insulating layer forming section forms at least one of an insulating layer having ionic conductivity, an insulating layer having a porous structure, an insulating layer having a co-continuous structure, an insulating layer mainly composed of a resin, and an insulating layer having a cross-linked structure.

2. A method for manufacturing a battery stack using an apparatus for manufacturing a battery stack, comprising: The battery laminate manufacturing apparatus includes: The transport unit transports the electrode to a stacking surface of a stage on which the electrodes are stacked. an alignment unit aligns the electrodes on the stacking surface; At least a portion of the alignment portion is disposed on the stacking surface, The method for manufacturing a stack for a battery, wherein the alignment unit is capable of contacting an end of the electrode transported to the stacking surface by the transport unit.

3. the alignment unit is movable on the stage, The method for producing a battery stack according to claim 2 , wherein the end of the electrode comes into contact with the alignment part by the alignment part moving on the stage.

4. the electrode is slidable on the stage or on another electrode disposed on the stage; 3. The method for manufacturing a battery stack according to claim 2, wherein the end of the electrode comes into contact with the alignment portion by sliding the electrode over the stage or over another electrode placed on the stage.

5. The method for producing a battery stack according to claim 2 , wherein the battery stack production device detects, by a sensor unit, that the electrodes have been stacked on the stage.

6. 6. The manufacturing method of the battery stack according to claim 5, wherein the battery stack manufacturing apparatus controls the operation of the alignment unit based on at least one of the transport state of the transport unit and the detection result of the sensor unit using a control unit.

7. 3. The method for producing a battery stack according to claim 2, wherein the battery stack production apparatus includes a friction reduction unit that reduces frictional force generated between the electrodes after the electrodes are stacked on the stage.

8. The method for producing a battery stack according to claim 2 , wherein the battery stack production apparatus forms an insulating layer by an insulating layer forming section.

9. The battery laminate manufacturing apparatus includes: An insulating layer is formed by an insulating layer forming unit; The method for producing a battery stack according to claim 2 , wherein the electrode on which the insulating layer has been formed by the insulating layer forming section is cut by an electrode cutting section.

10. a stage on which electrodes are stacked; a transport unit that transports the electrode to the stacking surface of the stage; an alignment portion for aligning the electrodes on the stacking surface; At least a portion of the alignment portion is disposed on the stacking surface, the alignment unit is capable of contacting an end of the electrode transported to the stacking surface by the transport unit; the alignment unit is movable on the stage, the end of the electrode comes into contact with the alignment unit as the alignment unit moves on the stage.

11. the electrode is slidable on the stage or on another electrode stacked on the stage; 11. The battery stack manufacturing apparatus according to claim 10, wherein the end of the electrode comes into contact with the alignment portion by the electrode sliding on the stage or on another electrode stacked on the stage.

12. A tilt mechanism for tilting the stage is provided, The manufacturing apparatus according to claim 10 , wherein the electrode slides on the stage due to gravity acting on the stage when the tilting mechanism tilts the stage.

13. The battery stack manufacturing apparatus according to claim 10 , further comprising a sensor unit that detects that the electrode is placed on the stage.

14. 14. The battery stack manufacturing apparatus according to claim 13, further comprising a control unit that controls an operation of the alignment unit based on at least one of a conveying state of the conveying unit and a detection result of the sensor unit.

15. The battery stack manufacturing apparatus according to claim 10 , further comprising a friction reducing section that reduces a frictional force generated between the electrode and the stage after the electrode is stacked on the stage.

16. The battery stack manufacturing apparatus according to claim 10 , further comprising an insulating layer forming section.

17. An insulating layer forming unit; 11. The manufacturing apparatus for a battery laminate according to claim 10, further comprising: an electrode cutting section that cuts the electrode on which the insulating layer has been formed by the insulating layer forming section.

Citation Information

Patent Citations

  • Lithium secondary battery

    JP2011124220A

  • Electrode body for all-solid-state batteries, and method for producing same

    WO2019103008A1

  • Laminating device and electrode laminating method

    WO2017073677A1