Polymer, electrolyte material, electrolyte membrane, electrolyte membrane with catalyst layer, membrane electrode assembly, solid polymer fuel cell and solid polymer water electrolysis device
A polymer with a structured ion exchange and arylene group arrangement addresses the conductivity and durability issues of non-fluorine-based electrolytes, offering high proton conductivity and chemical stability.
Patent Information
- Application Number
- JP2023055178
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Non-fluorine-based polymers used in electrolytes for polymer electrolyte fuel cells lack sufficient proton conductivity and chemical durability.
A polymer with a specific structural formula comprising ion exchange groups and arylene groups, linked by sulfone or sulfonyl groups, forming a microphase-separated structure for enhanced proton conductivity and chemical durability.
The polymer exhibits high proton conductivity and excellent chemical durability, particularly in humid environments, with improved gas barrier properties and mechanical stability.
Smart Images

Figure 2024142829000001 
Figure 2024142829000002 
Figure 2024142829000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer, an electrolyte material, an electrolyte membrane, an electrolyte membrane with a catalyst layer, a membrane electrode assembly, a solid polymer fuel cell, and a solid polymer water electrolysis device. [Background technology]
[0002] In recent years, fuel cells have been in the spotlight as a new, highly energy-efficient energy technology against the backdrop of environmental issues. Among them, solid polymer electrolyte fuel cells, which use polymer materials as electrolytes, have attracted particular attention because they have a high maximum current density and can operate at low temperatures, making them suitable for use as a mobile power source for automobiles and other vehicles, as well as small-capacity power sources for portable electronic devices.
[0003] Fluorine-based polymers are known as polymers (electrolyte polymers) used as electrolytes in polymer electrolyte fuel cells (see, for example, Patent Document 1). Fluorine-based polymers are widely used in electrolyte applications due to their high proton conductivity and excellent chemical durability, but they have problems such as high cost and a large environmental impact.
[0004] For these reasons, development of electrolyte polymers that do not use fluorine is also underway. For example, Patent Document 2 discloses an invention relating to a polymer electrolyte membrane made of a block copolymer containing one or more segments (A1) containing an ionic group and one or more segments (A2) not containing an ionic group. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-204119 [Patent Document 2] International Publication No. 2013-031675 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the non-fluorinated polymer obtained by block copolymerization as disclosed in the above Patent Document 2 does not necessarily have sufficient proton conductivity and is also insufficient in chemical durability.
[0007] An object of one aspect of the present invention is to provide a polymer that has sufficient proton conductivity as an electrolyte and is also excellent in chemical durability. [Means for solving the problem]
[0008] In some aspects, the present invention provides the following [1] to
[11] .
[0009] [1] A polymer having a structure represented by the following formula (1): [ka] [In formula (1), A 1 represents a structural unit represented by the following formula (a1): A 2 represents a structural unit represented by the following formula (a2): L 1 and L 2 each independently represents a single bond or -SO 2 - indicates n is a number between 10 and 100. * indicates a bond. Multiple A's 1 are identical to each other, Multiple A's 2 are identical to each other, Multiple L's 1 may be the same or different, Multiple L's 2 may be the same or different. [ka] [In formula (a1), IExG represents an ion exchange group, L 3 is a single bond or -SO 2 - indicates x represents an integer from 1 to 10; * indicates a bond. The multiple IExGs may be identical to or different from each other, Multiple L's 3 may be the same or different. [ka] [In formula (a2), Ar represents an arylene group having no ion exchange group; L 4 is a single bond or -SO 2 - indicates y represents an integer from 2 to 20; * indicates a bond. A plurality of Ar may be the same or different, Multiple L's 4 may be the same or different.
[0010] [2] The polymer according to [1], wherein the constitutional unit represented by the formula (a1) contains, as the ion exchange group, at least one selected from the group consisting of a sulfone group, an alkylsulfone group, and a sulfonimide group.
[0011] [3] The polymer according to [1] or [2], wherein the constitutional unit represented by the formula (a2) contains, as the arylene group, at least one selected from the group consisting of a phenylene group, a naphthylene group, and a fluorene group.
[0012] [4] The polymer according to any one of [1] to [3], having a number average molecular weight of 20,000 to 300,000.
[0013] [5] An oxide of a polymer having a sulfide group, The polymer is a polymer of a compound represented by the following formula (b1) and a compound represented by the following formula (b2): [ka] [In formula (b1), IExG represents an ion exchange group, L 5 is a single bond, -S- or -SO 2 - indicates X 1b and X 2b each independently represents a halogen atom, x represents an integer of 1 to 10. The multiple IExGs may be identical to or different from each other, Multiple L's 5 may be the same or different. [ka] [In formula (b2), Ar represents an arylene group having no ion exchange group; L 6 is a single bond, -S- or -SO 2 - indicates Z 1b and Z 2b each independently represents a thiol group, a halogen atom, a boronic acid group, an alkylborane group, or a boronic acid ester group, and y represents an integer of 2 to 20. A plurality of Ar may be the same or different, Multiple L's 6 may be the same or different.
[0014] [6] An electrolyte material comprising the polymer according to any one of [1] to [5].
[0015] [7] An electrolyte membrane comprising the polymer according to any one of [1] to [5].
[0016] [8] [7] A catalyst layer-attached electrolyte membrane comprising: the electrolyte membrane according to [7]; and a catalyst layer disposed on one or both sides of the electrolyte membrane.
[0017] [9] [7] A membrane electrode assembly comprising the electrolyte membrane according to [7] and an electrode layer disposed on one or both sides of the electrolyte membrane.
[0018]
[10] A polymer electrolyte fuel cell comprising the membrane electrode assembly according to [9].
[0019]
[11] A solid polymer water electrolysis apparatus comprising the membrane electrode assembly according to [9]. Effect of the Invention
[0020] According to one aspect of the present invention, it is possible to provide a polymer that has sufficient proton conductivity as an electrolyte and is excellent in chemical durability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, exemplary embodiments of the present invention will be described. However, the present invention is not limited to the following embodiments. In this specification, a numerical range indicated using "~" indicates a range including the numerical values before and after "~" as the minimum and maximum values, respectively. In addition, unless specifically stated otherwise, the units of the numerical values before and after "~" are the same. In addition, the upper limit value and the lower limit value described individually can be arbitrarily combined.
[0022] <Polymer> The polymer of one embodiment (hereinafter also referred to as "polymer (P-1)") has a structure represented by the following formula (1).
[0023] [ka]
[0024] In formula (1), A 1 is a structural unit represented by the following formula (a1) (hereinafter, “structural unit A 1 ") and A 2 is a structural unit represented by the following formula (a2) (hereinafter, “structural unit A 2 ") and L 1 and L 2 each independently represents a single bond or -SO 2 -, n is a number from 10 to 100, and * is a bond. 1 are identical to each other, and multiple A 2 are identical to each other, and multiple L 1 may be the same or different, and multiple L 2 may be the same or different from each other.
[0025] [ka]
[0026] In formula (a1), IExG represents an ion exchange group, L 3 is a single bond or -SO 2 -, x represents an integer of 1 to 10, and * represents a bond. A plurality of IExG may be the same or different, and a plurality of L 3 may be the same or different from each other.
[0027] [ka]
[0028] In formula (a2), Ar represents an arylene group having no ion exchange group, L 4 is a single bond or -SO 2 -, y represents an integer of 2 to 20, and * represents a bond. A plurality of Ar may be the same or different, and a plurality of L 4 may be the same or different from each other.
[0029] The polymer of another embodiment (hereinafter also referred to as "polymer (P-2)") is an oxide of a polymer having a sulfide group (-S-), and the polymer is a polymer of a compound represented by the following formula (b1) (hereinafter also referred to as "compound (b1)") and a compound represented by the following formula (b2) (hereinafter also referred to as "compound (b2)").
[0030] [ka]
[0031] In formula (b1), A 1b IExG and x are as defined above, and L 5 is a single bond, -S- or -SO 2 - indicates X 1b and X 2b Each independently represents a halogen atom. Examples of halogen atoms include a fluorine atom (F), a chlorine atom (Cl), a bromine atom (Br) and an iodine atom (I). Multiple IExG may be the same or different, and multiple L 5 may be the same or different from each other.
[0032] [ka]
[0033] In formula (b2), Ar and y are as defined above; L 6 is a single bond, -S- or -SO 2 - indicates Z 1b and Z 2bEach of the Ar independently represents a thiol group, a halogen atom, a boronic acid group, an alkylborane group, or a boronic acid ester group. Examples of halogen atoms include a fluorine atom (F), a chlorine atom (Cl), a bromine atom (Br), and an iodine atom (I). Examples of alkylborane groups include a diethylborane group, a disiamylborane group, a dicyclohexylborane group, and a 9-borabicyclo[3.3.1]nonane group. Examples of boronic acid ester groups include a pinacol boronic acid ester group, a 1,3-propanediol boronic acid ester group, a biscyclohexyldiol boronic acid ester group, a neopentyl glycol boronic acid ester group, and a catechol boronic acid ester group. A plurality of Ar may be the same or different from each other, and a plurality of L 6 may be the same or different from each other.
[0034] Compound (b1) and compound (b2) can also be represented by the following formulas (b1-1) and (b2-1), respectively.
[0035] [ka]
[0036] [ka]
[0037] A in formula (b1-1) 1b represents a structural unit represented by the following formula (b1-2), and A in formula (b2-1) 2b represents a structural unit represented by the following formula (b2-2): In addition, in formulas (b1-2) and (b2-2), * represents a bond.
[0038] [ka]
[0039] [ka]
[0040] Polymer (P-1) and polymer (P-2) (hereinafter sometimes collectively referred to as "polymer (P)") are so-called electrolyte polymers, and have sufficient proton conductivity as an electrolyte. Therefore, a membrane (polymer electrolyte membrane) formed from polymer (P) exhibits sufficiently high proton conductivity. The reason why polymer (P) has sufficiently high proton conductivity is not clear, but it is thought that polymer (P) has a sufficiently high proton conductivity when it contains a plurality of identical hydrophilic structural units (for example, A in formula (1)). 1 Or, A in formula (b1) 1b A structural unit derived from the compound (A) and a plurality of identical hydrophobic structural units (e.g., A 2 Or, A in formula (b2) 2b Since the hydrophilic structural units (structural units derived from ethylene glycol) are precisely arranged, the ion exchange groups are arranged at equal intervals, and it is presumed that the ion exchange groups self-accumulate in a higher-order structure to induce a microphase-separated structure, which in turn forms a good proton-conducting path within the polymer. In addition, it is presumed that the presence of two or more ion exchange groups densely packed in the hydrophilic structural units also contributes to the improvement of phase separation and proton conductivity. The above effect is particularly remarkable in a high-humidity environment (for example, at a humidity of 80% RH or higher).
[0041] The polymer (P) also has excellent chemical durability. The reason for this is unclear, but it is believed that the linking groups between the benzene rings (for example, L 1 and L 2 , L in formula (a1) 3 , L in formula (a2) 4 ) are all or most of single bonds or -SO 2 This is presumably because the linking group is difficult to cleave.
[0042] The polymer (P) also tends to have excellent gas barrier properties when made into a film. The reason for this is presumed to be as follows: Since the polymer (P) has a main chain composed of an arylene group containing a benzene ring, the solubility of hydrogen and oxygen is low, and the segment motion is restricted, suppressing gas diffusion in the film, which is thought to result in excellent gas barrier properties when made into a film.
[0043] (Polymer (P-1)) As represented by formula (1), the polymer (P-1) comprises a structural unit A 1 and structural unit A 2 and the linking group (L 1 Or L 2 The repeating number (n) of the structure is 10 to 100, and may be 15 or more or 20 or more, and may be 80 or less or 50 or less. When the repeating number (n) is 15 or more, the gas barrier property tends to be excellent, and when the repeating number (n) is 50 or less, the solubility in a solvent and the film-forming property tend to be excellent.
[0044] [Structural unit A 1 ] Building block A 1 The aromatic ring having an ion exchange group (IExG) is connected to a linking group (L 3 ) and has a continuous structure.
[0045] Ion exchange groups, also called ionic groups, have the property of being able to exchange ions with other ions by releasing ions (e.g., cations). Examples of ion exchange groups include sulfone groups, alkylsulfone groups, perfluoroalkylsulfone groups, sulfonimide groups, phosphonic acid groups, phosphoric acid groups, and carboxy groups. These ion exchange groups also include those that are in the form of salts. For example, a "sulfone group" is -SO 3 M 1 / q(M represents a metal such as H or Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Ti, Al, Fe, Pt, Rh, Ru, Ir, or Pd, and q represents the valence of M (e.g., an integer of 1 to 4). The metal represented by M exists as an ion (cation) and is represented by -SO 3 - and forms salt.
[0046] An alkylsulfone group is, for example, -R 1 SO 3 M 1 / q It is expressed as R 1 R is an alkanediyl group, the number of carbon atoms of which is preferably 1 to 12. 1 Specific examples of include a methylene group, a butane-1,4-diyl group, a hexane-1,6-diyl group, etc. M and q are as defined above.
[0047] The sulfonimide group is, for example, -SO 2 NM 1 / q SO 2 R 2 It is expressed as R 2 R is an alkyl group, the number of carbon atoms of which is preferably 1 to 6. 2 Specific examples of include a methyl group, an ethyl group, a propyl group, etc. M and q are as defined above.
[0048] Building block A 1 From the viewpoint of obtaining better proton conductivity, the structural unit A preferably contains, as an ion exchange group, at least one group selected from the group consisting of a sulfone group, an alkylsulfone group, and a sulfonimide group, and more preferably contains a sulfone group. 1 It is more preferable that the majority of the ion exchange groups present in the structural unit A are those of the above-mentioned preferred embodiment. 1 It is particularly preferred that all of the ion exchange groups present therein are of the above-mentioned preferred embodiment.
[0049] Building block A 1 From the viewpoint of obtaining better proton conductivity, 3) as -SO 2 From the same viewpoint, it is preferable that the structural unit A 1 There are multiple linking groups (L 3 It is further preferred that the majority of the above-mentioned preferred embodiments.
[0050] Linking group (L 3 The bonding position of the structural unit A is not particularly limited, but is preferably the ortho or meta position relative to the ion exchange group, and more preferably the ortho position. 1 It is preferable that the linking group (L 3 ) is -SO 2 When the ratio is -, the elimination of the ion exchange group is easily suppressed, and further excellent chemical durability tends to be obtained.
[0051] Building block A 1 The repeat number (x) of the structure in [ ] in formula (a1) in the above formula is preferably 2 to 8, and more preferably 3 to 5, from the viewpoints of obtaining better proton conductivity and excellent hot water resistance.
[0052] Building block A 1 From the viewpoint of obtaining better proton conductivity, it is preferable that the polyimide compound contains at least one structure selected from the group consisting of a structure represented by the following formula (a1-1) (hereinafter referred to as "structure (a1-1)") and a structure represented by the following formula (a1-2) (hereinafter referred to as "structure (a1-2)").
[0053] [ka]
[0054] [ka]
[0055] In formula (a1-1) and formula (a1-2), IExG and * are the same as defined above. Multiple IExG may be the same or different. x in formula (a1-1) 1 represents an integer of 2 to 10, and x in formula (a1-2) 2 represents an integer of 2 to 5. 1 If contains both structure (a1-1) and structure (a1-2), then x 1 and 2x 2 The sum of is 2 to 10. x 1 is preferably 2 to 5, and more preferably 2 to 3. 2 is preferably 2 to 3, and more preferably 2.
[0056] Building block A 1 may consist of only the structure (a1-1), or may contain the structure (a1-1) and a structure other than the structure (a1-1). In the latter case, the structure (a1-1) and the structure other than the structure (a1-1) are connected via a linking group (L 3 Similarly, the structural unit A may be linked by 1 may consist of only the structure (a1-2), or may contain the structure (a1-2) and a structure other than the structure (a1-2). In the latter case, the structure (a1-2) and the structure other than the structure (a1-2) are connected via a linking group (L 3 ) may be connected.
[0057] Building block A 1 Specific examples of the structural units include those represented by the following formulae (A1-1) to (A1-4).
[0058] [ka]
[0059] IExG and * in formulae (A1-1) to (A1-4), and L in formulae (A1-3) to (A1-4) 3 The multiple IExGs may be the same or different, and multiple L 3 may be the same or different from each other.
[0060] Structural unit A in polymer (P-1) 1 From the viewpoints of obtaining better proton conductivity and better chemical durability, it is preferably any one of the constitutional units represented by formulae (A1-1) to (A1-4), and more preferably a constitutional unit represented by formula (A1-2).
[0061] [Structural unit A 2 ] Building block A 2 is an arylene group (Ar) that does not have an ion exchange group and a linking group (L 4 ) and has a continuous structure.
[0062] The arylene group is a divalent aromatic hydrocarbon group, and has a structure in which two hydrogen atoms have been removed from an aromatic hydrocarbon. From the viewpoints of solubility in a solvent and film-forming properties, the number of aromatic rings in the arylene group is preferably 1 to 4, more preferably 1 to 2, and even more preferably 1. The arylene group may have a substituent other than an ion-exchange group, but preferably has no substituent.
[0063] Specific examples of the arylene group include a phenylene group, a naphthylene group, a fluorene group, an anthracylene group, a phenanthrylene group, a triphenylene group, a pyrenylene group, and a tetracenylene group.
[0064] Building block A 2 From the viewpoints of solubility in a solvent and film-forming properties, the structural unit A preferably contains, as an arylene group, at least one selected from the group consisting of a phenylene group, a naphthylene group, and a fluorene group, more preferably contains a phenylene group, and further preferably contains a 1,4-phenylene group. 2 It is more preferable that the majority of the arylene groups present in the structural unit A are those of the above-mentioned preferred embodiment. 2 It is particularly preferable that all of the arylene groups present in the copolymer are each independently a phenylene group, a naphthylene group or a fluorene group.
[0065] Building block A 2 From the viewpoints of excellent solubility in a solvent, excellent film-forming property, and excellent mechanical strength during film formation, 4 ) as -SO 2 From the same viewpoint, it is preferable that the structural unit A 2 There are multiple linking groups (L 4 It is more preferable that the majority of the structural units A 2 There are multiple linking groups (L 4 ) may all be of the preferred embodiments described above.
[0066] Building block A 2 The repeat number (y) of the structure in [ ] in formula (a2) in the above formula is preferably 4 to 12, and more preferably 5 to 10, from the viewpoints of obtaining better proton conductivity and excellent hot water resistance.
[0067] Building block A 2 In order to achieve both better proton conductivity and hot water resistance, the repeat number (y) of the structure in [ ] in formula (a2) in this case is preferably a number (x+(2 to 7)) larger by 2 to 7 than the repeat number (x) of the structure in [ ] in formula (a1).
[0068] Building block A 2 From the viewpoints of excellent solubility in a solvent, excellent film-forming ability, and excellent mechanical strength during film formation, it is preferable for the compound to contain a structure represented by the following formula (a2-1).
[0069] [ka]
[0070] In the formula (a2-1), Ar and * have the same meaning as defined above. A plurality of Ar may be the same or different.
[0071] Building block A 2 A specific example of the structural unit is the structural unit represented by the following formula (A2).
[0072] [ka]
[0073] Ar and L in formula (A2) 4 and * are as defined above, Q represents a group having a structure represented by formula (a2-1), y 1 and y 2 Each independently represents an integer of 2 to 4. 1 and y 2 is preferably 2 to 3. A plurality of Ar may be the same or different, and a plurality of L 4 may be the same or different from each other.
[0074] [Linking group] The polymer (P-1) is made of the structural unit A from the viewpoint of obtaining superior proton conductivity and superior chemical durability. 1 and building block A 2 The linking group (L 1 Or L 2 ) as -SO 2 From the same viewpoint, it is preferable that the polymer (P-1) contains a plurality of the structural units A 1 and building block A 2 The linking group (L 1 and L 2 It is more preferable that the majority of the structural units A) are those of the above-mentioned preferred embodiment, and 1 and building block A 2 The linking group (L 1 and L 2 It is particularly preferred that all of the above are of the preferred embodiments.
[0075] The polymer (P-1) may be composed of a structure represented by formula (1) and a terminal structure bonded to the structure. The polymer (P-1) may be, for example, a compound represented by the following formulae (1-1) to (1-3).
[0076] [ka]
[0077] A in formulas (1-1) to (1-3) 1 , A 2 , L 1 , L 2 and n are as defined above. However, in formula (1-1) and formula (1-2), Z 2 L binds to 2 is a single bond. Z 1 and Z 2 each independently represents a thiol group, a halogen atom, a boronic acid group, an alkylborane group, or a boronic acid ester group. Examples of the halogen atom, the alkylborane group, and the boronic acid ester group are the same as those described above in Z 1b and Z 2b These are the same as the examples of the halogen atom, alkylborane group and boronic acid ester group represented by the following formula:
[0078] The proportion of the structure represented by formula (1) in the entire polymer (P-1) is preferably 80% by mass or more from the viewpoint of obtaining better proton conductivity. From the same viewpoint, the proportion of the structure represented by formula (1) in the entire polymer (P-1) may be 85% by mass or more or 90% by mass or more. The proportion of the structure represented by formula (1) in the entire polymer (P-1) may be about 100% by mass (97% by mass or more and less than 100% by mass).
[0079] The polymer (P-1) may contain fluorine atoms, but the fluorine content in the polymer (P-1) is preferably 5 mass% or less, and it is preferable that the polymer (P-1) does not contain fluorine atoms (the fluorine content is below the detection limit).
[0080] The number average molecular weight of the polymer (P-1) may be 20,000 or more, 25,000 or more, or 30,000 or more from the viewpoint of excellent proton conductivity and excellent mechanical strength during film formation, and may be 300,000 or less, 200,000 or less, or 150,000 or less from the viewpoint of excellent solubility in a solvent and film formability. From these viewpoints, the number average molecular weight of the polymer (P-1) may be 20,000 to 300,000, 25,000 to 200,000, or 30,000 to 150,000. The number average molecular weight is a standard polyethylene glycol / oxide (PEG / PEO) equivalent value measured by gel permeation chromatography (GPC).
[0081] The polymer (P-1) can be obtained by oxidizing a polymer of the above compound (b1) and the above compound (b2). That is, the polymer (P-1) and the polymer (P-2) can be the same.
[0082] (Polymer (P-2)) The polymer (P-2) is an oxide of a polymer having a sulfide group (hereinafter, also referred to as "polymer (P-2')").
[0083] The polymer (P-2) has, for example, a structure represented by formula (1) (wherein the polymer does not contain a sulfonyl group (-SO 2 The polymer (P-2) preferably has a structure represented by the following formula (2):
[0084] [ka]
[0085] A in formula (2) 1 , A 2 , n and * are the same as defined above, and the preferred embodiments thereof are the same as those of the polymer (P-1). 1 are identical to each other, and multiple A 2 are identical to each other.
[0086] The polymer (P-2') is a polymer of the compound (b1) and the compound (b2), and has, for example, a structure represented by the following formula (2').
[0087] [ka]
[0088] A in formula (2') 1b The structural unit represented by formula (c1) is as described above, and L 3 Instead of L 5 The details (including preferred embodiments) of the compound are as follows: 1 It is the same as A in formula (2'). 2b The structural unit represented by formula (c2) is as described above, and L 4 Instead of L 6 The details (including preferred embodiments) of the compound are as follows: 2 It is the same as L in formula (2'). 1x and L 2x Each of A independently represents a single bond or -S-. In formula (2'), n and * are the same as defined above, and the preferred embodiments thereof are the same as those in the polymer (P-1). 1b are identical to each other, and multiple A 2b are identical to each other, and multiple L 1x may be the same or different, and multiple L 2x may be the same or different. However, A 1b and A 2b If does not contain -S-, multiple L 1x and multiple L 2x At least one of is -S-.
[0089] The method for oxidizing the polymer (P-2′) is not particularly limited, and may be, for example, by oxidizing a sulfide group (—S—) to a sulfonyl group (—SO 2The method may be a known method for obtaining a polymer (P-2') having a structure similar to that described above. An example of such a method is a method of immersing the polymer (P-2') in a mixed solution containing acetic acid, sulfuric acid, and hydrogen peroxide. The concentration of acetic acid in the mixed solution may be, for example, 50 to 90 mass %. The concentration of sulfuric acid in the mixed solution may be, for example, 5 to 25 mass %. The concentration of hydrogen peroxide in the mixed solution may be, for example, 1 to 15 mass %. The immersion time may be, for example, 1 to 100 hours. In the above method, heating may be performed after the immersion. The heating temperature may be, for example, 30 to 120°C, and the heating time may be, for example, 0.1 to 24 hours. According to these methods, the structural unit A in the polymer (P-2') can be easily obtained. 1b and structural unit A 2b A sulfide group (-S-) between the structural unit A and the structural unit B 1b and structural unit A 2b to a linking group (L 5 , L 6 All or most of the sulfide groups (-S-) that may be included as -SO 2 The degree of oxidation can be adjusted by the impregnation time, heating temperature, heating time, etc.
[0090] The compound (b1) for obtaining the polymer (P-2') is X 1b and / or X 2b Similarly, as the compound (b2), Z 1b and / or Z 2b It is possible to use multiple compounds with different
[0091] The reaction (polymerization) of compound (b1) and compound (b2) can be carried out, for example, by aromatic nucleophilic substitution reaction in a solvent in the presence of a base.
[0092] The solvent used in the reaction is preferably a good solvent for the compound (b1), the compound (b2), and the polymer (P-2'), and capable of increasing the molecular weight of the polymer (P-2') during polymerization. For example, N-methyl-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethylsulfoxide, diphenylsulfone, sulfolane, 1,3-dimethyl-2-imidazolidinone, tetramethylurea, etc. are preferably used. These solvents may be used alone or in a mixture of two or more kinds.
[0093] The base is used to improve the nucleophilicity of compound (b2). The base is not particularly limited as long as it can deprotonate compound (b2). For example, hydroxides and carbonates of alkali metals (lithium, sodium, potassium, rubidium, cesium), hydroxides and carbonates of alkaline earth metals (magnesium, calcium, strontium, barium), organic bases such as amines, etc. can be used.
[0094] The reaction temperature may be in the range of 25° C. to 350° C. From the viewpoint of excellent reaction rate, the reaction temperature is preferably 60° C. or higher, and more preferably 100° C. or higher. From the viewpoint of suppressing decomposition of the polymer, the reaction temperature is preferably 300° C. or lower, and more preferably 250° C. or lower.
[0095] Compound (b1) and compound (b2) can also be reacted (polymerized) by, for example, a cross-coupling reaction in a solvent in the presence of a catalyst. Examples of solvents that can be used in the reaction are the same as the examples of solvents that can be used in the aromatic nucleophilic substitution reaction.
[0096] The catalyst is not particularly limited as long as it can promote the cross-coupling reaction, and a conventionally known catalyst can be used. For example, in the case of a coupling reaction between halogens, a copper catalyst, a nickel catalyst, a palladium catalyst, etc. can be used. For example, in the case of a coupling reaction between a halogen and a boronic acid group, an alkylborane group, or a boronic acid ester group, a conventionally known catalyst (palladium catalyst, nickel catalyst, etc.) used in the Suzuki-Miyaura coupling reaction can be used.
[0097] Examples of the copper catalyst include copper(I) 2-thiophenecarboxylate and copper(I) tetrakis(acetonitrile)hexafluorophosphate.
[0098] Examples of nickel catalysts include bis(1,5-cyclooctadiene)nickel(0), dibromobis(triphenylphosphine)nickel(II), [1,1'-bis(diphenylphosphino)ferrocene]dichloronickel(II), and the like.
[0099] Examples of the palladium catalyst include tetrakis(triphenylphosphine)palladium(0), palladium(II) acetate, bis(triphenylphosphine)palladium(II) dichloride, [1,1'-bis(diphenylphosphino)ferrocene]dichloropalladium(II), and the like.
[0100] The reaction temperature may be in the range of 0° C. to 350° C. From the viewpoint of excellent reaction rate, the reaction temperature is preferably 30° C. or higher, and more preferably 60° C. or higher. From the viewpoint of suppressing decomposition of the polymer, the reaction temperature is preferably 300° C. or lower, and more preferably 250° C. or lower.
[0101] In the aromatic nucleophilic substitution reaction and cross-coupling reaction, it is preferable to remove water from the reaction system in order to increase the molecular weight of the polymer (P-2'). The dehydration method is not particularly limited, but for example, a method of azeotropic dehydration by making an azeotropic solvent coexist in the reaction system, a method of heating above the boiling point of water to continuously remove it from the reaction system, a method of making a water absorbent such as a molecular sieve coexist, etc. can be used. The azeotropic solvent is not particularly limited as long as it can remove water, and examples thereof include benzene, toluene, cyclohexane, xylene, etc.
[0102] The aromatic nucleophilic substitution reaction and the cross-coupling reaction are preferably carried out under an inert atmosphere (such as a nitrogen atmosphere or an argon atmosphere). After the polymerization reaction is completed, the polymer is recovered from the reaction solution and purified to obtain the desired polymer. Examples of the method for recovering the polymer from the reaction solution include a method in which the reaction solution is added to a solvent in which the polymer has low solubility, and the polymer is precipitated as a solid and recovered, and a method in which the solvent is removed from the reaction solution by evaporation and the polymer is recovered as a solid. Examples of the method for purifying the polymer include a method of washing in a solvent in which the polymer has low solubility and in which by-produced inorganic salts and compounds derived from the remaining monomers have high solubility, and a washing method using a Soxhlet extractor. The method for recovering and purifying the polymer is not limited to these methods.
[0103] In the above-mentioned method for synthesizing the polymer (P-2) using the polymer (P-2′) as an intermediate, a hydrophilic structural unit (e.g., structural unit A 1 ) and hydrophobic building blocks (e.g. building block A 2 ) are arranged alternately (repeated structure) throughout the polymer. Therefore, according to the above method, the repeat number n in formula (2) can be easily set to 10 or more.
[0104] <Electrolyte materials and electrolyte membranes> The electrolyte material of one embodiment is a material containing an electrolyte, and contains the above-mentioned polymer (P) as the electrolyte. The electrolyte membrane of one embodiment is a membrane containing an electrolyte, and contains the above-mentioned polymer (P) as the electrolyte. The electrolyte material is used to form the electrolyte membrane. That is, the electrolyte membrane may be made of the electrolyte material.
[0105] The electrolyte material and the electrolyte membrane contain the polymer (P), and therefore have excellent proton conductivity and chemical durability.
[0106] The electrolyte material and the electrolyte membrane may also have a microphase-separated structure when immersed in water (wet state). Specifically, when the electrolyte membrane is immersed in water and subjected to small-angle X-ray scattering (SAXS) measurement, the peak interplanar spacing obtained may be 4.0 nm or more.
[0107] The electrolyte material and the electrolyte membrane may also have a microphase-separated structure in a vacuum-dried state (dry state). Specifically, when the electrolyte membrane is subjected to small-angle X-ray scattering (SAXS) measurement in a vacuum-dried state, the peak interplanar spacing obtained may be 2.5 nm or more.
[0108] The electrolyte material and electrolyte membrane may consist of only the polymer (P) (for example, only the polymer (P-1) or only the polymer (P-2)), or may contain the polymer (P) and a component (additive, etc.) other than the polymer (P). That is, the electrolyte material may be a composition. The content of the polymer (P) in the electrolyte material and electrolyte membrane may be 90 to 100 mass%, 94 to 100 mass%, or 97 to 100 mass%. The above content is based on the total solid content of the electrolyte material or electrolyte membrane.
[0109] Examples of components other than the polymer (P) that may be contained in the electrolyte material and electrolyte membrane include water, water-retentive inorganic substances such as silica, and radical scavengers such as cerium oxide and manganese oxide.
[0110] The thickness of the electrolyte membrane is not particularly limited and can be changed depending on the size of the fuel cell, etc. From the viewpoint of increasing the mechanical strength of the membrane and reducing the membrane resistance, the thickness of the electrolyte membrane may be, for example, 1 to 200 μm, 1 to 100 μm, or 1 to 50 μm.
[0111] The method for producing the electrolyte membrane is not particularly limited, and the electrolyte membrane can be produced by a method known in the art for producing a membrane of an electrolyte polymer, such as a solution casting method, a dispersion casting method, a melt pressing method, a melt extrusion method, etc.
[0112] In the solution casting method, for example, a solution containing a polymer (P) is used as an electrolyte material, the solution is cast onto a substrate, the solvent is removed, and then the membrane is peeled off from the substrate to obtain an electrolyte membrane.
[0113] The solvent used in the solution casting method is not particularly limited as long as it is a solvent capable of dissolving the polymer (P), and examples of the solvent that can be used include N-methyl-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethylsulfoxide, diphenylsulfone, sulfolane, 1,3-dimethyl-2-imidazolidinone, tetramethylurea, etc. These may be used alone or in combination.
[0114] In the dispersion casting method, for example, a dispersion containing a polymer (P) is used as an electrolyte material, and the dispersion is cast onto a substrate, the dispersion medium is removed, and then the membrane is peeled off from the substrate to obtain an electrolyte membrane.
[0115] The dispersion medium used in the dispersion casting method is not particularly limited as long as it is a dispersion medium capable of dispersing the polymer (P), and examples of the dispersion medium that can be used include water, ethers such as tetrahydrofuran and diethyl ether, alcohols such as methanol, ethanol, 1-propanol, 2-propanol and 1-butanol, ketones such as acetone and cyclohexanone, acetonitrile, nitromethane, toluene, xylene, chlorobenzene, chloroform, etc. These may be used alone or in combination.
[0116] The electrolyte material and the electrolyte membrane are suitable for use in polymer electrolyte fuel cells and polymer electrolyte water electrolysis devices. The electrolyte material and the electrolyte membrane can also be used in redox flow batteries, electrochemical hydrogen pumps, chloralkali electrolysis devices, solid acid catalysts, membrane humidity control devices, gas separation membranes, and the like.
[0117] The electrolyte membrane can also be used by being attached to a microporous membrane, a nonwoven fabric, a mesh, etc. That is, another embodiment of the present invention is a laminate including an electrolyte membrane and another membrane (a microporous membrane, a nonwoven fabric, a mesh, etc.).
[0118] <Catalyst-coated electrolyte membrane> An electrolyte membrane with a catalyst layer in one embodiment includes the electrolyte membrane of the above embodiment and a catalyst layer disposed on one or both sides of the electrolyte membrane.
[0119] The catalyst layer is, for example, a layer composed of an anode catalyst or a cathode catalyst in a solid polymer fuel cell, a solid polymer water electrolysis device, etc. Hereinafter, a layer composed of an anode catalyst is referred to as an anode catalyst layer, and a layer composed of a cathode catalyst is referred to as a cathode catalyst layer.
[0120] The configuration of the catalyst layer is not particularly limited, and may be a conventionally known configuration as a catalyst layer (anode catalyst layer, cathode catalyst layer) of a polymer electrolyte fuel cell or a polymer electrolyte water electrolysis device. The catalyst layer may be formed of, for example, a conductive composition containing an anode catalyst or a cathode catalyst and a conductive material. The catalyst layer may contain an ionomer.
[0121] As the anode catalyst in a polymer electrolyte fuel cell, a metal catalyst capable of promoting the oxidation reaction of a fuel such as hydrogen can be used, and as the anode catalyst in a polymer electrolyte water electrolysis device, a metal catalyst capable of promoting an oxygen generation reaction can be used, for example, platinum, gold, silver, palladium, iridium, rhodium, ruthenium, iron, cobalt, nickel, chromium, tungsten, manganese, vanadium, and alloys of two or more of these metals can be used. These metals may be used alone or in combination of two or more.
[0122] As the cathode catalyst in a polymer electrolyte fuel cell, a metal catalyst capable of promoting an oxygen reduction reaction can be used, and as the cathode catalyst in a polymer electrolyte water electrolysis device, a metal catalyst capable of promoting a hydrogen generation reaction can be used, for example, platinum, gold, silver, palladium, iridium, rhodium, ruthenium, iron, cobalt, nickel, chromium, tungsten, manganese, vanadium, and alloys of two or more of these metals can be used. These metals may be used alone or in combination of two or more.
[0123] As the conductive material, for example, carbon blacks such as furnace black, ketjen black, channel black, and acetylene black, activated carbon, graphite, etc. These may be used alone or in combination of two or more.
[0124] As the ionomer, a conventionally known material can be used, for example, an ionomer containing a perfluoro electrolyte can be used. Also, the above-mentioned polymer (P) can be used as the ionomer. As the ionomer, it is preferable to use a material with high oxygen permeability. There is no particular limit to the amount of ionomer added in the catalyst layer, but it is preferable to adjust the amount added within a range where oxygen diffusion is not easily inhibited.
[0125] The catalyst layer may further contain, as additives, a water repellent such as fluorinated carbon, and a binder such as a fluorine-containing resin or a hydrocarbon-based resin having a sulfone group.
[0126] A laminate having an anode catalyst layer and a cathode catalyst layer on both sides of an electrolyte membrane (e.g., a layer structure of "anode catalyst layer / electrolyte membrane / cathode catalyst layer") is also called a CCM (Catalyst Coated Membrane), and is suitably used in solid polymer electrolyte fuel cells and solid polymer electrolyte water electrolysis devices.
[0127] In the above embodiment, instead of the electrolyte membrane, a laminate including the other membranes (microporous membrane, nonwoven fabric, mesh, etc.) described above may be used.
[0128] <Membrane electrode assembly> A membrane electrode assembly of one embodiment includes the electrolyte membrane of the above embodiment and an electrode layer disposed on one or both sides of the electrolyte membrane.
[0129] The electrode layer includes, for example, the catalyst layer (anode catalyst layer or cathode catalyst layer) in the catalyst-layered electrolyte membrane of the above embodiment. Hereinafter, the electrode layer including the anode catalyst layer is referred to as the anode layer, and the electrode layer including the cathode catalyst layer is referred to as the cathode layer.
[0130] The configuration of the electrode layer is not particularly limited, and may be a conventionally known configuration as the electrode layer (anode layer, cathode layer) of a polymer electrolyte fuel cell or a polymer electrolyte water electrolysis device. The electrode layer may be composed of, for example, the above-mentioned catalyst layer (anode catalyst layer or cathode catalyst layer) and a gas diffusion substrate. When the catalyst layer itself has gas diffusion properties, the electrode layer may be composed of only the catalyst layer. For example, a porous membrane can be used as the gas diffusion substrate. As the gas diffusion substrate, a substrate having water repellency and electrical conductivity in addition to gas diffusion properties (for example, a carbon fiber substrate such as a carbon nonwoven fabric or carbon paper, or a titanium fiber sintered body) can also be used.
[0131] A laminate having an anode layer and a cathode layer as electrode layers on both sides of an electrolyte membrane (for example, a laminate having a layer structure of "gas diffusion substrate / anode catalyst layer / electrolyte membrane / cathode catalyst layer / gas diffusion substrate") is also called an MEA (Membrane Electrode Assembly), and is suitably used in solid polymer fuel cells and solid polymer water electrolysis devices.
[0132] In the above embodiment, instead of the electrolyte membrane, a laminate including the other membranes (microporous membrane, nonwoven fabric, mesh, etc.) described above may be used.
[0133] <Polymer electrolyte fuel cell> A polymer electrolyte fuel cell according to one embodiment includes the membrane electrode assembly according to the above embodiment.
[0134] The configuration of the polymer electrolyte fuel cell is not particularly limited, and may be a conventionally known configuration, except for using the membrane electrode assembly of the above embodiment. The polymer electrolyte fuel cell may, for example, include two or more membrane electrode assemblies. The two or more membrane electrode assemblies may be stacked (laminated) via a separator. As the separator, a conventionally known separator for polymer electrolyte fuel cells may be used.
[0135] <Solid polymer water electrolysis device> A solid polymer water electrolysis device of one embodiment includes the membrane electrode assembly of the above embodiment.
[0136] The configuration of the solid polymer water electrolysis device is not particularly limited, and may be a conventionally known configuration, except for the use of the membrane electrode assembly of the above embodiment. The solid polymer water electrolysis device may further include, for example, a power feeder on the outside of the membrane electrode assembly. Also, the solid polymer water electrolysis device may include two or more membrane electrode assemblies. EXAMPLES
[0137] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0138] <Synthesis Example 1> (Synthesis of hydrophilic monomer (M1)) A 10L flask equipped with a dropping funnel, a reflux condenser, and a mechanical stirrer was replaced with nitrogen, and 101g of 4,4'-bis[(4-chlorophenyl)sulfonyl]-1,1'-biphenyl and 4L of dehydrated tetrahydrofuran were charged and stirring was started. The flask was cooled to -70°C in a methanol-dry ice bath, and 320mL of 2.6mol / L n-butyllithium-hexane solution was added dropwise. The flask was stirred for 1 hour while cooled in the bath. 40mL of sulfurous acid gas was introduced into the flask with nitrogen gas. The flask was stirred for 30 minutes while cooled in the bath. The bath was then removed and the internal temperature was raised to 0°C. The precipitated solid was filtered off by suction filtration and washed with 200mL of tetrahydrofuran. The collected solid was dissolved in 2L of pure water, 260mL of 35% hydrogen peroxide was added, and the mixture was stirred for 18 hours. The solid was removed by suction filtration, and 600g of sodium chloride was added to the collected filtrate. The precipitated white solid was collected by suction filtration and purified by recrystallization from water / isopropyl alcohol. The obtained solid was dried under reduced pressure to obtain a hydrophilic monomer represented by the following formula (M1). The yield was 65%.
[0139] [ka]
[0140] <Synthesis Example 2> (Synthesis of hydrophobic monomer (M2)) In a 200 mL flask equipped with a stirrer, a Dean-Stark tube, a reflux condenser, and a calcium chloride tube, 4.0 g of 4,4'-bis[(4-chlorophenyl)sulfonyl]-1,1'-biphenyl, 14.8 g of [1,1'-biphenyl]-4,4'-diol, and 13.2 g of potassium carbonate were charged, and 50 mL of N,N-dimethylacetamide (DMAc) and 50 mL of toluene were added. The temperature was raised to 160 ° C in an oil bath while stirring, and heating and stirring were continued for 4 hours. Toluene was extracted from the Dean-Stark tube, and the temperature was raised to 180 ° C in an oil bath. After the temperature was raised, heating and stirring were continued for 8 hours. After the reaction solution was allowed to cool to room temperature, the reaction solution was poured into 200 mL of 10% hydrochloric acid, and the precipitated white solid was filtered off. The filtered solid was washed with 300 mL of ethanol and dried. The dried solid was purified by recrystallization from NMP / ethanol. The resulting solid was dried under reduced pressure to obtain a hydrophobic monomer (M2) represented by the following formula (M2) in a yield of 50%.
[0141] [ka]
[0142] <Synthesis Example 3> (Synthesis of hydrophobic monomer (M3)) A 500 mL flask equipped with a stirrer and a cooling tube was replaced with nitrogen. 41 g of 4,4'-thiobisbenzenethiol, 14 g of 4,4'-bis[(4-chlorophenyl)sulfonyl]-1,1'-biphenyl, 80 mL of DMAc, and 4 g of potassium carbonate were added to the flask. The temperature was raised to 100°C in an oil bath while stirring, and heating and stirring were continued for 6 hours. After the reaction solution was allowed to cool, 100 mL of 1 M hydrochloric acid was added, and the precipitated solid was collected by suction filtration. The collected solid was dissolved in dichloromethane and purified by silica column chromatography using dichloromethane as a developing solvent. The fraction containing the target product was collected, and the solvent was removed by an evaporator. The obtained solid was purified by recrystallization from dichloromethane. The obtained solid was dried under reduced pressure to obtain a hydrophobic monomer (M3) represented by the following formula (M3). The yield was 40%.
[0143] [ka]
[0144] <Example 1> (Synthesis of polymer (P1)) In a 100 mL three-neck flask equipped with a nitrogen inlet tube, a stirrer, and a Dean-Stark tube, 2.711 g of the hydrophobic monomer (M3) obtained in Synthesis Example 3, 2.664 g of the hydrophilic monomer (M1) obtained in Synthesis Example 1, and 1.352 g of potassium carbonate were added, and nitrogen replacement was performed. Then, 25 mL of DMSO and 25 mL of cyclohexane were added. After heating to 130°C and reflux dehydration for 4 hours, cyclohexane was extracted from the Dean-Stark tube. The reaction solution was heated to 140°C and polymerization was performed for 260 hours. After cooling to room temperature, reprecipitation purification was performed from 500 mL of isopropyl alcohol (IPA), and a solid was collected by suction filtration. The collected solid was washed with water and dried under reduced pressure to obtain a polymer (P1) having a structure represented by the following formula (P1). The yield was 88%. Note that n in formula (P1) was calculated from the number average molecular weight described later. The same applies to n in formulas (P2) to (P3) described later.
[0145] [ka] [In formula (P1), M represents Na, K or H, and n represents a positive number (about 20).]
[0146] (molecular weight measurement) The number average molecular weight of the polymer (P1) was measured under the following conditions. The number average molecular weight was 33,000. [Measurement conditions] The number average molecular weight was measured by GPC. The polymer (P1) was dissolved in an eluent (N,N-dimethylformamide solvent containing 10 mmol / L lithium bromide) at a concentration of 1 mg / mL to prepare a sample solution. The apparatus used was a Tosoh HLC-8320GPC. Two Tosoh TSKgel SuperAWM-H columns (inner diameter 6.0 mm, length 15 cm) were used. A differential refractometer detector was used. The flow rate was 0.6 mL / min, and the temperature was 40°C. The number average molecular weight was calculated in terms of standard polyethylene glycol / oxide (PEG / PEO).
[0147] (Synthesis of polymer (P2) and preparation of electrolyte membrane) The obtained polymer (P1) was dissolved in DMSO to obtain a solution containing 10% by mass of polymer (P1). The obtained solution was cast onto a glass substrate and dried at 60°C for 12 hours to obtain a film (thickness 37 μm). The obtained film was immersed in a mixed solution consisting of 80 mL of acetic acid, 8 mL of sulfuric acid, and 7 mL of hydrogen peroxide, and stirred at 30°C for 48 hours. Then, the mixture was heated and stirred at 105°C for 10 minutes. The obtained film was immersed in pure water, thoroughly washed, and dried under reduced pressure to obtain a film (thickness 37 μm) made of polymer (P2) having a structure represented by the following formula (P2). The number average molecular weight of polymer (P2) measured in the same manner as above was 37,000. When the infrared absorption spectrum of the polymer film before and after the oxidation reaction was measured, it was found to have a peak at 1570 cm -1 and 1470cm -1 The absorption peak at 1330 cm completely disappeared after oxidation, and -1 The absorption peak intensity at 1570cm increased. -1 and 1470cm -1 The absorption peak at 1330 cm is due to the ring stretching vibration of the benzene ring with the -S- bond. -1 The absorption peak of -SO 2 -bond stretching vibration, all -S- bonds are converted to -SO 2 - bonds were confirmed to be oxidized.
[0148] [ka] [In formula (P2), M represents Na, K or H, and n represents a positive number (about 20).]
[0149] The obtained membrane was immersed in 1M hydrochloric acid for 24 hours to remove metal ions (Na + Or K + ) to proton (H + ), then it was immersed in pure water to thoroughly wash, and dried under reduced pressure to obtain the polymer electrolyte membrane of Example 1 (electrolyte membrane made of proton-substituted polymer (P2)).
[0150] (evaluation) [Proton conductivity evaluation] The proton conductivity of the resulting polymer electrolyte membrane was measured by the following method. A Teflon (registered trademark) measuring cell (Scribner, BT-115) was used, and the prepared electrolyte membrane was placed in the cell in contact with four platinum wires. After holding at 70% relative humidity for 2 hours, the humidity was increased from 20% relative humidity, and DC resistance measurement was performed by the four-terminal method while maintaining the set humidity. The proton conductivity in the in-plane direction of the electrolyte membrane was calculated from the obtained resistance value, the thickness of the polymer electrolyte membrane, and the distance between the terminals. The proton conductivity of the polymer electrolyte membrane of this example was 172 mS / cm (80°C, 100% relative humidity).
[0151] [Chemical durability evaluation] The chemical durability of the obtained polymer electrolyte membrane was evaluated by a Fenton test under the following conditions. A polymer electrolyte membrane measuring 1 cm in length and 3 cm in width was prepared, and the mass and proton conductivity were measured before the Fenton test. The measurement of proton conductivity was performed in the same manner as above. The polymer electrolyte membrane was placed in 50 mL of Fenton solution (3% aqueous hydrogen peroxide solution containing 2 ppm of iron (II) sulfate) and immersed at 80° C. for 1 hour to perform the Fenton test. The polymer electrolyte membrane after the Fenton test was dried, and the mass and proton conductivity were measured. The mass and proton conductivity retention rates were calculated from the values before and after the Fenton test. The mass retention rate and proton conductivity retention rate of the polymer electrolyte membrane of this example were both 100%.
[0152] [Gas permeability test] The gas permeability of the resulting polymer electrolyte membrane was evaluated according to the gas permeability test method (JIS K 7126-2) using the constant pressure method. Specifically, first, the polymer electrolyte membrane was mounted in a state in which it was hermetically sealed between the two chambers of the permeation cell. Hydrogen, which is the measurement gas, was supplied to one side of the polymer electrolyte membrane, and Ar gas, which is the carrier gas, was supplied to the other side. The relative humidity was adjusted by the humidifier temperature of each supply gas and the cell temperature. The measurement gas that had permeated the polymer electrolyte membrane was supplied to a gas chromatograph together with the carrier gas, and the gas permeability was measured from the detection data and flow rate. The gas permeability (cm) was calculated from the obtained gas permeability and the thickness of the polymer electrolyte membrane. 3 mm / (cm 2 The hydrogen gas permeability of the polymer electrolyte membrane of this example was calculated to be 0.11×10 -7 cm 3 mm / (cm 2 ·s·kPa) (80°C, relative humidity 60%).
[0153] [Small angle X-ray scattering (SAXS) measurement] Small angle X-ray scattering (SAXS) measurements of the polymer electrolyte membrane were carried out in a dry state (under vacuum) and in a wet state (immersed in water) according to the following conditions. Device name: Bruker Japan NanoSTAR Voltage / Current: 45kV / 120mA X-ray wavelength: Cu Kα ray Camera length: 104.3cm Exposure time: 60 minutes (dry state), 180 minutes (wet state)
[0154] For the obtained small-angle scattering profile, the peak top position q max Therefore, the interplanar spacing d(=2π / q max) was calculated. The interplanar spacing d in the dry state was 3.9 nm, and the interplanar spacing d in the wet state was 5.2 nm. This confirmed that the polymer electrolyte membrane of this example had a microphase-separated structure in both the dry and wet states.
[0155] <Comparative Example 1> (Synthesis of polymer (P3)) In a 100mL three-neck flask equipped with a nitrogen inlet tube, a stirrer, and a Dean-Stark tube, 0.983g of the hydrophobic monomer (M2) obtained in Synthesis Example 2, 1.181g of the hydrophilic monomer (M1) obtained in Synthesis Example 1, and 0.507g of potassium carbonate were added and nitrogen substitution was performed. Then, 10mL of dimethyl sulfoxide (DMSO) and 10mL of cyclohexane were added. After heating to 130°C and reflux dehydration for 4 hours, cyclohexane was extracted from the Dean-Stark tube. Polymerization was performed for 150 hours while heating at 130°C. After cooling the reaction solution to room temperature, reprecipitation purification was performed from 300mL of isopropyl alcohol (IPA), and a solid was collected by suction filtration. The collected solid was washed with water and dried under reduced pressure to obtain a polymer (P3) having a structure represented by the following formula (P3). The yield was 97%. The number average molecular weight of the polymer (P3) measured in the same manner as in Example 1 was 30,000. [ka] [In formula (P3), M represents Na, K or H, and n represents a positive number (about 20).]
[0156] (Preparation of electrolyte membrane) The obtained polymer (P3) was dissolved in DMSO to obtain a solution containing 10% by mass of polymer (P3). The obtained solution was cast onto a glass substrate and dried at 60° C. for 12 hours to obtain a membrane (thickness: 49 μm). The obtained membrane was immersed in 1 M hydrochloric acid for 24 hours to remove metal ions (Na + Or K + ) to proton (H +), then it was immersed in pure water to thoroughly wash, and dried under reduced pressure to obtain a polymer electrolyte membrane of Comparative Example 1 (an electrolyte membrane made of a proton-substituted polymer (P3)).
[0157] (evaluation) The polymer electrolyte membrane of this comparative example was subjected to various evaluations (proton conductivity evaluation, chemical durability evaluation, hydrogen gas permeability test, and SAXS measurement) in the same manner as in Example 1. The proton conductivity was 231 mS / cm (80°C, 100% relative humidity). In the Fenton test, the polymer electrolyte membrane was completely dissolved during the test and could not maintain the membrane shape, so the mass retention rate and proton conductivity retention rate were both 0%. The hydrogen gas permeability was 0.15×10 -7 cm 3 mm / (cm 2 The temperature was 80°C and the relative humidity was 60%. The interplanar spacing d in the dry and wet states measured by SAXS was 3.6 nm and 5.5 nm, respectively.
[0158] <Comparative Example 2> (Preparation of electrolyte membrane) Except for using the polymer (P1) obtained in Example 1 instead of the polymer (P3), a polymer electrolyte membrane of Comparative Example 2 (an electrolyte membrane made of proton-substituted polymer (P1)) was obtained in the same manner as in Comparative Example 1. The thickness of the electrolyte membrane was 37 μm.
[0159] (evaluation) The polymer electrolyte membrane of this comparative example was subjected to various evaluations (proton conductivity evaluation, chemical durability evaluation, hydrogen gas permeability test, and SAXS measurement) in the same manner as in Example 1. The proton conductivity was 185 mS / cm (80°C, 100% relative humidity). In the Fenton test, the polymer electrolyte membrane was completely dissolved during the test and could not maintain the membrane shape, so the mass retention rate and proton conductivity retention rate were both 0%. The hydrogen gas permeability was 0.14×10 -7 cm 3 mm / (cm 2The temperature was 80°C and the relative humidity was 60%. The interplanar spacing d in the dry and wet states measured by SAXS was 3.9 nm and 5.4 nm, respectively.
[0160] <Comparative Example 3> In Comparative Example 3, a commercially available Nafion was used as an evaluation sample. TM Using NR211, various evaluations (proton conductivity evaluation, chemical durability evaluation, hydrogen gas permeability test, and SAXS measurement) were performed in the same manner as in Example 1. The proton conductivity was 130 mS / cm (80°C, relative humidity 100%). The mass retention rate and proton conductivity retention rate in the Fenton test were 100%. The hydrogen gas permeability was 1.03×10 -7 cm 3 mm / (cm 2 The temperature was 80°C and the relative humidity was 60%. The interplanar spacing d in the dry and wet states measured by SAXS was 3.3 nm and 5.3 nm, respectively.
[0161] [Table 1]
Claims
1. A polymer having a structure represented by the following formula (1): 【Chemistry 1】 [In formula (1), A 1 represents a structural unit represented by the following formula (a1): A 2 represents a structural unit represented by the following formula (a2): L 1 and L 2 each independently represents a single bond or -SO 2 - indicates n is a number from 10 to 100, * indicates a bond. Multiple A's 1 are identical to each other, Multiple A's 2 are identical to each other, Multiple L 1 may be the same or different, Multiple L 2 may be the same or different. 【Chemistry 2】 [In formula (a1), IExG represents an ion exchange group; L 3 is a single bond or -SO 2 - indicates x represents an integer from 1 to 10; * indicates a bond. The multiple IExGs may be the same or different from each other, Multiple L 3 may be the same or different. 【Chemistry 3】 [In formula (a2), Ar represents an arylene group having no ion exchange group; L 4 is a single bond or -SO 2 - indicates y represents an integer from 2 to 20; * indicates a bond. A plurality of Ar may be the same or different, Multiple L 4 may be the same or different.
2. The polymer according to claim 1, wherein the constitutional unit represented by formula (a1) contains, as the ion exchange group, at least one selected from the group consisting of a sulfone group, an alkylsulfone group, and a sulfonimide group.
3. The polymer according to claim 1, wherein the constitutional unit represented by formula (a2) contains, as the arylene group, at least one selected from the group consisting of a phenylene group, a naphthylene group, and a fluorene group.
4. 2. The polymer of claim 1, having a number average molecular weight of 20,000 to 300,000.
5. An oxide of a polymer having a sulfide group, The polymer is a polymer of a compound represented by the following formula (b1) and a compound represented by the following formula (b2): 【Chemistry 4】 [In formula (b1), IExG represents an ion exchange group; L 5 is a single bond, -S- or -SO 2 - indicates X 1b and X 2b each independently represents a halogen atom, x represents an integer of 1 to 10. The multiple IExGs may be the same or different from each other, Multiple L 5 may be the same or different. 【Chemistry 5】 [In formula (b2), Ar represents an arylene group having no ion exchange group; L 6 is a single bond, -S- or -SO 2 - indicates Z 1b and Z 2b each independently represents a thiol group, a halogen atom, a boronic acid group, an alkylborane group, or a boronic acid ester group, y represents an integer of 2 to 20. A plurality of Ar may be the same or different, Multiple L 6 may be the same or different.
6. An electrolyte material comprising the polymer according to any one of claims 1 to 5.
7. An electrolyte membrane comprising the polymer according to any one of claims 1 to 5.
8. A catalyst layer-coated electrolyte membrane comprising the electrolyte membrane according to claim 7 and a catalyst layer disposed on one or both sides of the electrolyte membrane.
9. A membrane electrode assembly comprising the electrolyte membrane according to claim 7 and an electrode layer disposed on one or both sides of the electrolyte membrane.
10. A polymer electrolyte fuel cell comprising the membrane electrode assembly according to claim 9.
11. A solid polymer water electrolysis device comprising the membrane electrode assembly according to claim 9.
Citation Information
Patent Citations
Solid polyelectrolyte fuel cell and manufacture thereof
JP1999204119A
Polymer electrolyte membrane, membrane electrode assembly using same, and solid polymer fuel cell
WO2013031675A1
Cited By
Polymer, electrolyte material, electrolyte membrane, electrolyte membrane with catalyst layer, membrane electrode assembly, solid polymer-type fuel cell, and solid polymer-type water electrolysis device
JP2025023971A
Polymer, electrolyte material, electrolyte membrane, electrolyte membrane with catalyst layer, membrane electrode assembly, polymer electrolyte fuel cell, and polymer electrolyte water electrolysis device
JP7711830B2
Polymer, electrolyte material, electrolyte membrane, electrolyte membrane with catalyst layer, membrane electrode assembly, polymer electrolyte fuel cell, and polymer electrolyte water electrolysis device
JP7711855B2
Electrolyte membrane, electrolyte membrane with catalyst layer, membrane electrode assembly, polymer electrolyte fuel cell, and polymer electrolyte water electrolysis device
JP7925485B1
JPWO2024204267A1