Method for producing polyvinyl alcohol-based resin containing acetoacetate ester group

The reaction of polyvinyl alcohol resin with acetoacetate in a mixed solvent of amide and aliphatic carboxylic acid addresses solubility and coloring issues in AA-PVA production, resulting in high-quality AA-PVA suitable for diverse applications.

JP2024143111APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023055617
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for producing acetoacetyl group-containing polyvinyl alcohol resin (AA-PVA) face issues such as low solubility and coloring, particularly when using diketene or N-methyl-2-pyrrolidone (NMP) as solvents, necessitating the use of additional inhibitors.

Method used

A method involving the reaction of polyvinyl alcohol resin with acetoacetate in the presence of a mixed solvent comprising an amide compound and an aliphatic carboxylic acid, optimizing the mass ratios and reaction conditions to enhance solubility and suppress coloring.

Benefits of technology

The method produces AA-PVA with improved solubility and no coloring, allowing for efficient and safe production without the need for additional inhibitors, and can be used in various applications including molded products, adhesives, coatings, and stabilizers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143111000001
    Figure 2024143111000001
  • Figure 2024143111000002
    Figure 2024143111000002
Patent Text Reader

Abstract

To provide a production method that yields a polyvinyl alcohol-based resin containing an acetoacetate ester group with superior solubility and resistance to coloration.SOLUTION: A method for producing a polyvinyl alcohol-based resin containing an acetoacetate ester group includes reacting a polyvinyl alcohol-based resin (A) and an acetoacetate ester (B) in the presence of a solvent (C) containing an amide compound (c1) and an aliphatic carboxylic acid (c2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polyvinyl alcohol resin containing acetoacetate groups. [Background technology]

[0002] Acetoacetyl group-containing polyvinyl alcohol resins (hereinafter sometimes referred to as "AA PVA") are known to have excellent water resistance due to their high reactivity with various crosslinking agents, and are widely used in a variety of fields.

[0003] Conventionally, various methods have been proposed for producing AA PVA. For example, a method has been proposed in which a polyvinyl alcohol resin is swollen with acetic acid and the swollen polyvinyl alcohol resin is reacted with diketene to produce the desired AA PVA (Patent Document 1).

[0004] The production method of Patent Document 1 has concerns about the acute toxicity inherent to diketene, and so in recent years, an alternative production method in which a polyvinyl alcohol resin is reacted with an acetoacetic ester has attracted attention.

[0005] Specifically, a method has been proposed in which a polyvinyl alcohol resin is swollen with acetic acid and the swollen polyvinyl alcohol resin is reacted with an acetoacetate to produce the desired AA PVA (Patent Document 2). Also, for example, a method has been proposed in which a polyvinyl alcohol resin is swollen with N-methyl-2-pyrrolidone (NMP) and the swollen polyvinyl alcohol resin is reacted with an acetoacetate to produce the desired AA PVA (Patent Document 3). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 9-110925 [Patent Document 2] U.S. Patent No. 5,719,231 [Patent Document 3] International Publication No. 2022 / 065358 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the manufacturing method of Patent Document 2, the swelling degree of the polyvinyl alcohol resin is low and self-crosslinking of the acetoacetyl group tends to proceed during the reaction, so there is still room for improvement in that the solubility of the AA-PVA is low. Also, in the manufacturing method of Patent Document 3, there is still room for improvement in that the solubility of the AA-PVA may be insufficient and the obtained AA-PVA is colored, so that a separate coloring inhibitor must be used. [Means for solving the problem]

[0008] In the course of intensive research against such a background, the present inventors have focused on the technical relationship between the composition of the solvent used in the production method of AA-PVA and the solubility and coloration of the obtained AA-PVA. As a result of further research from such a perspective, the present inventors have unexpectedly found that an AA-PVA having excellent solubility and suppressed coloration can be obtained by reacting a polyvinyl alcohol resin with an acetoacetate ester in the presence of a mixed solvent of a specific combination of solvents.

[0009] That is, the present invention provides the following [1] to [6]. [1] A method for producing a polyvinyl alcohol-based resin containing an acetoacetate group, comprising reacting a polyvinyl alcohol-based resin (A) with an acetoacetate (B) in the presence of a solvent (C) containing an amide compound (c1) and an aliphatic carboxylic acid (c2). [2] The method for producing a polyvinyl alcohol resin containing an acetoacetate group according to [1], wherein a mass ratio (c1:c2) of the amide compound (c1) to the aliphatic carboxylic acid (c2) is 50:50 to 99:1. [3] The method for producing a polyvinyl alcohol-based resin containing an acetoacetate group according to [1] or [2], wherein a mass ratio (C / A) of the solvent (C) to the polyvinyl alcohol-based resin (A) is 1 to 10. [4] The method for producing a polyvinyl alcohol-based resin containing an acetoacetate group according to any one of [1] to [3], wherein a mass ratio (C / A) of the solvent (C) to the polyvinyl alcohol-based resin (A) is 2.5 to 8. [5] The method for producing a polyvinyl alcohol-based resin containing an acetoacetate group according to any one of [1] to [4], wherein the amount of the acetoacetate (B) is 50 to 250 parts by mass per 100 parts by mass of the polyvinyl alcohol-based resin (A). [6] The method for producing a polyvinyl alcohol-based resin containing an acetoacetate ester group according to any one of [1] to [5], wherein the polyvinyl alcohol-based resin (A) is a polyvinyl alcohol-based resin containing a fatty acid metal salt, and the content of the fatty acid metal salt is 1.0 mass% or less. Effect of the Invention

[0010] According to the production method of the present invention, it is possible to provide an acetoacetate group-containing polyvinyl alcohol resin which is excellent in solubility and suppressed in discoloration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. However, the following description is an example of an embodiment of the present invention, and the present invention is not limited to the contents of the following description as long as it does not deviate from the gist of the present invention.

[0012] The method for producing AA-PVA according to one embodiment of the present invention (hereinafter, may be referred to as "this production method") is characterized in that a polyvinyl alcohol resin (A) (hereinafter, may be referred to as "PVA (A)") is reacted with an acetoacetic ester (B) in the presence of a solvent (C) containing an amide compound (c1) and an aliphatic carboxylic acid (c2). According to this production method, since the reaction is carried out in the presence of a solvent (C) containing an amide compound (c1) and an aliphatic carboxylic acid (c2), an AA-PVA having high solubility can be obtained, and further, coloration can be suppressed.

[0013] Although the reason why the present production method provides the above-mentioned excellent effects is not entirely clear, the inventors speculate that the above-mentioned excellent effects are provided because the PVA (A) swollen with the above-mentioned specific mixed solvent is reacted with the acetoacetic ester (B), which allows the PVA (A) to react with an optimal degree of swelling.

[0014] The PVA (A), acetoacetic ester (B), and solvent (C) used as raw materials in this production method will be explained below, and this production method will be explained in detail.

[0015] (PVA(A)) The PVA (A) used in the present production method is not particularly limited, and various types of PVA can be used. PVA (A) is a saponified polymer of a vinyl ester monomer or a derivative thereof. Examples of the vinyl ester monomer include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl versatate. From the viewpoint of economy, vinyl acetate is preferably used.

[0016] PVA (A) may be PVA which is a saponification product of the polymer of the vinyl ester monomer, or may be modified PVA in which a monomer copolymerizable with the vinyl ester monomer is partially contained in the molecular chain. Examples of the copolymerizable monomer include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene, hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, 5-hexen-1-ol, and 3,4-dihydroxy-1-butene, and derivatives thereof such as acylated products, unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, itaconic acid, and undecylenic acid, salts thereof, monoesters thereof, and dialkyl esters thereof, nitriles such as acrylonitrile and methacrylonitrile, diacetone acrylamide, Examples of the vinyl acetate include amides such as acrylamide and methacrylamide, olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid, or salts thereof, alkyl vinyl ethers, dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxolane, and glycerin monoallyl ether, and other vinyl compounds, substituted vinyl acetates such as isopropenyl acetate and 1-methoxyvinyl acetate, vinylidene chloride, 1,4-diacetoxy-2-butene, 1,4-dihydroxy-2-butene, and vinylene carbonate.

[0017] Further, examples of the copolymerizable monomer include polyoxyalkylene group-containing monomers such as polyoxyethylene (meth)acryl ether, polyoxyethylene (meth)acrylamide, polyoxypropylene (meth)acrylamide, polyoxyethylene (meth)acrylate, polyoxypropylene (meth)acrylate, polyoxyethylene (1-(meth)acrylamide-1,1-dimethylpropyl) ester, polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, polyoxyethylene allylamine, polyoxypropylene allylamine, polyoxyethylene vinylamine, and polyoxypropylene vinylamine; N-acrylamide; Also included are cationic group-containing monomers such as N-acrylamidoethyltrimethylammonium chloride, N-acrylamidopropyltrimethylammonium chloride, 2-acryloxyethyltrimethylammonium chloride, 2-methacryloxyethyltrimethylammonium chloride, 2-hydroxy-3-methacryloyloxypropyltrimethylammonium chloride, allyltrimethylammonium chloride, methallyltrimethylammonium chloride, 3-butenetrimethylammonium chloride, dimethyldiallylammonium chloride, and diethyldiallylammonium chloride. In the present invention, (meth)acrylic refers to acrylic or methacrylic, and (meth)acrylate refers to acrylate or methacrylate.

[0018] The amount of the copolymerizable monomer introduced is appropriately set depending on the type of monomer, but is usually 10 mol % or less, particularly 5 mol % or less. If the amount introduced is too large, water solubility and chemical resistance may be impaired, which is not preferable.

[0019] In the case of a typical polyvinyl alcohol resin, the bonding mode of the main chain is mainly 1,3-diol bonds, and the content of 1,2-diol bonds is about 1.5 to 1.7 mol %, but it is also possible to use one in which the content is 1.7 to 3.5 mol % by increasing the polymerization temperature when polymerizing a vinyl ester monomer.

[0020] The PVA (A) can be produced according to a conventional method. For example, any known polymerization method such as solution polymerization, emulsion polymerization, suspension polymerization, etc. can be used. In addition, the PVA (A) is preferably formed into a powder by pulverizing and drying using a wet pulverizer or the like according to a conventional method.

[0021] The average particle size of the powdered PVA (A) is not limited to the following, but is preferably 100 to 800 μm, more preferably 200 to 700 μm, and even more preferably 300 to 600 μm, from the viewpoint of controlling the degree of swelling by a specific solvent composition. The average particle size means the particle size at which the cumulative value of the particle size distribution obtained by sieving is 50 mass%.

[0022] The saponification degree of PVA (A) (based on JIS K6726) is usually 75 to 99.9 mol%, more preferably 80 to 99.5 mol%, and particularly preferably 85 to 99.3 mol%. If the saponification degree is too low, the solubility in water tends to decrease, which is undesirable.

[0023] The average degree of polymerization of the PVA (A) (based on JIS K6726) is preferably 200 to 4000, more preferably 400 to 3500, and further preferably 500 to 3000. If the average degree of polymerization is too low, the water resistance tends to decrease, and if it is too high, the viscosity tends to increase, making it difficult to handle.

[0024] The viscosity of a 4% by mass aqueous solution of PVA (A) at 20° C. (based on JIS K6726) is usually 1.5 to 100 mPa s, preferably 4 to 80 mPa s, and more preferably 5 to 70 mPa s. If the viscosity of the 4% by mass aqueous solution is too high, the viscosity increases and the solution tends to become difficult to handle, whereas if the viscosity of the 4% by mass aqueous solution is too low, the water resistance tends to decrease.

[0025] The PVA (A) used in the present production method may be one type alone or two or more types in any combination.

[0026] (Acetoacetate (B)) Examples of the acetoacetate (B) include methyl acetoacetate, ethyl acetoacetate, n-propyl acetoacetate, isopropyl acetoacetate, n-butyl acetoacetate, s-butyl acetoacetate, t-butyl acetoacetate, octyl acetoacetate, oleyl acetoacetate, lauryl acetoacetate, stearyl acetoacetate, benzyl acetoacetate, and phenyl acetoacetate. The number of carbon atoms in the alkyl group of the acetoacetate is preferably 1 to 10, and more preferably 1 to 5. Among these, methyl acetoacetate and t-butyl acetoacetate are particularly preferred. These can be used alone or in any combination and ratio of two or more kinds.

[0027] In the present production method, the amount of acetoacetic ester (B) is preferably 50 to 250 parts by mass, more preferably 65 to 200 parts by mass, and even more preferably 80 to 150 parts by mass, relative to 100 parts by mass of PVA (A), from the viewpoints of increasing the solubility of AA PVA and effectively suppressing coloration. If the amount of acetoacetic ester is too large, the degree of swelling tends to decrease, which causes the AA PVA to become insoluble in water. If the amount is too small, the reaction rate tends to decrease, which causes the reaction time to be prolonged.

[0028] In the present production method, the molar ratio of the acetoacetate (B) to the vinyl alcohol units in the PVA (A) (moles of acetoacetate (B) / moles of vinyl alcohol units in the PVA (A) × 100) is preferably 10 to 50, more preferably 15 to 45, and even more preferably 20 to 40.

[0029] (Solvent (C)) In this production method, it is important to use a solvent (C) containing an amide compound (c1) and an aliphatic carboxylic acid (c2) as the solvent. By using a solvent (C) containing an amide compound (c1) and an aliphatic carboxylic acid (c2), the generation of insoluble matters can be suppressed, so that an AA-PVA having high solubility can be obtained, and further, coloring of the obtained AA-PVA can be suppressed. The mass ratio of the amide compound (c1) and the aliphatic carboxylic acid (c2) contained in the solvent (C) (amide compound (c1):aliphatic carboxylic acid (c2)) is preferably 50:50 to 99:1, more preferably 60:40 to 98.5:1.5, even more preferably 70:30 to 98:2, particularly preferably 80:20 to 97.5:2.5, and especially preferably 87.5:12.5 to 97:3, from the viewpoints of increasing the solubility of the AA-PVA and effectively suppressing coloration. If the amount of the amide compound (c1) is too small or the amount of the aliphatic carboxylic acid (c2) is too large, the degree of swelling tends to be low, which causes the product to become insoluble in water.

[0030] In addition to the above (c1) and (c2), the solvent (C) may contain other solvents such as water within the scope of not impairing the effects of the present invention. However, the total content of the amide compound (c1) and the aliphatic carboxylic acid (c2) in the total amount (100 mass%) of the solvent (C) is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 98 to 100 mass%.

[0031] The mass ratio (C / A) of the solvent (C) to the PVA (A) (hereinafter, this mass ratio may be referred to as the "bath ratio") is preferably 1 to 10, more preferably 2 to 9, even more preferably 3 to 8, and particularly preferably 4 to 6, from the viewpoint of stirring efficiency.

[0032] Examples of the amide compound (c1) include compounds having at least one amide group (solvents having an amide group).Specific examples of the amide compound include lactam compounds such as 2-pyrrolidone, N-methyl-2-pyrrolidone (NMP), N-methyl-2-piperidone, N-methylcaprolactam, N-acetylpyrrolidine, and N-ethyl-2-pyrrolidone; urea derivatives such as 1,3-dimethyl-2-imidazolidinone (DMI), tetramethylurea, N,N-dimethylethyleneurea, and N,N'-dimethylpropyleneurea (DMPU); and other amide compounds such as hexamethylphosphoramide, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N,N',N'-tetramethylmalonamide, N,N-diethylacetamide, N,N-dimethylpropionamide, N,N-dimethylisobutylamide, and N-methylformamide. These may be used alone as one type, or as two or more types in any combination and ratio.

[0033] The aliphatic carboxylic acid (c2) may be an organic acid having at least one carboxy group, specifically, formic acid, acetic acid, propionic acid, butyric acid, etc. These may be used alone or in any combination and ratio of two or more kinds.

[0034] Among these, a combination of at least one selected from the group consisting of 2-pyrrolidone, N-methyl-2-pyrrolidone (NMP), N-methyl-2-piperidone, N-methylcaprolactam, N-acetylpyrrolidine, and N-ethyl-2-pyrrolidone with at least one selected from the group consisting of formic acid, acetic acid, propionic acid, and butyric acid is preferred, and a combination of N-methyl-2-pyrrolidone (NMP) and acetic acid is more preferred.

[0035] Examples of the "other solvent" include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and diacetone alcohol; and nitrile solvents such as propanenitrile and acetonitrile.

[0036] This production method includes a step of subjecting PVA (A) to an ester exchange reaction with an acetoacetate (B) in the presence of a solvent (C) and a catalyst.

[0037] As the catalyst, for example, a Bronsted organic acid, a Bronsted inorganic acid, a Lewis inorganic acid, a Lewis organic base, or a combination thereof can be used. Specific examples of Bronsted organic acids include acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, benzoic acid, phthalic acid, gallic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, malic acid, citric acid, and aconitic acid; Bronsted inorganic acids include sulfuric acid, nitric acid, phosphoric acid, boric acid, hydrofluoric acid, hydrochloric acid, hydrobromic acid, hydroiodic acid, and partial esters thereof; Lewis inorganic acids include fatty acid metal salts such as sodium acetate, potassium acetate, magnesium acetate, calcium acetate, and zinc acetate, lithium triflate, magnesium triflate, zinc triflate, ytterbium triflate, bisacetylacetonate zinc, tetrakisacetylacetonate zirconium, tin dioctylate, and tetrabutoxytitanium; and Lewis organic bases include primary amines, secondary amines, tertiary amines, pyridine, primary phosphines, secondary phosphines, and tertiary phosphines. These may be used alone as one type, or as two or more types in any combination and ratio.

[0038] From the viewpoint of reaction rate, the catalyst is preferably a fatty acid metal salt contained in PVA(A), and more preferably sodium acetate contained in PVA(A). The content of the fatty acid metal salt (e.g., sodium acetate) contained in PVA(A) is, for example, 1.0 mass% or less of PVA(A) (total amount), preferably 0.01 to 1.0 mass%, more preferably 0.05 to 0.5 mass%, and even more preferably 0.1 to 0.3 mass%. The content of fatty acid metal salt contained in PVA (A) can be measured by a known method, for example, in accordance with JIS K 6726 (1994), 3.6.1, titration method.

[0039] When the catalyst is added separately, the amount of the catalyst added is usually 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of PVA (A). If the amount of the catalyst added is too large, it is not economically advantageous and tends to be difficult to remove the catalyst, which is undesirable.

[0040] The transesterification reaction in the present production method can be carried out according to a conventional method. However, from the viewpoint of increasing the reaction efficiency by swelling the PVA (A) and facilitating separation and washing of the reaction product after the reaction, it is preferable to carry out the transesterification reaction as a heterogeneous reaction in which the solid (powdered) PVA (A) is put into a solvent (C) and dispersed or stirred, while the acetoacetic ester (B) is added.

[0041] The reaction apparatus used in the transesterification reaction in the present production method may be any known reaction apparatus capable of mixing and heating, and may be a vertical or horizontal reactor. Specifically, a kneader, a Henschel mixer, a ribbon blender, or any other blender may be used.

[0042] In addition, the temperature at which the PVA (A) and the acetoacetate (B) are reacted in the reaction apparatus is not particularly limited, but the lower limit is preferably 60°C or higher, more preferably 70°C or higher, and particularly preferably 80°C or higher. If the temperature is 60°C or higher, the reaction rate tends to be high, which is preferable from the viewpoint of productivity. If the temperature is 60°C or higher, the upper limit is preferably 120°C or lower, more preferably 100°C or lower, and particularly preferably 95°C or lower. If the temperature is 120°C or lower, self-crosslinking between acetoacetyl groups tends to be easily suppressed, which is preferable.

[0043] The reaction time in the transesterification step is not particularly limited, but the lower limit is preferably 1 hour or more, more preferably 2 hours or more, and the upper limit is preferably 10 hours or less, more preferably 9 hours or less.

[0044] In the present production method, in the step of reacting PVA (A) with acetoacetate (B), acetoacetate (B) may be added all at once or dropwise. The drop time of acetoacetate (B) is optional and depends on the reaction scale and the capacity of the cooling equipment, but the lower limit is preferably 0.5 hours or more, more preferably 1 hour or more, and particularly preferably 2 hours or more. The upper limit is preferably 8 hours or less, more preferably 6 hours or less, and particularly preferably 5 hours or less. A drop time of 8 hours or less is preferable from the viewpoint of productivity.

[0045] After the transesterification reaction, the solvent is removed through a washing step in which washing is performed with a washing solvent of an alcohol having 1 to 3 carbon atoms, and a drying step. Specific examples of the alcohol having 1 to 3 carbon atoms used in the washing step include ethanol, methanol, and n-butyl alcohol. These can be used alone or in any combination and ratio of two or more. Among these, methanol is preferably used because it has a low boiling point and requires less energy for removal. The drying time in the drying step is appropriately selected in consideration of the temperature and pressure conditions, the mass of the object to be treated, etc., but is preferably set in the range of usually 0.5 to 10 hours. The temperature of the drying treatment is also appropriately selected, but is preferably set in the range of usually 20 to 80°C.

[0046] (AA PVA) In the manner described above, an AA-PVA is obtained by introducing an acetoacetyl group into the side chain of PVA (A). For example, the AA-PVA has a structural unit represented by the following formula (1), and in addition to the structural unit having an acetoacetyl group represented by formula (1), it has a vinyl alcohol structural unit and further a vinyl acetate structural unit which is an unsaponified portion.

[0047] [ka]

[0048] According to the present production method, a colorless, white powdery AA PVA can be obtained, and the AA PVA has excellent solubility. Therefore, according to the present production method, for example, when an aqueous solution of AA PVA is prepared, the occurrence of insoluble matters and the decrease in transparency can be suppressed.

[0049] Furthermore, the present production method can increase the AA conversion efficiency, and the AA conversion efficiency is, for example, 5 to 20 mol%, preferably 7.5 to 17.5 mol%, and more preferably 10 to 15 mol%. The AA conversion efficiency is calculated by the following formula. (formula) [AA degree of AA PVA (mol%) / Amount of acetoacetic ester charged (mol%)]×100

[0050] In particular, in the present production method, acetoacetylation can be performed in a heterogeneous system with a high liquid ratio (e.g., liquid ratio = 4 to 7) by using a small amount of acetoacetic ester (B) relative to PVA (A) (e.g., 200 parts by mass or less relative to 100 parts by mass of PVA (A)), and therefore the AA conversion efficiency of the obtained AA-PVA can be increased.

[0051] The degree of AA conversion of the AA-PVA obtained by the present production method can be appropriately set depending on the application, etc., and is, for example, 1 to 10 mol%, preferably 2 to 8 mol%, and more preferably 3 to 6 mol%. The degree of AA conversion can be determined by the method described in the Examples below.

[0052] Furthermore, in conventional methods for producing AA-PVA, when only N-methyl-2-pyrrolidone (NMP) or only acetic acid is used as the solvent, the bath ratio of the solvent to PVA must be kept low (for example, a bath ratio of about 1), and the slurry concentration is about 50 mass %. This means that the stirring efficiency is not improved in a general-purpose vertical reactor, and the reaction does not proceed, and uneven reaction progress occurs depending on the reaction position, making it necessary to carry out the reaction in a horizontal reactor such as a kneader. When a solvent (C) containing an amide compound (c1) and an aliphatic carboxylic acid (c2) is used as in the present production method, the bath ratio can be increased to, for example, 3 to 7, and the slurry concentration can be reduced to, for example, 25 mass% or less. This is also useful in that the reaction can be carried out evenly using a general-purpose vertical reactor which has few limitations in terms of equipment.

[0053] In the present production method, the slurry concentration is preferably 5 to 30 mass%, more preferably 7.5 to 25 mass%, and particularly preferably 10 to 20 mass%. The slurry concentration is calculated from the blended masses of each component according to the following formula: (Formula) Slurry concentration (%) = PVA (A) / (solvent (C) + acetoacetate (B)) x 100

[0054] Furthermore, according to the present production method, since it is not necessary to use diketene, it is possible to safely produce AA PVA.

[0055] The AA PVA obtained by the present production method can be used in the following applications (1) to (10), for example. (1) Molded products: fibers, films, sheets, pipes, tubes, leak-proof membranes, temporary coatings, chemical lace, water-soluble fibers, etc. (2) Adhesives: adhesives for wood, paper, aluminum foil, plastics, etc., pressure sensitive adhesives, rewetting agents, binders for nonwoven fabrics, binders for various building materials such as gypsum board and fiberboard, binders for various powder granulations, additives for cement and mortar, hot melt adhesives, pressure sensitive adhesives, fixing agents for anionic paints, etc. (3) Coating agents: clear coating agents for paper, pigment coating agents for paper, internal sizing agents for paper, sizing agents for textile products, warp size agents, textile processing agents, leather finishing agents, paints, anti-fogging agents, metal corrosion inhibitors, gloss agents for zinc plating, antistatic agents, conductive agents, temporary paints, etc. (4) Blending agents for hydrophobic resins: antistatic agents for hydrophobic resins, hydrophilic agents, additives for composite fibers, films and other molded products, etc. (5) Suspension and dispersion stabilizers: Pigment dispersion stabilizers for paints, ink, water-based colors, adhesives, etc.; dispersion stabilizers for suspension polymerization of various vinyl compounds such as vinyl chloride, vinylidene chloride, styrene, (meth)acrylates, and vinyl acetate, etc. (6) Emulsion dispersion stabilizers: emulsifiers for emulsion polymerization of various acrylic monomers, ethylenically unsaturated compounds, butadiene compounds, post-emulsifiers for hydrophobic resins such as polyolefins and polyester resins, epoxy resins, paraffin, bitumen, etc. (7) Thickeners: Thickeners for various aqueous solutions, emulsions, and oil drilling fluids, etc. (8) Flocculants: Flocculants for suspended and dissolved matter in water, drainage of pulp and slurry, etc. (9) Exchange resins, etc.: ion exchange resins, chelating exchange resins, ion exchange membranes, etc. (10) Others: soil conditioners, photosensitizers, photosensitive resist resins, etc. EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples and comparative examples. Note that the following examples are presented to explain the present invention in detail, and the present invention is not limited to the following examples unless it is contrary to the gist of the present invention. Note that in the examples, "parts" refers to mass standards.

[0057] Example 1 A test tube containing a mixture containing 100 parts of raw material PVA (saponification degree 99.1 mol%, viscosity of 4 mass% aqueous solution at 20℃ 13.3 mPa·s, average polymerization degree 1200, sodium acetate content 0.1 mass%), 270 parts of N-methyl-2-pyrrolidone (NMP), 30 parts of acetic acid, and 107 parts of t-butyl acetoacetate (t-BAA) was placed in a thermostatic bath (aluminum block bath, Tokyo Rikakikai Co., Ltd., ChemStation) set at 90℃, and a rotor (magnetic stirrer) was placed in the test tube to heat and stir (rotation speed 200 rpm). After 7 hours had passed since the internal temperature of the test tube reached 87℃, the test tube was removed from the thermostatic bath and cooled with water to terminate the reaction. The obtained slurry was subjected to solid-liquid separation, washed with methanol, and then dried under vacuum at 40°C for 3 hours to obtain powdered AA PVA (average polymerization degree 1200, AA degree 2.41 mol%, AA efficiency 8.02 mol%).

[0058] [Coloring evaluation] The appearance of the resulting AA PVA was visually observed and evaluated according to the following criteria, and the results are shown in Table 1. (Evaluation Criteria) ◯: No coloring, white powder. ×: Colored, yellow powder or mochi-like.

[0059] [Solubility evaluation] 30 mg of AA-PVA was placed in a test tube containing 1 mL of DMSO-d6 (dimethyl sulfoxide-D6), and the test tube was placed in a thermostatic bath (aluminum block bath, Tokyo Rikakikai Co., Ltd., Chemstation) set to 60°C. A rotor (magnetic stirrer) was placed in the test tube, and the mixture was heated and stirred for 1 hour (rotation speed 200 rpm) to obtain a solution. The resulting solution was visually observed and evaluated according to the following criteria, and the results are shown in Table 1. (Evaluation Criteria) ◯: The solution did not gel. ×: The solution gelled.

[0060] The methods for measuring the degree of AA (mol %) and the AA efficiency (mol %) of the obtained AA PVA are as follows.

[0061] [Measurement of AA content] The degree of AA of each AA-PVA was measured using a nuclear magnetic resonance spectrometer "Ascend 400 (400 MHz), AVANCE III 400, Cryo-probe" manufactured by Bruker. Specifically, each AA-PVA was dissolved in DMSO-d6 (dimethyl sulfoxide-D6) (concentration 4%) and measured under the conditions of 16 cumulative cycles at 50°C. 1 The degree of AA conversion (mol%) was calculated from the ratio of the peak area derived from the acetoacetyl group appearing at 2.2 ppm in H-NMR to the peak area derived from the CH2 unit of PVA.

[0062] [Calculation of AA efficiency] Based on the degree of AA (mol %) of the AA PVA and the amount of acetoacetic ester charged (mol %), the AA efficiency (mol %) was calculated by the following formula. (Formula) [AA degree of AA PVA (mol%) / Amount of acetoacetic ester charged (mol%)]×100

[0063] Example 2 A powdered AA-PVA (average polymerization degree 1200, AA degree 3.1 mol%, AA efficiency 10.33 mol%) was obtained in the same manner as in Example 1, except that 450 parts of N-methyl-2-pyrrolidone (NMP) and 50 parts of acetic acid were used. The coloring and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0064] Example 3 A powdered AA-PVA (average polymerization degree 1200, AA degree 2.53 mol%, AA efficiency 8.42 mol%) was obtained in the same manner as in Example 1, except that 630 parts of N-methyl-2-pyrrolidone (NMP) and 70 parts of acetic acid were used. The coloring and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0065] Example 4 A powdered AA-PVA (average polymerization degree 1200, AA degree 2.47 mol%, AA efficiency 5.48 mol%) was obtained in the same manner as in Example 1, except that 270 parts of N-methyl-2-pyrrolidone (NMP), 30 parts of acetic acid, and 160.5 parts of t-butyl acetoacetate (t-BAA) were used. Coloration and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0066] Example 5 A powdered AA-PVA (average polymerization degree 1200, AA degree 4.06 mol%, AA efficiency 9.03 mol%) was obtained in the same manner as in Example 1, except that 450 parts of N-methyl-2-pyrrolidone (NMP), 50 parts of acetic acid, and 160.5 parts of t-butyl acetoacetate (t-BAA) were used. Coloration and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0067] Example 6 A powdered AA-PVA (average polymerization degree 1200, AA degree 2.87 mol%, AA efficiency 6.37 mol%) was obtained in the same manner as in Example 1, except that 630 parts of N-methyl-2-pyrrolidone (NMP), 70 parts of acetic acid, and 160.5 parts of t-butyl acetoacetate (t-BAA) were used. Coloration and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0068] Example 7 A powdered AA-PVA (average polymerization degree 1200, AA degree 4.24 mol%, AA efficiency 7.06 mol%) was obtained in the same manner as in Example 1, except that 450 parts of N-methyl-2-pyrrolidone (NMP), 50 parts of acetic acid, and 214 parts of t-butyl acetoacetate (t-BAA) were used. Coloration and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0069] Example 8 A powdered AA-PVA (average polymerization degree 1200, AA degree 4.09 mol%, AA efficiency 13.64 mol%) was obtained in the same manner as in Example 1, except that 475 parts of N-methyl-2-pyrrolidone (NMP), 25 parts of acetic acid, and 107 parts of t-butyl acetoacetate (t-BAA) were used. The coloring and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0070] Example 9 A powdered AA-PVA (average polymerization degree 1200, AA degree 5.58 mol%, AA efficiency 12.4 mol%) was obtained in the same manner as in Example 1, except that 475 parts of N-methyl-2-pyrrolidone (NMP), 25 parts of acetic acid, and 160.5 parts of t-butyl acetoacetate (t-BAA) were used. Coloration and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0071] Example 10 A powdered AA-PVA (average polymerization degree 1200, AA degree 2.08 mol%, AA efficiency 4.62 mol%) was obtained in the same manner as in Example 1, except that 425 parts of N-methyl-2-pyrrolidone (NMP), 75 parts of acetic acid, and 160.5 parts of t-butyl acetoacetate (t-BAA) were used. Coloration and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0072] Comparative Example 1 100 parts of raw material PVA (saponification degree 99.1 mol%, viscosity of 4 mass% aqueous solution 13.3 mPa·s, average polymerization degree 1200, sodium acetate content 0.4 mass%) was charged into a kneader heated to 90°C, and 100 parts of N-methyl-2-pyrrolidone (NMP) was added dropwise over 1 hour, followed by swelling. Then, 71 parts of t-butyl acetoacetate (t-BAA) was added dropwise over 3 hours, and the reaction was allowed to proceed for another 4 hours. After the reaction was completed, the mixture was washed with methanol and dried under vacuum at 40°C to obtain powdered AA-PVA (average polymerization degree 1200, AA degree 4.7 mol%, AA efficiency 28.5 mol%). Coloration and solubility were evaluated by the same method as above. The results are shown in Table 1.

[0073] Comparative Example 2 560 parts of N-methyl-2-pyrrolidone (NMP), 240 parts of t-butyl acetoacetate (t-BAA), and 100 parts of raw material PVA (saponification degree 99.1 mol%, viscosity of 4 mass% aqueous solution 13.3 mPa·s, average polymerization degree 1200, sodium acetate content 0.4 mass%) were charged when the internal temperature of the test tube reached 90°C. Powdered AA-PVA (average polymerization degree 1200, AA degree 6.6 mol%, AA efficiency 9.8 mol%) was obtained in the same manner as in Example 1, except that the test tube was removed from the thermostatic bath after 4 hours had elapsed. Coloration and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0074] Comparative Example 3 100 parts of raw material PVA (saponification degree 99.1 mol%, viscosity of 4 mass% aqueous solution 13.3 mPa s, average polymerization degree 1200, sodium acetate content 0.4 mass%) was charged into a kneader heated to 90°C, and 100 parts of acetic acid was added dropwise thereto over 1 hour, followed by swelling. Then, 71 parts of t-butyl acetoacetate (t-BAA) was added dropwise over 3 hours, and the reaction was allowed to proceed for a further 7 hours. After the reaction was completed, the product was washed with methanol and dried under vacuum at 40°C to obtain a powdered AA-PVA (AA degree 2.7 mol%, AA efficiency 13.5 mol%). Coloration and solubility were evaluated in the same manner as above. The results are shown in Table 1.

[0075] Comparative Example 4 A test tube containing 100 parts of raw material PVA (saponification degree 99.1 mol%, viscosity of 4 mass% aqueous solution at 20℃ 13.3 mPa·s, average polymerization degree 1200, sodium acetate content 0.1 mass%), 500 parts of N-methyl-2-pyrrolidone (NMP), and 107 parts of t-butyl acetoacetate (t-BAA) was placed in a thermostatic bath (aluminum block bath, Tokyo Rikakikai Co., Ltd., ChemStation) set at 90℃, and a rotor (magnetic stirrer) was placed in the test tube to heat and stir (rotation speed 200 rpm). After 7 hours had passed since the internal temperature of the test tube reached 87℃, the test tube was removed from the thermostatic bath and cooled with water to terminate the reaction. Methanol was added to the gel solution obtained, and the solid matter was precipitated and separated into solid and liquid. After washing with methanol, the solid matter was dried under vacuum at 40°C for 3 hours to obtain a rice cake-like AA PVA (average polymerization degree 1200, AA degree 10.17 mol%, AA efficiency 33.9 mol%). The coloring and solubility were evaluated by the same method as above. The results are shown in Table 1.

[0076] Comparative Example 5 A test tube containing 100 parts of raw material PVA (saponification degree 99.1 mol%, viscosity of 4 mass% aqueous solution at 20℃ 13.3 mPa·s, average polymerization degree 1200, sodium acetate content 0.1 mass%), 500 parts of acetic acid, and 107 parts of t-butyl acetoacetate (t-BAA) was placed in a thermostatic bath (aluminum block bath, Tokyo Rikakikai Co., Ltd., ChemStation) set at 90℃, and a rotor (magnetic stirrer) was placed in the test tube and heated and stirred (rotation speed 200 rpm). After 7 hours had elapsed since the internal temperature of the test tube reached 87℃, the test tube was removed from the thermostatic bath and cooled with water to terminate the reaction. The obtained slurry was separated into solid and liquid, washed with methanol, and then dried under vacuum at 40℃ for 3 hours to obtain powdered AA-PVA (average polymerization degree 1200, AA degree 2.84 mol%, AA efficiency 9.5 mol%). The coloration and solubility were evaluated in the same manner as above, and the results are shown in Table 1.

[0077] [Table 1]

[0078] As shown in Table 1, in Examples 1 to 10, in which a mixed solvent containing an amide compound (c1) and an aliphatic carboxylic acid (c2) was used, it was confirmed that an AA-PVA having excellent solubility and suppressed coloration was obtained. On the other hand, in Comparative Examples 1 to 5 in which either the amide compound (c1) or the aliphatic carboxylic acid (c2) was used as the solvent, it was confirmed that the solubility was poor or coloring occurred.

[0079] Moreover, in Examples 1 to 10, powdery AA PVA was obtained that had excellent solubility and was suppressed from coloring. On the other hand, in Comparative Example 4, coloring occurred, and mochi-like AA PVA was obtained. There are concerns that mochi-like AA PVA may require an additional precipitation step in the production process or that the bulk density may decrease, resulting in, for example, packaging bags that are larger than necessary. However, Examples 1 to 10 are excellent in that they do not have such concerns.

[0080] From the above results, it was confirmed that the production method of the present invention can provide AA PVA which is excellent in solubility and suppressed in coloration. [Industrial Applicability]

[0081] The AA PVA obtained by the production method of the present invention is of high quality and is suitably used for various applications, such as various molding materials, various adhesive materials, coating materials, blending agents for hydrophobic resins, suspension dispersion stabilizers, emulsion dispersion stabilizers, thickeners, flocculants, and exchange resins.

Claims

1. A method for producing a polyvinyl alcohol-based resin containing an acetoacetate group, comprising reacting a polyvinyl alcohol-based resin (A) with an acetoacetate ester (B) in the presence of a solvent (C) containing an amide compound (c1) and an aliphatic carboxylic acid (c2).

2. The method for producing an acetoacetate group-containing polyvinyl alcohol resin according to claim 1, wherein the mass ratio (c1:c2) of the amide compound (c1) to the aliphatic carboxylic acid (c2) is 50:50 to 99:

1.

3. The method for producing an acetoacetate group-containing polyvinyl alcohol-based resin according to claim 1 or 2, wherein a mass ratio (C / A) of the solvent (C) to the polyvinyl alcohol-based resin (A) is 1 to 10.

4. The method for producing an acetoacetate group-containing polyvinyl alcohol-based resin according to claim 1 or 2, wherein the mass ratio (C / A) of the solvent (C) to the polyvinyl alcohol-based resin (A) is 2.5 to 8.

5. The method for producing an acetoacetate group-containing polyvinyl alcohol-based resin according to claim 1 or 2, wherein the amount of the acetoacetate (B) is 50 to 250 parts by mass per 100 parts by mass of the polyvinyl alcohol-based resin (A).

6. 3. The method for producing an acetoacetate group-containing polyvinyl alcohol resin according to claim 1, wherein the polyvinyl alcohol resin (A) is a polyvinyl alcohol resin containing a fatty acid metal salt, and the content of the fatty acid metal salt is 1.0 mass% or less.

Citation Information

Patent Citations

  • Production of modified cement molded body

    JP1997157069A

  • Acetoacetate group-containing polyvinyl alcohol resin composition, rapidly curable adhesive, and method of adhesion

    JP1997291185A

  • Polyvinyl alcohol resin composition

    JP2005120115A

  • Method of producing acetoacetyl group-containing polyvinyl alcohol resin

    JP2015124261A

  • High alcohol tolerant copolymers and terpolymers based on polyvinyl alcohols

    JP2020079409A

Cited By

  • Hydrolysis-resistant acetoacetamido modified polyvinyl alcohol and preparation method thereof

    CN119529145A

  • Acetylated polyvinyl alcohol modified resin as well as preparation method and application thereof

    CN121159743A

  • An acetoacetylated polyvinyl alcohol modified resin, a preparation method and application thereof

    CN121159743B