Method for producing block copolymer

The photopolymerization of hydrophobic monomers using a vinyl ether polymer as an initiator addresses the cost and limitations of existing methods, enabling the production of block copolymers with diverse hydrophobic monomers for various applications.

JP2024134328APending Publication Date: 2024-10-03UNIVERSITY OF FUKUI +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023044568
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for producing block copolymers of vinyl ether monomers and hydrophobic monomers are costly and limited in the types of hydrophobic monomers that can be used, and require purification steps or do not proceed with certain monomers like styrene or (meth)acrylic acid esters.

Method used

A method involving photopolymerization of hydrophobic monomers using a specific vinyl ether polymer as a photopolymerization initiator, allowing for the production of block copolymers with a wide variety of hydrophobic monomers at low cost without the need for prior purification.

Benefits of technology

Enables the easy and cost-effective production of block copolymers with segments derived from vinyl ether and hydrophobic monomers, including hydrophobic conjugated monomers, suitable for applications such as polymeric surfactants, thermoplastic elastomers, paints, and adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134328000012
    Figure 2024134328000012
  • Figure 2024134328000013
    Figure 2024134328000013
  • Figure 2024134328000014
    Figure 2024134328000014
Patent Text Reader

Abstract

To provide a method for simply and inexpensively producing a block copolymer of a vinyl ether monomer and a wide variety of hydrophobic monomers.SOLUTION: A method for producing a block copolymer of a vinyl ether polymer and a hydrophobic monomer, represented by formula (2), comprises a step for photopolymerizing the hydrophobic monomer through light irradiation in the presence of a vinyl ether polymer having a thioester group at the end.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a block copolymer, and more particularly to a method for producing a vinyl ether block copolymer, fine particles containing a vinyl ether block copolymer, and a photopolymerization initiator. [Background technology]

[0002] Block copolymers of vinyl ether monomers and hydrophobic monomers are used as polymeric surfactants, thermoplastic elastomers, paints, adhesives, template agents for lithography, and the like. Living cationic polymerization is known as a method for producing such block copolymers (Patent Document 1, Non-Patent Documents 1-2), but the living cationic polymerization requires a metal catalyst, which increases costs. In addition, the types of hydrophobic monomers that undergo polymerization reactions with vinyl ether monomers in the living cationic polymerization are limited. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-40245 A [Patent Document 2] JP 2016-210887 A [Non-patent literature]

[0004] [Non-Patent Document 1] Macromolecules,27,3714-3720(1994) [Non-Patent Document 2] Polymer Journal, 72, 486-490(2015) Summary of the Invention [Problem to be solved by the invention]

[0005] Also, as a method for producing a copolymer of 2-hydroxyethyl vinyl ether and vinyl acetate or N-vinylpyrrolidone, a method is known in which poly(2-hydroxyethyl vinyl ether) polymerized using S-cyanomethyl-N-methyl-N-phenylcarbamodithioate is used as a macro chain transfer agent to carry out radical RAFT polymerization of vinyl acetate or N-vinylpyrrolidone in the presence of a radical polymerization initiator (Patent Document 2). However, the radical RAFT polymerization method described in Patent Document 2 requires that the macro chain transfer agent be purified in advance prior to the copolymerization reaction. In addition, when a conjugated monomer such as styrene or a (meth)acrylic acid ester is used, the polymerization reaction sometimes does not proceed.

[0006] An object of the present invention is to provide a method for easily and inexpensively producing block copolymers of vinyl ether monomers and a wide variety of hydrophobic monomers. [Means for solving the problem]

[0007] As a result of intensive research, the present inventors have found that block copolymers of vinyl ether monomers and a wide variety of hydrophobic monomers can be produced simply and at low cost by photopolymerizing hydrophobic monomers using a specific vinyl ether polymer as a photopolymerization initiator, and have completed the present invention.

[0008] That is, the present invention provides the following: <1> ~ <11> This provides: <1> A method for producing a block copolymer represented by the following formula (2) (hereinafter also referred to as "block copolymer (2)"), comprising a step of photopolymerizing a hydrophobic monomer by irradiating it with light in the presence of a vinyl ether polymer represented by the following formula (1) (hereinafter also referred to as "vinyl ether polymer (1)") (hereinafter also referred to as "the production method of the present invention").

[0009] [ka]

[0010] [In formula (1), R 1 represents an alkanediyl group having 1 to 5 carbon atoms, R 2 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 3 is -C(R 5 )(R 6 )-CN, -C(R 7 )(R 8 )-X 1 , -C(R 9 )(R 10 )(R 11 ), -C(R 12 )(R 13 )-(CH2) a -COOR 14 , -C(R 15 )(X 2 )-(CH2) b -COOR 16 , -C(R 17 )(CN)-(CH2) c -COOR 18 , -C(R 19 )(CN)-(CH2) d -OH, -C(R 20 )(R 21 )-CON(R 22 )H, or -C(R 23 )(R 24 )-CON(R 25 )(R 26 ) and (R 5 ~R 21 , R 23 and R 24 each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 22 , R 25 and R 26 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; 1 ~X 2each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group, and a to d each independently represent an integer of 0 to 8. R 4 -SR 27 , -SX 3 , -SR 28 -X 4 , -N(R 29 )(R 30 ), -N(R 31 )(X 5 ), -N(X 6 )(X 7 ), -N(R 32 X 8 )(R 33 X 9 ), or -N(X 10 )(R 34 X 11 ) and (R 27 and R 29 ~R 31 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 28 and R 32 ~R 34 each independently represents a substituted or unsubstituted alkanediyl group having 1 to 12 carbon atoms; X 3 ~X 11 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group. 29 and R 30 may form a heterocycle together with the adjacent nitrogen atom; n represents an integer from 1 to 10; p represents the number of repeating units.

[0011] [ka]

[0012] [In formula (2), Z represents a repeating unit derived from the hydrophobic monomer, q represents the number of repeating units derived from the hydrophobic monomer, R 1 , R 2 , R 3 , R 4 , n and p are as defined above.

[0013] <2> the hydrophobic monomer is one or more hydrophobic monomers selected from the group consisting of aromatic vinyl hydrophobic monomers, (meth)acrylic acid ester hydrophobic monomers, N-substituted (meth)acrylamide hydrophobic monomers, olefin hydrophobic monomers, (meth)acrylonitrile hydrophobic monomers, N-vinyl group-containing heterocyclic hydrophobic monomers, halogenated vinyl hydrophobic monomers, and vinyl carboxylate hydrophobic monomers; <1> The manufacturing method described in <3> The hydrophobic monomer is a hydrophobic conjugated monomer; <1> The manufacturing method described in <4> The hydrophobic monomer is one or more hydrophobic monomers selected from the group consisting of aromatic vinyl hydrophobic monomers, (meth)acrylic acid ester hydrophobic monomers, and N-substituted (meth)acrylamide hydrophobic monomers. <1> The manufacturing method described in

[0014] <5> R 3 But -C(R 5 )(R 6 )-CN, -C(R 12 )(R 13 )-(CH2) a -COOR 14 , -C(R 15 )(X 2 )-(CH2) b -COOR 16 , -C(R 17 )(CN)-(CH2) c -COOR 18 , or -C(R 19 )(CN)-(CH2) d -OH, <1> ~ <4> 13. The method for producing a semiconductor device according to any one of the preceding claims. <6> R 4 But -N(R29 )(R 30 ), -N(R 31 )(X 5 ), -N(X 6 )(X 7 ), -N(R 32 X 8 )(R 33 X 9 ), or -N(X 10 )(R 34 X 11 ), <1> ~ <5> 13. The method for producing a semiconductor device according to any one of the preceding claims. <7> The block copolymer is a particulate block copolymer. <1> ~ <6> 13. The method for producing a semiconductor device according to any one of the preceding claims.

[0015] <8> Microparticles containing a block copolymer (2) (hereinafter also referred to as "microparticles of the present invention"). <9> The hydrophobic monomer is a hydrophobic conjugated monomer; <8> The microparticle according to claim 1. <10> A photopolymerization initiator containing a vinyl ether polymer (1) (hereinafter also referred to as "the photopolymerization initiator of the present invention"). <11> A photo-RAFT polymerization initiator, <10> The photopolymerization initiator according to claim 1. Effect of the Invention

[0016] According to the production method of the present invention and the photopolymerization initiator of the present invention, block copolymers of vinyl ether monomers and a wide variety of hydrophobic monomers can be produced simply and at low cost. The fine particles of the present invention have a segment composed of repeating units derived from a vinyl ether monomer and a segment composed of repeating units derived from a hydrophobic monomer, and yet can be produced easily and at low cost. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a GPC chromatogram showing the synthesis of the block copolymer obtained in Example 1. [Diagram 2]FIG. 2 is a GPC chromatogram showing the synthesis of a block copolymer obtained in Example 2. [Diagram 3] FIG. 2 is a GPC chromatogram showing the synthesis of a block copolymer obtained in Example 3. [Figure 4] FIG. 1 is a GPC chromatogram showing the synthesis of a block copolymer obtained in Example 4. [Diagram 5] FIG. 1 is a GPC chromatogram showing the synthesis of a block copolymer obtained in Example 5. [Figure 6] FIG. 1 is a GPC chromatogram showing the synthesis of a block copolymer obtained in Example 6. [Figure 7] FIG. 13 is a diagram showing an AFM image of the fine particles obtained in Example 7. [Figure 8] FIG. 13 is a diagram showing an AFM image of the fine particles obtained in Example 8. [Figure 9] FIG. 13 is a diagram showing an AFM image of the fine particles obtained in Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] [Method for producing block copolymer] The production method of the present invention includes a step of irradiating a hydrophobic monomer with light in the presence of a vinyl ether polymer represented by the following formula (1) to photopolymerize it. This step produces a block copolymer represented by the following formula (2). In this specification, the term "vinyl ether polymer" refers to a polymer having at least a repeating unit derived from a vinyl ether monomer.

[0019] [ka]

[0020] [In formula (1), R 1 represents an alkanediyl group having 1 to 5 carbon atoms, R 2 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R3 is -C(R 5 )(R 6 )-CN, -C(R 7 )(R 8 )-X 1 , -C(R 9 )(R 10 )(R 11 ), -C(R 12 )(R 13 )-(CH2) a -COOR 14 , -C(R 15 )(X 2 )-(CH2) b -COOR 16 , -C(R 17 )(CN)-(CH2) c -COOR 18 , -C(R 19 )(CN)-(CH2) d -OH, -C(R 20 )(R 21 )-CON(R 22 )H, or -C(R 23 )(R 24 )-CON(R 25 )(R 26 ) and (R 5 ~R 21 , R 23 and R 24 each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 22 , R 25 and R 26 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; 1 ~X 2 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group, and a to d each independently represent an integer of 0 to 8. R 4 -SR 27 , -SX 3 , -SR 28 -X 4 , -N(R 29 )(R 30), -N(R 31 )(X 5 ), -N(X 6 )(X 7 ), -N(R 32 X 8 )(R 33 X 9 ), or -N(X 10 )(R 34 X 11 ) and (R 27 and R 29 ~R 31 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 28 and R 32 ~R 34 each independently represents a substituted or unsubstituted alkanediyl group having 1 to 12 carbon atoms; X 3 ~X 11 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group. 29 and R 30 may form a heterocycle together with the adjacent nitrogen atom; n represents an integer from 1 to 10; p represents the number of repeating units.

[0021] [ka]

[0022] [In formula (2), Z represents a repeating unit derived from the hydrophobic monomer, q represents the number of repeating units derived from the hydrophobic monomer, R 1 , R 2 , R 3 , R 4 , n and p are as defined above.

[0023] Each symbol in formulas (1) and (2) will be explained. In formulas (1) and (2), R 1 represents an alkanediyl group having 1 to 5 carbon atoms. R 1 The alkanediyl group represented by R may be linear or branched. 1 The alkanediyl group represented by the following formula (I) preferably has 1 to 4 carbon atoms, and more preferably 2 or 3 carbon atoms. R 1 Examples of the alkanediyl group represented by the formula (I) include a methane-1,1-diyl group, an ethane-1,1-diyl group, an ethane-1,2-diyl group, a propane-1,1-diyl group, a propane-1,2-diyl group, a propane-1,3-diyl group, a propane-2,2-diyl group, a butane-1,2-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, and a pentane-1,5-diyl group. Among these, R 1 The alkanediyl group represented by the formula: is preferably an ethane-1,2-diyl group or a propane-1,2-diyl group, and more preferably an ethane-1,2-diyl group.

[0024] In the formulas (1) and (2), n represents an integer of 1 to 10, preferably an integer of 1 to 6, more preferably an integer of 1 to 4, and particularly preferably an integer of 1 to 3. When n is an integer of 2 to 10, n R 1 may be the same or different.

[0025] In formulas (1) and (2), R 2 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. R 2 The alkyl group represented by R may be linear or branched. 2 The number of carbon atoms of the alkyl group represented by the formula (I) is preferably 1 or 2. Specific examples include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. Among these, a methyl group and an ethyl group are preferred, and a methyl group is more preferred. Among these, R 2 From the viewpoint of availability, a hydrogen atom is preferable as the alkyl group.

[0026] In formulas (1) and (2), R3 is -C(R 5 )(R 6 )-CN, -C(R 7 )(R 8 )-X 1 , -C(R 9 )(R 10 )(R 11 ), -C(R 12 )(R 13 )-(CH2) a -COOR 14 , -C(R 15 )(X 2 )-(CH2) b -COOR 16 , -C(R 17 )(CN)-(CH2) c -COOR 18 , -C(R 19 )(CN)-(CH2) d -OH, -C(R 20 )(R 21 )-CON(R 22 )H, or -C(R 23 )(R 24 )-CON(R 25 )(R 26 ) Among these, R 3 From the viewpoint of availability, -C(R 5 )(R 6 )-CN, -C(R 12 )(R 13 )-(CH2) a -COOR 14 , -C(R 15 )(X 2 )-(CH2) b -COOR 16 , -C(R 17 )(CN)-(CH2) c -COOR 18 , -C(R 19 )(CN)-(CH2) d -OH is preferred, and -C(R 17 )(CN)-(CH2) c -COOR 18 , -C(R 19 )(CN)-(CH2) d -OH, -C(R 5 )(R 6)-CN is more preferred, and -C(R 5 )(R 6 )-CN is particularly preferred.

[0027] In formulas (1) and (2), R 4 -SR 27 , -SX 3 , -SR 28 -X 4 , -N(R 29 )(R 30 ), -N(R 31 )(X 5 ), -N(X 6 )(X 7 ), -N(R 32 X 8 )(R 33 X 9 ), or -N(X 10 )(R 34 X 11 ) Among these, R 4 From the viewpoint of availability, -N(R 29 )(R 30 ), -N(R 31 )(X 5 ), -N(X 6 )(X 7 ), -N(R 32 X 8 )(R 33 X 9 ), -N(X 10 )(R 34 X 11 ) is preferred, and -N(R 29 )(R 30 ), -N(R 31 )(X 5 ), -N(X 6 )(X 7 ) is more preferred, and -N(R 31 )(X 5 ) is particularly preferred.

[0028] Above R 5 ~R 21 , R 23 and R 24 Each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms, preferably a hydrogen atom. 22, R 25 and R 26 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms. In addition, the above R 27 and R 29 ~R 31 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms. R 5 ~R 26 , R 27 and R 29 ~R 31 The alkyl group represented by R may be linear or branched. 5 ~R 26 , R 27 and R 29 ~R 31 The number of carbon atoms of the alkyl group represented by is preferably 1 to 8, more preferably 1 to 4, and particularly preferably 1 or 2. Specific examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, n-pentyl group, n-hexyl group, 2-methylpentyl group, 1,3-dimethylbutyl group, 1,1,2-trimethylpropyl group, n-heptyl group, n-octyl group, isooctyl group, 2-ethylhexyl group, n-decyl group, and n-dodecyl group. Among these, methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, and tert-butyl group are preferred, and methyl group and ethyl group are more preferred. -N(R 29 )(R 30 ) in R 29 and R 30 may form a heterocycle together with the adjacent nitrogen atom. Examples of the heterocycle include a pyrrole ring, an imidazole ring, a pyridine ring, an indole ring, and a pyrimidine ring.

[0029] R 28 and R 32 ~R 34 each independently represents a substituted or unsubstituted alkanediyl group having 1 to 12 carbon atoms. R 28 and R32 ~R 34 The alkanediyl group represented by R may be linear or branched. 28 and R 32 ~R 34 The number of carbon atoms in the alkanediyl group represented by the formula (I) is preferably 1 to 4, and more preferably 1 or 2. 28 and R 32 ~R 34 The alkanediyl group represented by the formula R 1 Examples of the alkanediyl group include those similar to the alkanediyl group represented by the following formula:

[0030] X 1 ~X 2 , X 3 ~X 11 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group. Among these, X 1 ~X 11 As the alkyl group, a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, or a substituted or unsubstituted pyridyl group is preferable, and a substituted or unsubstituted phenyl group is more preferable.

[0031] a to d each independently represent an integer of 0 to 8, preferably 0 to 4, and more preferably 0 to 2.

[0032] R 5 ~R 34 , X 1 ~X 11 Examples of the substituent in include halogen atoms such as a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom; a haloalkyl group, etc. The substitution position and the number of the substituents are optional, and when there are two or more substituents, the substituents may be the same or different.

[0033] In the formulas (1) and (2), p represents the number of repeating units (degree of polymerization). From the viewpoint of fine particle formation and functional expression as a polymer, p is preferably an integer of 5 to 1000, more preferably an integer of 10 to 500, and particularly preferably an integer of 20 to 300. The number of repeating units (degree of polymerization) in this specification can be determined, for example, as a number average molecular weight in terms of polystyrene by gel permeation chromatography (GPC) analysis (developing solvent: N,N-dimethylformamide containing 10 mmol / L lithium bromide).

[0034] In formula (2), Z represents a repeating unit derived from a hydrophobic monomer. In this specification, the term "hydrophobic monomer" refers to a monomer having a solubility in water of less than 1 wt %. The hydrophobic monomer may be one or more hydrophobic monomers selected from the group consisting of aromatic vinyl hydrophobic monomers, (meth)acrylic acid ester hydrophobic monomers, N-substituted (meth)acrylamide hydrophobic monomers, olefin hydrophobic monomers, (meth)acrylonitrile hydrophobic monomers, N-vinyl group-containing heterocyclic hydrophobic monomers, halogenated vinyl hydrophobic monomers, and vinyl carboxylate hydrophobic monomers. These hydrophobic monomers may be used alone or in combination of two or more.

[0035] The hydrophobic monomer is preferably a hydrophobic conjugated monomer, more preferably one or more hydrophobic monomers selected from aromatic vinyl hydrophobic monomers, (meth)acrylic acid ester hydrophobic monomers, and N-substituted (meth)acrylamide hydrophobic monomers, and particularly preferably one or more hydrophobic monomers selected from aromatic vinyl hydrophobic monomers and (meth)acrylic acid ester hydrophobic monomers. According to the present invention, even when a hydrophobic conjugated monomer is used as the hydrophobic monomer, a block copolymer can be produced easily and at low cost. In addition, when a hydrophobic conjugated monomer (preferably one or more hydrophobic monomers selected from an aromatic vinyl hydrophobic monomer and a (meth)acrylic acid ester hydrophobic monomer) is used, a fine particle block copolymer can be easily obtained, and a stable polymer without a hemiacetal dithioester at the terminal can be obtained.

[0036] Examples of aromatic vinyl hydrophobic monomers include styrene hydrophobic monomers such as styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4,6-trimethylstyrene, ethylvinylbenzene, 2-n-butylstyrene, 3-n-butylstyrene, 4-n-butylstyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, 2-tert-butoxystyrene, 3-tert-butoxystyrene, 4-tert-butoxystyrene, and halogenated styrenes; and vinylnaphthalene hydrophobic monomers such as 1-vinylnaphthalene and 2-vinylnaphthalene, with styrene hydrophobic monomers being more preferred. As the (meth)acrylic acid ester-based hydrophobic monomer, a (meth)acrylic acid alkyl-based hydrophobic monomer is preferred, and (meth)acrylic acid C 1-8 Alkyl hydrophobic monomers are more preferred, and (meth)acrylic acid C 1-4 Alkyl hydrophobic monomers are particularly preferred, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. As the N-substituted (meth)acrylamide hydrophobic monomer, N-alkyl (meth)acrylamide hydrophobic monomer and N,N-dialkyl (meth)acrylamide hydrophobic monomer are preferred. 1-10 Alkyl (meth)acrylamide hydrophobic monomer, N,N-diC1-10 Alkyl (meth)acrylamide-based hydrophobic monomers are more preferred, and NC 1-6 Alkyl (meth)acrylamide hydrophobic monomer, N,N-diC 1-6 Particularly preferred are alkyl(meth)acrylamide hydrophobic monomers, such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, and N,N-diethyl(meth)acrylamide.

[0037] The olefin-based hydrophobic monomer may be a linear olefin-based hydrophobic monomer or a cyclic olefin-based hydrophobic monomer, and examples thereof include ethylene, propylene, isoprene, 1,3-butadiene, hexene, octene, cyclohexene, cyclooctene, and vinylcyclohexene. An example of the (meth)acrylonitrile-based hydrophobic monomer is (meth)acrylonitrile. Examples of the N-vinyl group-containing heterocyclic hydrophobic monomer include N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylindole, N-vinylphthalimide, and N-vinylcarbazole. Examples of the vinyl halide hydrophobic monomer include vinyl chloride and vinylidene chloride. As the vinyl carboxylate hydrophobic monomer, a saturated aliphatic carboxylate vinyl ester hydrophobic monomer is preferable, for example, vinyl acetate, vinyl propionate, vinyl hexanoate, vinyl laurate, etc.

[0038] In formula (2), q represents the number of repetitions (degree of polymerization) of the repeating unit derived from the hydrophobic monomer. From the viewpoint of fine particle formation and functional expression as a polymer, q is preferably an integer of 5 to 1000, more preferably an integer of 10 to 500, and particularly preferably an integer of 20 to 300.

[0039] The vinyl ether polymer (1) may be a commercially available product or may be synthesized according to a known method. For example, the vinyl ether polymer (1) can be synthesized by the method described in JP 2016-210887 A. Specifically, the vinyl ether polymer (1) can be synthesized by living radical polymerization of a compound represented by the following formula (4) (hereinafter also referred to as "compound (4)") in the presence of a compound represented by the following formula (3) (hereinafter also referred to as "compound (3)") and a radical polymerization initiator. The compound represented by formula (3) acts as a chain transfer agent.

[0040] [ka]

[0041] [In formula (3), R 3 and R 4 has the same meaning as above.

[0042] [ka]

[0043] [In formula (4), R 1 , R 2 and n are as defined above.

[0044] Examples of the compound (4) include 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, propylene glycol monovinyl ether, 1-hydroxypropan-2-yl vinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, dipropylene glycol monovinyl ether, triethylene glycol monovinyl ether, 2-methoxyethyl vinyl ether, 2-ethoxyethyl vinyl ether, 2-(2-methoxyethoxy)ethyl vinyl ether, 2-(2-ethoxyethoxy)ethyl vinyl ether, 2-(2-(2-methoxyethoxy)ethoxy)ethyl vinyl ether, 2-(2-(2-ethoxyethoxy)ethoxy)ethyl vinyl ether, etc. Compound (4) can be used alone or in combination of two or more. Among these, 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 2-methoxyethyl vinyl ether, and 4-hydroxybutyl vinyl ether are preferred, 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 2-methoxyethyl vinyl ether are more preferred, and 2-hydroxyethyl vinyl ether is particularly preferred.

[0045] Examples of compound (3) include S-cyanomethyl-N-methyl-N-phenylcarbamodithioate, S-cyanomethyl-N,N-diphenylcarbamodithioate, S-2-cyanopropan-2-yl-N-methyl-N-(4-pyridyl)carbamodithioate, S-cyanomethyl-N-methyl-N-(4-pyridyl)carbamodithioate, methyl 2-[N-methyl-N(4-pyridyl)carbamothioylthio]propanoate, benzyl 1H-pyrrole-1-carbodithioate, etc. These chain transfer agents may be used alone or in combination of two or more. Among these chain transfer agents, in terms of good reactivity and ease of polymerization control, S-cyanomethyl-N-methyl-N-phenylcarbamodithioate, S-cyanomethyl-N,N-diphenylcarbamodithioate, and benzyl 1H-pyrrole-1-carbodithioate are preferred, and S-cyanomethyl-N-methyl-N-phenylcarbamodithioate is more preferred.

[0046] The amount of the chain transfer agent used is usually in the range of 0.001 to 20 parts by mole, preferably 0.01 to 10 parts by mole, and more preferably 0.1 to 5 parts by mole, based on 100 parts by mole of compound (4).

[0047] Examples of the radical polymerization initiator include an azo-based radical polymerization initiator and a peroxide-based radical polymerization initiator.

[0048] Examples of the azo radical polymerization initiator include oil-soluble azo radical polymerization initiators such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexanecarbonitrile), 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], and 2,2'-azobis[N-butyl-2-methylpropionamide]; and water-soluble azo radical polymerization initiators such as 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamide], 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate, 2,2'-azobis(2-methylpropionamide) dihydrate, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamide) tetrahydrate, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], and 2,2'-azobis[1-imino-1-pyrrolidino-2-methylpropane] dihydrochloride.

[0049] Examples of peroxide-based radical polymerization initiators include t-butyl hydroperoxide, cumene hydroperoxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, t-butyl peroxyoctanoate, t-butyl peroxyneodecanoate, t-butyl peroxyisobutyrate, lauroyl peroxide, t-amyl peroxypivalate, t-butyl peroxypivalate, dicumyl peroxide, benzoyl peroxide, potassium persulfate, and ammonium persulfate.

[0050] The radical polymerization initiator may be used alone or in combination of two or more kinds. The amount of the radical polymerization initiator used is not particularly limited, but is usually in the range of 0.001 to 20 parts by mole, preferably 0.01 to 10 parts by mole, and more preferably 0.05 to 5 parts by mole, per 100 parts by mole of compound (4).

[0051] The living radical polymerization can be carried out in the presence or absence of a solvent. Examples of the solvent include water; monoalcohols such as methanol, ethanol, isopropanol, n-butyl alcohol, isobutyl alcohol, tert-butyl alcohol, sec-butyl alcohol, and tetrahydrofurfuryl alcohol; polyhydric alcohols such as ethylene glycol, glycerin, and diethylene glycol; ether alcohols such as methyl cellosolve, cellosolve, isopropyl cellosolve, butyl cellosolve, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, and diethylene glycol monoethyl ether; alkyl amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; alkyl sulfoxides such as dimethyl sulfoxide; ketones such as acetone and methyl ethyl ketone; and cyclic ethers such as tetrahydrofuran and dioxane. These solvents can be used alone or in combination of two or more. The amount of the solvent used is not particularly limited, but is usually 10 to 1000 parts by mass, and preferably 20 to 500 parts by mass, per 100 parts by mass of compound (4).

[0052] The polymerization temperature for the living radical polymerization is preferably from −20° C. to 200° C., more preferably from 40° C. to 160° C. The polymerization time is usually from 1 to 144 hours, preferably from 3 to 108 hours.

[0053] The number average molecular weight (Mn) of the vinyl ether polymer (1) in terms of polystyrene by GPC analysis is usually 1,000 to 1,000,000, preferably 1,500 to 500,000, more preferably 2,000 to 200,000. The molecular weight distribution (Mw / Mn) is usually 1.0 to 2.0, preferably 1.0 to 1.8, more preferably 1.0 to 1.6. The number average molecular weight of the vinyl ether polymer (1) can be adjusted by the amounts of the compound (3) and the radical initiator used.

[0054] Next, the photopolymerization step will be described in detail. The photopolymerization step is a step in which a hydrophobic monomer is irradiated with light in the presence of the vinyl ether polymer (1) to cause photopolymerization. Examples of the hydrophobic monomer include those which provide a repeating unit derived from the hydrophobic monomer represented by Z. The vinyl ether polymer (1) acts as a photopolymerization initiator (preferably a photo-RAFT polymerization initiator). The vinyl ether polymer (1) may be obtained by living radical polymerization and used as it is, or may be isolated from the reaction solution. The amount of the vinyl ether polymer (1) used is not particularly limited, but is usually in the range of 1 to 10,000 parts by mole, preferably 5 to 5,000 parts by mole, and more preferably 10 to 1,000 parts by mole, per 100 parts by mole of the hydrophobic monomer.

[0055] Examples of light to be irradiated include ultraviolet light, visible light, and X-rays, with ultraviolet light being preferred. Examples of ultraviolet irradiating devices include low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, metal halide lamps, black light lamps, UV electrodeless lamps, and LEDs. The irradiation intensity is usually 0.1 to 100 mW / cm 2 , preferably 0.5 to 20 mW / cm 2 It is.

[0056] The photopolymerization step can be carried out by a general polymerization method such as bulk polymerization, dispersion polymerization, emulsion polymerization, solution polymerization, or suspension polymerization. The photopolymerization step can be carried out in the presence or absence of a solvent or dispersion medium, but is preferably carried out in the presence of a solvent or dispersion medium. Examples of the solvent or dispersion medium that can be used include water; monoalcohols such as methanol, ethanol, isopropanol, n-butyl alcohol, isobutyl alcohol, tert-butyl alcohol, sec-butyl alcohol, and tetrahydrofurfuryl alcohol; polyhydric alcohols such as ethylene glycol, glycerin, and diethylene glycol; ether alcohols such as methyl cellosolve, cellosolve, isopropyl cellosolve, butyl cellosolve, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, and diethylene glycol monoethyl ether; alkylamides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; alkyl sulfoxides such as dimethyl sulfoxide; ketones such as acetone and methyl ethyl ketone; and cyclic ethers such as tetrahydrofuran and dioxane. These solvents or dispersion media can be used alone or in combination of two or more.

[0057] The amount of the solvent or dispersion medium used is not particularly limited, but is usually 50 to 2000 parts by mass, and preferably 100 to 1000 parts by mass, per 100 parts by mass of the hydrophobic monomer.

[0058] When photopolymerization is carried out by emulsion polymerization, the photopolymerization step is preferably carried out in the presence of water, and may also be carried out in the presence of an emulsifier together with water. Examples of emulsifiers include anionic surfactants such as sodium laurate, sodium polyoxyethylene methyl ether carboxylate, sodium 2-ethylhexyl sulfate, sodium dioctyl sulfosuccinate, sodium polyacrylate, and sodium polymethacrylate; cationic surfactants such as alkyl trimethyl ammonium salts and alkyl benzyl ammonium chloride; nonionic surfactants such as polyoxyethylene alkyl ethers, polyvinyl alcohol, poly N-vinyl pyrrolidone, and polyethylene glycol monomethacrylate; and amphoteric surfactants such as alkyl dimethyl amino acetate betaine and alkyloyl amidopropyl dimethyl glycine. The emulsifiers can be used alone or in combination of two or more. The amount of the emulsifier used is not particularly limited, but is usually 1 to 400 parts by mass, and preferably 10 to 100 parts by mass, per 100 parts by mass of the hydrophobic monomer.

[0059] When photopolymerization is carried out by the dispersion polymerization method, the photopolymerization step is preferably carried out in the presence of a dispersion medium, more preferably in the presence of a dispersion medium and a dispersion stabilizer. Examples of the dispersion stabilizer include polyvinyl alcohol, partially saponified polyvinyl alcohol, polyoxyethylene alkyl ether, poly-N-vinylpyrrolidone, etc. The dispersion stabilizer may be used alone or in combination of two or more.

[0060] From the viewpoint of reaction efficiency, the polymerization temperature for photopolymerization is preferably from 10 to 160° C., more preferably from 15 to 120° C. The polymerization time is usually from 0.5 to 96 hours, preferably from 1 to 72 hours.

[0061] The polymerization can be carried out by any of a batch polymerization method, a semi-batch polymerization method, a continuous polymerization method, and the like.

[0062] The reaction product obtained in the photopolymerization step may be purified, if necessary. According to the production method of the present invention, block copolymers of vinyl ether monomers and a wide variety of hydrophobic monomers can be produced easily and at low cost. In addition, when the vinyl ether polymer (1) is prepared by living radical polymerization, the vinyl ether polymer (1) can be used in a photopolymerization step without purification, which is extremely useful industrially. In particular, even when a hydrophobic conjugated monomer is used as the hydrophobic monomer, a block copolymer can be produced easily and at low cost. The block copolymer thus obtained is useful as a polymer surfactant, a thermoplastic elastomer, a coating material, an adhesive, a template agent for lithography, a surface modifier, and the like. The block copolymer (2) has a polystyrene-equivalent number average molecular weight (Mn) determined by GPC analysis of usually 1,000 to 500,000, preferably 2,500 to 200,000, more preferably 5,000 to 100,000. The molecular weight distribution (Mw / Mn) is usually 1.0 to 4.0, preferably 1.0 to 5.0, more preferably 1.0 to 4.5. The block copolymer (2) is preferably a fine particle block copolymer, which is useful as a cosmetic material, etc.

[0063] [Fine particles] The fine particles of the present invention contain a block copolymer (2). In the microparticles of the present invention, each symbol in formula (2) has the same meaning as above. That is, as the hydrophobic monomer that gives the repeating unit represented by Z in formula (2), a hydrophobic conjugated monomer is preferable, one or more hydrophobic monomers selected from aromatic vinyl hydrophobic monomers, (meth)acrylic acid ester hydrophobic monomers, and N-substituted (meth)acrylamide hydrophobic monomers are more preferable, and one or more hydrophobic monomers selected from aromatic vinyl hydrophobic monomers and (meth)acrylic acid ester hydrophobic monomers are particularly preferable.

[0064] In addition, from the viewpoint of the size being dispersible in a solvent or a dispersion medium, the average particle diameter (Dh) of the fine particles of the present invention is preferably 1 to 1000 nm, more preferably 5 to 500 nm, and particularly preferably 10 to 300 nm. From the viewpoint of uniformity, the particle size distribution (PDI) is preferably 0.01 to 0.8, more preferably 0.01 to 0.65, and particularly preferably 0.01 to 0.5. From the viewpoint of reproducibility in particle size measurement, the coefficient of variation (CV) is preferably 0 to 20%, more preferably 0 to 10%, and particularly preferably 0 to 5%. In this specification, the average particle diameter means the volume average particle diameter measured by the dynamic light scattering method, and the average particle diameter, the particle size distribution (PDI), and the coefficient of variation (CV) can be specifically measured by the methods described in the examples below.

[0065] And the fine particles of the present invention can be produced simply and at low cost while having a segment composed of repetitions of repeating units derived from a vinyl ether-based monomer and a segment composed of repetitions of repeating units derived from a hydrophobic monomer. In addition, the vinyl ether unit has a feature of low cytotoxicity. Therefore, the fine particles of the present invention are useful as cosmetic materials and the like.

[0066] 〔Photoinitiator〕 The photoinitiator of the present invention contains a vinyl ether-based polymer (1). According to the photoinitiator of the present invention, a block copolymer of a vinyl ether-based monomer and a wide variety of hydrophobic monomers can be produced simply and at low cost. The photoinitiator of the present invention is particularly useful as a photo-RAFT polymerization initiator.

Examples

[0067] Hereinafter, the present invention will be described in detail with reference to examples, but the present invention is not limited to these examples.

[0068] <GPC Measurement> The analysis of Mn and Mw / Mn was carried out using GPC in terms of polystyrene. The analysis conditions were as follows: column: TSKgel column G-MHHR-M × 2 (manufactured by Tosoh Corporation), solvent: N,N-dimethylformamide (containing 10 mmol / L lithium bromide), measurement temperature: 40°C, and flow rate: 1.0 mL / min.

[0069] < 1 H NMR measurement> 1 H NMR measurements were performed using a JNM-ECX500 II manufactured by JEOL Corp. The monomer conversion (the ratio of monomers incorporated into the polymer by the polymerization reaction to the total amount of monomers present at the beginning) was determined from the peak area ratio of the produced polymer to the remaining monomers by dissolving the reaction solution after polymerization in a solvent that dissolves the polymer homogeneously (heavy water, deuterated methanol, deuterated dimethyl sulfoxide, or deuterated chloroform).

[0070] <Particle size measurement by dynamic light scattering (DLS)> DLS particle size measurements were performed using a Malvern Zetasizer Nano-ZSP at a scattering angle of 173°. The measurement data was analyzed using the cumulant method with Zeta Software Ver. 7.02, and the particle diameter (D h The mean particle size was obtained from measurements taken nine or more times, and the coefficient of variation (CV) was calculated from the standard deviation of the particle size measurement results.

[0071] <Atomic Force Microscope (AFM) Measurement> The shape of the particles was observed using a Shimadzu SPM-9600. A sample (aqueous dispersion of particles) was applied to a mica substrate, and after sufficient air drying, it was measured in dynamic mode. A silicon cantilever (Olympus OMCL-AC160TS-C3) was used for the measurement.

[0072] <Preparation Example 1: Synthesis of poly(2-hydroxyethyl vinyl ether)> A stirrer was placed in the test tube, and 0.050 g of S-cyanomethyl-N-methyl-N-phenylcarbamodithioate (hereinafter referred to as "CMPCD"), 4.011 g (200 molar equivalents per mole of CMPCD) of 2-hydroxyethyl vinyl ether (hereinafter referred to as "HEVE") as a monomer, and 0.021 g (0.4 molar equivalents per mole of CMPCD) of dimethyl 2,2'-azobis(2-methylpropionate) ("V-601" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added and thoroughly stirred. Next, the mixture was subjected to freezing and degassing three times, after which the test tube was sealed and the polymerization reaction was started in an oil bath at 70°C. After 6 or 24 hours had elapsed since the start of the reaction, the polymerization was stopped by cooling and exposure to air. 1 1 H NMR analysis and GPC analysis were carried out. After 6 hours of polymerization, the monomer conversion (the proportion of the monomer HEVE incorporated into the polymer through the polymerization reaction relative to the total amount of monomer initially present) was 13%, and the Mn of the resulting poly(2-hydroxyethyl vinyl ether) (hereinafter referred to as "PHEVE") was 2100 and the Mw / Mn was 1.52. In addition, after 24 hours of polymerization, the monomer conversion was 21%, and the Mn of the resulting PHEVE was 3,800 and the Mw / Mn was 1.40.

[0073] <Preparation Example 2: Synthesis of poly(diethylene glycol monovinyl ether)> The polymerization reaction was carried out in the same manner as in Preparation Example 1, except that the monomer was changed to 5.999 g (200 moles per mole of CMPCD) of diethylene glycol monovinyl ether (hereinafter, referred to as "DEGV"). After 24 hours, the polymerization was stopped by cooling and exposure to air. 1 1 H NMR analysis and GPC analysis were carried out. As a result, the monomer conversion was 25%, and the resulting poly(diethylene glycol monovinyl ether) (hereinafter referred to as "PDEGV") had an Mn of 6,300 and an Mw / Mn of 1.46.

[0074] <Preparation Example 3: Synthesis of poly(2-methoxyethyl vinyl ether)> A stirrer was placed in the test tube, and 0.218 g of CMPCD, 20.000 g of 2-methoxyethyl vinyl ether (hereinafter referred to as "MOVE") as a monomer (200 molar times relative to 1 mole of CMPCD), 0.093 g of V-601 (0.4 molar times relative to 1 mole of CMPCD), 0.017 g of lithium hydroxide monohydrate (0.4 molar times relative to 1 mole of CMPCD), and 20.000 g of ultrapure water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added and thoroughly stirred. Next, after performing freezing and degassing three times, the test tube was sealed and a polymerization reaction was started in an oil bath at 70°C. After 72 hours had passed since the start of the reaction, the polymerization was stopped by cooling and exposure to air, 1 1 H NMR analysis and GPC analysis were carried out. As a result, the monomer conversion was 28%, and the resulting poly(2-methoxyethyl vinyl ether) (hereinafter referred to as "PMOVE") had an Mn of 5500 and an Mw / Mn of 1.31.

[0075] <Reference Example 1: Irradiation of PHEVE solution containing HEVE monomer> In the test tube after the completion of the 24-hour polymerization in Preparation Example 1, in addition to the produced PHEVE (Mn=3800, Mw / Mn=1.40), unreacted HEVE was contained (3.762 mol% based on PHEVE). The solution in the test tube was subjected to freezing and degassing three times again, and then the test tube was sealed and heated at room temperature with a UV-LED (peak wavelength 365 nm, 14.2 mW / cm 2 The test tubes were then exposed to UV-LED light for two days. The light source used was a Technosigma PER-365 (output 507 mW) that was inserted directly into the test tube (hereafter, this light source will be referred to as "UV-LED"). After that, the test tubes were exposed to air. 1 1 H NMR analysis and GPC analysis were carried out. As a result, PHEVE was exactly the same as before light irradiation (Mn = 3800, Mw / Mn = 1.40). Thus, it was confirmed that the remaining unreacted HEVE did not react with light irradiation in the presence of PHEVE obtained in Preparation Example 1. Similarly, a PDEGV solution containing DEGV and a PMOVE solution containing MOVE were also irradiated with light for 2 days each, but no change was observed.

[0076] Example 1: Irradiation of PHEVE solution containing styrene (1) After 24 hours of polymerization in Preparation Example 1, 3.377 g of solution (containing 0.799 g of PHEVE) was taken from the test tube and placed in a new test tube, to which 4.030 g (200 mol % relative to PHEVE) of styrene (hereinafter referred to as "St") and 9.428 g of N,N-dimethylformamide (hereinafter referred to as "DMF") as a solvent were added and thoroughly dissolved. After freeze-degassing was performed three times, the test tube was sealed and irradiated with UV-LED light at room temperature for three days. (2) During this time, the reaction solution is withdrawn after 1 hour, 2 hours, 4 hours, 8 hours, 24 hours, 48 ​​hours, and 72 hours, and the withdrawn solution is exposed to air to terminate the polymerization. 1 H NMR and GPC analyses were performed. As time passed, the product changed to a higher molecular weight product and the amount of St remaining decreased, confirming the synthesis of a block copolymer consisting of PHEVE and polystyrene (hereafter referred to as "PSt"). The GPC analysis results obtained at each time are shown in Figure 1.

[0077] Example 2: Irradiation of PHEVE solution containing vinyl acetate After 24 hours of polymerization in Preparation Example 1, a mixed solution containing 0.691 g of PHEVE was collected from the test tube and placed in a new test tube, to which 3.235 g of vinyl acetate (200 mol % relative to PHEVE) and 6.519 g of methanol as a solvent were added and thoroughly dissolved. Next, after three freeze-degassing cycles, the test tube was sealed and irradiated with UV-LED light at room temperature for 25 hours. During this time, the reaction solution was removed after 1 hour, 2 hours, 4 hours, 8 hours, and 25 hours, and the removed solution was exposed to air to terminate the polymerization. 1 H NMR and GPC analyses were performed. As time passed, the product changed to a higher molecular weight product and the amount of remaining vinyl acetate decreased, confirming the synthesis of a block copolymer consisting of PHEVE and polyvinyl acetate. The GPC analysis results obtained at each time point are shown in Figure 2.

[0078] <Example 3: Irradiation of PHEVE solution containing N-vinylpyrrolidone> After 24 hours of polymerization in Preparation Example 1, a mixed solution containing 1.100 g of PHEVE was collected from the test tube and placed in a new test tube, to which 5.914 g of N-vinylpyrrolidone (200 mol % relative to PHEVE) and 3.486 g of methanol as a solvent were added and thoroughly dissolved. Next, freeze-degassing was performed three times, after which the test tube was sealed and immersed in a water bath heated to 70°C while simultaneously being irradiated with UV-LED light for 25 hours. During this time, the reaction solution was removed after 1 hour, 2 hours, 4 hours, 8 hours, and 25 hours, and the removed solution was exposed to air to terminate the polymerization. 1 H NMR and GPC analyses were performed. As time passed, the product changed to a higher molecular weight product and the amount of remaining N-vinylpyrrolidone decreased, confirming the synthesis of a block copolymer consisting of PHEVE and poly(N-vinylpyrrolidone). The GPC analysis results obtained at each time point are shown in Figure 3.

[0079] <Example 4: Irradiation of PHEVE solution containing N,N-diethylacrylamide> After 24 hours of polymerization in Preparation Example 1, a mixed solution containing 0.420 g of PHEVE was collected from the test tube and placed in a new test tube, to which 2.580 g of N,N-diethylacrylamide (200 mol % relative to PHEVE) and 10.649 g of methanol as a solvent were added and thoroughly dissolved. Next, after performing freeze-degassing three times, the test tube was sealed and irradiated with UV-LED light at room temperature for 24 hours, and then exposed to air to terminate the polymerization. 1 H NMR and GPC analyses were performed. GPC analysis of the PHEVE used and the resulting polymer confirmed that the resulting polymer had changed to a higher molecular weight than PHEVE, and that all of the N,N-diethylacrylamide had polymerized. In this way, the synthesis of a block copolymer (Mn=40600, Mw / Mn=1.46) consisting of PHEVE and poly(N,N-diethylacrylamide) was confirmed. The results of the GPC analysis are shown in Figure 4.

[0080] <Example 5: Irradiation of PHEVE solution containing methyl methacrylate> After 24 hours of polymerization in Preparation Example 1, a mixed solution containing 0.478 g of PHEVE was collected from the test tube and placed in a new test tube, to which 2.526 g (200 mol % relative to PHEVE) of methyl methacrylate (hereinafter referred to as "MMA") and 10.283 g of DMF as a solvent were added and thoroughly dissolved. Next, after performing freeze-degassing three times, the test tube was sealed and immersed in a water bath heated to 70°C while simultaneously irradiating it with UV-LED light for 46 hours, and then exposed to air to terminate the polymerization. 1 H NMR analysis and GPC analysis were performed. GPC analysis of the PHEVE used and the resulting polymer confirmed that the resulting polymer had changed to a higher molecular weight than PHEVE, and that MMA had polymerized at a conversion rate of 80%. In this way, the synthesis of a block copolymer (Mn=27500, Mw / Mn=1.41) of PHEVE and polymethyl methacrylate (hereinafter referred to as "PMMA") was confirmed. The results of the GPC analysis are shown in Figure 5.

[0081] Example 6: Irradiation of PMOVE solution containing MMA 0.706 g of PMOVE obtained in Preparation Example 3, 1.894 g of MMA (200 mol % based on PMOVE), and 10.401 g of DMF as a solvent were added to a test tube and thoroughly dissolved. Next, freeze-degassing was performed three times, and then the test tube was sealed and irradiated with UV-LED light at room temperature for 24 hours, and then exposed to air to terminate the polymerization. 1 H NMR and GPC analyses were performed. GPC analysis of the PMOVE used and the resulting polymer confirmed that the resulting polymer had changed to a higher molecular weight than PMOVE, and that MMA had polymerized at a conversion rate of 88%. In this way, the synthesis of a block copolymer of PMOVE and PMMA (Mn=14900, Mw / Mn=1.85) was confirmed. The results of the GPC analysis are shown in Figure 6.

[0082] Example 7 Preparation of PHEVE-PSt Copolymer Microparticles Photopolymerization was carried out in the same manner as in Example 1(1), except that DMF was changed to ethanol and the mixture was irradiated with UV-LED light for 45.5 hours while being stirred at a speed of 600 rpm. After that, the polymerization was stopped by exposing it to air, and DLS and AFM measurements were performed. 1 H NMR and GPC analyses were performed. GPC analysis of the PHEVE used and the resulting polymer confirmed that the resulting polymer had changed to a higher molecular weight than PHEVE, and that St had polymerized at a conversion rate of 92%. In this way, the synthesis of a block copolymer of PHEVE and PSt (Mn = 14,300, Mw / Mn = 3.42) was confirmed. The block copolymer was obtained in ethanol as fine particles with the PSt portion as the core and the PHEVE portion as the shell, and particle size measurements by DLS revealed that the particle size (D h The particle diameter distribution (PDI) was 0.413, and the coefficient of variation (CV) was 2.0%. The results of AFM observation of the obtained microparticles are shown in FIG.

[0083] Example 8: Preparation of PDEGV-PSt copolymer microparticles (1) 0.145 g of PDEGV obtained in Preparation Example 2, 0.456 g of St (200 mol % relative to PDEGV), and 2.399 g of 1-butanol as a solvent were added to a test tube and thoroughly dissolved. Next, after performing freeze-degassing three times, the test tube was sealed and immersed in an oil bath heated to 70°C or 110°C, and at the same time, irradiated with UV-LED light for 24 hours while stirring at a speed of 600 rpm. (2) After that, the polymerization was stopped by exposing to air, and DLS and AFM measurements were performed. 1H NMR analysis and GPC analysis were performed. GPC analysis of the PDEGV used and the resulting polymer confirmed that the resulting polymer had changed to a higher molecular weight than PDEGV, and that St was polymerized at a conversion rate of 91% in the polymerization at 70°C and 81% in the polymerization at 110°C. In this way, the synthesis of a block copolymer of PDEGV and PSt was confirmed (polymerization at 70°C: Mn = 24,800, Mw / Mn = 4.02, polymerization at 110°C: Mn = 11,800, Mw / Mn = 2.09). The block copolymer was obtained as fine particles in 1-butanol, and particle size measurement by DLS showed that the particle size (D h ) was 197 nm, the particle size distribution (PDI) was 0.031, and the coefficient of variation (CV) was 2.1%. In addition, in the polymerization at 110°C, the particle diameter (D h The particle diameter distribution (PDI) was 0.145, and the coefficient of variation (CV) was 1.2%. The results of AFM observation of the obtained microparticles (2 μm × 2 μm height image) are shown in FIG.

[0084] Example 9: Preparation of PDEGV-PSt copolymer microparticles in water (1) Photopolymerization was carried out in the same manner as in Example 8(1), except that 1-butanol was replaced with ultrapure water and the reaction temperature was changed to 70°C. (2) After that, the polymerization was stopped by exposing to air, and DLS and AFM measurements were performed. 1 H NMR analysis and GPC analysis were performed. GPC analysis of the PDEGV used and the resulting polymer confirmed that the resulting polymer had changed to a higher molecular weight than PDEGV, and that St had polymerized at a conversion rate of 98%. In this way, the synthesis of a block copolymer of PDEGV and PSt (Mn = 29,000, Mw / Mn = 4.06) was confirmed. The block copolymer was obtained in water as fine particles with the PSt portion as the core and the PDEGV portion as the shell, and particle size measurement by DLS revealed that the particle size (D h The particle diameter distribution (PDI) was 0.073, and the coefficient of variation (CV) was 1.1%. The results of AFM observation of the obtained microparticles (2 μm × 2 μm height image) are shown in FIG.

[0085] <Comparative Example 1> 0.145 g of PDEGV obtained in Preparation Example 2, 0.456 g of St (200 mol % relative to PDEGV), 0.002 g of V-601 (0.4 mol % relative to PDEGV), and 2.399 g of ultrapure water as a solvent were added to a test tube and thoroughly dissolved. Next, freeze-degassing was performed three times, and then the test tube was sealed and stirred at 600 rpm in a 70°C oil bath for 24 hours. After that, when the sample was exposed to air and DLS measurements were performed, no fine particles were observed, and no progress of the copolymerization reaction could be confirmed.

[0086] <Comparative Example 2> 0.478 g of PHEVE obtained in Preparation Example 1, 2.526 g of MMA (200 mol % relative to PHEVE), 0.012 g of V-601 (0.4 mol % relative to PHEVE), and 10.271 g of DMF as a solvent were added to a test tube and thoroughly dissolved. Next, after freeze-degassing was performed three times, the test tube was sealed and reacted in an oil bath at 70°C for 24 hours. After exposure to air, the reaction mixture was dissolved in 50 mL of water, but the PHEVE used was recovered as it was, and the progress of the block copolymerization reaction of PHEVE and PMMA could not be confirmed.

[0087] As shown in the results of Comparative Examples 1 and 2, when a vinyl ether polymer was used as a macro chain transfer agent to carry out radical RAFT polymerization of hydrophobic conjugated monomers such as St and MMA, no progress of the block copolymerization reaction was observed.

Claims

1. A method for producing a block copolymer represented by the following formula (2), comprising a step of irradiating a hydrophobic monomer with light in the presence of a vinyl ether polymer represented by the following formula (1) to photopolymerize the monomer: 【Chemistry 1】 [In formula (1), R 1 represents an alkanediyl group having 1 to 5 carbon atoms, R 2 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 3 is -C(R 5 ) (R 6 )-CN, -C(R 7 ) (R 8 ) -X 1 , -C(R 9 ) (R 10 ) (R 11 ), -C(R 12 ) (R 13 )-(CH 2 ) a -COOR 14 , -C(R 15 ) (X 2 )-(CH 2 ) b -COOR 16 , -C(R 17 )(CN)-(CH 2 ) c -COOR 18 , -C(R 19 )(CN)-(CH 2 ) d -OH, -C(R 20 ) (R 21 ) -CON(R 22 ) H, or -C(R 23 ) (R 24 ) -CON(R 25 ) (R 26 ) (R 5 ~R 21 , R 23 and R 24 each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 22 , R 25 and R 26 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; 1 ~X 2 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group, and a to d each independently represent an integer of 0 to 8. R 4 is -S-R 27 , -S-X 3 , -S-R 28 -X 4 , -N(R 29 ) (R 30 ), -N(R 31 ) (X 5 ), -N(X 6 ) (X 7 ), -N(R 32 X 8 ) (R 33 X 9 ), or -N(X 10 ) (R 34 X 11 ) (R 27 and R 29 ~R 31 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 28 and R 32 ~R 34 each independently represents a substituted or unsubstituted alkanediyl group having 1 to 12 carbon atoms; X 3 ~X 11 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group. 29 and R 30 may form a heterocycle together with the adjacent nitrogen atom; n represents an integer from 1 to 10; p represents the number of repeating units. 【Chemistry 2】 [In formula (2), Z represents a repeating unit derived from the hydrophobic monomer, q represents the number of repeating units derived from the hydrophobic monomer, R 1 , R 2 , R 3 , R 4 , n and p are as defined above.

2. The method according to claim 1, wherein the hydrophobic monomer is at least one hydrophobic monomer selected from the group consisting of aromatic vinyl hydrophobic monomers, (meth)acrylic acid ester hydrophobic monomers, N-substituted (meth)acrylamide hydrophobic monomers, olefin hydrophobic monomers, (meth)acrylonitrile hydrophobic monomers, N-vinyl group-containing heterocyclic hydrophobic monomers, halogenated vinyl hydrophobic monomers, and vinyl carboxylate hydrophobic monomers.

3. The method of claim 1 , wherein the hydrophobic monomer is a hydrophobic conjugated monomer.

4. The method according to claim 1, wherein the hydrophobic monomer is at least one hydrophobic monomer selected from the group consisting of aromatic vinyl hydrophobic monomers, (meth)acrylic acid ester hydrophobic monomers, and N-substituted (meth)acrylamide hydrophobic monomers.

5. R 3 But -C(R 5 ) (R 6 )-CN, -C(R 12 ) (R 13 )-(CH 2 ) a -COOR 14 , -C(R 15 ) (X 2 )-(CH 2 ) b -COOR 16 , -C(R 17 )(CN)-(CH 2 ) c -COOR 18 , or -C(R 19 )(CN)-(CH 2 ) d The method according to claim 1, wherein the alkyl group is —OH.

6. R 4 But -N(R 29 ) (R 30 ), -N(R 31 ) (X 5 ), -N(X 6 ) (X 7 ), -N(R 32 X 8 ) (R 33 X 9 ), or -N(X 10 ) (R 34 X 11 2. The method according to claim 1 , wherein

7. The method according to claim 1 , wherein the block copolymer is a particulate block copolymer.

8. A fine particle comprising a block copolymer represented by the following formula (2): 【Chemistry 3】 [In formula (2), R 1 represents an alkanediyl group having 1 to 5 carbon atoms, R 2 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 3 is -C(R 5 ) (R 6 )-CN, -C(R 7 ) (R 8 ) -X 1 , -C(R 9 ) (R 10 ) (R 11 ), -C(R 12 ) (R 13 )-(CH 2 ) a -COOR 14 , -C(R 15 ) (X 2 )-(CH 2 ) b -COOR 16 , -C(R 17 )(CN)-(CH 2 ) c -COOR 18 , -C(R 19 )(CN)-(CH 2 ) d -OH, -C(R 20 ) (R 21 ) -CON(R 22 ) H, or -C(R 23 ) (R 24 ) -CON(R 25 ) (R 26 ) (R 5 ~R 21 , R 23 and R 24 each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 22 , R 25 and R 26 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; 1 ~X 2 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group, and a to d each independently represent an integer of 0 to 8. R 4 is -S-R 27 , -S-X 3 , -S-R 28 -X 4 , -N(R 29 ) (R 30 ), -N(R 31 ) (X 5 ), -N(X 6 ) (X 7 ), -N(R 32 X 8 ) (R 33 X 9 ), or -N(X 10 ) (R 34 X 11 ) (R 27 and R 29 ~R 31 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 28 and R 32 ~R 34 each independently represents a substituted or unsubstituted alkanediyl group having 1 to 12 carbon atoms; X 3 ~X 11 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group. 29 and R 30 may form a heterocycle together with the adjacent nitrogen atom; n represents an integer from 1 to 10; p represents the number of repeating units, Z represents a repeating unit derived from a hydrophobic monomer, and q represents the number of repeating units derived from a hydrophobic monomer.

9. The microparticle of claim 8 , wherein the hydrophobic monomer is a hydrophobic conjugated monomer.

10. A photopolymerization initiator containing a vinyl ether polymer represented by the following formula (1): 【Chemistry 4】 [In formula (1), R 1 represents an alkanediyl group having 1 to 5 carbon atoms, R 2 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 3 is -C(R 5 ) (R 6 )-CN, -C(R 7 ) (R 8 ) -X 1 , -C(R 9 ) (R 10 ) (R 11 ), -C(R 12 ) (R 13 )-(CH 2 ) a -COOR 14 , -C(R 15 ) (X 2 )-(CH 2 ) b -COOR 16 , -C(R 17 )(CN)-(CH 2 ) c -COOR 18 , -C(R 19 )(CN)-(CH 2 ) d -OH, -C(R 20 ) (R 21 ) -CON(R 22 ) H, or -C(R 23 ) (R 24 ) -CON(R 25 ) (R 26 ) (R 5 ~R 21 , R 23 and R 24 each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 22 , R 25 and R 26 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; 1 ~X 2 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group, and a to d each independently represent an integer of 0 to 8. R 4 is -S-R 27 , -S-X 3 , -S-R 28 -X 4 , -N(R 29 ) (R 30 ), -N(R 31 ) (X 5 ), -N(X 6 ) (X 7 ), -N(R 32 X 8 ) (R 33 X 9 ), or -N(X 10 ) (R 34 X 11 ) (R 27 and R 29 ~R 31 each independently represents a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms; R 28 and R 32 ~R 34 each independently represents a substituted or unsubstituted alkanediyl group having 1 to 12 carbon atoms; X 3 ~X 11 each independently represents a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted pyrenyl group, or a substituted or unsubstituted pyridyl group. 29 and R 30 may form a heterocycle together with the adjacent nitrogen atom; n represents an integer from 1 to 10; p represents the number of repeating units.

11. The photoinitiator of claim 10 which is a photo-RAFT polymerization initiator.

Citation Information

Patent Citations

  • Method of producing block copolymer

    JP2013040245A

  • Method for producing alkenyl ether-based polymer

    JP2016210887A