Copper terminal material with film and manufacturing method of the same
A copper terminal material with a controlled tin layer thickness and surface texture, combined with copper-tin alloy and nickel layers, addresses adhesion and force issues in connectors, ensuring stable and low-friction operation.
Patent Information
- Application Number
- JP2024023852
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-02-20
- Publication Date
- 2024-10-09
AI Technical Summary
Existing copper terminal materials face issues with adhesion and increased insertion/extraction force due to the softness of the tin layer, especially in multi-pin connectors, leading to difficulties in connector assembly.
A copper terminal material with a controlled surface texture and composition, featuring a tin layer with specific thickness and curvature, along with optional copper-tin alloy and nickel layers, is manufactured through precise plating and reflow processes to stabilize the dynamic friction coefficient and prevent adhesion.
The material achieves stable and reduced insertion/extraction forces, preventing adhesion and maintaining low dynamic friction, while preserving electrical properties and heat resistance.
Smart Images

Figure 2024139698000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a film-coated copper terminal material useful as a connector terminal used for connecting electrical wiring in automobiles, consumer devices, etc., particularly as a terminal for a multi-pin connector, and a method for producing the same. [Background technology]
[0002] As a coated copper terminal material, there is a type in which a copper (Cu) plating layer and a tin (Sn) plating layer are formed on a base material made of a copper alloy, and then a reflow process is performed to suppress the generation of whiskers, forming a copper-tin (CuSn) alloy layer under the tin layer on the surface. This coated copper terminal material is widely used as a terminal material because it has high connection reliability and can be manufactured inexpensively.
[0003] For example, Patent Document 1 discloses a conductive material in which a Cu-Sn alloy coating layer mainly composed of a Cu6Sn5 phase and a Sn coating layer are formed in this order on the surface of a base material made of a Cu alloy strip. This conductive material is produced by roughening the surface of the base material to a surface roughness of 0.15 μm or more in at least one direction and 4.0 μm or less in all directions, forming a Cu plating layer and a Sn plating layer in this order on the surface of the base material, and then performing a reflow treatment.
[0004] Patent Document 2 discloses a Sn-plated material in which a Cu-Sn alloy layer made of many Cu-Sn alloy crystal grains and a top layer made of a Sn layer in the recesses between adjacent Cu-Sn alloy crystal grains on the top surface are formed on the surface of an underlayer on a substrate made of copper or a copper alloy. It is described that the area ratio of the Sn layer 16 on the top surface is 20 to 80%, and the maximum thickness of the Sn layer 16 is smaller than the average grain size of the Cu-Sn alloy crystal grains.
[0005] However, because the tin layer (Sn layer) is soft, adhesion is likely to occur between the contacts. In addition, the contact area between the contacts becomes larger, which causes excessive friction when inserting the connector, making insertion difficult, especially in multi-pin terminals.
[0006] Patent Document 3 discloses a plating material in which a base layer of Ni or the like is provided on a conductive substrate, an intermediate layer of copper or a copper alloy is provided on that, and an outermost layer made of a Cu-Sn intermetallic compound is provided on that. It is described that because the outermost layer is made of a hard Cu-Sn intermetallic compound layer, fretting is unlikely to occur even if the contact pressure between terminals is reduced.
[0007] However, when the outermost layer is a Cu-Sn intermetallic compound layer, copper (Cu) diffuses at high temperatures, and copper oxide is likely to form on the surface. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2006-077307 A [Patent Document 2] JP 2015-180770 A [Patent Document 3] JP 2007-247060 A Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made in consideration of the above circumstances, and aims to provide a coated copper terminal material that prevents adhesion when used as a connector and stably reduces insertion and removal force. [Means for solving the problem]
[0010] The film-coated copper terminal material of the present invention has a substrate made of copper or a copper alloy and a film formed on the substrate, the film having a tin layer made of tin or a tin alloy with an average thickness of 0.2 μm or more and 2.0 μm or less on the surface thereof, and the arithmetic mean curvature Spc of the peaks on the surface of the film is 10 mm -1 More than 70mm -1or less, and the standard deviation / average value (CV value) of the Spc when measuring 10 visual fields is within 30%.
[0011] This coated copper terminal material has a tin layer on the surface, and therefore has good electrical properties inherent to the tin layer. If the average thickness of this tin layer is less than 0.2 μm, Cu diffuses at high temperatures, and Cu oxides are likely to form on the surface, which may increase the contact resistance. If it exceeds 2.0 μm, the soft tin layer increases the insertion and removal force when used as a connector, making it difficult to reduce the insertion and removal force associated with the increased number of pins in the connector. The average thickness of the tin layer is preferably 0.3 μm or more and 1.8 μm or less.
[0012] The arithmetic mean curvature Spc of the peaks on the coating surface is 10 mm -1 More than 70mm -1 By setting it to below, the dynamic friction coefficient can be reduced, and by setting the standard deviation / average value of Spc when measuring 10 visual fields to below 30%, the dynamic friction coefficient is stabilized and local fluctuations are also suppressed.
[0013] The arithmetic mean curvature Spc of the peak is specified in ISO-25178, and the larger the value, the sharper the point that contacts the mating terminal. -1 If the Spc is less than 70mm, the surface becomes nearly flat, so the contact area when it comes into contact with the mating terminal as a connector becomes large, and the dynamic friction coefficient increases. -1 If it exceeds this value, the surface irregularities become too steep, causing the mating terminal to be dug up. If the standard deviation / average value of Spc exceeds 30%, local fluctuations occur in the dynamic friction coefficient, making it unstable.
[0014] Spc is 20mm -1 More than 60mm -1 More preferably, the standard deviation / average value of Spc is 25% or less.
[0015] In the plating film-coated copper terminal material of the present invention, the plating film may have a copper-tin alloy layer made of an alloy of copper and tin under the tin layer. The average thickness of the copper-tin alloy layer is preferably 0.2 μm or more and 2.5 μm or less.
[0016] In the plating film-coated copper terminal material of the present invention, the film may have a nickel layer made of nickel or a nickel alloy in contact with the base material.
[0017] The nickel layer can prevent the diffusion of copper from the substrate and improve heat resistance. The average thickness of this nickel layer is preferably 0.05 μm or more and 1.0 μm or less.
[0018] The method for producing a film-coated copper terminal material of the present invention includes a plating step of forming a plated material on the substrate by forming a plating layer having a tin plating layer made of tin or a tin alloy on the surface thereof, and a reflow step of heating and reflowing the plated material. The thickness of the tin plating layer in the plating step is 0.2 μm or more and 3.0 μm or less. The reflow treatment includes a heating step of heating the plated material to a peak temperature of 240° C. or more and 300° C. or less, a primary cooling step of passing the plated material through a cooling furnace having an internal temperature of 20° C. or more and 70° C. or less to reduce the material temperature of the plated material to 150° C. or more and 220° C. or less after the heating step, and a secondary cooling step of cooling the plated material at a cooling rate of 100° C. / sec. or more and 300° C. / sec. after the primary cooling step. In the primary cooling step, cooling air is blown onto the surface of the plated material at a rate of 10 m / s. 3 / min more than 300m 3 Spray at a rate of less than 1 / min.
[0019] If the thickness of the tin plating layer made of tin or a tin alloy is less than 0.2 μm or exceeds 3.0 μm, the average thickness of the tin layer after reflow treatment will be less than 0.2 μm or exceed 2.0 μm, and the desired tin layer cannot be obtained.
[0020] If the peak temperature in the heating step is less than 240° C., the tin will not melt uniformly, and if the peak temperature exceeds 300° C., the copper-tin intermetallic compound will grow rapidly and the unevenness of the copper-tin alloy layer will become large, which is undesirable.
[0021] In the cooling process of the reflow treatment, a primary cooling process is provided in which the plated material is passed through a cooling furnace with an internal temperature of 20°C to 70°C in order to bring the material temperature to 150°C to 220°C inclusive, thereby cooling it to a temperature below the melting point of tin, and then the plated material is rapidly cooled at a high cooling rate in the secondary cooling process.
[0022] In the primary cooling process, a specified amount of cooling air is blown onto the surface of the plated material in a cooling furnace at a specified furnace temperature, thereby appropriately controlling the surface shape at a temperature below the melting point of tin, and the arithmetic mean curvature Spc of the peaks on the plated film surface is adjusted to 10 mm -1 More than 70mm -1 With the above, the standard deviation / average value (CV value: coefficient of variation) of Spc when measuring 10 visual fields can be kept at 30% or less.
[0023] In this case, if the temperature inside the cooling furnace is less than 20°C, the cooling rate will be too fast, and the Spc and CV values (standard deviation / average value) of Spc will be too large. -1 In the following, the CV value (standard deviation / average value) of Spc cannot be set below 30%. If the temperature inside the furnace exceeds 70°C, the cooling time to the temperature below the melting point of tin is too long, and the CV value (standard deviation / average value) of Spc becomes excessively large.
[0024] Regarding the material temperature of the plated material, if it is less than 150°C, the cooling time is too long, and the CV value (standard deviation / average value) of Spc becomes excessively large. If the material temperature exceeds 220°C, the tin is secondary cooled while still in a semi-molten state, and the CV value (standard deviation / average value) of Spc becomes excessively large. The material temperature is preferably 160°C or higher and 210°C or lower, and more preferably 170°C or higher and 200°C or lower.
[0025] Cooling air volume is 10m 3 At less than 10 mm / min, cooling is insufficient and Spc becomes too small. -1 On the other hand, the cooling air volume cannot be more than 300 m 3If the cooling air temperature exceeds 100°C / min, the molten tin will flow due to the large amount of air blown, and the Spc and CV values of Spc (standard deviation / average value) will become excessively large. The temperature of the cooling air is preferably 30°C or higher and 60°C or lower.
[0026] Then, the material is rapidly cooled in a secondary cooling step to obtain the desired surface shape. If the cooling rate in the secondary cooling step is less than 100° C. / sec, the desired surface shape cannot be obtained. It is difficult to achieve a cooling rate of more than 300° C. / sec.
[0027] In the method for producing a film-coated copper terminal material of the present invention, in the plating step, the tin plating layer may be formed after a copper plating layer made of copper or a copper alloy is formed on the base material.
[0028] When a copper plating layer is formed, the heating rate of the plated material in the heating step is preferably 20° C. / sec or more and 75° C. / sec or less. If the heating rate is less than 20° C. / sec, copper atoms preferentially diffuse into the grain boundaries of tin before the tin melts, and copper-tin intermetallic compounds grow abnormally near the grain boundaries, making it impossible to obtain a desired copper-tin alloy layer. On the other hand, if the heating rate exceeds 75° C. / sec, the growth of the copper-tin intermetallic compounds is insufficient, making it impossible to obtain a desired copper-tin alloy layer.
[0029] When a copper plating layer is formed, if the peak temperature in the heating step is less than 240° C., the tin does not melt uniformly, and if the peak temperature exceeds 300° C., the copper-tin intermetallic compounds grow rapidly and the copper-tin alloy layer becomes uneven, which is not preferable. Also, if the cooling rate in the secondary cooling step is less than 100° C. / sec, the copper-tin intermetallic compounds grow, and the desired copper-tin alloy layer cannot be obtained.
[0030] In the method for producing a film-coated copper terminal material of the present invention, the plating step may include forming a nickel plating layer made of nickel or a nickel alloy on the surface of the base material. Effect of the Invention
[0031] According to the present invention, the arithmetic mean curvature Spc of the peaks on the surface of the tin layer forming the surface of the terminal material is set to 10 mm -1 More than 70mm -1 By setting the standard deviation / average value of Spc when measuring from 10 visual fields at 30% or less, it is possible to provide a coated copper terminal material that prevents adhesion when used as a connector, reduces the dynamic friction coefficient and stabilizes the dynamic friction coefficient, thereby stably reducing the insertion / removal force. [Brief description of the drawings]
[0032] [Figure 1] 1 is a cross-sectional view showing a schematic diagram of a first embodiment of a film-coated copper terminal material of the present invention. [Diagram 2] 2 is a cross-sectional view showing the plated material in the process of being manufactured as the film-coated copper terminal material of FIG. 1. [Diagram 3] FIG. 2 is a cross-sectional view showing a schematic diagram of a second embodiment of the film-coated copper terminal material of the present invention. [Figure 4] 4 is a cross-sectional view showing the plated material in the process of being manufactured as the film-coated copper terminal material of FIG. 3. [Diagram 5] FIG. 3 is a cross-sectional view showing a schematic diagram of a third embodiment of the film-coated copper terminal material of the present invention. [Figure 6] 6 is a cross-sectional view showing the plated material in the middle of the production of the film-coated copper terminal material of FIG. 5. [Figure 7] FIG. 4 is a cross-sectional view showing a schematic diagram of a fourth embodiment of the film-coated copper terminal material of the present invention. [Figure 8] 8 is a cross-sectional view showing the plated material in the process of being manufactured as the film-coated copper terminal material of FIG. 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] An embodiment of the film-coated copper terminal material of the present invention will be described.
[0034] (First embodiment) As shown in FIG. 1, the film-coated copper terminal material 1 of the first embodiment has a film 5 formed by laminating a tin layer 3 made of tin or a tin alloy on a substrate 2 made of copper or a copper alloy.
[0035] The substrate 2 is a strip material formed into a band-like plate shape, and the composition thereof is not particularly limited as long as the surface thereof is made of copper or a copper alloy.
[0036] The tin layer 3 is formed by forming a plating layer made of tin or a tin alloy on the base material 2 and then performing a reflow treatment.
[0037] The average thickness of the tin layer 3 is 0.2 μm or more and 2.0 μm or less. The tin layer 3 has lubricity that reduces the insertion and removal force required for the connector, and also reduces contact resistance to provide excellent electrical properties. However, if the average thickness is less than 0.2 μm, it becomes difficult to obtain the excellent properties of tin. In addition, solderability and corrosion resistance may also be reduced.
[0038] On the other hand, if the average thickness of the tin layer 3 exceeds 2.0 μm, it becomes soft and adhesion occurs easily, and the insertion and extraction force during use as a connector increases, making it difficult to reduce the insertion and extraction force associated with an increase in the number of pins in the connector. The average thickness of this tin layer 3 is preferably 0.3 μm or more and 1.8 μm or less.
[0039] The arithmetic mean curvature Spc of the peaks on the surface of the tin layer 3 is 10 mm -1 More than 70mm -1 and the standard deviation / average value (coefficient of variation) of Spc when measuring 10 visual fields is 30% or less.
[0040] The arithmetic mean curvature Spc of the peak is specified in ISO-25178, and the larger the value, the sharper the point of contact with another object. -1 If the thickness is less than this, the surface becomes nearly flat, so that the contact area when the connector comes into contact with a mating terminal becomes large, and the dynamic friction coefficient increases.
[0041] Spc is 70mm -1If the standard deviation / average value of Spc exceeds 30%, the dynamic friction coefficient will fluctuate locally and become unstable. Spc is 20mm -1 More than 60mm -1 More preferably, the standard deviation / average value of Spc is 25% or less.
[0042] A method for producing the film-coated copper terminal material 1 thus constructed will be described. This coated copper terminal material 1 is formed by applying tin plating made of tin or a tin alloy onto a substrate 2 to form a plated material 7 having a tin plating layer 4 laminated on the substrate 2 as shown in FIG. 2, and then performing a reflow treatment.
[0043] As the substrate 2, a plate made of copper or a copper alloy is prepared, and the surface of this plate is cleaned by degreasing, pickling, and other treatments.
[0044] As a plating bath for tin plating, a general tin plating bath may be used, for example, a sulfuric acid bath mainly composed of sulfuric acid (H2SO4) and stannous sulfate (SnSO4). The temperature of the plating bath is 15 to 35°C, and the current density is 1 to 30 A / dm 2 The thickness of the tin plating layer 4 is set to be 0.2 μm or more and 3.0 μm or less.
[0045] If the thickness of the tin plating layer 4 is less than 0.2 μm or exceeds 3.0 μm, the average thickness of the tin layer 3 after reflow treatment will be less than 0.2 μm or exceed 2.0 μm, and the desired tin layer 3 cannot be obtained.
[0046] The reflow treatment involves heating the plated material 7 to melt the tin plating layer 4 once and then rapidly cooling it. Specifically, the treatment includes a heating step in which the plated material 7 is heated to a temperature of 240°C to 300°C, which is higher than the melting point of tin, in a heating furnace with a CO reducing atmosphere, a primary cooling step in which the plated material 7 is passed through a cooling furnace with an internal temperature of 20°C to 70°C after the heating step to make the material temperature of the plated material 7 150°C to 220°C, and a secondary cooling step in which the plated material 7 is cooled at a cooling rate of 100°C / sec to 300°C / sec after the primary cooling.
[0047] In this case, in the primary cooling process, cooling air is blown to the surface of the plating material 7 at a speed of 10 m 3 / min more than 300m 3 The temperature of the cooling air is preferably 30°C or higher and 60°C or lower.
[0048] By carrying out the heating step in a reducing atmosphere, it is possible to prevent the formation of a tin oxide film, which has a high melting temperature, on the surface of the tin plating layer 4, and to carry out the reflow treatment at a lower temperature in a shorter time.
[0049] If the peak temperature in the heating process is less than 240°C, the tin will not melt uniformly, and if the peak temperature exceeds 300°C, the copper of the substrate 2 will diffuse into the tin plating layer 4, forming voids at the interface between the substrate 2 and the tin layer 3, which may cause the tin layer to peel off.
[0050] The cooling process after heating is divided into two stages. In the first cooling process, the plated material 7 is passed through a cooling furnace with an internal temperature of 20°C to 70°C and the material temperature reached by the plated material 7 is cooled to below the melting point of tin, and then in the second cooling process, it is rapidly cooled at a faster cooling rate.
[0051] In the primary cooling process, a predetermined cooling air is blown onto the surface of the plating material 7 in a cooling furnace at a predetermined furnace temperature to appropriately control the surface shape at a temperature below the melting point of tin. This allows the arithmetic mean curvature Spc of the peaks on the surface of the coating 5 (tin layer 3) to be reduced to 10 mm -1 More than 70mm -1Hereinafter, the standard deviation / average value (CV value) of Spc when measuring 10 visual fields can be made 30% or less.
[0052] In this case, if the temperature inside the cooling furnace is less than 20°C, the cooling rate is too fast, and the Spc and CV values (standard deviation / average value) of Spc become excessively large. -1 In the following cases, the CV value (standard deviation / average value) of Spc cannot be set below 30%. If the temperature inside the furnace exceeds 70°C, the cooling time required to reach a temperature below the melting point of tin is too long, and the CV value (standard deviation / average value) of Spc becomes excessively large.
[0053] If the material temperature of the plating material 7 in the primary cooling process is less than 150°C, the cooling time is too long and the CV value (standard deviation / average value) of Spc becomes excessively large. If the temperature of the plating material 7 does not drop to 220°C or less in the primary cooling process, the tin will be in a semi-molten state during secondary cooling, and the CV value (standard deviation / average value) of Spc will become excessively large. The material temperature of the plating material 7 in the primary cooling process is preferably 160°C or more and 210°C or less, and more preferably 170°C or more and 200°C or less.
[0054] The volume of cooling air in the primary cooling process is 10 m 3 At less than 10 mm / min, cooling is insufficient and Spc becomes too small. -1 On the other hand, the cooling air volume cannot be more than 300m 3 If the speed exceeds 1 / min, the molten tin will flow due to the large amount of air hitting it, and the Spc and CV values of Spc (standard deviation / average value) will become excessively large.
[0055] The cooling air is blown perpendicularly to the plated material 7 from a height of about 10 cm above the surface of the plated material 7.
[0056] Next, in the secondary cooling step, the plated material 7 is quenched to complete the process with a desired surface shape. If the cooling rate in this secondary cooling step is less than 100°C / sec, the desired surface shape cannot be obtained. It is difficult to achieve a cooling rate of more than 300°C / sec.
[0057] The coating 5 of the copper terminal material 1 with a plating film manufactured in this manner has a surface made of the tin layer 3, and therefore has good electrical properties inherent to tin. In addition, the arithmetic mean curvature Spc of the peaks on the surface of the coating 5 (tin layer 3) is 10 mm -1 More than 70mm -1 Since the coefficient of dynamic friction is less than or equal to 100 kPa, the coefficient of dynamic friction can be reduced.
[0058] Furthermore, by setting the standard deviation / average value of Spc when measuring in 10 visual fields to 30% or less, the dynamic friction coefficient is stabilized and local fluctuations are also suppressed.
[0059] Therefore, by using the film-coated copper terminal material 1 as a terminal material for a connector, the insertion and withdrawal force can be stably reduced, and adhesion with the mating terminal can be prevented.
[0060] Second embodiment 3, the film-coated copper terminal material 11 of the second embodiment is formed by laminating a copper-tin alloy layer 13 made of an alloy of copper and tin and a tin layer 14 in this order on a film 12 provided on a substrate 2. In other words, the film 12 has a copper-tin alloy layer 13 below the tin layer 14.
[0061] The copper-tin alloy layer 13 and the tin layer 14 are formed by sequentially plating the base material 2 with copper or a copper alloy and tin or a tin alloy, followed by a reflow treatment, as described below.
[0062] The copper-tin alloy layer 13 is formed to an average thickness of 0.2 μm or more and 2.5 μm or less. If the thickness is less than 0.2 μm, the contact resistance may increase in a high-temperature environment. If the thickness exceeds 2.5 μm, the copper-tin alloy layer 13 is hard and may cause cracks during bending. The copper-tin alloy layer 13 preferably has an average crystal grain size of 0.2 μm or more and 1.5 μm or less.
[0063] This copper-tin alloy layer 13 is composed of a lower Cu3Sn layer 15 and a Cu6Sn5 layer 16 disposed on the Cu3Sn layer 15. The Cu3Sn layer 15 is partially formed on the surface of the base material 2, and therefore the Cu6Sn5 alloy layer 16 is formed so as to extend over both the Cu3Sn alloy layer 15 on the base material 2 and the portion of the base material 2 where the Cu3Sn alloy layer 15 is not present.
[0064] As in the first embodiment, the average thickness of the tin layer 14 is 0.2 μm or more and 2.0 μm or less. If the thickness of the tin layer 14 is less than 0.2 μm, copper diffuses at high temperatures and copper oxide is easily formed on the surface, which may increase the contact resistance and cause a decrease in connection reliability. In addition, solderability and corrosion resistance may also decrease.
[0065] On the other hand, if the average thickness of the tin layer 14 exceeds 2.0 μm, the effect of hardening the surface base by the copper-tin alloy layer 13 existing under the soft tin layer 14 is weakened, the insertion and removal force during use as a connector increases, and it is difficult to reduce the insertion and removal force associated with an increase in the number of pins of the connector. The average thickness of this tin layer 14 is preferably 0.3 μm or more and 1.8 μm or less.
[0066] As in the first embodiment, the arithmetic mean curvature Spc of the peaks on the surface of the tin layer 14 is 10 mm -1 More than 70mm -1 and the standard deviation / average value of Spc when measuring 10 visual fields is 30% or less.
[0067] The arithmetic mean curvature Spc of the peak is specified in ISO-25178, and the larger the value, the sharper the point of contact with another object. -1 If the Spc is less than 70mm, the surface becomes nearly flat, so the contact area when it comes into contact with the mating terminal as a connector becomes large, and the dynamic friction coefficient increases. -1 If the surface unevenness exceeds this value, the mating terminal will be dug up because the surface irregularities will be too steep.
[0068] If the standard deviation / average value of Spc exceeds 30%, the dynamic friction coefficient will fluctuate locally and become unstable. Spc is 20mm -1 More than 60mm -1 More preferably, the standard deviation / average value of Spc is 25% or less.
[0069] A method for producing the film-coated copper terminal material 11 thus constructed will be described. This film-coated copper terminal material 11 is formed by sequentially applying copper plating made of copper or a copper alloy and tin plating made of tin or a tin alloy to a base material 2 to form a plating material 19 having a copper plating layer 17 and a tin plating layer 18 laminated on the base material 2 as shown in FIG. 4, and then heating and performing a reflow treatment.
[0070] As the substrate 2, a plate made of copper or a copper alloy is prepared, and the surface of this plate is cleaned by degreasing, pickling, and other treatments.
[0071] Copper plating can be performed using a general copper plating bath, for example, a copper sulfate bath mainly composed of copper sulfate (CuSO4) and sulfuric acid (H2SO4). The plating bath temperature is 20 to 50°C, and the current density is 1 to 50 A / dm 2 The thickness of the copper plating layer 21 formed by this Cu plating is set to be 0.05 μm or more and 0.50 μm or less.
[0072] As a plating bath for tin plating, a general tin plating bath may be used, for example, a sulfuric acid bath mainly composed of sulfuric acid (H2SO4) and stannous sulfate (SnSO4). The temperature of the plating bath is 15 to 35°C, and the current density is 1 to 30 A / dm 2 The thickness of the tin plating layer 18 is set to be 0.2 μm or more and 3.0 μm or less.
[0073] If the thickness of the tin plating layer 18 is less than 0.2 μm or exceeds 3.0 μm, the average thickness of the tin layer 14 after the reflow treatment will be less than 0.2 μm or exceed 2.0 μm, and the desired tin layer 14 will not be obtained.
[0074] By carrying out these plating processes, a plated material 19 is formed in which a copper plating layer 17 and a tin plating layer 18 are laminated in this order on the base material 2.
[0075] In the reflow treatment, the plated material 19 is heated to melt the copper plating layer 17 and the tin plating layer 18 once, and then rapidly cooled. Specifically, the reflow treatment includes a heating step in which the plated material 19 is heated to a temperature of 240° C. to 300° C. at a heating rate of 20° C. / sec to 75° C. / sec in a heating furnace in a CO reducing atmosphere, a primary cooling step in which the plated material is passed through a cooling furnace having an internal temperature of 20° C. to 70° C. so that the material reaches a temperature of 150° C. to 220° C. after the primary cooling step, and a secondary cooling step in which the plated material is cooled at a cooling rate of 100° C. / sec to 300° C. / sec after the primary cooling step.
[0076] In this case, in the primary cooling process, cooling air is blown to the surface of the plating material 19 at a speed of 10 m 3 / min more than 300m 3 The temperature of the cooling air is preferably 30°C or higher and 60°C or lower.
[0077] By carrying out the heating process in a reducing atmosphere, the formation of a tin oxide film with a high melting temperature on the surface of the tin plating layer 18 is prevented, and the reflow process can be carried out at a lower temperature and in a shorter time, making it easier to produce the desired copper-tin alloy structure.
[0078] If the heating rate in the heating step is less than 20° C. / sec, copper atoms will preferentially diffuse through the grain boundaries of the tin before the tin melts, causing abnormal growth of copper-tin intermetallic compounds near the grain boundaries, making it impossible to obtain the desired copper-tin alloy layer 13. On the other hand, if the heating rate exceeds 75° C. / sec, growth of the copper-tin intermetallic compounds will be insufficient, making it impossible to obtain the desired copper-tin alloy layer.
[0079] If the peak temperature in the heating step is less than 240° C., the tin does not melt uniformly, and if the peak temperature exceeds 300° C., the copper-tin intermetallic compound grows rapidly and the unevenness of the copper-tin alloy layer 13 becomes large, which is undesirable.
[0080] In the primary cooling process, a predetermined cooling air is blown onto the surface of the plated material 19 in a cooling furnace at a predetermined furnace temperature, thereby appropriately controlling the surface shape at a temperature below the melting point of tin. -1 More than 70mm -1 Hereinafter, the standard deviation / average value of Spc when measuring 10 visual fields can be kept below 30%.
[0081] In this case, if the temperature inside the cooling furnace is less than 20°C, the cooling rate is too fast, and the Spc and CV values (standard deviation / average value) of Spc become excessively large. -1 In the following, the CV value (standard deviation / average value) of Spc cannot be set below 30%. If the temperature inside the furnace exceeds 70°C, the cooling time to reach a temperature below the melting point of tin is too long, and the CV value (standard deviation / average value) of Spc becomes excessively large.
[0082] If the material temperature of the plating material 19 in the primary cooling process is less than 150°C, the cooling time is too long, and the CV value (standard deviation / average value) of Spc becomes excessively large. If the temperature of the plating material 19 in the primary cooling process does not drop to 220°C or less, the tin will be in a semi-molten state during secondary cooling, and the CV value (standard deviation / average value) of Spc will become excessively large. The material temperature of the plating material 19 in the primary cooling process is preferably 160°C or more and 210°C or less, and more preferably 170°C or more and 200°C or less.
[0083] The volume of cooling air in the primary cooling process is 10 m 3 At less than 10 mm / min, cooling is insufficient and Spc becomes too small. -1 On the other hand, the cooling air volume cannot be more than 300 m 3 If the speed exceeds 1 / min, the molten tin will flow due to the large amount of air hitting it, and the Spc and CV values of Spc (standard deviation / average value) will become excessively large.
[0084] The cooling air is blown perpendicularly to the plated material 19 from a height of about 10 cm above the surface of the plated material 19 .
[0085] Next, in the secondary cooling step, the plated material 19 is quenched to complete the desired surface shape. If the cooling rate in this secondary cooling step is less than 100°C / sec, the copper-tin intermetallic compound grows excessively, and the desired copper-tin alloy layer cannot be obtained. It is difficult to achieve a cooling rate of more than 300°C / sec.
[0086] The coating 12 of the plated copper terminal material 11 manufactured in this manner has a composite structure formed by the uneven interface between the copper-tin alloy layer 13 and the tin layer 14, and the relatively soft tin layer 14 is supported by the hard copper-tin alloy layer 13. The arithmetic mean curvature Spc of the peaks on the surface of the coating 12 is 10 mm. -1 More than 70mm -1 Since the coefficient of dynamic friction is less than or equal to 100 kPa, the coefficient of dynamic friction can be reduced.
[0087] Furthermore, by setting the standard deviation / average value of Spc when measuring in 10 visual fields to 30% or less, the dynamic friction coefficient is stabilized and local fluctuations are also suppressed.
[0088] Therefore, by using the film-coated copper terminal material 11 as a terminal material for a connector, the insertion and withdrawal force can be stably reduced, and adhesion with the mating terminal can be prevented.
[0089] Third embodiment 5, the coating-coated copper terminal material 21 of the third embodiment has a coating 22 having a nickel layer 23 made of nickel or a nickel alloy on the side in contact with the substrate 2, and a tin layer 24 made of tin or a tin alloy laminated on the nickel layer 23. In other words, the coating 22 has the nickel layer 23 below the tin layer 24.
[0090] By providing the nickel layer 23, it is possible to prevent copper from the base material 2 from diffusing into the coating 22, thereby improving the heat resistance.
[0091] The average thickness of the nickel layer 23 is set to 0.05 μm or more and 1.0 μm or less. If it is less than 0.05 μm, the effect of preventing copper diffusion from the base material 2 is reduced, and if it exceeds 1.0 μm, bending and other processes may become difficult.
[0092] On the surface of the tin layer 24, the arithmetic mean curvature Spc of the peak is 10 mm -1 More than 70mm -1 or less, and the standard deviation / average value of Spc when measuring 10 visual fields is 30% or less, which is the same as in the first embodiment.
[0093] The Spc on the surface of the tin layer 24 is 20 mm -1 More than 60mm -1 More preferably, the standard deviation / average value of Spc is 25% or less.
[0094] The film-coated copper terminal material 21 thus constructed is formed by sequentially applying nickel plating made of nickel or a nickel alloy and tin plating made of tin or a tin alloy onto the base material 2 to form a plating material 27 in which a nickel plating layer 25 and a tin plating layer 26 are laminated on the base material 2 as shown in FIG. 6, and then subjecting the resulting material to a reflow treatment.
[0095] A typical nickel plating bath may be used for nickel plating to form the nickel plating layer 25. For example, a sulfuric acid bath containing sulfuric acid (H2SO4) and nickel sulfate (NiSO4) as main components may be used. The temperature of the plating bath is 20°C or higher and 60°C or lower, and the current density is 5 to 60 A / dm 2 The thickness of the nickel plating layer 25 is set to be 0.05 μm or more and 1.0 μm or less.
[0096] The conditions for the tin plating and the reflow treatment are the same as those described in the first embodiment.
[0097] The film-coated copper terminal material 21 thus manufactured has the nickel layer 23, which prevents copper from diffusing and improves heat resistance.
[0098] (Fourth embodiment) 7, in the film-coated copper terminal material 31 of the fourth embodiment, the film 32 has a nickel layer 33 made of nickel or a nickel alloy in contact with the substrate 2, a copper-tin alloy layer 34 made of an alloy of copper and tin laminated on the nickel layer 33, and a tin layer 35 made of tin or a tin alloy laminated on the copper-tin alloy layer 34. In other words, the film 32 has a tin layer 35 on the surface, a copper-tin alloy layer 34 below the tin layer 35, and a nickel layer 33 in contact with the substrate 2 below the copper-tin alloy layer 34.
[0099] By providing the nickel layer 33, it is possible to prevent copper from the base material 2 from diffusing into the coating 32, thereby improving the heat resistance.
[0100] The average thickness of the nickel layer 33 is set to 0.05 μm or more and 1.0 μm or less. If it is less than 0.05 μm, the effect of preventing copper diffusion from the base material 2 decreases, and if it exceeds 1.0 μm, bending and other processes may become difficult.
[0101] The copper-tin alloy layer 34 is composed of a Cu3Sn alloy layer 36 partially formed on the substrate 2 side and a Cu6Sn5 alloy layer 37 formed so as to cover the Cu3Sn alloy layer 36. Therefore, the Cu6Sn5 alloy layer 37 is formed so as to cover both the Cu3Sn alloy layer 36 on the nickel layer 33 and the nickel layer 33 where the Cu3Sn alloy layer 36 is not present.
[0102] The copper-tin alloy layer 34 preferably has an average thickness of 0.2 μm to 2.5 μm and an average crystal grain size of 0.2 μm to 1.5 μm. The tin layer 35 has an average thickness of 0.2 μm to 2.0 μm.
[0103] As in the first embodiment, the arithmetic mean curvature Spc of the peaks on the surface of the tin layer 35 is 10 mm -1 More than 70mm -1 The standard deviation / average value of Spc when measuring 10 visual fields is 30% or less, which is the same as in the first embodiment. -1 More than 60mm -1It is more preferable that the standard deviation / average value of Spc is 25% or less.
[0104] The film-coated copper terminal material 31 thus constructed is formed by sequentially applying nickel plating made of nickel or a nickel alloy, copper plating made of copper or a copper alloy, and tin plating made of tin or a tin alloy to the base material 2, to form a plating material 44 having a nickel plating layer 41, a copper plating layer 42, and a tin plating layer 43 laminated on the base material 2 as shown in FIG. 8, and then performing a reflow treatment.
[0105] The conditions for nickel plating, copper plating, and tin plating are the same as those described in the first to third embodiments.
[0106] The plating material 44 having the nickel plating layer 41, the copper plating layer 42, and the tin plating layer 43 formed thereon is subjected to a reflow treatment to form the film-coated copper terminal material 31. This reflow treatment is similar to that in the second embodiment, and therefore a description thereof will be omitted.
[0107] The thus-manufactured coated copper terminal material 31 has a nickel layer 33 below the coating 32, which prevents copper diffusion and improves heat resistance. In addition, the copper-tin alloy layer 34 and the tin layer 35 have an uneven interface, the copper-tin alloy layer 34 supports the tin layer 35, and the arithmetic mean curvature of the peaks on the surface and the CV value when measuring 10 fields of view are within a predetermined range, so that the dynamic friction coefficient is uniformly low and stable. EXAMPLES
[0108] A copper alloy plate having a thickness of 0.25 mm was used as the substrate, and various plating processes were carried out under the following plating bath conditions.
[0109] (nickel plating) Nickel sulfate: 300g / L Sulfuric acid: 2g / L Liquid temperature: 45℃ Current density: 20ASD(A / dm 2 )
[0110] (Copper plating) Copper sulfate: 250g / L Sulfuric acid: 50g / L Liquid temperature: 25℃ Current density: 5ASD
[0111] (Tin plating) Tin sulfate: 75g / L Sulfuric acid: 85g / L Additive: 10g / L Liquid temperature: 25℃ Current density: 2ASD
[0112] Of these platings, plated materials in which a tin plating layer was formed on the base material (Examples 1, 5, 9; Comparative Examples 1, 5), plated materials in which a copper plating layer and a tin plating layer were formed in that order on the base material (Examples 2, 6, 10; Comparative Examples 2, 6), plated materials in which a nickel plating layer and a tin plating layer were formed in that order on the base material (Examples 3, 7, 11; Comparative Example 3), and plated materials in which a nickel plating layer, a copper plating layer, and a tin plating layer were formed in that order on the base material (Examples 4, 8, 12; Comparative Examples 4, 7) were each produced and subjected to a reflow treatment under the conditions shown in Table 1.
[0113] [Table 1]
[0114] The average thickness of the tin layer on the surface, the arithmetic mean curvature Spc of the peaks, and the dynamic friction coefficient were measured for the obtained samples, and the stability was evaluated.
[0115] [Average thickness of tin layer] The average thickness of the tin layer was measured using a fluorescent X-ray film thickness meter (SEA5120A) manufactured by SII NanoTechnology Inc.
[0116] For samples having a copper-tin alloy layer, the thickness of the total tin-containing layer containing tin of the sample after reflow treatment was first measured, and then the tin layer was removed to expose the copper-tin alloy layer underneath, and the thickness of the copper-tin alloy layer was measured. The thickness of the tin layer was defined as (thickness of the total tin-containing layer containing tin - thickness of the copper-tin alloy layer). The thickness of the total tin-containing layer containing tin includes the copper-tin alloy layer portion and the tin layer portion, but since the tin solidified matter has irregularities, it is calculated as the average thickness. The tin layer was removed by immersing the sample for 5 minutes in an etching solution for removing the plating film, which is made of a component that does not corrode the copper-tin alloy layer.
[0117] [Arithmetic mean curvature of peak Spc] Ten fields of view were observed using a laser microscope (Keyence Corporation VKX-1100, objective lens ×10), and Spc was measured over the entire field of view in accordance with ISO25178, and the CV value of Spc (standard deviation / average value) was calculated.
[0118] [Kinematic friction coefficient and stability] To simulate the contact area between the male and female terminals of a mating connector, a hemispherical female test piece with an inner diameter of 1.5 mm and a plate-shaped male test piece were prepared for each sample. Using a friction measuring machine (horizontal load tester, model M-2152ENR) manufactured by Aiko Engineering Co., Ltd., a load of 100 gf to 500 gf was applied between the female and male test pieces, and the male test piece was pulled 10 mm horizontally at a sliding speed of 80 mm / min to measure the friction force, thereby determining the dynamic friction coefficient.
[0119] The dynamic friction coefficient increases as the tin layer becomes thicker, since it is less susceptible to the influence of the hard substrate, nickel layer, and copper-tin alloy layer underneath, and the influence of the soft tin layer becomes greater. Test pieces with a dynamic friction coefficient of 0.3 or less when the average thickness of the tin layer was less than 1.0 μm, 0.4 or less when the average thickness of the tin layer was between 1.0 μm and 1.5 μm, and 0.45 or less when the average thickness of the tin layer was 1.5 μm or more were classified as passing (A), and test pieces with a dynamic friction coefficient exceeding these values were classified as failing (B).
[0120] The average value of 30 measurements was calculated using the above method, and test pieces with 30 measured values within the range of the average value ±25% were rated as stability "A," and test pieces with measured values of ±25% or more were rated as stability "B."
[0121] [Contact resistance value] To evaluate electrical reliability, the samples were heated in air at 150°C for 500 hours and the contact resistance was measured. The measurement method was in accordance with JIS-C-5402, and a four-terminal contact resistance tester (Yamazaki Seiki Kenkyusho: CRS-113-AU) was used to measure the contact resistance as a function of load change from 0 to 50g using a sliding type (1mm), and the contact resistance was evaluated at a load of 50g.
[0122] The results are shown in Table 2.
[0123] [Table 2]
[0124] As is clear from Tables 1 and 2, all of the Examples had small dynamic friction coefficients depending on the average thickness of the tin layer, and showed good stability of the dynamic friction coefficient. For example, in Example 8, the tin layer was a little thick at 1.2 μm, and was less susceptible to the influence of the hard substrate, nickel layer, and copper-tin alloy layer underneath, but was more susceptible to the influence of the soft tin layer, but the dynamic friction coefficient was 0.37, showing good stability.
[0125] In contrast, the following problems were observed in each of the comparative examples. In comparative example 1, the temperature inside the cooling furnace exceeded 70°C, so the CV value of Spc was excessively large, and the stability of the dynamic friction coefficient was poor. In comparative example 2, the cooling air volume in the primary cooling was too weak, so Spc was too small, the real contact area between the platings became large, and the dynamic friction coefficient was poor compared to the thickness of the tin layer, and the stability was poor. In comparative example 3, the cooling air volume in the primary cooling was too strong, so Spc was excessively large, and piercing occurred due to the unevenness of the surface during the insertion / extraction test, so the dynamic friction coefficient became excessive, and the CV value of Spc was excessive, and the stability of the dynamic friction coefficient was poor.
[0126] In Comparative Example 4, the temperature inside the cooling furnace is less than 20°C, so Spc and CV values of Spc are excessively large, and the dynamic friction coefficient is excessively large and its stability is poor. In Comparative Example 5, the material end temperature is less than 150°C, so the CV value of Spc is excessively large and the stability of the dynamic friction coefficient is poor. In Comparative Example 6, the material end temperature exceeds 220°C, so the CV value of Spc is excessively large and the stability of the dynamic friction coefficient is poor. In Comparative Example 7, the cooling air volume of the primary cooling is too strong, so Spc and CV values of Spc are excessively large, and the dynamic friction coefficient is excessively large and its stability is poor.
[0127] In Comparative Example 8, the tin plating layer was too thin, resulting in a thin tin layer and a poor contact resistance value, whereas in Comparative Example 9, the tin plating layer was too thick, resulting in a thick tin layer and a poor dynamic friction coefficient. [Explanation of symbols]
[0128] 1. Coated copper terminal material 2 Base material 3 tin layer 5. Coating 4 Tin plating layer 7 Plating materials 11 Coated copper terminal material 12. Membrane 13 Copper-tin alloy layer 14 Tin layer 15 Cu3Sn alloy layer 16 Cu6Sn5 alloy layer 17 Copper plating layer 18 Tin plating layer 19 Plating materials 21 Coated copper terminal material 22 Membrane 23 Nickel layer 24 Tin layer 25 Nickel plating layer 26 Tin plating layer 27 Plating materials 31 Coated copper terminal material 32 Membrane 33 Nickel layer 34 Copper-tin alloy layer 35 Tin layer 36 Cu3Sn alloy layer 37 Cu6Sn5 alloy layer 41 Nickel plating layer 42 Copper plating layer 43 Tin plating layer 44 Plating materials
Claims
1. A film-coated copper terminal material having a substrate made of copper or a copper alloy and a coating formed on the substrate, The coating has a tin layer made of tin or a tin alloy and having an average thickness of 0.2 μm or more and 2.0 μm or less on a surface thereof, The arithmetic mean curvature Spc of the peaks on the surface of the coating is 10 mm -1 More than 70 mm -1 The coated copper terminal material is characterized in that the standard deviation / average value of Spc when measured in 10 visual fields is 30% or less.
2. The film-coated copper terminal material according to claim 1, The coating has a copper-tin alloy layer made of an alloy of copper and tin under the tin layer. A coated copper terminal material characterized by the above.
3. The film-coated copper terminal material according to claim 1 or 2, The coating has a nickel layer made of nickel or a nickel alloy in contact with the substrate. A coated copper terminal material characterized by the above.
4. A method for producing a coated copper terminal material having a coating formed on a substrate made of copper or a copper alloy, comprising: The method includes a plating step of forming a plated material by forming a plating layer having a surface made of tin or a tin alloy on the base material, and a reflow step of heating the plated material to perform a reflow treatment, The thickness of the tin plating layer in the plating step is 0.2 μm or more and 3.0 μm or less, The reflow treatment includes a heating step of heating the plated material to a peak temperature of 240° C. or more and 300° C. or less, a primary cooling step of passing the plated material through a cooling furnace having an internal temperature of 20° C. or more and 70° C. or less to reduce the material temperature of the plated material to 150° C. or more and 220° C. or less, and a secondary cooling step of cooling the plated material at a cooling rate of 100° C. / sec. or more and 300° C. / sec. or less after the primary cooling step, In the primary cooling step, cooling air is blown onto the surface of the plated material at a speed of 10 m 3 / min or more 300m 3 Spray at a rate of less than 1 / min. A method for producing a film-coated copper terminal material, comprising the steps of:
5. A method for producing the film-coated copper terminal material according to claim 4, The method for producing a film-coated copper terminal material, wherein in the plating step, a copper plating layer made of copper or a copper alloy is formed under the tin plating layer.
6. A method for producing the film-coated copper terminal material according to claim 5, The heating rate of the plated material in the heating step is 20° C. / sec or more and 75° C. / sec or less. A method for producing a film-coated copper terminal material, comprising the steps of:
7. A method for producing the film-coated copper terminal material according to claim 4, The method for producing a film-coated copper terminal material, wherein the plating step comprises forming a nickel plating layer made of nickel or a nickel alloy in contact with the surface of the base material.
8. A method for producing the film-coated copper terminal material according to claim 6, The method for producing a film-coated copper terminal material, wherein the plating step comprises forming a nickel plating layer made of nickel or a nickel alloy in contact with the surface of the base material.
Citation Information
Patent Citations
Electrically conductive material for connecting parts and production method therefor
JP2006077307A
Plating material and electrical and electronic component using the plating material
JP2007247060A
Sn PLATED MATERIAL AND PRODUCTION METHOD THEREOF
JP2015180770A
Cited By
Copper terminal material with plating film and method for manufacturing same
WO2025197299A1