Toner for developing electrostatic charge image, electrostatic charge image developing agent, toner cartridge, process cartridge and image formation device

The toner formulation with crosslinked resin particles and controlled porosity addresses the issue of image gloss instability at high temperatures, ensuring both low-temperature fixability and gloss stability during storage.

JP2024137414APending Publication Date: 2024-10-07FUJIFILM BUSINESS INNOVATION CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023048935
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing toners with low glass transition temperature resin particles exhibit increased image glossiness when stored at high temperatures, compromising low-temperature fixability and image gloss stability during high-pressure storage.

Method used

A toner formulation containing crosslinked resin particles with specific porosity and glass transition temperature ranges, along with a controlled void ratio, to enhance both low-temperature fixability and image gloss stability.

Benefits of technology

The toner achieves both low-temperature fixability and image gloss stability during high-pressure storage by controlling the exposure of crosslinked resin particles and maintaining image quality under varying conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137414000001_ABST
    Figure 2024137414000001_ABST
Patent Text Reader

Abstract

To achieve both low-temperature fixability and image gloss stability in high-pressure storage, as compared with the case that in a toner to which crosslinked resin particles are added, a porosity in the toner is less than 1% or more than 10%.SOLUTION: Provided is a toner for developing an electrostatic charge image. On a cut surface of the toner for developing an electrostatic charge image, an area ratio (Sc) of the crosslinked resin particles, a porosity (Se) on the cut surface, and a ratio Se / Sc of the porosity (Se) to the area ratio (Sc) are 5% or more and 40% or less, 1% more and 10% or less, and 0.05 or more and 1.5 or less, respectively.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner for developing an electrostatic image, an electrostatic image developer, a toner cartridge, a process cartridge and an image forming apparatus. [Background technology]

[0002] Patent Document 1 discloses a toner for developing electrostatic images, which comprises toner particles containing a binder resin having a domain-matrix structure and a colorant, the toner particles having a volume-based median diameter of 4.3 to 7.0 μm, the matrix phase in the binder resin is composed of a polymer of a styrene-acrylic resin or a polyester resin, and the domain phase in the binder resin is composed of a polymer containing a structural unit derived from a diene monomer, the size of the domain phase is 50 to 300 nm in Feret diameter, and the glass transition temperature of the polymer constituting the domain phase is in the range of -85 to +35°C. Patent Document 2 discloses an electrophotographic toner obtained by agglomerating and coalescing particles containing a binder resin including polyester in an aqueous medium in the presence of a monovalent salt, the toner having a volume median particle size (D50) of 2 to 7 μm and a ratio of the total pore area to the particle area (total pore area / particle area) in the cross section of the toner particle of 1.0 to 6%. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2011-257744 A [Patent Document 2] JP 2008-257056 A Summary of the Invention [Problem to be solved by the invention]

[0004] It is known that resin particles with a low glass transition temperature are added to the toner to improve the fixing property of the toner. However, when fixed images using such toners are stored in a stacked state at high temperatures, the image glossiness may increase. For this reason, it has been difficult to achieve both low-temperature fixing property and image gloss stability during high-pressure storage. The present invention aims to achieve both low-temperature fixability and image gloss stability during high-pressure storage in a toner to which crosslinked resin particles have been added, compared to toners with a void ratio of less than 1% or more than 10%. [Means for solving the problem]

[0005] The invention of claim 1 is a toner for developing electrostatic images comprising a binder resin and crosslinked resin particles, wherein, on a surface obtained by cutting the toner for developing electrostatic images, the area ratio (Sc) of the crosslinked resin particles is 5% or more and 40% or less, the porosity (Se) of the cut surface is 1% or more and 10% or less, and the ratio Se / Sc of the porosity (Se) to the area ratio (Sc) is 0.05 or more and 1.5 or less. A second aspect of the present invention provides the toner for developing electrostatic images according to the first aspect, wherein the glass transition temperature Tg of the crosslinked resin particles is 0° C. or higher and 30° C. or lower. The invention of claim 3 is the toner for developing electrostatic images according to claim 1, wherein the crosslinked resin particles have a tetrahydrofuran insoluble content of 90% by mass or more and a swelling degree of 2 or more and 10 or less when permeated in tetrahydrofuran for 24 hours. The invention of claim 4 provides the toner for developing electrostatic images according to claim 1, wherein the crosslinked resin particles contain a styrene-(meth)acrylate copolymer. The invention of claim 5 is the toner for developing electrostatic images according to claim 1, wherein the crosslinked resin particles have, as units derived from a (meth)acrylate monomer, units derived from a monofunctional (meth)acrylate monomer and a bifunctional (meth)acrylate monomer, and the units derived from the monofunctional (meth)acrylate monomer include a unit derived from a (meth)acrylate monomer having a carboxyl group and a unit derived from a (meth)acrylate monomer not having a carboxyl group. The invention of claim 6 is the toner for developing electrostatic images according to claim 5, wherein the mass ratio of the units derived from the (meth)acrylate monomer having a carboxyl group in the crosslinked resin particles is from 0.01 mass % to 0.50 mass %. The invention of claim 7 provides the toner for developing electrostatic images according to claim 1, wherein the binder resin contains an amorphous polyester resin. The invention of claim 8 is the toner for developing electrostatic images according to claim 7, wherein, when the glass transition temperature of the amorphous polyester resin is T1 (°C) and the glass transition temperature of the crosslinked resin particles is T2 (°C), 30≦T1-T2≦70 (°C). The invention of claim 9 provides the toner for developing electrostatic images according to claim 7, wherein the acid value of the amorphous polyester resin is 5 mgKOH / g or more and 20 mgKOH / g or less. The invention of claim 10 provides the toner for developing electrostatic images according to claim 7, wherein the sum of the acid value (mgKOH / g) and the hydroxyl value (mgKOH / g) of the amorphous polyester resin is 15 or more and 40 or less. The invention of claim 11 is the toner for developing electrostatic images according to claim 7, wherein the amorphous polyester resin contains units derived from an aliphatic dicarboxylic acid represented by formula (1), and the proportion of units derived from an aliphatic dicarboxylic acid in the entire units derived from dicarboxylic acid of the amorphous polyester resin is 1 mol % or more and 30 mol % or less. Formula (1) -OC-(CH2) n -CO- (wherein n is an integer of 4 or more and 12 or less). The invention of claim 12 provides the toner for developing electrostatic images according to claim 1, wherein the binder resin contains 15% by mass or more and 40% by mass or less of a crystalline resin. The invention of claim 13 provides the toner for developing electrostatic images according to claim 1, wherein the average equivalent circle diameter of the domains formed by the crosslinked resin particles is 50 nm or more and 300 nm or less. The invention of claim 14 provides the toner for developing electrostatic images according to claim 1, wherein the average shape factor SF-1 of the domains formed by the crosslinked resin particles is 130 or less. The invention of claim 15 provides the toner for developing electrostatic images according to claim 1, wherein in the number average particle size distribution of the toner for developing electrostatic images, a particle size distribution index GSD(p) represented by the formula (2) is 1.20 or more and 1.35 or less. Equation (2) GSD(p)=1+(D50(p)-D16(p)) / D50(p) (In the formula, D16(p) and D50(p) are the particle sizes at which the cumulative numbers are 16% and 50%, respectively, in the cumulative curve of the number particle size distribution.) The invention of claim 16 is the toner for developing electrostatic images according to claim 1, wherein the toner for developing electrostatic images contains one or more elements selected from the group consisting of aluminum, molybdenum, and magnesium. The invention of claim 17 is an electrostatic image developer containing the toner for developing electrostatic images according to any one of claims 1 to 16. The invention of claim 18 is a toner cartridge that contains the electrostatic image developing toner according to any one of claims 1 to 16 and is detachably mountable to an image forming apparatus. The invention of claim 19 is a process cartridge that contains the electrostatic image developer according to claim 17, has a developing means that develops an electrostatic image formed on the surface of an image carrier using the electrostatic image developer into a toner image, and is detachably attached to an image forming apparatus. The invention of claim 20 is an image forming apparatus comprising an image holder, a charging means for charging the surface of the image holder, an electrostatic image forming means for forming an electrostatic image on the charged surface of the image holder, a developing means that contains the electrostatic image developer described in claim 17 and develops the electrostatic image formed on the surface of the image holder as a toner image using the electrostatic image developer, a transfer means that transfers the toner image formed on the surface of the image holder to the surface of a recording medium, and a fixing means that fixes the toner image transferred to the surface of the recording medium. Effect of the Invention

[0006] According to the invention of claim 1, in a toner for developing electrostatic images containing a binder resin and crosslinked resin particles, it is possible to achieve both low-temperature fixability and image gloss stability during high-pressure storage, compared to when the ratio Se / Sc of the void ratio (Se) to the area ratio (Sc) is less than 0.05 or exceeds 1.5. According to the invention of claim 2, a toner for developing electrostatic images having good low-temperature fixing properties can be provided, as compared with a toner having a glass transition temperature Tg of less than 0°C or more than 30°C. According to the invention of claim 3, the crosslinked resin particles have an appropriate degree of crosslinking and swelling compared to when the crosslinked resin particles have a tetrahydrofuran insoluble content of less than 90% by mass, or when the swelling degree when soaked in tetrahydrofuran for 24 hours is less than 2 or more than 10, and therefore it is possible to prevent the crosslinked resin particles from flowing and being exposed to the toner surface during fixing. According to the invention of claim 4, the crosslinked resin particles can be controlled so that they aggregate more easily than a case in which the crosslinked resin particles do not contain a styrene-(meth)acrylate copolymer, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of claim 5, compared to a case in which the units derived from a monofunctional (meth)acrylate monomer do not include the three types of units derived from a (meth)acrylate monomer having a carboxyl group, a unit derived from a (meth)acrylate monomer not having a carboxyl group, and a unit derived from a bifunctional (meth)acrylate monomer, the crosslinked resin particles can be controlled to be more easily aggregated, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of claim 6, the crosslinked resin particles can be controlled so that they are more likely to aggregate than crosslinked resin particles having a mass ratio of units derived from a (meth)acrylate monomer having a carboxyl group that is less than 0.01 mass % or more than 0.50 mass %, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of claim 7, the binder resin can be controlled so that the crosslinked resin particles are more likely to aggregate than when the binder resin does not contain an amorphous polyester resin, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of claim 8, when the glass transition temperature of the amorphous polyester resin is T1 (°C) and the glass transition temperature of the crosslinked resin particles is T2 (°C), the crosslinked resin particles can be controlled to be more likely to aggregate than when (T1-T2) is less than 30°C or exceeds 70°C, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of claim 9, it is possible to provide a toner for developing electrostatic images in which the crosslinked resin particles can be controlled to be more easily aggregated than when the acid value of the amorphous polyester resin is less than 5 mgKOH / g or more than 20 mgKOH / g, and the void ratio is controlled within a suitable range. According to the invention of claim 10, the sum of the acid value (mg KOH / g) and the hydroxyl value (mg KOH / g) of the amorphous polyester resin can be controlled so that the crosslinked resin particles are more likely to aggregate than when the sum is less than 15 or more than 40, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided.

[0007] According to the invention of claim 11, the amorphous polyester resin contains units derived from an aliphatic dicarboxylic acid represented by formula (1), and compared with a case in which the ratio of units derived from an aliphatic dicarboxylic acid in the entire dicarboxylic acid-derived units of the amorphous polyester resin is less than 1 mol % or exceeds 30 mol %, the crosslinked resin particles can be controlled to be more easily aggregated, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of claim 12, by setting the binder resin to a suitable ratio of crystalline resin to amorphous resin, it is possible to provide a toner for developing electrostatic images having improved low-temperature fixing properties, compared to a case where the binder resin contains less than 15% by mass or more than 40% by mass of crystalline resin. According to the invention of claim 13, it is possible to provide a toner for developing electrostatic images, which is more effectively prevented from being exposed to the surface of a fixed image by controlling the domain size of the crosslinked resin particles, compared to a case where the average equivalent circular diameter of the domains formed by the crosslinked resin particles is less than 50 nm or more than 300 nm. According to the invention of claim 14, it is possible to provide a toner for developing electrostatic images, which is more prevented from being exposed to the surface of a fixed image by controlling the domain size of the crosslinked resin particles, compared to a case where the average shape factor SF-1 of the domains formed by the crosslinked resin particles exceeds 130. According to the invention of claim 15, in the number-average particle size distribution of the toner for developing electrostatic images, compared with the case where the particle size distribution index GSD(p) represented by the formula (2) is less than 1.20 or exceeds 1.35, small diameter particles are more likely to be exposed to the surface. However, by controlling the number of small diameter particles, it is possible to provide a toner for developing electrostatic images in which exposure to the surface of a fixed image is more effectively prevented. According to the invention of claim 16, it is possible to provide a toner for developing electrostatic images having improved fixing properties by including an element having high thermal conductivity in the toner particles, compared to a toner for developing electrostatic images not including one or more elements selected from the group consisting of aluminum, molybdenum, and magnesium, which increases thermal conductivity outside the voids. According to the invention of claim 17, 18, 19 or 20, in a toner for developing electrostatic images containing a binder resin and crosslinked resin particles, it is possible to provide an electrostatic image developer, a toner cartridge, a process cartridge, or an image forming apparatus which can achieve both low-temperature fixing ability and image gloss stability during high-pressure storage, compared with a case in which the ratio Se / Sc of the void ratio (Se) to the area ratio (Sc) is less than 0.05 or exceeds 1.5. [Brief description of the drawings]

[0008] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a process cartridge that is detachably mounted to the image forming apparatus according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the present invention will be described. The description and examples are merely illustrative of the embodiments, and do not limit the scope of the present invention.

[0010] In the present disclosure, the descriptions "from XX to XX" or "XX to XX" expressing a numerical range mean a numerical range including the stated upper and lower limits, unless otherwise specified. In addition, in the present disclosure, when referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the description means the total amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the "toner for developing electrostatic images" may be simply referred to as "toner", the "carrier for developing electrostatic images" may be simply referred to as "carrier", and the "electrostatic image developer" may be simply referred to as "developer". In the present disclosure, (meth)acrylic means both acrylic and methacrylic.

[0011] <Toner for developing electrostatic images> The electrostatic image developing toner according to this embodiment is a toner for developing electrostatic images comprising a binder resin and crosslinked resin particles, and on a surface obtained by cutting the electrostatic image developing toner, the area ratio (Sc) of the crosslinked resin particles is 5% or more and 40% or less, the porosity (Se) of the cut surface is 1% or more and 10% or less, and the ratio Se / Sc of the porosity (Se) to the area ratio (Sc) is 0.01 or more and 0.5 or less.

[0012] Toners that contain crosslinked resin particles with a low glass transition temperature and rubber elasticity have been disclosed. When such toners are used, the toner particles are heated and deformed during fixing, which may expose the crosslinked resin particles on the image surface. It is presumed that if an image with exposed particles is stacked at high temperatures, the crosslinked resin particles will not deform during fixing because of their low glass transition temperature, but will be smoothed by being exposed to high pressure for a long period of time after image formation, leading to an increase in the glossiness of the image. On the other hand, the toner according to the present embodiment has the above-mentioned constitution, and therefore can achieve both low-temperature fixability and image gloss stability during high-pressure storage. The mechanism behind this is presumed to be as follows.

[0013] When a toner structure as in this embodiment is formed, it is presumed that the formation of appropriate voids inside the toner reduces thermal conduction to the center of the toner, suppressing the temperature rise inside the toner compared to the toner surface, and as a result, it is possible to suppress the exposure of the crosslinked resin particles to the surface during fixing. Furthermore, due to the presence of voids, it is believed that the crosslinked resin particles tend to spread into the voids rather than being exposed to the outside of the toner even during fixing, and exposure of the particles to the toner surface is suppressed, which is presumably why changes in image gloss can be suppressed even during stacking. From the above, it is presumed that the toner structure of this embodiment can achieve both low-temperature fixability and image gloss stability during high-pressure storage.

[0014] The configuration of the toner for developing electrostatic images according to this embodiment will be described in detail below. The toner for developing electrostatic images according to the present embodiment contains a binder resin and crosslinked resin particles. The toner particles contain, for example, a binder resin, crosslinked resin particles, and, if necessary, a colorant, a release agent, and other additives.

[0015] -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.

[0016] The binder resin preferably contains a polyester resin. By including a polyester resin as the binder resin, when a styrene-(meth)acrylic copolymer is used as the crosslinked resin particles as described below, the crosslinked resin particles can be controlled to be more likely to aggregate, and the void ratio can be controlled within a suitable range. The binder resin preferably contains an amorphous resin and a crystalline resin. Here, the term "amorphous resin" refers to a resin that, in a thermal analysis measurement using differential scanning calorimetry (DSC), has only a stepwise endothermic change rather than a clear endothermic peak, is a solid at room temperature, and is thermoplasticized at a temperature equal to or higher than the glass transition temperature. On the other hand, a crystalline resin is one that has a clear endothermic peak rather than a stepwise change in endothermic amount in differential scanning calorimetry (DSC). For example, a crystalline resin is one whose endothermic peak has a half-width of 10°C or less when measured at a heating rate of 10°C / min.

[0017] The amorphous resin will be described. Examples of the amorphous resin include known amorphous resins such as amorphous polyester resin, amorphous vinyl resin (e.g., styrene-acrylic resin, etc.), epoxy resin, polycarbonate resin, polyurethane resin, etc. Among these, amorphous polyester resin and amorphous vinyl resin (particularly styrene-acrylic resin) are preferred, and amorphous polyester resin is more preferred.

[0018] Amorphous polyester resin The amorphous polyester resin may be, for example, a condensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. The amorphous polyester resin may be a commercially available product or a synthesized product.

[0019] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). Among these, aliphatic dicarboxylic acids such as adipic acid and sebacic acid, which are units represented by formula (1), are preferred as polyvalent carboxylic acids. Formula (1) -OC-(CH2) n -CO- (In the formula, n is an integer of 4 or more and 12 or less.) When the unit of formula (1) is used, the unit derived from the aliphatic dicarboxylic acid is preferably 1 mol% or more and 30 mol% or less, more preferably 3 mol% or more and 20 mol% or less, of the units derived from the acid component monomer of the amorphous polyester resin. By using the unit of formula (1), it is possible to control the crosslinked resin particles to be more easily aggregated, and the void ratio can be controlled to a suitable range. In addition, when two or more kinds of amorphous polyester resins are used in combination, it is preferable that the unit derived from the aliphatic dicarboxylic acid is included in the above range in the weighted average.

[0020] The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower (e.g., carbon number 1 to 5) alkyl esters thereof. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0021] Examples of polyhydric alcohols include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol, a polyhydric alcohol having a crosslinked or branched structure of three or more may be used in combination with the diol. Examples of the polyhydric alcohol having a trihydric or higher valence include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.

[0022] The acid value of the amorphous polyester resin is preferably 5 mgKOH / g or more and 20 mgKOH / g or less, more preferably 7 mgKOH / g or more and 16 mgKOH / g or less, from the viewpoint of being able to control the crosslinked resin particles to be more easily aggregated and being able to control the void ratio within a suitable range. Furthermore, the sum of the acid value and the hydroxyl value is preferably 15 to 40. The acid value and hydroxyl value of the amorphous polyester resin are measured as follows. The toner to be measured is dissolved in tetrahydrofuran (THF) to remove insoluble components, and then the amorphous polyester resin is separated. The separated amorphous polyester resin is used to measure the acid value and hydroxyl value of the resin according to the method (neutralization titration method) specified in JIS K0070-1992. The acid value refers to the number of milligrams of potassium hydroxide required to neutralize the acid groups (e.g., carboxyl groups) in 1 g of sample, and the hydroxyl value refers to the number of milligrams of potassium hydroxide required to neutralize the acetic acid bonded to the hydroxyl groups when 1 g of sample is acetylated.

[0023] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 70°C or lower. The glass transition temperature is determined from a DSC curve obtained by a differential scanning calorimeter (DSC), more specifically, from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics". The method for determining the glass transition temperature is the same for other resins. The glass transition temperature of the amorphous polyester resin is measured for the melt-separated amorphous polyester resin by the method described in the acid value measurement.

[0024] The weight average molecular weight (Mw) of the amorphous polyester resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the amorphous polyester resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the amorphous polyester resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.

[0025] The amorphous polyester resin can be obtained by a known manufacturing method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.

[0026] The crystalline resin will now be described. The crystalline resin may be a crystalline polyester resin, a crystalline vinyl resin (e.g., polyal Examples of the crystalline resin include known crystalline resins such as xylene resins and long-chain alkyl (meth)acrylate resins. Among these, crystalline polyester resins are preferred from the viewpoints of the mechanical strength and low-temperature fixability of the toner.

[0027] Crystalline polyester resin The crystalline polyester resin may be, for example, a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol. The crystalline polyester resin may be a commercially available product or a synthesized product. Here, the crystalline polyester resin is preferably a polycondensate using a polymerizable monomer having a linear aliphatic group rather than a polymerizable monomer having an aromatic group, since the crystalline polyester resin can easily form a crystalline structure.

[0028] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower alkyl esters (e.g., carbon number 1 to 5). As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0029] Examples of polyhydric alcohols include aliphatic diols (for example, straight-chain aliphatic diols having 7 to 20 carbon atoms in the main chain). Examples of aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred as aliphatic diols. The polyhydric alcohol may be a trihydric or higher alcohol having a crosslinked or branched structure in combination with the diol. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds. Here, the polyhydric alcohol has an aliphatic diol content of 80 mol % or more, preferably 90 mol % or more.

[0030] The melting temperature of the crystalline polyester resin is preferably 50°C or higher and 100°C or lower, more preferably 55°C or higher and 90°C or lower, and even more preferably 60°C or higher and 85°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics." The weight average molecular weight (Mw) of the crystalline polyester resin is preferably 6,000 or more and 50,000 or less.

[0031] The crystalline polyester resin can be obtained, for example, by a known production method, like the amorphous polyester resin.

[0032] When the toner contains a crystalline resin, the content of the crystalline resin in the entire binder resin is preferably from 15% by mass to 40% by mass, and more preferably from 17% by mass to 37% by mass. By setting the content of the crystalline resin within the above range and by setting the ratio of the crystalline resin to the amorphous resin at an appropriate ratio, the low temperature fixability of the toner can be improved.

[0033] In order to ensure the affinity between the binder resin and the crosslinked resin particles, the binder resin preferably contains an amorphous polyester resin and a crystalline polyester resin. When the binder resin contains an amorphous polyester resin and a crystalline polyester resin, the crosslinked resin particles can be more uniformly dispersed by having both of them have an aliphatic dicarboxylic acid unit. In addition, examples of the aliphatic dicarboxylic acid include the dicarboxylic acid represented by the general formula "HOOC-(CH2) n In the above general formula, n is preferably 4 to 20, and more preferably 4 to 12.

[0034] The content of the binder resin is, for example, preferably from 40% by mass to 98% by mass, more preferably from 50% by mass to 95% by mass, and even more preferably from 60% by mass to 93% by mass, based on the entire toner.

[0035] -Crosslinked resin particles- As described above, the electrostatic image developing toner according to this embodiment contains a binder resin and crosslinked resin particles. Examples of the crosslinked resin particles include crosslinked resin particles crosslinked by ionic bonds (ion-crosslinked particles), crosslinked resin particles crosslinked by covalent bonds (covalent bond crosslinked particles), etc. Among these, crosslinked resin particles crosslinked by covalent bonds are preferred.

[0036] The types of resins used in the crosslinked resin particles include polyolefin resins (polyethylene, polypropylene, etc.), styrene resins (polystyrene, α-polymethylstyrene, etc.), (meth)acrylic resins (polymethyl methacrylate, polyacrylonitrile, etc.), epoxy resins, polyurethane resins, polyurea resins, polyamide resins, polycarbonate resins, polyether resins, polyester resins, and copolymer resins thereof. These resins may be used alone or in combination of two or more types, as necessary.

[0037] Among the above resins, the resin used for the crosslinked resin particles preferably contains a styrene-(meth)acrylic copolymer. Specifically, the crosslinked resin particles preferably contain 50% by mass or more, 80% by mass or more, and more preferably 90% by mass or more of the styrene-(meth)acrylic copolymer as the main component. In particular, it is preferable that the crosslinked resin particles are substantially all styrene-(meth)acrylic copolymers. In addition, as the monomers constituting the copolymer, the total of the styrene monomer and the (meth)acrylic monomer is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The remainder is a crosslinking agent described later, and the crosslinking agent causes the crosslinked resin particles to become crosslinked particles. When the crosslinked resin particles are styrene-(meth)acrylic copolymer particles, the crosslinked resin particles can be controlled so as to be more easily aggregated, and the void ratio can be controlled within a suitable range.

[0038] The styrene-(meth)acrylic copolymer may be, for example, a resin obtained by radical polymerization of the following styrene monomer and (meth)acrylic acid monomer.

[0039] Examples of styrene-based monomers include styrene, α-methylstyrene, vinylnaphthalene, alkyl-substituted styrenes having alkyl chains such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene, halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene, and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene, etc. Among these, styrene and α-methylstyrene are preferred.

[0040] Examples of (meth)acrylic acid monomers include (meth)acrylic acid, n-methyl (meth)acrylate, n-ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, n-hexadecyl (meth)acrylate, n-octadecyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, amyl (meth)acrylate, Examples of such acrylates include neopentyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, phenyl (meth)acrylate, biphenyl (meth)acrylate, diphenylethyl (meth)acrylate, t-butylphenyl (meth)acrylate, terphenyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-carboxyethyl (meth)acrylate, (meth)acrylonitrile, and (meth)acrylamide. Among these, n-butyl (meth)acrylate and 2-carboxyethyl (meth)acrylate are preferred.

[0041] Examples of crosslinking agents for crosslinking the resin in the crosslinked resin particles include aromatic polyvinyl compounds such as divinylbenzene and divinylnaphthalene; polyvinyl esters of aromatic polyvalent carboxylic acids such as divinyl phthalate, divinyl isophthalate, divinyl terephthalate, divinyl homophthalate, divinyl trimesate, trivinyl trimesate, divinyl naphthalenedicarboxylate, and divinyl biphenylcarboxylate; divinyl esters of nitrogen-containing aromatic compounds such as divinyl pyridinedicarboxylate; vinyl esters of unsaturated heterocyclic compound carboxylic acids such as vinyl pyrromucate, vinyl furancarboxylate, vinyl pyrrole-2-carboxylate, and vinyl thiophenecarboxylate; butanediol diacrylate, butanediol dimethacrylate, hexanediol diacrylate, hexanediol dimethacrylate, octanediol diacrylate, octanediol dimethacrylate, nonanediol diacrylate, nonanediol dimethacrylate, decanediol diacrylate, decanedi ... (Meth)acrylic acid esters of linear polyhydric alcohols such as diol dimethacrylate, dodecane diol diacrylate, and dodecane diol dimethacrylate; (meth)acrylic acid esters of branched or substituted polyhydric alcohols such as neopentyl glycol dimethacrylate and 2-hydroxy, 1,3-diacryloxypropane; polyethylene glycol di(meth)acrylate, polypropylene polyethylene glycol di(meth)acrylates, divinyl succinate, divinyl fumarate, and maleic acid Examples of the crosslinking agent include polyvinyl esters of polyvalent carboxylic acids such as vinyl, divinyl maleate, divinyl diglycolate, vinyl itaconate, divinyl itaconate, divinyl acetonedicarboxylate, divinyl glutarate, divinyl 3,3'-thiodipropionate, divinyl trans-aconitate, trivinyl trans-aconitate, divinyl adipate, divinyl pimelate, divinyl suberate, divinyl azelaate, divinyl sebacate, divinyl dodecanedioate, and divinyl brassylate. The crosslinking agent may be used alone or in combination of two or more.

[0042] Among these, it is preferable to use a bifunctional alkyl acrylate having an alkylene chain with 6 or more carbon atoms as a crosslinking agent for crosslinking the resin. In other words, it is preferable that the crosslinked resin particles have a bifunctional alkyl acrylate as a constituent unit, and the alkylene chain in the bifunctional alkyl acrylate has 6 or more carbon atoms. By using crosslinked particles having a bifunctional alkyl acrylate as a constituent unit and an alkylene chain with 6 or more carbon atoms, it becomes easier to obtain a toner with an appropriate range of toner deformation during fixing and particularly good low-temperature fixing properties. When the crosslinking density of the crosslinked resin particles is high (i.e., the distance between crosslinking points is short), the elasticity becomes too high, whereas when a bifunctional acrylate having a long alkylene chain is used as a crosslinking agent, the crosslinking density becomes low (i.e., the distance between crosslinking points becomes long), and it is possible to prevent the elasticity of the crosslinked resin particles from becoming too high.

[0043] From the viewpoint of adjusting the crosslink density to an appropriate range, the number of carbon atoms in the alkylene chain in the bifunctional alkyl acrylate is preferably 6 or more, more preferably 6 to 12, and even more preferably 8 to 12. More specific examples of the bifunctional alkyl acrylate include 1,6-hexanediol acrylate, 1,6-hexanediol methacrylate, 1,8-octanediol diacrylate, 1,8-octanediol dimethacrylate, 1,9-nonanediol diacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol diacrylate, 1,10-decanediol dimethacrylate, 1,12-dodecanediol diacrylate, and 1,12-dodecanediol dimethacrylate, and among these, 1,10-decanediol diacrylate and 1,10-decanediol dimethacrylate are preferred.

[0044] As the (meth)acrylic acid-based monomer ((meth)acrylate monomer) used for the crosslinked resin particles, it is preferable to use a monofunctional (meth)acrylate monomer and a bifunctional (meth)acrylate monomer, and as the monofunctional (meth)acrylate monomer, it is preferable to use a (meth)acrylate monomer having a carboxyl group and a (meth)acrylate monomer not having a carboxyl group. By using these monomers, it is possible to control the crosslinked resin particles so that they are more likely to aggregate, and it is possible to control the void ratio within a suitable range. An example of the (meth)acrylate monomer having a carboxyl group is 2-carboxyethyl (meth)acrylate. The ratio of the unit derived from the (meth)acrylate monomer having a carboxyl group can be controlled so that the crosslinked resin particles are more likely to aggregate, and from the viewpoint of controlling the void ratio within a suitable range, it is preferably 0.01% by mass or more and 0.50% by mass or less in the crosslinked resin particles. In addition, an example of the (meth)acrylate monomer not having a carboxyl group is (meth)acrylic acid ester such as n-butyl (meth)acrylate, ethyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. An example of the bifunctional (meth)acrylate monomer is the bifunctional alkyl acrylate described as a crosslinking agent.

[0045] In addition, when the crosslinked resin particles are polymers of a composition for forming crosslinked resin particles containing a styrene-based monomer, a (meth)acrylic acid-based monomer, and a crosslinking agent, the fixability of the crosslinked resin particles may be controlled by adjusting the amount of the crosslinking agent contained in the composition. For example, by increasing the amount of the crosslinking agent contained in the composition, crosslinked resin particles with good fixability are easily obtained. The content of the crosslinking agent in the composition for forming crosslinked resin particles is, for example, preferably 0.3 parts by mass or more and 5.0 parts by mass or less, more preferably 0.5 parts by mass or more and 2.5 parts by mass or less, and even more preferably 1.0 parts by mass or more and 2.0 parts by mass or less, relative to 100 parts by mass of the total of the styrene-based monomer, the (meth)acrylic acid-based monomer, and the crosslinking agent.

[0046] The glass transition temperature Tg of the crosslinked resin particles measured by a differential scanning calorimeter is preferably 0° C. or more and 30° C. or less, and more preferably 5° C. or more and 25° C. or less. When the glass transition temperature Tg of the crosslinked resin particles is 0° C. or more and 30° C. or less, the toner has good low-temperature fixability. When the glass transition temperature of the crosslinked resin particles exceeds 30° C., the toner containing the crosslinked resin particles having a high glass transition temperature tends to have poor adhesion to paper and to have difficulty in obtaining low-temperature fixability. In addition, when particles having a glass transition temperature of less than 0° C., such as rubber particles, are used, the toner always exhibits elastic behavior from room temperature to high temperatures, and it tends to have difficulty in obtaining low-temperature fixability. The glass transition temperature of the crosslinked resin particles can be determined by extracting the crosslinked resin particles as THF insoluble matter from the toner. The constituent monomers and their ratio in the crosslinked resin particles can be determined by measuring the constituent monomer ratio in the crosslinked resin particles extracted as the insoluble matter.

[0047] When the binder resin contains an amorphous polyester resin, the glass transition temperature of the amorphous polyester resin is T1 (°C) and the glass transition temperature of the crosslinked resin particles is T2 (°C), 30≦ T1-T2 ≦70 (℃) When this relationship is satisfied, the crosslinked resin particles can be controlled so as to aggregate more easily, and the void ratio can be controlled within a suitable range. The glass transition temperature T1 of the amorphous polyester resin can be measured by dissolving the toner in THF, removing the insoluble components, and then taking out the amorphous polyester resin.

[0048] The crosslinked resin particles preferably have a THF insoluble content of 90% by mass or more, and a swelling degree of 2 to 10 when soaked in THF for 24 hours. The crosslinked resin particles have an appropriate crosslinking and swelling degree, so that the crosslinked resin particles can be prevented from flowing and being exposed to the toner surface during fixing. It is more preferable that the THF insoluble content is 95% by mass or more, and the swelling degree is 3 to 8.

[0049] In the crosslinked resin particles, the glass transition temperature, THF insoluble content, swelling degree, etc. can be adjusted by adjusting the monomer composition ratio of the copolymer, polymerization conditions, etc. For example, the progress of the reaction can be controlled by adjusting the polymerization conditions such as the polymerization temperature, polymerization time, and the method of adding the polymerization initiator. The THF insoluble content and swelling degree of the crosslinked resin particles can be determined as follows. The mass of the mesh encasing the resin is measured (measured mass: m1). Next, the sample to be measured (crosslinked resin particles) is dried, wrapped and sealed in the mesh, and then the mass is measured (measured mass: m2). The mesh-wrapped sample is immersed in THF for 24 hours and then removed. The solvent on the surface of the removed sample is wiped off and the mass is measured (measured mass: m3). Next, the sample is dried while still wrapped in the mesh, and the mass after drying is measured (measured mass: m4). Using each of the measured masses m1 to m4, the THF insoluble content and the degree of swelling are calculated according to the following formulas. THF insoluble amount (mass%)=(m4-m1) / (m2-m1)×100 Swelling degree = (m3-m1) / (m4-m1)

[0050] The content of the crosslinked resin particles is preferably from 2% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the entire toner. When the content of the crosslinked resin particles is within the above range, it is possible to prevent images from adhering to each other and to achieve low-temperature fixability at the same time. The ratio w1 / w2 of the content w1 of the crosslinked resin particles in the toner to the content w2 of the crystalline resin in the toner is preferably 0.2 or more and 2.0 or less, and more preferably 0.3 or more and 1.5 or less. When w1 / w2 is in the above range, the ratio of the crystalline resin to the crosslinked resin particles is in a specific range, the toner deforms appropriately during fixing, and low-temperature fixing properties of the toner can be obtained.

[0051] When the crosslinked resin particles are crosslinked particles, the constituent monomer ratio of the entire crosslinked resin particles can be obtained by measuring the constituent monomer ratio for the crosslinked resin particles extracted as tetrahydrofuran (THF) insoluble matter from the toner.

[0052] The average equivalent circle diameter of the domains formed in the toner by the individual crosslinked resin particles is preferably 50 nm to 300 nm, more preferably 80 nm to 250 nm. By controlling the domain size of the crosslinked resin particles, exposure to the fixed image surface can be further prevented. The measurement is carried out by the following method. The toner is mixed into the epoxy resin and embedded, and the epoxy resin is solidified. The solidified material obtained is cut using an ultramicrotome (Ultracut UCT, manufactured by Leica) to prepare a thin section sample with a thickness of 80 nm to 130 nm. Next, the obtained thin section sample is stained with ruthenium tetroxide for 3 hours in a desiccator at 30°C. Then, an SEM image of the stained thin section sample is obtained using an ultra-high resolution field emission scanning electron microscope (FE-SEM, Hitachi High-Technologies Corporation, S-4800). Since the ease with which the release agent, styrene-(meth)acrylic resin, and polyester resin are stained by ruthenium tetroxide differs, each component is identified by the shade due to the degree of staining. If it is difficult to distinguish the shade due to the condition of the sample, the staining time is adjusted. In the cross section of a toner particle, the colorant domain is smaller than the release agent domain and the crosslinked resin particle domain, and therefore is distinguished by size.

[0053] The average equivalent circular diameter of the domains of the individual crosslinked resin particles is a value measured by the following method. In the SEM image, 30 toner cross sections whose maximum length is 85% or more of the volume average particle diameter of the toner particles are selected, and a total of 100 domains of the dyed crosslinked resin particles are observed. The maximum length of each domain is measured, and the maximum length is regarded as the diameter of the domain, and the arithmetic average of the maximum lengths is regarded as the average equivalent circle diameter. The average equivalent circular diameter of the domains of the crosslinked resin particles can be adjusted, for example, by producing toner particles by aggregation and coalescence and adjusting the volume average particle diameter of the crosslinked resin particles contained in the crosslinked resin particle dispersion used in the production; by preparing a plurality of crosslinked resin particle dispersions having different volume average particle diameters and using them in combination; or the like.

[0054] The average shape factor SF-1 of the domains of the individual crosslinked resin particles is preferably equal to or less than 130. By making SF-1 equal to or less than 130, fixing is not hindered and post-processing machine staining can be prevented. The average shape factor SF-1 is calculated by the following formula: SF-1=(ML / A) × (π / 4) × 100 In the above formula, ML represents the absolute maximum length of the toner, and A represents the projected area of ​​the toner. Specifically, samples are prepared in the same manner as in the measurement of the average circle equivalent diameter of the domains. Thirty toner cross sections whose maximum length is 85% or more of the volume average particle diameter of the toner particles are selected from the SEM images, and a total of 100 domains of dyed resin particles are observed. The observed SEM images are imported into an image analysis processing system, Luzex (manufactured by Nireco Corporation), and the maximum length and projected area of ​​the 100 particles are obtained, and the average value is calculated using the above formula.

[0055] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, ultramarine blue, and tetrahydrofuran. Examples of the dyes include various pigments such as phosphorus blue, chalcoil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate, and various dyes such as acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes. The colorant may be used alone or in combination of two or more kinds.

[0056] The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination. The content of the colorant is, for example, preferably from 1% by mass to 30% by mass, and more preferably from 3% by mass to 15% by mass, based on the total mass of the toner particles.

[0057] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.

[0058] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" as described in the method for determining melting temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics." The content of the release agent is, for example, preferably from 1% by mass to 20% by mass, and more preferably from 4% by mass to 15% by mass, based on the total amount of the toner particles.

[0059] -Other additives- Examples of other additives include well-known additives such as magnetic materials, charge control agents, inorganic powders, etc. These additives are contained in the toner particles as internal additives.

[0060] -Characteristics of toner, etc.- The toner may be toner particles having a single layer structure, or toner particles having a so-called core-shell structure composed of a core part (core particle) and a coating layer (shell layer) that coats the core part. Here, the toner particles having a core-shell structure may be composed of, for example, a core portion containing a binder resin, crosslinked resin particles, and, if necessary, other additives such as a colorant and a release agent, and a coating layer containing a binder resin and crosslinked resin particles.

[0061] As described above, the area ratio (Sc) of the crosslinked resin particles on the cut surface of the toner is 5% to 40%, the porosity (Se) of the cut surface is 1% to 10%, and the ratio Se / Sc of the porosity (Se) to the area ratio (Sc) is 0.05 to 1.5. By satisfying these relationships, it is possible to achieve both low-temperature fixability and image gloss stability during high-pressure storage. More preferred ranges are the area ratio (Sc) of 8% to 35%, the porosity (Se) of the cut surface is 1.5% to 8%, and Se / Sc is 0.08 to 1.3. The area ratio (Sc) and void ratio (Se) are measured in the same manner as in the measurement of the average equivalent circle diameter of the domains formed in the toner by the crosslinked resin particles described above, by staining a thin sample with ruthenium tetroxide and obtaining an SEM image.

[0062] In the number-average particle size distribution of the toner, the particle size distribution index GSD(p) represented by formula (2) is preferably 1.20 to 1.35. When GSD(p) is within this range, small diameter particles are more likely to be exposed to the surface, but exposure to the fixed image surface can be prevented by controlling the number of small diameter particles. Formula (2): GSD(p)=1+(D50(p)-D16(p)) / D50(p) (In the formula, D16(p) and D50(p) are the particle sizes at which the cumulative numbers are 16% and 50%, respectively, in the cumulative curve of the number particle size distribution.)

[0063] The volume average particle size D50(v) of the toner particles is preferably from 2 μm to 10 μm, more preferably from 4 μm to 8 μm, and even more preferably from 4 μm to 7 μm. The various average particle sizes and particle size distribution indexes of the toner particles are measured using a Coulter Multisizer 3 (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer 3 with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the particle size distribution measured, cumulative distributions are drawn for the volume and number of particles for each divided particle size range (channel), starting from the smallest diameter side. The particle size at 16% of the cumulative total is defined as the volumetric particle size D16(v) and number particle size D16(p), and the particle size at 50% of the cumulative total is defined as the volume average particle size D50(v) and cumulative number average particle size D50(p). The volume average particle diameter D50(v) is calculated using this method. Using these, the number particle size distribution index GSD(p) is Formula (2): GSD(p)=1+(D50(p)-D16(p)) / D50(p) It is calculated as:

[0064] The average circularity of the toner particles is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less. The average circularity of toner particles is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. First, the toner particles to be measured are sucked and collected, flattened, and a still image of the particles is captured by instantaneous strobe light emission, and the particle image is analyzed by a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation). The number of samples to be taken in order to calculate the average circularity is 3,500. When the toner contains an external additive, the toner (developer) to be measured is dispersed in water containing a surfactant, and then ultrasonic treatment is performed to obtain toner particles from which the external additive has been removed.

[0065] -External additives- Examples of the external additive include inorganic particles, such as SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, K2O·(TiO2)n, Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, and MgSO4. Among them, it is preferable to contain one or more elements selected from the group consisting of aluminum, molybdenum, and magnesium. By containing an element with high thermal conductivity in the toner particles, it is possible to increase the thermal conductivity in the areas other than the voids, thereby improving the fixing property. These elements are preferably contained in the toner as external additives, but can also be contained as internal additives.

[0066] The surface of the inorganic particles as an external additive may be subjected to a hydrophobic treatment. The hydrophobic treatment may be performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the inorganic particles.

[0067] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate (PMMA), and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles). The amount of the external additive added is, for example, preferably from 0.01% by mass to 8.0% by mass, and more preferably from 0.01% by mass to 6.0% by mass, based on the toner particles.

[0068] (Toner manufacturing method) Next, a method for producing the toner according to the present embodiment will be described. The toner according to the exemplary embodiment can be obtained by producing toner particles and then adding an external additive to the toner particles, if necessary.

[0069] The toner particles may be produced by any of a dry production method (e.g., a kneading and pulverizing method, etc.) and a wet production method (e.g., an aggregation-coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). The method for producing the toner particles is not particularly limited, and a well-known production method is adopted. Among these, it is preferable to obtain toner particles by an aggregation / coalescence method, which is one of the emulsion aggregation methods, in order to control the void ratio and domain size. In the emulsion aggregation method, the void ratio can be controlled by controlling the aggregation state when the dispersion of the toner raw materials is mixed. Specifically, when the dispersion liquid of the raw material is aggregated, if the crosslinked resin particles are preferentially aggregated and the dispersion liquid of the binder resin is attached around them, the crosslinked resin particles will not be integrated even in the toner fusing process, and the gaps formed when the crosslinked resin particles aggregate will tend to remain as voids even after the toner particles are dried. The aggregability of the crosslinked resin particles can be controlled by adjusting the amount of (meth)acrylate monomer having a carboxyl group in the crosslinked resin particles, and the acid value and hydroxyl value of the amorphous polyester resin. Furthermore, the aggregability can be controlled more stably by adjusting the pH of the crosslinked resin particle dispersion, the surfactant concentration in the system during aggregation, the amount of the aggregating agent, and the temperature when the aggregating agent is added. Furthermore, during aggregation or fusion, a foaming liquid such as carbonated water may be added to make it easier to entrap air inside the toner, thereby adjusting the voids.

[0070] Specifically, for example, when toner particles are produced by the aggregation and coalescence method, The toner particles are manufactured through a process including a step of preparing a binder resin particle dispersion in which resin particles that become the binder resin are dispersed, and a crosslinked resin particle dispersion in which the crosslinked resin particles become the crosslinked resin particles (crosslinked resin particle dispersion preparation process), a step of aggregating the crosslinked resin particles (or other particles, if necessary) in the crosslinked resin particle dispersion (in a dispersion after mixing other particle dispersions, if necessary) to form aggregated particles (aggregated particle formation process), and a step of heating the aggregated particle dispersion in which the aggregated particles are dispersed, fusing and coalescing the aggregated particles, and forming toner particles (fusion and coalescence process).

[0071] Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described, but the colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may be used.

[0072] - Binder resin particle dispersion preparation process - First, a binder resin particle dispersion liquid in which resin particles serving as a binder resin are dispersed, as well as, for example, a colorant particle dispersion liquid in which colorant particles are dispersed and a release agent particle dispersion liquid in which release agent particles are dispersed are prepared. Here, the binder resin particle dispersion liquid is prepared, for example, by dispersing binder resin particles in a dispersion medium with the aid of a surfactant. The dispersion medium used in the binder resin particle dispersion liquid is, for example, an aqueous medium. Examples of the aqueous medium include water such as distilled water and ion-exchanged water, alcohols, etc. These may be used alone or in combination of two or more.

[0073] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Among these, anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. The surfactant may be used alone or in combination of two or more kinds.

[0074] In the binder resin particle dispersion liquid, examples of a method for dispersing the binder resin particles in a dispersion medium include general dispersion methods using, for example, a rotary shear type homogenizer, a ball mill having a medium, a sand mill, a dyno mill, etc. Depending on the type of resin particles, the resin particles may be dispersed in the resin particle dispersion liquid using, for example, a phase inversion emulsification method. The phase inversion emulsification method is a method in which the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) to neutralize it, and then an aqueous medium (W phase) is added to effect conversion of the resin from W / O to O / W (so-called phase inversion), resulting in a discontinuous phase, and the resin is dispersed in particulate form in the aqueous medium.

[0075] The volume average particle size of the crosslinked resin particles dispersed in the crosslinked resin particle dispersion is, for example, preferably from 0.01 μm to 1 μm, more preferably from 0.08 μm to 0.8 μm, and even more preferably from 0.1 μm to 0.6 μm. The volume average particle size of the crosslinked resin particles is measured by using a particle size distribution obtained by measurement using a laser diffraction particle size distribution measuring device (e.g., LA-700 manufactured by Horiba, Ltd.), subtracting the cumulative distribution from the small particle size side for the volume of the divided particle size range (channel), and measuring the particle size at which the cumulative distribution is 50% of all particles as the volume average particle size D50(v). The volume average particle sizes of particles in other dispersions are also measured in the same manner.

[0076] The content of the crosslinked resin particles in the crosslinked resin particle dispersion is, for example, preferably from 5% by mass to 50% by mass, and more preferably from 10% by mass to 40% by mass.

[0077] In addition, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared in the same manner as the binder resin particle dispersion. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion are the same for the colorant particles dispersed in the colorant particle dispersion and the release agent particles dispersed in the release agent particle dispersion.

[0078] Preparation of crosslinked resin particle dispersion The crosslinked resin particle dispersion can be prepared by any known method, such as emulsion polymerization, melt kneading using a Banbury mixer or a kneader, suspension polymerization, spray drying, etc., with emulsion polymerization being preferred. It is preferable to use a styrene-based monomer and a (meth)acrylic acid-based monomer as the monomers and polymerize them in the presence of a crosslinking agent. In the production of the crosslinked resin particles, it is preferable to carry out emulsion polymerization a number of times. The method for producing the crosslinked resin particles will now be described in more detail.

[0079] The method for preparing the crosslinked resin particle dispersion includes the steps of: A step of obtaining an emulsion containing a monomer, a crosslinking agent, a surfactant, and water (an emulsion preparation step); a step of adding a polymerization initiator to the emulsion and polymerizing the monomers by heating (first emulsion polymerization step); It is preferable to include a step (second emulsion polymerization step) of adding an emulsion containing a monomer and a crosslinking agent to the reaction solution after the first emulsion polymerization step and heating the mixture to polymerize the monomer.

[0080] -Emulsion preparation process- This is a process for obtaining an emulsion containing a monomer, a crosslinking agent, a surfactant, and water. It is preferable to obtain an emulsion by emulsifying a monomer, a crosslinking agent, a surfactant, and water using an emulsifier. Examples of emulsifiers include rotary mixers equipped with propeller-type, anchor-type, paddle-type, or turbine-type stirring blades, static mixers such as static mixers, rotor-stator type emulsifiers such as homogenizers and Clearmix, mill-type emulsifiers equipped with a grinding function, high-pressure emulsifiers such as Manton-Gaulin pressure emulsifiers, high-pressure nozzle type emulsifiers that generate cavitation under high pressure, high-pressure collision type emulsifiers such as microfluidizers that apply shear force by colliding liquids together under high pressure, ultrasonic emulsifiers that generate cavitation using ultrasound, and membrane emulsifiers that perform uniform emulsification through fine pores.

[0081] As the monomer, it is preferable to use a styrene-based monomer and a (meth)acrylic acid-based monomer. As the crosslinking agent, those already mentioned are applicable.

[0082] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. Among these, anionic surfactants are preferred. The surfactants may be used alone or in combination with two or more.

[0083] The emulsion may contain a chain transfer agent. There is no particular limitation on the chain transfer agent, but a compound having a thiol component can be used. Specifically, alkyl mercaptans such as hexyl mercaptan, heptyl mercaptan, octyl mercaptan, nonyl mercaptan, decyl mercaptan, and dodecyl mercaptan are preferred. The mass ratio of the styrene-based monomer to the (meth)acrylic acid-based monomer in the emulsion (styrene-based monomer / (meth)acrylic acid-based monomer) is preferably 0.2 or more and 1.1 or less. The content of the crosslinking agent in the entire emulsion is preferably 0.5% by mass or more and 3% by mass or less.

[0084] -First emulsion polymerization process- This is a process in which a polymerization initiator is added to the emulsion and then heated to polymerize the monomers. During polymerization, it is preferable to stir the emulsion (reaction solution) containing the polymerization initiator with a stirrer. The agitator may be a rotary agitator equipped with a propeller-type, anchor-type, paddle-type, or turbine-type agitator blade. As the polymerization initiator, ammonium persulfate is preferably used.

[0085] -Second emulsion polymerization process- This is a step in which an emulsion containing a monomer is added to the reaction solution after the first emulsion polymerization step, and the monomer is polymerized by heating. During the polymerization, it is preferable to stir the reaction solution in the same manner as in the first emulsion polymerization step. In this step, the emulsion may be added in portions by changing the ratio of the styrene monomer and the (meth)acrylate monomer in the emulsion. The emulsion containing the monomer is preferably obtained by emulsifying the monomer, a surfactant, and water using an emulsifier.

[0086] -Agglomerated particle formation process- Next, the colorant particle dispersion, the release agent particle dispersion, and the crosslinked resin particle dispersion are mixed together with the binder resin particle dispersion. Then, in the mixed dispersion, the resin particles, the colorant particles, and the release agent particles are hetero-aggregated to form aggregated particles containing the resin particles, the colorant particles, and the release agent particles and having a diameter close to that of the target toner particles.

[0087] Specifically, for example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic (e.g., pH 2 or more and 5 or less), a dispersion stabilizer is added as necessary, and then the mixed dispersion is heated to a temperature of the glass transition temperature of the resin particles (specifically, for example, a temperature of the glass transition temperature of the resin particles -30°C or more and the glass transition temperature -10°C or less), and the particles dispersed in the mixed dispersion are aggregated to form aggregated particles. In the aggregated particle formation process, for example, the above-mentioned aggregating agent may be added to the mixed dispersion at room temperature (e.g., 25°C) while stirring the mixed dispersion with a rotary shear homogenizer, the pH of the mixed dispersion may be adjusted to an acidic state (e.g., pH 2 or more and 5 or less), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.

[0088] In this process, the temperature of the mixed dispersion liquid when the coagulant is added may be adjusted to control the dispersion state of the resin particles in the toner particles obtained. For example, the dispersibility of the resin particles is improved by lowering the temperature of the mixed dispersion liquid. The temperature of the mixed dispersion liquid may be, for example, in the range of 5°C to 40°C. In this step, the dispersion state of the resin particles in the toner particles obtained may be controlled by adjusting the stirring speed after the addition of the aggregating agent. For example, the dispersion of the resin particles is improved by increasing the stirring speed after the addition of the aggregating agent.

[0089] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved. If necessary, an additive that forms a complex or a similar bond with the metal ions of the flocculant may be used, and a chelating agent is preferably used as this additive.

[0090] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The chelating agent may be a water-soluble chelating agent, for example, oxycarboxylic acid such as tartaric acid, citric acid, gluconic acid, iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), ethylenediaminetetraacetic acid (EDTA), etc. The amount of the chelating agent added is, for example, preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the resin particles.

[0091] -Fusion / unification process- Next, the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the crosslinked resin particles (for example, a temperature 10° C. to 30° C. higher than the glass transition temperature of the resin particles) to fuse and coalesce the aggregated particles, thereby forming toner particles.

[0092] Through the above steps, toner particles are obtained. Note that, after obtaining an aggregated particle dispersion in which the aggregated particles are dispersed, the toner particles may be manufactured through a process of further mixing the aggregated particle dispersion, a resin particle dispersion in which resin particles are dispersed, and another resin particle dispersion in which other resin particles are dispersed, and aggregating the aggregated particles so that the resin particles and the other resin particles are attached to the surfaces of the aggregated particles to form second aggregated particles, and a process of heating the second aggregated particle dispersion in which the second aggregated particles are dispersed, to fuse and coalesce the second aggregated particles, thereby forming toner particles having a core / shell structure.

[0093] In the step of forming the second aggregated particles, the addition of the resin particle dispersion and the adhesion of the resin particles to the surfaces of the aggregated particles may be repeated multiple times.

[0094] After the fusion and coalescence process, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process, and drying process to obtain toner particles in a dried state. In the washing step, it is preferable to carry out sufficient replacement washing with ion-exchanged water from the viewpoint of electrostatic charge. In addition, the solid-liquid separation step is not particularly limited, but it is preferable to carry out suction filtration, pressure filtration, etc. from the viewpoint of productivity. In addition, in the drying step, there is no particular limit to the method, but it is preferable to carry out freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc. from the viewpoint of productivity.

[0095] The toner according to the present embodiment is produced, for example, by adding an external additive to the obtained toner particles in a dry state and mixing them. The mixing may be performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.

[0096] <Electrostatic image developer> The electrostatic image developer according to this embodiment contains at least the toner according to this embodiment or the toner according to the second embodiment. The electrostatic image developer according to this embodiment may be a one-component developer containing only the toner according to this embodiment or the second embodiment, or may be a two-component developer containing the toner mixed with a carrier.

[0097] The carrier is not particularly limited, and may be any known carrier, such as a coated carrier in which the surface of a core material made of magnetic powder is coated with a coating resin, a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin, or a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material and are coated with a coating resin.

[0098] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt, and magnetic oxides such as ferrite and magnetite.

[0099] Examples of the coating resin and matrix resin include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin containing an organosiloxane bond or a modified product thereof, fluororesin, polyester, polycarbonate, phenolic resin, and epoxy resin. The coating resin and the matrix resin may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.

[0100] Here, the method of coating the surface of the core material with the coating resin includes a method of coating with a solution for forming a coating layer in which the coating resin and, if necessary, various additives are dissolved in an appropriate solvent, etc. The solvent is not particularly limited and may be selected taking into consideration the coating resin to be used, the suitability for application, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer, a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material, a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air, and a kneader coater method in which the core material of a carrier and the solution for forming a coating layer are mixed in a kneader coater and the solvent is removed.

[0101] In a two-component developer, the mixture ratio (mass ratio) of toner and carrier is toner:carrier. = 1:100 to 30:100 is preferable, and 3:100 to 20:100 is more preferable.

[0102] <Image forming device, image forming method> An image forming apparatus / image forming method according to this embodiment will be described. The image forming apparatus according to the present embodiment includes an image carrier, a charging means for charging the surface of the image carrier, an electrostatic image forming means for forming an electrostatic image on the surface of the charged image carrier, a developing means for containing an electrostatic image developer and developing the electrostatic image formed on the surface of the image carrier as a toner image with the electrostatic image developer, a transfer means for transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium. The electrostatic image developer according to the present embodiment is used as the electrostatic image developer.

[0103] In the image forming apparatus according to this embodiment, an image forming method (the image forming method according to this embodiment) is carried out, which includes a charging step of charging the surface of an image carrier, an electrostatic image forming step of forming an electrostatic image on the surface of the charged image carrier, a developing step of developing the electrostatic image formed on the surface of the image carrier as a toner image using the electrostatic image developer according to this embodiment, a transfer step of transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.

[0104] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as a direct transfer type apparatus in which a toner image formed on the surface of an image holder is directly transferred to a recording medium; an intermediate transfer type apparatus in which a toner image formed on the surface of an image holder is primarily transferred to the surface of an intermediate transfer body, and the toner image transferred to the surface of the intermediate transfer body is secondarily transferred to the surface of a recording medium; an apparatus equipped with a cleaning means for cleaning the surface of the image holder after the transfer of the toner image and before charging; and an apparatus equipped with a discharging means for irradiating the surface of the image holder with discharging light to discharge it after the transfer of the toner image and before charging it. When the image forming apparatus according to the present embodiment is an intermediate transfer type apparatus, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the image carrier onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.

[0105] In the image forming apparatus according to the present embodiment, for example, a portion including the developing means may have a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge including the developing means that contains the electrostatic image developer according to the present embodiment is preferably used.

[0106] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. In the following description, the main parts shown in the drawings will be described, and the description of the rest will be omitted.

[0107] FIG. 1 is a schematic diagram showing the configuration of an image forming apparatus according to the present embodiment. The image forming apparatus shown in Fig. 1 includes first to fourth image forming units 10Y, 10M, 10C, and 10K (image forming means) of an electrophotographic type that output images of each color of yellow (Y), magenta (M), cyan (C), and black (K) based on color-separated image data. These image forming units (hereinafter sometimes simply referred to as "units") 10Y, 10M, 10C, and 10K are arranged in parallel at predetermined distances from each other in the horizontal direction. These units 10Y, 10M, 10C, and 10K may be process cartridges that are detachably attached to the image forming apparatus.

[0108] Above each of the units 10Y, 10M, 10C, and 10K, an intermediate transfer belt (an example of an intermediate transfer body) 20 is provided to extend through each unit. The intermediate transfer belt 20 is provided wound around a drive roll 22 and a support roll 24 that are in contact with the inner surface of the intermediate transfer belt 20, and runs in a direction from the first unit 10Y to the fourth unit 10K. A force is applied to the support roll 24 by a spring or the like (not shown) in a direction away from the drive roll 22, and tension is applied to the intermediate transfer belt 20 wound around them. An intermediate transfer belt cleaning device 30 is provided on the image bearing surface side of the intermediate transfer belt 20, facing the drive roll 22. The developing devices (an example of developing means) 4Y, 4M, 4C, and 4K of the units 10Y, 10M, 10C, and 10K are supplied with yellow, magenta, cyan, and black toners contained in toner cartridges 8Y, 8M, 8C, and 8K, respectively.

[0109] Since the first to fourth units 10Y, 10M, 10C, and 10K have the same configuration and operation, the first unit 10Y that forms a yellow image and is disposed upstream in the direction in which the intermediate transfer belt travels will be described here as a representative.

[0110] The first unit 10Y has a photoconductor 1Y that acts as an image carrier. Around the photoconductor 1Y, a charging roll (an example of a charging means) 2Y that charges the surface of the photoconductor 1Y to a predetermined potential, an exposure device (an example of an electrostatic image forming means) 3 that exposes the charged surface to a laser beam 3Y based on a color-separated image signal to form an electrostatic image, a developing device (an example of a developing means) 4Y that supplies charged toner to the electrostatic image to develop it, a primary transfer roll (an example of a primary transfer means) 5Y that transfers the developed toner image onto an intermediate transfer belt 20, and a photoconductor cleaning device (an example of an image carrier cleaning means) 6Y that removes toner remaining on the surface of the photoconductor 1Y after the primary transfer are arranged in this order.

[0111] The primary transfer roll 5Y is disposed inside the intermediate transfer belt 20, and is provided at a position facing the photoconductor 1Y. A bias power supply (not shown) that applies a primary transfer bias is connected to the primary transfer rolls 5Y, 5M, 5C, and 5K of each unit. Each bias power supply changes the value of the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).

[0112] Hereinafter, the operation of forming a yellow image in the first unit 10Y will be described. First, prior to operation, the surface of the photoconductor 1Y is charged to a potential of −600V to −800V by the charging roll 2Y. The photoconductor 1Y has a conductivity (for example, a volume resistivity of 1×10 at 20° C. -6 The photosensitive layer is formed by laminating a photosensitive layer on a substrate having a resistivity of Ωcm or less. This photosensitive layer is usually highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam, the resistivity of the portion irradiated with the laser beam changes. Therefore, the exposed surface of the charged photoreceptor 1Y is irradiated with a laser beam 3Y from the exposure device 3 in accordance with image data for yellow sent from a control unit (not shown). As a result, an electrostatic charge image of a yellow image pattern is formed on the surface of the photoreceptor 1Y.

[0113] An electrostatic image is an image formed on the surface of the photoconductor 1Y by electrostatic charging. The laser beam 3Y reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 1Y to flow, while the charges remain in the parts not irradiated by the laser beam 3Y. This is a so-called negative latent image. The electrostatic image formed on the photoconductor 1Y rotates to a predetermined developing position as the photoconductor 1Y travels. At this developing position, the electrostatic image on the photoconductor 1Y is developed into a toner image by the developing device 4Y and made visible.

[0114] The developing device 4Y contains an electrostatic image developer including at least yellow toner and a carrier, for example. The yellow toner is triboelectrically charged by being stirred inside the developing device 4Y, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 1Y. As the surface of the photoconductor 1Y passes through the developing device 4Y, the yellow toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 1Y, and the latent image is developed with the yellow toner. The photoconductor 1Y on which the yellow toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 1Y is transported to a predetermined primary transfer position.

[0115] When the yellow toner image on the photoreceptor 1Y is transported to the primary transfer position, a primary transfer bias is applied to the primary transfer roll 5Y, and an electrostatic force from the photoreceptor 1Y toward the primary transfer roll 5Y acts on the toner image, and the toner image on the photoreceptor 1Y is transferred onto the intermediate transfer belt 20. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and is controlled to, for example, +10 μA by a control unit (not shown) in the first unit 10Y. On the other hand, the toner remaining on the photoconductor 1Y is removed and collected by the photoconductor cleaning device 6Y.

[0116] The primary transfer bias applied to the primary transfer rolls 5M, 5C, and 5K in the second unit 10M and subsequent units is also controlled in accordance with the first unit. In this manner, the intermediate transfer belt 20 onto which the yellow toner image has been transferred by the first unit 10Y is conveyed successively through the second to fourth units 10M, 10C, and 10K, where the toner images of each color are transferred and superimposed.

[0117] The intermediate transfer belt 20 onto which the four color toner images have been transferred in multiple layers through the first to fourth units reaches a secondary transfer section that is composed of the intermediate transfer belt 20, a support roll 24 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer means) 26 arranged on the image bearing surface side of the intermediate transfer belt 20. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 26 and the intermediate transfer belt 20 via a supply mechanism, and a secondary transfer bias is applied to the support roll 24. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 20 toward the recording paper P acts on the toner image, and the toner image on the intermediate transfer belt 20 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection means (not shown) that detects the resistance of the secondary transfer section, and is voltage-controlled.

[0118] The recording paper P onto which the toner image has been transferred is sent to a pressure contact portion (nip portion) of a pair of fixing rolls in a fixing device (one example of a fixing means) 28, where the toner image is fixed onto the recording paper P to form a fixed image. After the color image has been fixed, the recording paper P is conveyed toward a discharge portion, and a series of color image forming operations is completed.

[0119] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets and the like. To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with a resin or the like, art paper for printing, etc. are preferably used.

[0120] <Process cartridge / toner cartridge> The process cartridge according to this embodiment will be described. The process cartridge according to this embodiment is a process cartridge that contains the electrostatic image developer according to this embodiment, is equipped with a developing means that develops an electrostatic image formed on the surface of an image carrier using the electrostatic image developer into a toner image, and is detachably attached to an image forming apparatus. The process cartridge according to this embodiment may be configured to include a developing means and, if necessary, at least one selected from other means such as an image carrier, a charging means, an electrostatic image forming means, and a transfer means.

[0121] An example of a process cartridge according to the present embodiment will be described below, but the present invention is not limited to this example. In the following description, the main parts shown in the drawings will be described, and the description of the rest will be omitted. FIG. 2 is a schematic diagram showing an example of a process cartridge according to the present embodiment. The process cartridge 200 shown in FIG. 2 is configured by, for example, a housing 117 having a mounting rail 116 and an opening 118 for exposure, and integrally holding a photoconductor 107 (an example of an image carrier), a charging roll 108 (an example of a charging means) provided around the photoconductor 107, a developing device 111 (an example of a developing means), and a photoconductor cleaning device 113 (an example of a cleaning means), which are combined and held in a cartridge form. In FIG. 2, 109 indicates an exposure device (an example of an electrostatic image forming means), 112 indicates a transfer device (an example of a transfer means), 115 indicates a fixing device (an example of a fixing means), and 300 indicates a recording paper (an example of a recording medium).

[0122] Next, the toner cartridge according to this embodiment will be described. The toner cartridge according to the present embodiment is a toner cartridge that contains the toner according to the present embodiment and is detachably attached to an image forming apparatus. The toner cartridge contains replenishment toner to be supplied to a developing unit provided in the image forming apparatus.

[0123] 1 is an image forming apparatus having a configuration in which toner cartridges 8Y, 8M, 8C, and 8K can be attached and detached, and the developing devices 4Y, 4M, 4C, and 4K are connected to the toner cartridges corresponding to the respective developing devices (colors) through toner supply pipes (not shown). When the toner contained in the toner cartridge becomes low, the toner cartridge is replaced. EXAMPLES

[0124] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the embodiments of the present invention are not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" are based on mass.

[0125] [Preparation of emulsion 1] Styrene: 49 parts n-Butyl acrylate: 49 parts 1,10-Decanediol diacrylate: 1.9 parts 2-Carboxyethyl acrylate: 0.1 parts Anionic surfactant (Dowfax2a-1, manufactured by Dow Chemical Japan Co., Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were charged into a mixing vessel equipped with a stirrer and stirred to prepare emulsion 1.

[0126] [Preparation of crosslinked resin particle dispersion 1] In a reaction vessel equipped with a stirrer and a nitrogen inlet tube, 0.3 parts of anionic surfactant (Dowfax2a-1) and 100 parts of ion-exchanged water were added after replacing the atmosphere in the reaction vessel with nitrogen. The reaction solution was heated in an oil bath while stirring, and the temperature of the reaction solution was adjusted to 65°C. Then, 12 parts of the emulsion were added, and 4 parts of an aqueous solution of ammonium persulfate with a concentration adjusted to 10% were added, and the mixture was maintained for 30 minutes. Thereafter, while maintaining the temperature of the reaction solution at 65° C., 198 parts of emulsion 1 was gradually added dropwise to the reaction vessel over a period of 180 minutes using a pump. After the dropwise addition, the mixture was held for 60 minutes, and then 2 parts of 10% ammonium persulfate was added, and the mixture was held for another 3 hours and then cooled to room temperature. Ion-exchanged water and nitric acid were then added to the mixture so that the solids concentration was 20% and the pH was 2.0, to obtain crosslinked resin particle dispersion 1. The crosslinked resin particles thus obtained had a volume average particle size of 160 nm and a glass transition temperature of 12° C. as measured by a differential scanning calorimeter.

[0127] [Preparation of crosslinked resin particle dispersion 2] [Preparation of emulsion 2] Styrene: 49 parts n-Butyl acrylate: 49.05 parts 1,10-Decanediol diacrylate: 1.9 parts 2-Carboxyethyl acrylate: 0.05 parts Anionic surfactant (Dowfax2a-1, manufactured by Dow Chemical Japan Co., Ltd.): 1.4 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare emulsion 2. Crosslinked resin particle dispersion 2 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 2 and the amount of nitric acid added was adjusted so that the pH of the dispersion was 2.0 to 3.0. The volume average particle size of the obtained crosslinked resin particles was 160 nm. The glass transition temperature measured by a differential scanning calorimeter was 12°C.

[0128] [Preparation of crosslinked resin particle dispersion 3] [Preparation of emulsion 3] Styrene: 49.0 parts n-Butyl acrylate: 48.7 parts 1,10-Decanediol diacrylate: 1.9 parts 2-Carboxyethyl acrylate: 0.3 parts Anionic surfactant (Dowfax2a-1, manufactured by Dow Chemical Japan Co., Ltd.): 1.0 part Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare emulsion 3. Crosslinked resin particle dispersion 3 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 3 and the amount of nitric acid added was adjusted so that the pH of the dispersion was 2.0 to 1.6. The volume average particle size of the obtained crosslinked resin particles was 160 nm. The glass transition temperature measured by a differential scanning calorimeter was 12°C.

[0129] [Preparation of crosslinked resin particle dispersion 4] [Preparation of emulsion 4] Styrene: 41 parts n-Butyl acrylate: 57 parts 1,10-Decanediol diacrylate: 1.9 parts 2-Carboxyethyl acrylate: 0.1 parts Anionic surfactant (Dowfax2a-1, manufactured by Dow Chemical Japan Co., Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare emulsion 4. Crosslinked resin particle dispersion 4 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 4. The volume average particle size of the obtained crosslinked resin particles was 170 nm. The glass transition temperature measured by a differential scanning calorimeter was -1°C.

[0130] [Preparation of crosslinked resin particle dispersion 5] [Preparation of emulsion 5] Styrene: 59 parts n-Butyl acrylate: 39 parts 1,10-Decanediol diacrylate: 1.9 parts 2-Carboxyethyl acrylate: 0.1 parts Anionic surfactant (Dowfax2a-1, manufactured by Dow Chemical Japan Co., Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were placed in a mixing vessel equipped with a stirrer and stirred to prepare emulsion 5. Crosslinked resin particle dispersion 5 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 5. The volume average particle size of the obtained crosslinked resin particles was 160 nm. The glass transition temperature measured by a differential scanning calorimeter was 31°C.

[0131] [Preparation of crosslinked resin particle dispersion 6] [Preparation of emulsion 6] Styrene: 49.5 parts n-Butyl acrylate: 49.5 parts 1,6-Hexanediol acrylate: 0.9 parts 2-Carboxyethyl acrylate: 0.1 parts Anionic surfactant (Dowfax2a-1, manufactured by Dow Chemical Japan Co., Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were charged into a mixing vessel equipped with a stirrer and stirred to prepare emulsion 6. Crosslinked resin particle dispersion 6 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 6 and the amount of ammonium persulfate aqueous solution added was changed from 4 parts to 3.5 parts, to prepare crosslinked resin particle dispersion 6. The volume average particle size of the obtained crosslinked resin particles was 160 nm. The glass transition temperature measured by a differential scanning calorimeter was 11°C.

[0132] [Preparation of crosslinked resin particle dispersion 7] Crosslinked resin particle dispersion 7 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that the temperature of the reaction vessel was changed from 65°C to 78°C and the amount of ammonium persulfate aqueous solution added was changed from 4 parts to 4.5 parts. The volume average particle size of the obtained crosslinked resin particles was 150 nm. The glass transition temperature measured by a differential scanning calorimeter was 13°C.

[0133] [Preparation of crosslinked resin particle dispersion 8] [Preparation of emulsion 8] Styrene: 49.5 parts n-Butyl acrylate: 49.5 parts 1,12-dodecanediol diacrylate: 1.0 part 2-Carboxyethyl acrylate: 0.1 parts Anionic surfactant (Dowfax2a-1, manufactured by Dow Chemical Japan Co., Ltd.): 1.2 parts Ion-exchanged water: 98.8 parts The above materials were charged into a mixing vessel equipped with a stirrer and stirred to prepare emulsion 8. Crosslinked resin particle dispersion 8 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 8 and the drop time of the emulsion was changed from 180 minutes to 150 minutes, to prepare crosslinked resin particle dispersion 8. The volume average particle size of the obtained crosslinked resin particles was 180 nm. The glass transition temperature measured by a differential scanning calorimeter was 11°C.

[0134] [Preparation of crosslinked resin particle dispersion 9] [Preparation of emulsion 9] Emulsion 9 was prepared in the same manner as in the preparation of emulsion 1, except that 1,10-decanediol diacrylate was changed to divinylbenzene. Crosslinked resin particle dispersion 9 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 9 and the drop time of the emulsion was changed from 180 minutes to 150 minutes, to prepare crosslinked resin particle dispersion 9. The volume average particle size of the obtained crosslinked resin particles was 180 nm. The glass transition temperature measured by a differential scanning calorimeter was 11°C.

[0135] [Preparation of Crosslinked Resin Particle Dispersion 10] Emulsion 10 was prepared in the same manner as in the preparation of emulsion 1, except that the amount of styrene was changed from 49 parts to 49.1 parts and the amount of 2-carboxyethyl acrylate was changed from 0.1 parts to 0 parts. Crosslinked resin particle dispersion 10 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 10 and the amount of nitric acid added was adjusted so that the pH of the dispersion was 2.0 to 3.5. The volume average particle size of the obtained crosslinked resin particles was 160 nm. The glass transition temperature measured by a differential scanning calorimeter was 12°C.

[0136] [Preparation of crosslinked resin particle dispersion 11] Emulsion 11 was prepared in the same manner as in preparation of emulsion 1, except that the amount of styrene was changed from 49 parts to 48.55 parts and the amount of 2-carboxyethyl acrylate was changed from 0.1 parts to 0.55 parts. Crosslinked resin particle dispersion 11 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 11. The volume average particle size of the obtained crosslinked resin particles was 160 nm. The glass transition temperature measured by a differential scanning calorimeter was 12°C.

[0137] [Preparation of crosslinked resin particle dispersion 12] Emulsion 12 was prepared in the same manner as in the preparation of emulsion 1, except that the amount of the anionic surfactant (Dowfax2a-1) added to the reaction vessel was changed from 0.3 parts to 0.9 parts. Crosslinked resin particle dispersion 12 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 12. The volume average particle size of the obtained crosslinked resin particles was 45 nm. The glass transition temperature measured by a differential scanning calorimeter was 12°C.

[0138] [Preparation of crosslinked resin particle dispersion 13] Emulsion 13 was prepared in the same manner as in the preparation of emulsion 1, except that the amount of the anionic surfactant (Dowfax2a-1) added to the reaction vessel was changed from 0.3 parts to 0.1 parts. Crosslinked resin particle dispersion 13 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 13 and the amount of nitric acid added was adjusted so that the pH of the dispersion was 2.0 to 1.6. The volume average particle size of the obtained crosslinked resin particles was 310 nm. The glass transition temperature measured by a differential scanning calorimeter was 12°C.

[0139] [Preparation of crosslinked resin particle dispersion 14] Emulsion 14 was prepared in the same manner as in the preparation of emulsion 1, except that the amount of n-butyl acrylate was changed from 49 parts to 49.6 parts, and the amount of 1,10-decanediol diacrylate was changed from 1.9 parts to 1.3 parts. Crosslinked resin particle dispersion 14 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that the temperature of the reaction vessel was changed from 65°C to 62°C and the drop time of the emulsion was changed from 180 minutes to 240 minutes, to obtain crosslinked resin particle dispersion 14. The volume average particle size of the obtained crosslinked resin particles was 220 nm. The glass transition temperature measured by a differential scanning calorimeter was 11°C.

[0140] [Preparation of crosslinked resin particle dispersion 15] Emulsion 15 was prepared in the same manner as in the preparation of emulsion 1, except that the amount of styrene was changed from 49 parts to 57 parts and the amount of n-butyl acrylate was changed from 49 parts to 41 parts. Crosslinked resin particle dispersion 15 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 15. The volume average particle size of the obtained crosslinked resin particles was 160 nm. The glass transition temperature measured by a differential scanning calorimeter was 27°C.

[0141] [Preparation of crosslinked resin particle dispersion 16] Emulsion 16 was prepared in the same manner as in preparation of emulsion 1, except that the amount of styrene was changed from 49 parts to 43 parts and the amount of n-butyl acrylate was changed from 49 parts to 55 parts. Crosslinked resin particle dispersion 16 was prepared in the same manner as in preparation of crosslinked resin particle dispersion 1, except that emulsion 1 was changed to emulsion 16. The volume average particle size of the obtained crosslinked resin particles was 160 nm. The glass transition temperature measured by a differential scanning calorimeter was 3°C.

[0142] [Preparation of crosslinked resin particle dispersion 17] Styrene: 48 parts Butadiene: 50 parts Acrylic acid: 1.9 parts tert-dodecanethiol: 0.1 parts Anionic surfactant (Dowfax2a-1): 1.2 parts - Ion-exchanged water: 200 parts Potassium persulfate: 1 part The above materials were placed in a polymerization reactor and polymerized for 2 hours under a nitrogen atmosphere at a temperature of 50°C, and then the reaction was continued for 3 hours to terminate the polymerization. Ion-exchanged water and nitric acid were added to the obtained dispersion to a solid concentration of 20% and a pH of 2.0, to obtain crosslinked resin particle dispersion 17.

[0143] [Preparation of amorphous polyester resin dispersion 1] Terephthalic acid: 30 parts by mole Isophthalic acid: 10 mol parts Adipic acid: 8.5 mol parts Trimellitic anhydride: 2 mol parts Bisphenol A propylene oxide 2 mole adduct: 49.5 mole parts The above materials were charged into a reaction vessel equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, the temperature was raised to 190°C over 1 hour, and 1.2 parts of dibutyltin oxide were added per 100 parts of the above materials. The temperature was raised to 240°C over 6 hours while distilling off the generated water, and then the temperature was maintained at 240°C for 3 hours to continue the dehydration condensation reaction, followed by cooling to obtain amorphous polyester resin 1. The amorphous polyester resin 1 had an acid value of 10, a hydroxyl value of 17, a weight average molecular weight of 27,000 and a glass transition temperature of 61°C.

[0144] Amorphous polyester resin 1:100 parts Methyl ethyl ketone: 60 parts Isopropanol: 10 parts 10% ammonia solution: 3.5 parts The above materials were charged into a jacketed reaction tank equipped with a condenser, a thermometer, a water dropping device, and an anchor blade, and the amorphous polyester resin 1 was dissolved while stirring and mixing at 100 rpm while maintaining the liquid temperature at 50° C. in a water circulation type thermostatic bath. Next, the water circulation type thermostatic bath was set to 40° C., and a total of 300 parts of ion-exchanged water kept at 40° C. was dropped at a rate of 3 parts / min to cause phase inversion and produce an emulsion. The obtained emulsion was placed in an eggplant flask and set in an evaporator equipped with a vacuum control unit via a trap bulb. The eggplant flask was rotated and heated in a hot water bath at 60°C, and the pressure was reduced to 7 kPa while taking care not to bump, and the solvent was removed. The pressure was then returned to normal pressure, and the eggplant flask was water-cooled to obtain a dispersion. Ion-exchanged water was added to the obtained dispersion to obtain amorphous polyester resin dispersion 1 with a solid content of 20%. The volume average particle size of the amorphous polyester resin particles in amorphous polyester resin dispersion 1 was 180 nm.

[0145] [Preparation of amorphous polyester resin dispersion 2] Amorphous polyester resin dispersion 2 was obtained in the same manner as in preparation of amorphous polyester resin dispersion 1, except that the amounts of materials charged were changed as follows. Terephthalic acid: 43 parts by mole Isophthalic acid: 2 mol parts Adipic acid: 3 mol parts Trimellitic anhydride: 2.5 mol parts Bisphenol A propylene oxide 2 mole adduct: 40 mole parts Bisphenol A ethylene oxide 2 mole adduct: 10 mole parts The amorphous polyester resin 2 had an acid value of 10, a hydroxyl value of 13, a weight average molecular weight of 32,000 and a glass transition temperature of 66°C. The volume average particle size of the amorphous polyester resin particles in the amorphous polyester resin dispersion 2 was 180 nm.

[0146] [Preparation of amorphous polyester resin dispersion 3] Amorphous polyester resin dispersion 3 was obtained in the same manner as in preparation of amorphous polyester resin dispersion 1, except that the amounts of materials charged were changed as follows. Terephthalic acid: 16.5 mol parts Isophthalic acid: 20 parts by mole Adipic acid: 12 molar parts Trimellitic anhydride: 2 mol parts Bisphenol A propylene oxide 2 mole adduct: 39.5 mole parts Bisphenol A propylene oxide 2 mole adduct: 10 mole parts The amorphous polyester resin 3 had an acid value of 12, a hydroxyl value of 20, a weight average molecular weight of 27,000, and a glass transition temperature of 55°C. The volume average particle size of the amorphous polyester resin particles in the amorphous polyester resin dispersion 3 was 180 nm.

[0147] [Preparation of amorphous polyester resin dispersion 4] Amorphous polyester resin dispersion 4 was obtained in the same manner as in preparation of amorphous polyester resin dispersion 1, except that the amounts of materials charged were changed as follows. Terephthalic acid: 44 parts by mole Isophthalic acid: 2 mol parts Sebacic acid: 1 molar part Trimellitic anhydride: 3 mol parts Bisphenol A propylene oxide 2 mole adduct: 36 mole parts Bisphenol A ethylene oxide 2 mole adduct: 15 mole parts The amorphous polyester resin 4 had an acid value of 9, a hydroxyl value of 15, a weight average molecular weight of 36,000 and a glass transition temperature of 74°C. The volume average particle size of the amorphous polyester resin particles in Amorphous Polyester Resin Dispersion 4 was 200 nm.

[0148] [Preparation of amorphous polyester resin dispersion 5] Amorphous polyester resin dispersion 5 was obtained in the same manner as in preparation of amorphous polyester resin dispersion 1, except that the amount of bisphenol A propylene oxide 2-mol adduct was changed from 49.5 parts by mol to 51.5 parts by mol. Amorphous polyester resin 5 had an acid value of 4.5, a hydroxyl value of 20.5, a weight average molecular weight of 28,000 and a glass transition temperature of 61°C. The volume average particle size of the amorphous polyester resin particles in Amorphous Polyester Resin Dispersion 5 was 195 nm.

[0149] [Preparation of amorphous polyester resin dispersion 6] Amorphous polyester resin dispersion 6 was obtained in the same manner as in preparation of amorphous polyester resin dispersion 1, except that the amount of bisphenol A propylene oxide 2-mol adduct was changed from 49.5 parts by mol to 47.5 parts by mol. The amorphous polyester resin 6 had an acid value of 21, a hydroxyl value of 11, a weight average molecular weight of 25,000 and a glass transition temperature of 61°C. The volume average particle size of the amorphous polyester resin particles in the amorphous polyester resin dispersion 6 was 195 nm.

[0150] [Preparation of amorphous polyester resin dispersion 7] Amorphous polyester resin dispersion 7 was obtained in the same manner as in preparation of amorphous polyester resin dispersion 1, except that the amount of dibutyltin oxide was changed from 1.2 parts to 1.5 parts and the polymerization time was changed from 6 hours to 9 hours. Amorphous polyester resin 7 had an acid value of 8, a hydroxyl value of 6, a weight average molecular weight of 38,000 and a glass transition temperature of 63°C. The volume average particle size of the amorphous polyester resin particles in the amorphous polyester resin dispersion 7 was 190 nm.

[0151] [Preparation of amorphous polyester resin dispersion 8] Amorphous polyester resin dispersion 8 was obtained in the same manner as in preparation of amorphous polyester resin dispersion 1, except that the amount of dibutyltin oxide was changed from 1.2 parts to 0.6 parts and the polymerization temperature was changed from 240°C to 230°C. The amorphous polyester resin 8 had an acid value of 15, a hydroxyl value of 26, a weight average molecular weight of 23,000 and a glass transition temperature of 58°C. The volume average particle size of the amorphous polyester resin particles in the amorphous polyester resin dispersion 8 was 170 nm.

[0152] [Preparation of amorphous polyester resin dispersion 9] Amorphous polyester resin dispersion 9 was obtained in the same manner as in preparation of amorphous polyester resin dispersion 1, except that the amounts of materials charged were changed as follows. Terephthalic acid: 30 parts by mole Isophthalic acid: 18 mol parts Adipic acid: 0.4 mol parts Trimellitic anhydride: 2 mol parts Bisphenol A propylene oxide 2 mole adduct: 49.6 mole parts The amorphous polyester resin 9 had an acid value of 10, a hydroxyl value of 18, a weight average molecular weight of 28,000 and a glass transition temperature of 63°C. The volume average particle size of the amorphous polyester resin particles in Amorphous Polyester Resin Dispersion 9 was 180 nm.

[0153] [Preparation of amorphous polyester resin dispersion 10] Amorphous polyester resin dispersion 10 was obtained in the same manner as in preparation of amorphous polyester resin dispersion 1, except that the amounts of materials charged were changed as follows. Terephthalic acid: 30 parts by mole Isophthalic acid: 3 mol parts Adipic acid: 15.5 mol parts Trimellitic anhydride: 2 mol parts Bisphenol A propylene oxide 2 mole adduct: 49.5 mole parts The amorphous polyester resin 10 had an acid value of 11, a hydroxyl value of 15, a weight average molecular weight of 29,000 and a glass transition temperature of 57°C. The volume average particle size of the amorphous polyester resin particles in the amorphous polyester resin dispersion 10 was 180 nm.

[0154] [Preparation of amorphous styrene acrylic resin dispersion] Styrene: 78 parts n-Butyl acrylate: 21 parts β-Carboxyethyl acrylate: 1 part The above materials were charged into a mixing vessel equipped with a stirrer and stirred. A mixed solution of 1.5 parts of an anionic surfactant (Dowfax2a-1, manufactured by Dow Chemical Japan Co., Ltd.) and 48.5 parts of ion-exchanged water was added to the mixing vessel with respect to 100 parts of the above materials and stirred to obtain emulsion 21. In a reaction vessel equipped with a stirrer and a nitrogen inlet tube, 1.5 parts of an anionic surfactant (Dowfax2a-1) and 90 parts of ion-exchanged water were added and stirred. 5 parts of emulsion 21 were added, and 1 part of a 10% aqueous solution of ammonium persulfate was further added. The atmosphere in the reaction vessel was replaced with nitrogen, and the reaction solution was heated in an oil bath while being stirred, the temperature of the reaction solution was raised to 80°C, and the reaction solution was stirred for 30 minutes. Further, 145 parts of emulsion 21 was added to the reaction vessel, and the reaction solution was stirred for 3 hours while maintaining the temperature at 80°C. Then, the reaction solution was cooled to room temperature, and ion-exchanged water was added to the dispersion to obtain an amorphous styrene-acrylic resin particle dispersion with a solid content of 20%. The volume average particle size of the resin particles in the amorphous styrene-acrylic resin particle dispersion was 200 nm, the weight average molecular weight of the amorphous styrene-acrylic resin was 33,000, and the glass transition temperature was 56°C.

[0155] [Preparation of crystalline polyester resin particle dispersion 1] Dodecanedioic acid: 50 parts by mole 1,6-Hexanediol: 50 parts by mole The above materials were charged into a reaction vessel equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 160°C over 1 hour, and 0.8 parts of dibutyltin oxide was added to 100 parts of the above materials. The temperature was raised to 180°C over 6 hours while distilling off the generated water, and the reaction was allowed to proceed by refluxing in the vessel while stirring for 5 hours while maintaining 180°C. Next, the temperature was gradually raised to 230°C under reduced pressure (3 kPa), and stirring was performed for 2 hours while maintaining 230°C. Then, the reactant was cooled. After cooling, solid-liquid separation was performed, and the solid was dried to obtain crystalline polyester resin 1. The weight average molecular weight of crystalline polyester resin 1 was 29,000.

[0156] Crystalline polyester resin 1: 100 parts Methyl ethyl ketone: 70 parts Isopropanol: 12 parts 10% ammonia solution: 3 parts The above materials were charged into a jacketed reaction tank equipped with a condenser, a thermometer, a water dropping device, and an anchor blade, and while maintaining the liquid temperature at 80° C. in a water circulation type thermostatic bath, the mixture was stirred and mixed at 100 rpm to dissolve the crystalline polyester resin 1. Next, the water circulation type thermostatic bath was set to 60° C., and a total of 300 parts of ion-exchanged water kept at 60° C. was dropped at a rate of 3 parts / min to cause phase inversion, thereby obtaining an emulsion. The obtained emulsion was placed in an eggplant flask and set in an evaporator equipped with a vacuum control unit via a trap bulb. The eggplant flask was heated in a hot water bath at 60°C while rotating, and the pressure was reduced to 7 kPa while taking care not to bump, and the solvent was removed. The pressure was then returned to normal pressure, and the eggplant flask was water-cooled to obtain a dispersion. Ion-exchanged water was added to the dispersion to obtain crystalline polyester resin particle dispersion 1 with a solid content of 20%. The volume average particle size of the crystalline polyester resin particles in crystalline polyester resin particle dispersion 1 was 160 nm.

[0157] [Preparation of colorant particle dispersion] ·CIPigment Blue 15:3 (manufactured by Dainichiseika Chemical Co., Ltd.): 100 copies Anionic surfactant (Neopelex G-65, Kao Corporation): 6 parts Ion-exchanged water: 300 parts The above materials were mixed and dispersed for 10 minutes using a homogenizer (Ultra Turrax T50, manufactured by IKA). Ion-exchanged water was added to the obtained dispersion to obtain a colorant particle dispersion with a solid content of 20%. The volume average particle size of the colorant particles in the colorant particle dispersion was 220 nm.

[0158] [Preparation of release agent particle dispersion] Fischer-Tropsch wax (Sasolwax H1, Sasol): 100 parts Anionic surfactant (Neopelex G-65): 6 parts Ion-exchanged water: 300 parts The above materials were mixed and heated to 100°C, and dispersed using a homogenizer (Ultra Turrax T50). Further, the mixture was dispersed using a Manton-Gaulin high pressure homogenizer (Gaulin Co., Ltd.), and ion-exchanged water was added to the dispersion to obtain a release agent particle dispersion with a solid content of 20%. The volume average particle size of the release agent particles in the release agent particle dispersion liquid was 210 nm.

[0159] [Preparation of composite silica particles 1] Into a glass reaction vessel equipped with a metallic stirring rod, a dropping nozzle, and a thermometer, 950 parts of methanol and 166 parts of aqueous ammonia (concentration: 9.6%) were placed and mixed with stirring to obtain an alkali catalyst solution. The temperature of the obtained alkaline catalyst solution was adjusted to 40°C, and the alkaline catalyst solution was replaced with nitrogen. Next, while stirring the alkaline catalyst solution, 1000 parts of tetramethoxysilane (TMOS) and 124 parts of ammonia water (NH4OH) with a concentration of 7.9% were simultaneously dropped to obtain a silica base particle suspension. The obtained silica base particle suspension was heated to 40° C. and stirred while 50 parts of a silane coupling agent (TMOS) was added to the suspension. Stirring was then continued for 120 minutes to react the silane coupling agent and form an adsorption structure. An alcohol solution was prepared by diluting Mo element-containing quaternary ammonium salt (TP-415, manufactured by Hodogaya Chemical Co., Ltd.) with butanol, and added to the suspension. This alcohol solution was added so that the number of parts of Mo element-containing quaternary ammonium salt was 5 parts per 100 parts of the solid content of the silica base particle suspension. The mixture was then stirred at 30°C for 100 minutes to obtain a suspension. Next, 300 parts of the suspension was placed in a reaction vessel, and carbon dioxide was added while stirring, and the temperature and pressure in the reaction vessel were raised to 150°C and 15 MPa. Carbon dioxide was introduced and discharged at a flow rate of 5 L / min while stirring while maintaining the temperature and pressure. The solvent was then removed over 120 minutes to obtain composite silica particles 1.

[0160] [Preparation of Toner 1] Amorphous polyester resin particle dispersion 1 (solid content 20%): 28 parts ·Crosslinked resin particle dispersion 1 (solid content 20%): 14 parts Crystalline polyester resin dispersion (20% solids): 20 parts Colorant particle dispersion (solid content 20%): 6 parts Release agent particle dispersion (solid content 20%): 8 parts Anionic surfactant (Eleminol MON-2, manufactured by Sanyo Chemical Industries, Ltd.): 0.7 parts Ion-exchanged water: 50 parts The above materials were placed in a reaction vessel equipped with a thermometer, a pH meter, and a stirrer, and the temperature of the reaction vessel was kept at 20° C. and the mixture was stirred at 150 rpm for 30 minutes. Then, a 0.3N aqueous nitric acid solution was added to adjust the pH to 4.5, and 20 parts of a 2% aqueous aluminum sulfate solution (flocculant) was added while dispersing with a homogenizer (Ultra Turrax T50). The mixture was then heated to 45° C. at a rate of 0.4° C. / min while stirring, and held for 30 minutes. Next, 124 parts of amorphous polyester resin particle dispersion was added and held for 30 minutes. Next, 0.1N sodium hydroxide aqueous solution was added to adjust the pH to 8.5 and held for 15 minutes, and then the temperature was raised to 80°C at a rate of 1°C / min while continuing stirring, and 80°C was held for 5 hours. Next, cooling and solid-liquid separation were performed, and the solid matter was washed with ion-exchanged water, and then dried in a vacuum freeze dryer for 24 hours to obtain toner particles 1 having a volume average particle size of 5.3 μm. The particle size distribution index GSD(p) of toner particles 1 was 1.25.

[0161] Toner particles 1:100 parts Composite silica particles 1:0.4 parts Hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.): 2.2 parts Aluminum oxide (ALuC805, manufactured by Nippon Aerosil Co., Ltd.): 0.2 parts The above materials were mixed in a Henschel mixer to obtain toner 1. The materials other than toner particles 1 were external additives. "Creating a carrier" Ferrite particles (average particle size 35 μm): 100 parts Toluene: 14 parts Styrene / methyl methacrylate copolymer (copolymer ratio 15 / 85): 3 parts Carbon black: 0.2 parts The above components except for the ferrite particles were dispersed in a sand mill to prepare a dispersion liquid, and this dispersion liquid was placed in a vacuum degassing kneader together with the ferrite particles, and the mixture was dried under reduced pressure while stirring to obtain a carrier. Developer 1 was obtained by mixing 8 parts of toner 1 and 92 parts of carrier.

[0162] [Preparation of toners 2 to 29 and 33 to 39] Toners 2 to 29 and 33 to 39 were obtained in the same manner as Toner 1, except that in the preparation of Toner 1, the type and amount of each material, the pH of the crosslinked resin particle dispersion, and the temperature when the coagulant was added were changed as shown in Table 1. [Preparation of Toner 30] Fine powder components were removed from the toner particles 1 using an elbow jet classifier (EJ-30, manufactured by Nittetsu Mining Co., Ltd.), to obtain toner particles 30 having a GSD(p) of 1.19. In the same manner as in the case of toner 1, external additives were mixed to obtain toner 30. [Preparation of Toner 31] Toner particles 31 having a GSD(p) of 1.36 were obtained in the same manner as in the preparation of toner particles 1, except that the rate of heating up to 45°C was changed from 0.4°C / min to 1.5°C / min, and the pH adjustment value when adding 0.1 N sodium hydroxide aqueous solution was changed from 8.5 to 9.0. In the same manner as in the case of toner 1, external additives were mixed to obtain toner 31. [Preparation of Toner 32] Toner particles 1:100 parts Hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.): 2.2 parts Hydrophobic silica (PM-20, manufactured by Tokuyama Corporation): 0.5 parts The above materials were mixed in a Henschel mixer to obtain Toner 32.

[0163] [Table 1]

[0164] For the toners obtained in Examples 1 to 32 and Comparative Examples 1 to 7, the following values ​​were determined and are shown in Tables 2 and 3. All of the values ​​were measured according to the above-mentioned methods or commonly used methods. "Items related to toner cutting surface" Area ratio of crosslinked resin particles: Described as "Sc". -Porosity of cut surface: Indicated as "Se". ·Se / Sc "Items related to crosslinked resin particles" Glass transition temperature THF insolubles · Swelling degree · Mass proportion of units derived from (meth)acrylate monomers having a carboxyl group: Described as "COOH monomer". · Domain average circle equivalent diameter: This is written as "domain circle equivalent diameter". · Average shape factor SF-1 of the domain: Described as "domain SF-1".

[0165] "Items related to amorphous polyester resins" Glass transition temperature of amorphous polyester resin: T1 T1 (glass transition temperature of amorphous polyester resin) - T2 (glass transition temperature of crosslinked resin particles) Acid number Acid value + hydroxyl value Proportion of aliphatic dicarboxylic acid units of formula (1): Described as "proportion of units of formula (1)". "others" - Crystalline resin ratio in binder resin Particle size distribution index in toner number-average particle size distribution: GSD(p) Toner elements: Aluminum, molybdenum, or magnesium

[0166] [Table 2]

[0167] [Table 3]

[0168] [evaluation] <Image gloss stability> Using the developers of the Examples and Comparative Examples, a solid image (toner amount on the paper: 8.0 g / m) was printed on coated paper (JD Coat 127, Fujifilm Business Innovation Co., Ltd.) in an A3 color multifunction printer (Apeos C3570, Fujifilm Business Innovation Co., Ltd.). 2 After the printed image was sandwiched between two sheets of white paper, the load on the image was adjusted to 60 g / cm 2 A weight was placed on the image so that the weight was 48° C. and the image was left for 60 days in an environment with a temperature of 48% and a humidity of 60%. The glossiness of the image was measured before and after the image was left for 60 days, and the change in glossiness was determined. The gloss level was measured using a micro gloss meter 60° (manufactured by BYK-Gardner). The change in gloss level was evaluated as follows, and the results are shown in Table 3. A: The change in glossiness after the image was left standing relative to the glossiness before the image was left standing was less than 2%, which was not problematic at all. B: The change in glossiness after the image was left standing is from 2% to less than 5% compared to the glossiness before the image was left standing, and although the change is slight, it is fully acceptable. C: The change in glossiness after the image was left standing is between 5% and 10% compared to the glossiness before the image was left standing, and although there is a change in glossiness, it is within the acceptable range. D: The change in glossiness after the image was left standing relative to the glossiness before the image was left standing was 10% or more, which was unacceptable.

[0169] <Low temperature image fixing ability> Using the developers of the Examples and Comparative Examples, a 50% halftone image was printed on "Waterproof White Film" (manufactured by Fujifilm Business Innovation Co., Ltd.) in an environment of 10°C using a modified monochrome printer Revorias Press E1136 (manufactured by Fujifilm Business Innovation Co., Ltd.). The fixing level of the image was evaluated by a tape peeling method. The evaluation criteria were as follows, and the results are shown in Table 2. A: No defects such as missing or blank areas were observed. B: Chips were found in some parts of the image, but they were minor and within the acceptable range. C: Image loss is evident, but is within the acceptable range. D: The image is clearly chipped, blanked, etc., and is at an unacceptable level.

[0170] As shown in Table 3, it was found that the electrostatic image developing toner of the embodiment can achieve both low-temperature fixing properties and image gloss stability during high-pressure storage, compared to the electrostatic image developing toner of the comparative example.

[0171] (Additional Note) (((1))) A toner for developing electrostatic images, comprising a binder resin and crosslinked resin particles, On the cut surface of the electrostatic image developing toner, The area ratio (Sc) of the crosslinked resin particles is 5% or more and 40% or less, The porosity (Se) of the cut surface is 1% or more and 10% or less, The ratio Se / Sc of the porosity (Se) to the area ratio (Sc) is 0.05 or more and 1.5 or less; Toner for developing electrostatic images. (((2))) The toner for developing electrostatic images according to (((1))), wherein the glass transition temperature Tg of the crosslinked resin particles is 0° C. or higher and 30° C. or lower. (((3))) The toner for developing electrostatic images according to (((1))) or (((2))), wherein the crosslinked resin particles have a tetrahydrofuran insoluble content of 90% by mass or more and a swelling degree of 2 or more and 10 or less when permeated in tetrahydrofuran for 24 hours. (((4))) The toner for developing electrostatic images according to any one of (((1))) to (((3))), wherein the crosslinked resin particles contain a styrene-(meth)acrylate copolymer. (((5))) The crosslinked resin particles have, as units derived from a (meth)acrylate monomer, units derived from a monofunctional (meth)acrylate monomer and a difunctional (meth)acrylate monomer, The unit derived from the monofunctional (meth)acrylate monomer includes a unit derived from a (meth)acrylate monomer having a carboxyl group and a unit derived from a (meth)acrylate monomer not having a carboxyl group. The toner for developing electrostatic images according to any one of (((1))) to (((4))). (((6))) The toner for developing electrostatic images according to (((5))), wherein the mass ratio of the units derived from the (meth)acrylate monomer having a carboxyl group in the crosslinked resin particles is from 0.01 mass % to 0.50 mass %. (((7))) The toner for developing electrostatic images according to any one of (((1))) to (((6))), wherein the binder resin contains an amorphous polyester resin. (((8))) When the glass transition temperature of the amorphous polyester resin is T1 (°C) and the glass transition temperature of the crosslinked resin particles is T2 (°C), 30≦ T1-T2 ≦70 (℃) The toner for developing electrostatic images according to (((7))), (((9))) The toner for developing electrostatic images according to (((7))) or (((8))), wherein the amorphous resin comprises an amorphous polyester resin, and the crystalline resin comprises a crystalline polyester resin. (((10))) The toner for developing electrostatic images according to any one of (((7))) to (((9))), wherein the sum of the acid value (mg KOH / g) and the hydroxyl value (mg KOH / g) of the amorphous polyester resin is 15 or more and 40 or less. (((11))) The amorphous polyester resin contains a unit derived from an aliphatic dicarboxylic acid represented by formula (1), In the units derived from dicarboxylic acid in the entirety of the amorphous polyester resin, the ratio of units derived from aliphatic dicarboxylic acid is 1 mol % or more and 30 mol % or less. The toner for developing electrostatic images according to any one of (((7))) to (((10))). Formula (1) -OC-(CH2) n -CO- (In the formula, n is an integer of 4 or more and 12 or less.)

[0172] (((12))) The toner for developing electrostatic images according to any one of ((1)) to (((11))), wherein the binder resin contains a crystalline resin in an amount of 15% by mass or more and 40% by mass or less. (((13))) The toner for developing electrostatic images according to any one of (((1))) to (((12))), wherein the average equivalent circle diameter of the domains formed by the crosslinked resin particles is 50 nm or more and 300 nm or less. (((14))) The toner for developing electrostatic images according to any one of ((1))) to (((13))), wherein an average shape factor SF-1 of domains formed by the crosslinked resin particles is 130 or less. (((15))) The toner for developing electrostatic images according to any one of (((1))) to (((14))), wherein in a number average particle size distribution of the toner for developing electrostatic images, a particle size distribution index GSD(p) represented by formula (2) is 1.20 or more and 1.35 or less. Equation (2) GSD(p)=1+(D50(p)-D16(p)) / D50(p) (In the formula, D16(p) and D50(p) are the particle sizes at which the cumulative numbers are 16% and 50%, respectively, in the cumulative curve of the number particle size distribution.) (((16))) The toner for developing electrostatic images according to any one of (((1))) to (((15))), further comprising one or more elements selected from the group consisting of aluminum, molybdenum and magnesium. (((17))) An electrostatic image developer comprising the toner for developing electrostatic images according to any one of (((1))) to (((16))). (((18))) The toner for developing electrostatic images according to any one of (((1))) to (((16))) is contained in the container, A toner cartridge that is detachably attached to an image forming apparatus. (((19)) a developing means for developing an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer according to (((17))), A process cartridge that is detachably attached to an image forming apparatus. (((20))) An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; a developing means for containing the electrostatic image developer according to (((17))) and developing the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:

[0173] According to the invention of (((1))), in a toner for developing electrostatic images containing a binder resin and crosslinked resin particles, it is possible to achieve both low-temperature fixability and image gloss stability during high-pressure storage, as compared with a case in which the ratio Se / Sc of the porosity (Se) to the area ratio (Sc) is less than 0.05 or exceeds 1.5. According to the invention (((2))), it is possible to provide a toner for developing electrostatic images which has good low-temperature fixing properties compared to a case in which the glass transition temperature Tg of the crosslinked resin particles is lower than 0°C or higher than 30°C. According to the invention of (((3))), the crosslinked resin particles have an appropriate degree of crosslinking and swelling compared to when the crosslinked resin particles have a tetrahydrofuran insoluble content of less than 90% by mass, or when the swelling degree when soaked in tetrahydrofuran for 24 hours is less than 2 or exceeds 10. This makes it possible to prevent the crosslinked resin particles from flowing and being exposed to the toner surface during fixing. According to the invention of (((4))), the crosslinked resin particles can be controlled so that they aggregate more easily than a case in which the crosslinked resin particles do not contain a styrene-(meth)acrylate copolymer, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of (((5))), it is possible to provide a toner for developing electrostatic images in which the crosslinked resin particles can be controlled to aggregate more easily and the void ratio is controlled within a suitable range, compared to a case in which the crosslinked resin particles do not contain three types of units derived from monofunctional (meth)acrylate monomers: a unit derived from a (meth)acrylate monomer having a carboxyl group, a unit derived from a (meth)acrylate monomer not having a carboxyl group, and a unit derived from a bifunctional (meth)acrylate monomer. According to the invention of (((6))), the crosslinked resin particles can be controlled so that they are more likely to aggregate than crosslinked resin particles having a mass ratio of units derived from a (meth)acrylate monomer having a carboxyl group that is less than 0.01 mass % or more than 0.50 mass %, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of (((7))), the binder resin can be controlled so that crosslinked resin particles are more likely to aggregate than when the binder resin does not contain an amorphous polyester resin, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of (((8))), when the glass transition temperature of the amorphous polyester resin is T1 (°C) and the glass transition temperature of the crosslinked resin particles is T2 (°C), the crosslinked resin particles can be controlled to aggregate more easily than when (T1-T2) is less than 30°C or exceeds 70°C, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of (((9))), the crosslinked resin particles can be controlled so as to be more easily aggregated than when the acid value of the amorphous polyester resin is less than 5 mg KOH / g or more than 20 mg KOH / g, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of (((10))), the sum of the acid value (mg KOH / g) and the hydroxyl value (mg KOH / g) of the amorphous polyester resin can be controlled so that the crosslinked resin particles are more likely to aggregate than when the sum is less than 15 or exceeds 40, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided.

[0174] According to the invention (((11))), the amorphous polyester resin contains units derived from an aliphatic dicarboxylic acid represented by formula (1), and compared with a case in which the proportion of units derived from an aliphatic dicarboxylic acid in the entire dicarboxylic acid-derived units of the amorphous polyester resin is less than 1 mol % or exceeds 30 mol %, the crosslinked resin particles can be controlled to be more easily aggregated, and a toner for developing electrostatic images in which the void ratio is controlled within a suitable range can be provided. According to the invention of (((12))), by setting the binder resin to a suitable ratio of crystalline resin to amorphous resin, it is possible to provide a toner for developing electrostatic images having improved low-temperature fixing properties, compared to a case where the binder resin contains less than 15% by mass or more than 40% by mass of crystalline resin. According to the invention of (((13))), it is possible to provide a toner for developing electrostatic images which is more effectively prevented from being exposed to the surface of a fixed image by controlling the domain size of the crosslinked resin particles, compared to a case where the average equivalent circular diameter of the domains formed by the crosslinked resin particles is less than 50 nm or exceeds 300 nm. According to the invention of (((14))), it is possible to provide a toner for developing electrostatic images which is more prevented from being exposed to the surface of a fixed image by controlling the domain size of the crosslinked resin particles, as compared with a case in which the average shape factor SF-1 of the domains formed by the crosslinked resin particles exceeds 130. According to the invention of (((15))), in the number average particle size distribution of the toner for developing electrostatic images, smaller diameter particles are more likely to be exposed to the surface than when the particle size distribution index GSD(p) represented by formula (2) is less than 1.20 or exceeds 1.35. However, by controlling the number of small diameter particles, it is possible to provide a toner for developing electrostatic images in which exposure to the surface of a fixed image is more effectively prevented. According to the invention of (((16))), by containing an element having high thermal conductivity in the toner particles, it is possible to provide a toner for developing electrostatic images having improved fixing properties by increasing thermal conductivity outside voids, compared to a toner for developing electrostatic images that does not contain one or more elements selected from the group consisting of aluminum, molybdenum, and magnesium. According to the invention of (((17))), (((18))), (((19))) or (((20))), it is possible to provide an electrostatic image developer, a toner cartridge, a process cartridge or an image forming apparatus which, in a toner for developing electrostatic images containing a binder resin and crosslinked resin particles, makes it possible to achieve both low-temperature fixing ability and image gloss stability during high-pressure storage, as compared with a case in which the ratio Se / Sc of the porosity (Se) to the area ratio (Sc) is less than 0.01 or exceeds 0.5. [Explanation of symbols]

[0175] 1Y, 1M, 1C, 1K Photoconductor (an example of an image carrier) 2Y, 2M, 2C, 2K Charging roll (an example of a charging means) 3 Exposure device (an example of an electrostatic image forming means) 3Y, 3M, 3C, 3K laser beam 4Y, 4M, 4C, 4K developing device (an example of developing means) 5Y, 5M, 5C, 5K Primary transfer roll (an example of a primary transfer means) 6Y, 6M, 6C, 6K: Photoconductor cleaning device (an example of an image carrier cleaning means) 8Y, 8M, 8C, 8K toner cartridges 10Y, 10M, 10C, 10K Image forming units 20 Intermediate transfer belt (an example of an intermediate transfer body) 22 Driving Roll 24 Support roll 26 Secondary transfer roll (an example of a secondary transfer means) 28 Fixing device (an example of a fixing means) 30 Intermediate transfer belt cleaning device (an example of an intermediate transfer body cleaning means) 107 Photoconductor (an example of an image carrier) 108 Charging roll (an example of charging means) 109 Exposure device (an example of electrostatic image forming means) 111 Developing device (an example of developing means) 112 Transfer device (an example of a transfer means) 113 Photoconductor cleaning device (an example of an image carrier cleaning means) 115 Fixing device (an example of fixing means) 116 Mounting Rail 117 Cabinet 118 Exposure Aperture 200 Process Cartridge 300 Recording paper (an example of a recording medium) P Recording paper (an example of a recording medium)

Claims

1. A toner for developing electrostatic images, comprising a binder resin and crosslinked resin particles, On the cut surface of the electrostatic image developing toner, The area ratio (Sc) of the crosslinked resin particles is 5% or more and 40% or less, The porosity (Se) of the cut surface is 1% or more and 10% or less, The ratio Se / Sc of the porosity (Se) to the area ratio (Sc) is 0.05 or more and 1.5 or less; Toner for developing electrostatic images.

2. 2. The toner for developing electrostatic images according to claim 1, wherein the glass transition temperature Tg of the crosslinked resin particles is from 0° C. to 30° C.

3. 2. The toner for developing electrostatic images according to claim 1, wherein the crosslinked resin particles have a tetrahydrofuran insoluble content of 90% by mass or more and a swelling degree of 2 to 10 when permeated in tetrahydrofuran for 24 hours.

4. 2. The toner for developing electrostatic images according to claim 1, wherein said crosslinked resin particles contain a styrene-(meth)acrylate copolymer.

5. The crosslinked resin particles have, as units derived from a (meth)acrylate monomer, units derived from a monofunctional (meth)acrylate monomer and units derived from a difunctional (meth)acrylate monomer, The unit derived from the monofunctional (meth)acrylate monomer includes a unit derived from a (meth)acrylate monomer having a carboxyl group and a unit derived from a (meth)acrylate monomer not having a carboxyl group.

2. The toner for developing electrostatic images according to claim 1.

6. 6. The toner for developing electrostatic images according to claim 5, wherein the mass ratio of the units derived from the (meth)acrylate monomer having a carboxyl group in the crosslinked resin particles is from 0.01% by mass to 0.50% by mass.

7. 2. The toner for developing electrostatic images according to claim 1, wherein the binder resin comprises an amorphous polyester resin.

8. When the glass transition temperature of the amorphous polyester resin is T1 (°C) and the glass transition temperature of the crosslinked resin particles is T2 (°C), 30≦T1-T2≦70 (℃) 8. The toner for developing electrostatic images according to claim 7, wherein

9. 8. The toner for developing electrostatic images according to claim 7, wherein the acid value of the amorphous polyester resin is from 5 mgKOH / g to 20 mgKOH / g.

10. 8. The toner for developing electrostatic images according to claim 7, wherein the sum of the acid value (mgKOH / g) and the hydroxyl value (mgKOH / g) of the amorphous polyester resin is 15 or more and 40 or less.

11. The amorphous polyester resin contains a unit derived from an aliphatic dicarboxylic acid represented by formula (1), the ratio of units derived from aliphatic dicarboxylic acids to units derived from dicarboxylic acids in the entire amorphous polyester resin is 1 mol % or more and 30 mol % or less; The toner for developing electrostatic images according to claim 7. Formula (1) -OC-(CH 2 ) n -CO- (In the formula, n is an integer of 4 or more and 12 or less.)

12. 2. The toner for developing electrostatic images according to claim 1, wherein the binder resin contains a crystalline resin in an amount of 15% by mass or more and 40% by mass or less.

13. 2. The toner for developing electrostatic images according to claim 1, wherein the average equivalent circle diameter of the domains formed by the crosslinked resin particles is 50 nm or more and 300 nm or less.

14. 2. The toner for developing electrostatic images according to claim 1, wherein the domains formed by the crosslinked resin particles have an average shape factor SF-1 of 130 or less.

15. 2. The toner for developing an electrostatic image according to claim 1, wherein in the number average particle size distribution of the toner for developing an electrostatic image, a particle size distribution index GSD(p) represented by the formula (2) is 1.20 or more and 1.35 or less. Formula (2) GSD(p)=1+(D50(p)-D16(p)) / D50(p) (In the formula, D16(p) and D50(p) are particle sizes at which the cumulative numbers are 16% and 50%, respectively, in the cumulative curve of the number particle size distribution.)

16. 2. The toner for developing an electrostatic image according to claim 1, further comprising at least one element selected from the group consisting of aluminum, molybdenum and magnesium.

17. An electrostatic image developer comprising the toner for developing electrostatic images according to any one of claims 1 to 16.

18. The toner for developing an electrostatic image according to any one of claims 1 to 16 is contained therein, A toner cartridge that is detachably attached to an image forming apparatus.

19. a developing unit that contains the electrostatic image developer according to claim 17 and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer, A process cartridge that is detachably attached to an image forming apparatus.

20. An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; a developing unit that contains the electrostatic image developer according to claim 17 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:

Citation Information

Patent Citations

  • Electrophotographic toner

    JP2008257056A

  • Toner for electrostatic charge image development

    JP2011257744A