Negative electrode protective film and battery

A copolymer-based negative electrode protective film for lithium ion batteries addresses dendrite issues by enhancing ionic conductivity and Coulombic efficiency, improving battery performance.

JP2024146091APending Publication Date: 2024-10-15LINTEC CORP

Patent Information

Application Number
JP2023058805
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing lithium ion secondary batteries face issues with dendrite formation on the negative electrode, leading to potential short circuits, and require improved protective films that enhance ionic conductivity and Coulombic efficiency.

Method used

A negative electrode protective film containing a specific copolymer with structural units represented by general formulas (1) and (2), and optionally (3) and (4), which allows for improved compatibility with electrolyte solutions, suppressing dendrite growth and enhancing ionic conductivity and Coulombic efficiency.

Benefits of technology

The protective film effectively suppresses dendrite formation and improves ionic conductivity and Coulombic efficiency, resulting in better battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146091000001_ABST
    Figure 2024146091000001_ABST
Patent Text Reader

Abstract

To provide a negative electrode protective film which suppresses generation of dendrites and is improved in ion conductivity and coulombic efficiency.SOLUTION: A negative electrode protective film 11 covering at least a part of a negative electrode 13 contains a copolymer containing a constituent unit represented by the following general formula (1) and 0.3 mol% or more and 20 mol% or less of a constituent unit represented by the following general formula (2). (In general formula (1) and general formula (2), R1 represents a hydrogen atom or a C1-3 alkyl group; L1 and L2 each independently represent a single bond or a C1-3 alkylene group; and L3 represents a single bond, a C1-5 alkylene group or a C1-5 oxyalkylene group.)SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a negative electrode protective film and a battery. [Background technology]

[0002] As one type of high-performance battery, secondary batteries using lithium ions or the like have attracted attention. A secondary battery using lithium ions or the like includes, for example, a positive electrode, a negative electrode, an electrolyte, and a separator disposed between the positive electrode and the negative electrode. Various materials for use in such secondary batteries have been studied.

[0003] Patent Document 1 discloses a lithium metal battery including a positive electrode, a lithium negative electrode, and a liquid electrolyte interposed therebetween, and a protective film disposed on at least a portion of the lithium negative electrode, the protective film including one or more first polymers selected from polyvinyl alcohol and polyvinyl alcohol blends. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2016-219411 Summary of the Invention [Problem to be solved by the invention]

[0005] The protective film disclosed in Patent Document 1 is formed by directly coating a protective film containing polyvinyl alcohol on lithium metal. Because metallic lithium reacts with moisture in the air, all steps for forming the protective film are performed in a dry environment. For this reason, the steps for forming the protective film disclosed in Patent Document 2 are complicated.

[0006] Meanwhile, lithium ion secondary batteries are being required to have even higher performance. For example, when a lithium negative electrode is used as the negative electrode of a lithium ion secondary battery, it is possible to increase the energy density of the battery. However, when a lithium negative electrode is used as the negative electrode, dendrites may be formed on the surface of the lithium negative electrode. When dendrites are formed and grow, they may eventually cause a short circuit in the lithium ion secondary battery. For this reason, further improvement is being required in the protective layer for protecting the negative electrode.

[0007] An object of the present invention is to provide an anode protective film that suppresses the generation of dendrites and has improved ionic conductivity and coulombic efficiency, and a battery that includes the anode protective film. [Means for solving the problem]

[0008] [1] A negative electrode protective film that covers at least a portion of a negative electrode, The copolymer contains a structural unit represented by the following general formula (1) and 0.3 mol % or more and 20.0 mol % or less of a structural unit represented by the following general formula (2): Negative electrode protective film.

[0009] [ka]

[0010] (In the general formula (1) and the general formula (2), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and L 1 and L 2 are each independently a single bond or an alkylene group having 1 to 3 carbon atoms, and L 3 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms, and X 1 is any one of the reactive groups represented by the following structural formula (2-1), (2-2), and (2-3).

[0011] [ka]

[0012] [2] The anode protective film according to [1], -L in the general formula (2) 3 -X 1 is any reactive group selected from the groups represented by the following structural formula (2-4), the following structural formula (2-5), and the following structural formula (2-6), Negative electrode protective film.

[0013] [ka]

[0014] [3] The anode protective film according to [1] or [2], The copolymer further contains 0.1 mol% to 30.0 mol% of at least one structural unit selected from the group consisting of structural units represented by the following general formula (3) and structural units represented by the following general formula (4): Negative electrode protective film.

[0015] [ka]

[0016] (In the general formula (3) and the general formula (4), R 2 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and L 4 and L 5 are each independently a single bond or an alkylene group having 1 to 3 carbon atoms, and L 6 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms, and X 2 is any one of the reactive groups represented by the following structural formula (4-1), (4-2), and (4-3).

[0017] [ka]

[0018] [4] The anode protective film according to any one of [1] to [3], the amount of the copolymer eluted in ethyl acetate is 10% or less; the degree of swelling of the copolymer in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is 100% or more; Negative electrode protective film.

[0019] [5] The anode protective film according to any one of [1] to [4], the anode protective film further contains an electrolyte solution, the electrolyte solution contains a carbonate-based solvent and a lithium salt, the molar ratio of the lithium salt to the carbonate-based solvent (the lithium salt / the carbonate-based solvent) is 1 / 6 or more and 1 / 1 or less; Negative electrode protective film.

[0020] [6] The anode protective film according to any one of [1] to [5], The negative electrode is a lithium negative electrode. Negative electrode protective film.

[0021] [7] The anode protective film according to any one of [1] to [6], battery. [Effects of the Invention]

[0022] According to one aspect of the present invention, it is possible to provide an anode protective film that suppresses the generation of dendrites and has improved ionic conductivity and Coulombic efficiency, and a battery that includes the anode protective film. [Brief explanation of the drawings]

[0023] [Figure 1] FIG. 1 is a cross-sectional view schematically illustrating an example in which the anode protective film according to the present embodiment is used. [Figure 2] 1 is a cross-sectional view schematically illustrating an example of a main part of a battery according to an embodiment of the present invention. [Figure 3] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 1. [Figure 4] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 3. [Figure 5] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 6. DETAILED DESCRIPTION OF THE INVENTION

[0024] The present invention will be described below by taking an embodiment as an example, but the present invention is not limited to the content of the embodiment.

[0025] [Negative electrode protective film] A preferred example of the negative electrode protective film according to this embodiment will be described.

[0026] The anode protective film according to this embodiment covers at least a portion of the anode, and includes a copolymer containing a structural unit represented by general formula (1) and 0.3 mol % to 20.0 mol % of a structural unit represented by general formula (2).

[0027] The anode protective film according to this embodiment has the above-described structure, which suppresses dendrite formation and provides an anode protective film with improved ionic conductivity and Coulombic efficiency. Coulombic efficiency is expressed as the ratio of the electrical capacity during discharge to the electrical capacity during charge. The reasons for the improved ionic conductivity and Coulombic efficiency are unclear, but are thought to be as follows. The copolymer used in the anode protective film according to this embodiment has a carbonate skeleton as the main polymer backbone, which improves compatibility with the electrolyte. Therefore, during battery assembly, the thin film serving as the anode protective film swells after the electrolyte is injected, thereby exhibiting ionic conductivity. Furthermore, by including 0.3 mol % or more and 20.0 mol % or less of a structural unit represented by general formula (2) having a reactive group, the crosslinking reaction proceeds appropriately, thereby achieving both a high degree of swelling and a low amount of elution. As a result, the anode protective film according to this embodiment is presumed to suppress dendrite formation and provide improved ionic conductivity and Coulombic efficiency. Furthermore, a battery using the anode protective film according to this embodiment suppresses the generation of dendrites and improves ionic conductivity and coulomb efficiency, thereby achieving excellent battery characteristics.

[0028] Furthermore, with the anode protective film according to this embodiment, even if the anode is a lithium anode, it is possible to easily provide a protective layer that covers the anode. Because the anode protective film according to this embodiment contains the specific copolymer having the above-described structure, it is possible to form a thin film by film formation in the atmosphere without maintaining a dry environment. Therefore, when assembling a battery, it is possible to inject an electrolyte after providing a thin film as a protective film on the surface of the anode. Therefore, by using the anode protective film according to this embodiment, it is possible to easily provide a protective layer that covers the anode.

[0029] The anode protective film according to this embodiment may contain other components as long as it contains the specific copolymer having the above-described structure, as long as the object of the present invention is not impaired.

[0030] The form of the anode protective film according to this embodiment is not particularly limited. From the viewpoint of easily providing the anode protective film on the anode, the form of the anode protective film according to this embodiment is preferably a thin film containing a specific copolymer having the above-described structure. The thin film containing this copolymer is preferably a free-standing film. The free-standing film of the thin film containing this copolymer refers to a film that can be self-supported by itself.

[0031] (copolymer) The copolymer contained in the anode protective film according to this embodiment includes a copolymer containing a constitutional unit represented by the following general formula (1) and 0.3 mol % or more and 20.0 mol % or less of a constitutional unit represented by the following general formula (2):

[0032] [ka]

[0033] In the general formula (1) and the general formula (2), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, preferably a hydrogen atom or a methyl group, and particularly preferably a methyl group. L 1 and L 2 are each independently a single bond or an alkylene group having 1 to 3 carbon atoms, preferably a methylene group or an ethylene group, and particularly preferably a methylene group. L 3 represents a single bond, an alkylene group having from 1 to 5 carbon atoms, or an oxyalkylene group having from 1 to 5 carbon atoms, preferably a single bond or an oxyalkylene group having from 1 to 5 carbon atoms, and particularly preferably a single bond or an oxyalkylene group having from 2 to 4 carbon atoms. X 1 is any reactive group among groups represented by the following structural formula (2-1), (2-2), and (2-3): The wavy line in the structural formula indicates a bonding position.

[0034] [ka]

[0035] From the viewpoint of ease of synthesis, -L in general formula (2) 3 -X 1 is preferably any one of the reactive groups represented by the following structural formula (2-4), (2-5), and (2-6): In the structural formula, the wavy line indicates the bonding position.

[0036] [ka]

[0037] Such a copolymer may be a random copolymer or a block copolymer, but from the viewpoint of ease of synthesis, the copolymer is preferably a random copolymer.

[0038] The copolymer contained in the anode protective film according to this embodiment has the following composition ratio, for example, when the copolymer is composed of a constitutional unit represented by general formula (1) and a constitutional unit represented by general formula (2). The ratio of the structural unit represented by general formula (2) must be 0.3 mol% or more and 20.0 mol% or less relative to all structural units. If this ratio is less than 0.3 mol%, the amount of elution increases and the Coulomb efficiency decreases. On the other hand, if this ratio exceeds 20.0 mol%, the crosslink density of the copolymer increases, resulting in problems such as reduced swelling properties. From the same viewpoint, the ratio of the structural unit represented by general formula (2) is preferably 1 mol% or more, more preferably 1.5 mol% or more, and even more preferably 1.8 mol% or more. On the other hand, the ratio of the structural unit represented by general formula (2) is preferably 19.0 mol% or less, more preferably 18.0 mol% or less, even more preferably 12.0 mol% or less, and particularly preferably 6.0 mol% or less.

[0039] The ratio of the structural units represented by general formula (1) must be 80.0 mol% or more and 99.7 mol% or less relative to all structural units. Furthermore, the ratio of the structural units represented by general formula (1) is preferably 81.0 mol% or more, more preferably 82.0 mol% or more, even more preferably 88.0 mol% or more, and particularly preferably 94.0 mol% or more. Meanwhile, the ratio of the structural units represented by general formula (1) is preferably 99.0 mol% or less, more preferably 98.5 mol% or less, and even more preferably 98.2 mol% or less.

[0040] The copolymer contained in the anode protective film according to this embodiment preferably further contains 0.1 mol % to 30.0 mol % of at least one structural unit selected from the group consisting of structural units represented by the following general formula (3) and structural units represented by the following general formula (4): By using a copolymer containing an ether skeleton such as the structural unit represented by general formula (3) or (4), the glass transition temperature of the copolymer is lowered and the thin film becomes flexible, which is expected to result in high ionic conductivity.

[0041] [ka]

[0042] In the general formula (3) and the general formula (4), R 2 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, preferably a hydrogen atom or a methyl group, and particularly preferably a methyl group. L 4 and L 5 are each independently a single bond or an alkylene group having 1 to 3 carbon atoms, preferably a methylene group or an ethylene group, and particularly preferably a methylene group. L 6represents a single bond, an alkylene group having from 1 to 5 carbon atoms, or an oxyalkylene group having from 1 to 5 carbon atoms, preferably a single bond or an oxyalkylene group having from 1 to 5 carbon atoms, and particularly preferably a single bond or an oxyalkylene group having from 2 to 4 carbon atoms. X 2 is any reactive group among groups represented by the following structural formula (4-1), (4-2), and (4-3): The wavy line in the structural formula indicates a bonding position.

[0043] [ka]

[0044] From the viewpoint of ease of synthesis, -L in general formula (4) 6 -X 2 is preferably any one of the reactive groups represented by the following structural formula (4-4), (4-5), and (4-6): The wavy line in the structural formula indicates the bonding position.

[0045] [ka]

[0046] The copolymer contained in the anode protective film according to this embodiment has the following composition ratio, for example, in the case of a copolymer consisting of a constituent unit represented by general formula (1), a constituent unit represented by general formula (2), a constituent unit represented by general formula (3), and a constituent unit represented by general formula (4). The ratio of the constitutional units represented by general formula (2) is as described above. The total ratio of the structural units represented by general formula (3) and the structural units represented by general formula (4) is preferably 0.1 mol% or more and 30.0 mol% or less relative to all structural units. If the total ratio is less than 0.1 mol%, the effect of the ether skeleton tends to be insufficient. On the other hand, if the total ratio exceeds 30.0 mol%, the compatibility with the electrolyte solution tends to deteriorate, the degree of swelling tends to decrease, and the ionic conductivity tends to decrease. From the same viewpoint, the total ratio of these is preferably 0.2 mol% or more, more preferably 0.6 mol% or more, while the total ratio of these is preferably 25.0 mol% or less, more preferably 20.0 mol% or less, and particularly preferably 10.0 mol% or less.

[0047] The ratio of the structural units represented by general formula (1) is preferably 50.0 mol% or more and 99.6 mol% or less relative to all structural units. Furthermore, the ratio of the structural units represented by general formula (1) is preferably 55.0 mol% or more, more preferably 60.0 mol% or more. On the other hand, the ratio of the structural units represented by general formula (1) is preferably 98.0 mol% or less, more preferably 94.0 mol% or less.

[0048] The molecular weight of the copolymer according to this embodiment, measured by the method shown in the measurement examples, is preferably 5,000 or more and 5,000,000 or less, and more preferably 10,000 or more and 1,000,000 or less, when expressed as a weight average molecular weight (Mw). Furthermore, the molecular weight of the copolymer according to this embodiment, measured by the method shown in the measurement example, is preferably 3,000 or more and 3,000,000 or less, and more preferably 5,000 or more and 500,000 or less, when expressed as a number average molecular weight (Mn). The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is preferably from 1 to 10, more preferably from 1.1 to 5. When the molecular weight and molecular weight distribution of the copolymer are within the above ranges, sufficient handleability can be achieved when the copolymer is formed into a film.

[0049] (Method of producing copolymer) The method for producing the copolymer contained in the negative electrode protective film according to this embodiment is not particularly limited, and the copolymer can be obtained by a known method, for example, the following method. As described in the Examples below, it can be produced by copolymerizing an epoxide monomer such as propylene oxide with carbon dioxide in the presence of a polymerization catalyst. Specifically, propylene oxide undergoes ring-opening to form a structural unit represented by general formula (3), and a portion of the propylene oxide undergoes ring-opening polymerization with carbon dioxide to form a structural unit represented by general formula (1).

[0050] The polymerization catalyst used in producing the copolymer is not particularly limited, and examples thereof include metal salen complex catalysts such as cobalt salen complex catalysts; and organozinc catalysts.

[0051] The amount of the polymerization catalyst used in the copolymerization reaction of the epoxide monomer with carbon dioxide, for example, in the case of a metal-salen complex catalyst, is preferably 0.05 mol or less, more preferably 0.01 mol or less, and particularly preferably 0.001 mol or less, per 1 mol of the epoxide monomer. Furthermore, when using a metal-salen complex catalyst, a co-catalyst can be used. For example, an onium salt compound is preferable as the co-catalyst. Specific examples of the onium salt compound are not particularly limited, but from the viewpoint of high reaction activity, bis(triphenylphosphoranylidene)ammonium chloride, piperidine, bis(triphenylphosphoranylidene)ammonium fluoride, ammonium pentafluorobenzoate, and tetra-n-butylammonium chloride are preferable.

[0052] The optimum polymerization conditions vary depending on the type of catalyst, but for example, the carbon dioxide pressure in the reaction vessel is 0.1 MPa or more and 10 MPa or less, preferably 0.5 MPa or more and 5 MPa or less. Furthermore, in the case of a cobalt salen complex catalyst, the polymerization temperature is preferably about room temperature (25° C.) from the viewpoint that the catalytic action works well and the reaction rate is accelerated.

[0053] In the method of copolymerizing an epoxide monomer with carbon dioxide, examples of the epoxide monomer used as a starting material include ethylene oxide, propylene oxide, 1,2-butylene oxide, allyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, and 4-hydroxybutyl acrylate glycidyl ether. Note that, due to differences in reactivity, the molar ratio of the constituent unit represented by general formula (1) to the constituent unit represented by general formula (2) in the copolymer may not match the molar mixing ratio of the epoxide monomer serving as the starting material for the constituent unit represented by general formula (1) and the epoxide monomer serving as the starting material for the constituent unit represented by general formula (2).

[0054] (Characteristics of the negative electrode protective film) In the anode protective film according to this embodiment, the amount of copolymer eluted in ethyl acetate is preferably 40% or less, more preferably 30% or less, even more preferably 20% or less, particularly preferably 10% or less, and most preferably 7% or less. Since the eluted low-molecular-weight components of the copolymer constitute irreversible capacity, it is desirable that the amount of elution be as low as possible. The lower limit of the amount of copolymer elution is not particularly limited and may be, for example, 1% or more, 0.1% or more, or even 0%.

[0055] In the negative electrode protective film according to this embodiment, it is preferable that the amount of elution of the copolymer with respect to ethyl acetate is within the above range, and that the degree of swelling of the copolymer with respect to a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is 100% or more.

[0056] When used in a lithium-ion secondary battery, for example, a thin film prepared using the copolymer does not exhibit ionic conductivity because it does not contain lithium ions before an electrolyte solution containing lithium ions is injected. When an electrolyte solution containing lithium ions is injected into a thin film containing the copolymer, the thin film containing the copolymer swells. The thin film swollen by the electrolyte exhibits ionic conductivity. Therefore, in the anode protective film according to this embodiment, the anode protective film preferably further contains an electrolyte in addition to the thin film containing the copolymer. To improve the performance of a battery using a thin film containing the copolymer as the anode protective film, high ionic conductivity of the thin film is preferred. From this perspective, it is preferable for the thin film to have high swelling properties in the electrolyte and carbonate-based solvents used as the solvent for the electrolyte. The degree of swelling of the copolymer in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is preferably 100% or more, more preferably 200% or more, even more preferably 300% by mass or more, particularly preferably 500% or more, very preferably 700% or more, and most preferably 900% or more. The upper limit of the swelling degree is not particularly limited, and may be, for example, 2000% or less.

[0057] When an electrolyte solution is contained in a thin film containing a copolymer, the electrolyte solution preferably contains a carbonate-based solvent and a lithium salt, and the molar ratio of the lithium salt to the carbonate-based solvent (the lithium salt / the carbonate-based solvent) is 1 / 6 or more and 1 / 1 or less. An electrolyte solution having a concentration where the molar ratio of the lithium salt to the carbonate-based solvent is 1 / 6 or more and 1 / 1 or less has a higher concentration than that of a general electrolyte solution. Use of such an electrolyte solution tends to make the dissolution and deposition of lithium uniform and improve the effect of suppressing the generation of dendrites.

[0058] From the viewpoint of film strength, the thickness of the anode protective film according to this embodiment is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more. From the viewpoint of reducing the resistance of the film, the thickness of the anode protective film according to this embodiment is preferably 20 μm or less, more preferably 16 μm or less, and even more preferably 12 μm or less.

[0059] (Method of manufacturing the negative electrode protective film) The anode protective film according to this embodiment preferably uses a photopolymerization initiator, from the viewpoint of facilitating the formation of a thin film (i.e., a thin film containing a copolymer) as the anode protective film. When a photopolymerization initiator is used in the anode protective film according to this embodiment, reactive groups (allyl groups and (meth)acryloyl groups) in the side chains of the copolymer in the thin film react to crosslink the thin film containing the copolymer.

[0060] An example of a preferred method for producing the anode protective film according to this embodiment will be described.

[0061] The method for producing the anode protective film according to this embodiment includes the following steps. A step of mixing the copolymer and a photopolymerization initiator to prepare a mixture (step 1). A step of molding the mixture to obtain a molded product (step 2). Step 3 is a step of irradiating the molded product with energy rays to obtain an anode protective film containing the copolymer. "Energy rays" refers to electromagnetic waves or charged particle rays that have an energy quantum. Examples of energy rays include ultraviolet rays, radioactive rays, and electron beams. Ultraviolet rays can be irradiated using an electrodeless lamp, a high-pressure mercury lamp, a metal halide lamp, a xenon lamp, a black light, an LED lamp, or the like. Electron beams generated by an electron beam accelerator or the like can be irradiated.

[0062] According to one aspect of the method for producing the anode protective film according to the present embodiment, a thin film containing the copolymer is obtained as the anode protective film, and a free-standing film of the thin film is easily obtained. Therefore, it is possible to form the anode protective film on the surface of the anode without maintaining a dry environment throughout the entire process. Furthermore, by using the anode protective film according to the present embodiment, it is possible to provide a protective layer that covers the anode through a simple process, and further, it is possible to obtain a battery according to the present embodiment through a simple process.

[0063] (Process 1) Step 1 is a step of mixing raw materials for obtaining the anode protective film to obtain a mixture. In step 1, first, the aforementioned copolymer and a photopolymerization initiator are prepared as raw materials for obtaining the anode protective film. The copolymer is obtained, for example, by the aforementioned manufacturing method. Next, the desired amounts of these prepared raw materials are weighed. Thereafter, the weighed raw materials are mixed, and a dilution solvent is further added, if necessary, to prepare a mixture. The mixture may be prepared by stirring the raw materials using a known stirring device or the like. The mixture prepared in step 1 is a mixture for forming the anode protective film.

[0064] The photopolymerization initiator is not particularly limited, and known compounds can be used. The photopolymerization initiator is preferably a photopolymerization initiator that is sensitive to ultraviolet light. The photopolymerization initiator may be used alone or in combination of two or more types.

[0065] Specific examples of the photopolymerization initiator include α-ketol compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and 1-hydroxycyclohexylphenyl ketone; acetophenone compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin ether compounds such as benzoin ethyl ether, benzoin isopropyl ether, and anisoin methyl ether; Examples of suitable oxime compounds include ketal compounds such as benzyl dimethyl ketal; aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, etc.; thioxanthone compounds (benzophenone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, etc.); camphorquinone, halogenated ketones, acylphosphinoxides, acylphosphonates, and oligo[2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone].

[0066] The content of the photopolymerization initiator is, for example, preferably 0.1 parts by mass or more and 10 parts by mass or less, more preferably 0.5 parts by mass or more and 7.5 parts by mass or less, and even more preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the copolymer.

[0067] (Process 2) Step 2 is a step of obtaining a molded product from the mixture prepared in Step 1. In Step 2, the molded product is obtained by molding the mixture prepared in Step 1. The molding of the mixture is not particularly limited, and for example, the mixture may be molded by applying it to the surface of a support to form a coating film. As the support, for example, a release film having a release-treated surface on at least one side of the substrate may be used. A molded product can be obtained by applying the mixture prepared in Step 1 to the release-treated surface of the release film to form a coating film. Furthermore, when a release film is used, a first release film having a release-treated surface on at least one side of the substrate may be used, and the mixture prepared in Step 1 may be applied to the release-treated surface to form a coating film to obtain a molded product, and then the release-treated surface of a second release film having a release-treated surface on at least one side of the substrate may be superimposed on the molded product. The molded product may be sandwiched between the first release film and the second release film and subjected to Step 3.

[0068] (Step 3) Step 3 is a step of obtaining an anode protective film containing a copolymer from the molded product obtained in step 2. In step 3, the molded product molded in step 2 is irradiated with energy rays, thereby crosslinking the copolymer and obtaining a thin film that is a crosslinked product of the copolymer. The type of energy rays is not particularly limited, but ultraviolet rays are preferred in terms of reactivity and workability. The device for irradiating the molded product with ultraviolet rays is not particularly limited, and may be, for example, a device equipped with an ultraviolet LED lamp, a device equipped with a high-pressure mercury lamp, or a device equipped with a metal halide lamp.

[0069] The conditions for irradiating the molded product with ultraviolet light are not particularly limited. The maximum irradiance and the integrated amount of light when irradiating with ultraviolet light are, for example, as follows: maximum irradiance: 5 to 1000 mW / cm 2 The integrated light amount is preferably 50 to 5000 mJ / cm 2 It is preferable that:

[0070] The anode protective film according to the present embodiment is obtained through the above steps 1, 2, and 3. The release film used in step 2 is irradiated with ultraviolet light in step 3, and then the release film is peeled off from the thin film, thereby obtaining the anode protective film according to the present embodiment.

[0071] [How to use the negative electrode protective film] The anode protective film according to this embodiment is used to cover at least a portion of the anode. The material of the anode is not particularly limited, and examples thereof include lithium metal, lithium alloy, metal oxide, metal sulfide, metal nitride, and graphite. Among these, the anode is preferably a lithium anode containing, for example, lithium metal or a lithium alloy. If the anode is a lithium anode, a battery with a high energy density can be easily obtained.

[0072] The lithium negative electrode is not particularly limited as long as it is a negative electrode containing lithium metal, a lithium alloy, etc. Specific examples of the lithium negative electrode include lithium foil, lithium alloy foil, a lithium metal film or lithium alloy film deposited on a negative electrode current collector, and a lithium metal film or lithium alloy film deposited on a resin film.

[0073] The anode protective film according to this embodiment is provided, for example, on the surface of the lithium anode facing the electrolyte layer, at the interface between the lithium anode and the electrolyte solution. In this case, the anode protective film may cover a part of the surface of the lithium anode facing the electrolyte layer, or may cover the entire surface. By providing the anode protective film according to this embodiment at the interface between the lithium anode and the electrolyte solution, it becomes easier to suppress the growth of dendrites.

[0074] Here, an example of a state in which a negative electrode is covered with the negative electrode protective film according to the present embodiment in order to protect the negative electrode will be described with reference to the drawings. In the drawings, some parts are illustrated enlarged or reduced in size for ease of explanation.

[0075] FIG. 1 shows a cross-sectional view of a negative electrode 10 with a negative electrode protective film in which a negative electrode 13 is protected. The negative electrode 10 with a negative electrode protective film is an example of a state in which a negative electrode protective film 11 according to the present embodiment is provided on the surface of the negative electrode 13. The negative electrode 10 with a negative electrode protective film shown in FIG. 1 includes a negative electrode 13 and a negative electrode protective film 11 that covers the negative electrode 13. In the negative electrode 10 with a negative electrode protective film shown in FIG. 1, a lithium negative electrode is used as the negative electrode 13. The negative electrode 13 is made of, for example, lithium metal foil. The negative electrode 13 has a first main surface 131 of the negative electrode 13 and a second main surface 132 of the negative electrode 13 that is the surface opposite to the first main surface 131. The negative electrode protective film 11 has a first main surface 111 of the negative electrode protective film 11 and a second main surface 112 that is the surface opposite to the first main surface 111. In the anode 10 with an anode protective film, the anode protective film 11 is provided on the first main surface 131 of the anode 13 so that the first main surface 131 of the anode 13 and the second main surface 112 of the anode protective film 11 are in direct contact with each other. The anode 10 with an anode protective film is provided with the anode protective film 11 covering the entire first main surface 131 of the anode 13. The second main surface 132 of the anode 13 is the surface on which an anode current collector (not shown) is provided. The first main surface 111 of the anode protective film 11 is the surface on which an electrolyte layer (not shown) is provided. The anode 10 with an anode protective film is obtained by attaching a thin film as the anode protective film 11 to the anode 13. By covering the surface of the anode 13 with the anode protective film 11, the generation of dendrites is suppressed and ionic conductivity and Coulombic efficiency are improved. Here, the main surface refers to the largest surface of the anode protective film 11 and the anode 13, and refers to the surface facing in the thickness direction (that is, the stacking direction of the anode protective film 11 and the anode 13).

[0076] 1, a negative electrode with a negative electrode protective film has been described as an example of a state in which a negative electrode is protected using the negative electrode protective film according to the present embodiment, but the example of protecting a negative electrode using the negative electrode protective film according to the present embodiment is not limited to this. The negative electrode protective film according to the present embodiment can adopt various forms as long as it can protect the negative electrode and obtain the effects of the negative electrode protective film according to the present embodiment.

[0077] [battery] Next, a preferred example of the battery according to this embodiment will be described.

[0078] The battery according to this embodiment includes the anode protective film according to this embodiment. In this embodiment, it is preferable that the anode protective film according to this embodiment be included as a constituent material of the battery. The battery is composed of a positive electrode, a negative electrode, and an electrolyte layer disposed between the positive electrode and the negative electrode. With this configuration, a battery with excellent characteristics can be obtained. Furthermore, the battery is preferably a secondary battery, and more preferably a lithium ion secondary battery. The structure of the battery according to this embodiment is not particularly limited, and may be a stacked structure or a wound structure.

[0079] Here, an example of a battery using the anode protective film according to this embodiment will be described with reference to the drawings. In the drawings, some parts are illustrated enlarged or reduced in size for ease of explanation.

[0080] FIG. 2 shows an example of a battery using the anode protective film according to this embodiment. The battery 100 shown in FIG. 2 is a lithium-ion secondary battery. As shown in FIG. 2, the battery 100 has a structure in which a cathode layer 20 is laminated on a cathode current collector 25 as the cathode side, and a structure in which an anode protective film-equipped anode 10 is laminated on an anode current collector 15 as the anode protective film-equipped anode 10. The anode protective film-equipped anode 10 shown in FIG. 1 is used as the anode protective film-equipped anode 10, and one surface of the anode 13 is covered with an anode protective film 11. The battery 100 also has an electrolyte layer 30 between the cathode layer 20 and the anode protective film 11. The electrolyte layer 30 is composed of an electrolyte solution 33 and a separator 31 impregnated with the electrolyte solution 33, and the separator 31 separates the cathode side from the anode side. The anode protective film 11 contains the electrolyte solution 33 of the electrolyte layer 30 and is swollen by the electrolyte solution 33. The battery 100 has a laminated structure in which a cathode current collector 25, a cathode layer 20, an electrolyte layer 30, anode protective film 11, an anode 13, and an anode current collector 15 are laminated in this order from the cathode current collector 25 toward the anode current collector 15, and the laminated structure is housed inside a container (not shown).

[0081] While an example of a battery using the anode protective film according to the present embodiment has been described above with reference to Fig. 2, examples of batteries using the anode protective film according to the present embodiment are not limited to this. The battery according to the present embodiment may adopt various forms as long as it can protect the anode using the anode protective film according to the present embodiment and can obtain the effects of using the anode protective film according to the present embodiment.

[0082] When the battery according to the present embodiment is a lithium ion secondary battery, the various components of the lithium ion secondary battery are not particularly limited as long as it is provided with the anode protective film according to the present embodiment, and for example, materials that are generally used in batteries can be used.

[0083] Examples of materials used for the positive electrode current collector and the negative electrode current collector include metal foils or metal plates such as copper, aluminum, nickel, titanium, and stainless steel, as well as carbon sheets and carbon nanotube sheets.

[0084] The positive electrode layer is composed of, for example, a positive electrode active material such as a lithium-containing composite oxide, a conductive additive such as a carbon-based material, a binder, and the like.

[0085] The electrolyte layer is composed of, for example, an electrolytic solution and a separator. When a separator is used, the material of the separator is not particularly limited, and examples thereof include a porous resin sheet containing a resin such as polyolefin, polyester, or polyamide.

[0086] In the battery according to this embodiment, the electrolyte preferably contains a lithium salt and a carbonate-based solvent. From the viewpoint of easily improving the effect of suppressing dendrite formation, the molar ratio of the lithium salt to the carbonate-based solvent (the lithium salt / the carbonate-based solvent) is preferably 1 / 6 or more and 1 / 1 or less. This molar ratio is more preferably 1 / 4 or more and 1 / 1 or less, and even more preferably 1 / 3 or more and 1 / 1 or less.

[0087] Specific examples of lithium salts include lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium 2-trifluoromethyl-4,5-dicyanoimidazolate, lithium 4,5-dicyano-1,2,3-triazolate, lithium bis(pentafluoroethylsulfonyl)imide, lithium borofluoride, lithium bis(oxalato)borate, lithium nitrate, lithium chloride, lithium bromide, and lithium fluoride. One or more of these exemplified lithium salts can be used as the lithium salt.

[0088] Specific examples of carbonate solvents include dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, and butylene carbonate. The carbonate solvent may be one or more of these lithium salts. The carbonate solvent in this embodiment refers to a compound having a carbonate skeleton in its molecular structure.

[0089] The negative electrode and the negative electrode protective film are as described above. The negative electrode protective film is the negative electrode protective film according to this embodiment.

[0090] The present invention is not limited to the above-described embodiment, and includes modifications and improvements within the scope of achieving the object of the present invention. [Example]

[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0092] Measurements and evaluations in the following examples and comparative examples were carried out by the methods shown below.

[0093] [Measurement of weight average molecular weight (Mw) and number average molecular weight (Mn)] Measurement was carried out using a gel permeation chromatograph (manufactured by Tosoh Corporation, product name "HLC-8320GPC") under the following conditions, and the values ​​measured were converted into standard polystyrene equivalents. (Measurement conditions) Column: "TSKgel guardcolumn SuperH-H", "TSKgel SuperHM-H", "TSKgel SuperHM-H", and "TSKgel SuperH2000" (all manufactured by Tosoh Corporation) connected in series Column temperature: 40℃ Developing solvent: tetrahydrofuran (copolymer concentration 1% by mass) Standard material: Polystyrene ·Injection volume: 20μL ·Flow rate: 0.60mL / min Detector: Differential refractometer

[0094] [Measurement of elution amount] The thin film obtained in each of the Examples and Comparative Examples described below was weighed to approximately 300 mg. The mass of the thin film at this time was designated M0. This thin film was wrapped in a polyester mesh (mesh size 200). The mass of the thin film wrapped in the polyester mesh was weighed, and the mass of the thin film was subtracted to calculate the mass of the polyester mesh alone. Next, the thin film wrapped in the polyester mesh was immersed in ethyl acetate at 23°C for 48 hours. Thereafter, the thin film wrapped in the polyester mesh was removed from the ethyl acetate and dried in an oven at 120°C for 2 hours, and then air-dried for 2 hours in an environment at a temperature of 23°C and a relative humidity of 50%. The mass after air-drying was weighed, and the mass of the thin film alone after immersion was calculated by subtracting the mass of the polyester mesh alone. This mass was designated M1. The amount of elution was then calculated using the following formula (F1): Elution amount (%)={(M0-M1) / M0}×100 (F1) In formula (F1), M0 represents the mass of the thin film weighed before being wrapped in the polyester mesh, and M1 represents the mass of the thin film alone after being immersed in ethyl acetate.

[0095] [Swelling degree measurement] The thin films obtained in each of the Examples and Comparative Examples described below were cut into pieces measuring approximately 3 cm (length) x 3 cm (width), and the resulting thin film pieces were weighed to approximately 1 g. The mass at this time was designated W0. The thin film pieces were wrapped in a polyester mesh (mesh size 200), and the mass of the thin film pieces wrapped in the polyester mesh was weighed. The mass of the polyester mesh alone was calculated by subtracting the mass of the thin film pieces from the weight. The pieces were immersed in a carbonate-based solvent [a mixed solvent of ethylene carbonate / dimethyl carbonate = 1 / 1 (volume ratio)] for 24 hours to allow swelling. The thin film pieces wrapped in the polyester mesh were then pulled out, the solvent on the surface was wiped with a paper wiper, and the mass was measured. The mass of the swollen thin film pieces was calculated by subtracting the mass of the polyester mesh alone. The mass at this time was designated W1. The swelling degree was then calculated using the following formula (F2): Swelling degree (%) = {(W1-W0) / W0} × 100 (F2) In formula (F2), W0 represents the mass of the thin film piece weighed before being wrapped in the polyester mesh, and W1 represents the mass of the thin film piece alone after swelling.

[0096] [Ionic conductivity measurement] The lithium half-cells obtained in each of the Examples and Comparative Examples described below were measured using the AC impedance method, which measures the resistance component by applying an AC voltage (applied voltage of 10 mV) between the electrodes. The ionic conductivity was calculated from the real impedance intercept of the resulting Cole-Cole plot. A potentiostat / galvanostat (VMP-300, manufactured by Biologic) was used for the measurements. Ionic conductivity (σ A ) was calculated using the following formula (F3). σ A =L A / (R A ×S A ) (F3) In formula (F3), σ A is the ionic conductivity (unit: S cm -1 ), R A is the resistance (unit: Ω), S A is the cross-sectional area of ​​the solid electrolyte membrane at the time of measurement (unit: cm 2 ), LA indicates the distance between electrodes (unit: cm). The measurement temperature was 25°C. The ionic conductivity (σ A ) was calculated.

[0097] [Coulomb efficiency measurement] The lithium half-cells obtained in each of the Examples and Comparative Examples described below were discharged for 1 hour at a constant current of 0.1 C at 25°C, and then charged to a cell voltage of 1.0 V at a constant current of 0.1 C at 25°C. This discharge and charge cycle constitutes one cycle, and this cycle was repeated two more times for a total of three cycles. The discharge capacity at the third cycle was designated C0, and the charge capacity at the third cycle was designated C1. The Coulombic efficiency was calculated using the following formula (F4). A potentiostat / galvanostat (VMP-300, manufactured by Biologic) was used for the measurements. Coulomb efficiency (%) = C1 / C0 × 100 (F4) In formula (F4), C0 represents the discharge capacity at the third cycle, and C1 represents the charge capacity at the third cycle.

[0098] The closer the Coulombic efficiency is to 100%, the better the battery performance, indicating the superior performance of the anode protective film. On the other hand, if the Coulombic efficiency exceeds 100%, it is likely that dendrites have grown and caused micro-short circuits, indicating that the film's ability to uniformly dissolve and deposit lithium is poor.

[0099] [Example 1] (Synthesis of polymerization catalyst) (R,R)-N,N'-bis(3,5-di-tert-butylsalicylidene)-1,2-diaminocyclohexanecobalt(II) and pentafluorobenzoic acid were weighed out in a molar ratio of 1:1.1 and placed in a flask, followed by the addition of dehydrated toluene. The flask was shielded from light with aluminum foil and the reaction was carried out at room temperature for 20 hours. The chemical reaction formula is as follows: After the reaction was completed, the solvent was removed under reduced pressure and the mixture was washed several times with excess hexane. The mixture was then vacuum dried at room temperature to obtain a cobalt salen complex.

[0100] [ka]

[0101] (Synthesis of Copolymer A) A mixture of propylene oxide and allyl glycidyl ether in a molar ratio of 97:3 was used as the epoxide monomer. The polymerization catalyst was a synthesized cobalt salen complex, and the cocatalyst was bis(triphenylphosphoranylidene)ammonium chloride. The molar ratio of epoxide monomer:catalyst:cocatalyst was 2000:1:1, and the mixture was placed in a pressure vessel. 200 ppm of phenothiazine was then added, followed by ethyl acetate to achieve a monomer:ethyl acetate ratio of 50:50 (by mass). All of these operations were carried out under argon. After purging the pressure vessel, carbon dioxide was introduced into the vessel using a liquid pump. The pressure inside the vessel was then increased to 2.0 MPa, and the polymerization reaction was carried out at 25°C for 20 hours. After the reaction was completed, chloroform was added to the contents of the pressure vessel to prepare a chloroform solution, and 1M hydrochloric acid was added. Next, the chloroform solution was dropped into stirring methanol to precipitate the product. The product was then dried under reduced pressure using a diaphragm pump in a desiccator, and then vacuum dried at 60°C to obtain copolymer A.

[0102] The structure of the obtained copolymer A was confirmed by nuclear magnetic resonance spectroscopy ( 1 When H-NMR (Biospin Avance 500, manufactured by Bruker) was performed using a solvent (CDCl3 containing 0.03% by volume of tetramethylsilane), the molar ratio of the structural unit represented by general formula (1) (hereinafter also referred to as structural unit (1)), the structural unit represented by general formula (2) (hereinafter also referred to as structural unit (2)), the structural unit represented by general formula (3) (hereinafter also referred to as structural unit (3)), and the structural unit represented by general formula (4) (hereinafter also referred to as structural unit (4)) in copolymer A was structural unit (1): structural unit (2): structural unit (3): structural unit (4) = 94.5:2.9:2.5:0.1 (see Figure 3). The number average molecular weight Mn of the obtained copolymer A was 24,000, and the molecular weight distribution Mw / Mn was 1.1.

[0103] (thin film preparation) To the resulting copolymer A, 1-hydroxycyclohexyl phenyl ketone was added as a photopolymerization initiator so that the copolymer:initiator ratio was 97:3% by mass. The mixture was then diluted with ethyl acetate and stirred to prepare a thin-film-forming solution with a solids concentration of 30% by mass. A first release film (manufactured by Lintec Corporation, product name "SP-PET381031") was prepared, and the prepared thin-film-forming solution was applied to the release-treated surface of this release film. The film was then dried at 120°C for 1 minute to form a 10-μm-thick thin-film layer. A second release film (manufactured by Lintec Corporation, product name "SP-PET382150") was then prepared, and the release-treated surface of this release film was attached to the surface of the thin-film layer. The thin-film laminate sandwiched between the first and second release films was then placed on a stainless steel plate and irradiated with ultraviolet light [illuminance: 200 mW / cm] at 50°C. 2 , Accumulated light intensity: 1000mJ / cm 2 The measured values ​​were measured using an illuminance actinometer manufactured by Eye Graphics Inc. (controller: EYE UV METER UVPF-A2, light-receiving part: EYE UV METER PD-365A2) to obtain a thin film having a thickness of 10 μm. The obtained thin film was a negative electrode protective film. The amount of elution and the degree of swelling of the obtained thin film were measured using the methods described above.

[0104] (Fabrication of lithium half-cells) The thin film prepared above was attached to a lithium foil approximately 400 μm thick as a protective film for the anode, and the foil was punched out to a diameter of 16 mm to produce a lithium anode with a protective film. A 19 mm diameter, 61 μm thick polyester mesh (UX-screen 150-035 / 380PW, manufactured by NBC Meshtec Co., Ltd.) was then placed on top of the thin film (the side opposite the lithium foil). A 12 μm thick, 16 mm diameter copper foil was then placed on top of the polyester mesh (the side opposite the thin film), producing a lithium half-cell. The resulting cell was filled with an electrolyte solution and allowed to stand at 25°C for 1.5 hours. The ionic conductivity and Coulombic efficiency were then measured using the methods described above. The electrolyte solution was a 1:2 molar mixture of lithium bis(fluorosulfonyl)imide and dimethyl carbonate.

[0105] [Example 2] (Polymerization of Copolymer B) Polymerization was carried out in the same manner as in Example 1, except that a mixture of propylene oxide and allyl glycidyl ether in a molar ratio of 90:10 was used as the epoxide monomer. The structure of the obtained copolymer B was determined in the same manner as in Example 1. 1 When confirmed by H-NMR, the molar ratio of structural unit (1), structural unit (2), structural unit (3), and structural unit (4) in copolymer B was structural unit (1):structural unit (2):structural unit (3):structural unit (4)=81.7:8.4:8.9:0.9. The number average molecular weight Mn of the obtained copolymer B was 25,000, and the molecular weight distribution Mw / Mn was 1.2.

[0106] (thin film preparation) A thin film having a thickness of 10 μm was obtained in the same manner as in Example 1, except that copolymer B was used.

[0107] (Fabrication of lithium half-cells) A lithium half-cell was produced in the same manner as in Example 1, except that a thin film obtained using copolymer B was used. Then, ionic conductivity and Coulomb efficiency were measured in the same manner as in Example 1.

[0108] [Example 3] (Polymerization of Copolymer C) Polymerization was carried out in the same manner as in Example 1, except that a mixture of propylene oxide and glycidyl methacrylate in a molar ratio of 98:2 was used as the epoxide monomer. The structure of the obtained copolymer C was determined in the same manner as in Example 1. 1 When confirmed by H-NMR, the molar ratio of structural unit (1), structural unit (2), structural unit (3), and structural unit (4) in copolymer C was structural unit (1):structural unit (2):structural unit (3):structural unit (4)=97.5:1.6:0.9:0.0 (see FIG. 4). The number average molecular weight Mn of the obtained copolymer C was 23,000, and the molecular weight distribution Mw / Mn was 1.3.

[0109] (thin film preparation) A thin film having a thickness of 10 μm was obtained in the same manner as in Example 1, except that Copolymer C was used.

[0110] (Fabrication of lithium half-cells) A lithium half-cell was produced in the same manner as in Example 1, except that a thin film obtained using copolymer C was used. Then, ionic conductivity and Coulomb efficiency were measured in the same manner as in Example 1.

[0111] [Example 4] (Polymerization of Copolymer D) Polymerization was carried out in the same manner as in Example 1, except that a mixture of propylene oxide and glycidyl methacrylate in a molar ratio of 96:4 was used as the epoxide monomer. The structure of the obtained copolymer D was determined in the same manner as in Example 1. 1 When confirmed by H-NMR, the molar ratio of structural unit (1), structural unit (2), structural unit (3), and structural unit (4) in copolymer D was structural unit (1):structural unit (2):structural unit (3):structural unit (4)=95.4:4.3:0.3:0.0. The number average molecular weight Mn of the obtained copolymer D was 30,000, and the molecular weight distribution Mw / Mn was 1.2.

[0112] (thin film preparation) A thin film having a thickness of 10 μm was obtained in the same manner as in Example 1, except that Copolymer D was used.

[0113] (Fabrication of lithium half-cells) A lithium half-cell was produced in the same manner as in Example 1, except that a thin film obtained using copolymer D was used. Then, ionic conductivity and Coulomb efficiency were measured in the same manner as in Example 1.

[0114] [Example 5] (Polymerization of Copolymer E) Polymerization was carried out in the same manner as in Example 1, except that a mixture of propylene oxide and glycidyl methacrylate in a molar ratio of 90:10 was used as the epoxide monomer. The structure of the obtained copolymer E was determined in the same manner as in Example 1. 1 When confirmed by H-NMR, the molar ratio of structural unit (1), structural unit (2), structural unit (3), and structural unit (4) in copolymer E was structural unit (1):structural unit (2):structural unit (3):structural unit (4)=83.7:15.0:1.1:0.2. The number average molecular weight Mn of the obtained copolymer E was 20,000, and the molecular weight distribution Mw / Mn was 1.2.

[0115] (thin film preparation) A thin film having a thickness of 10 μm was obtained in the same manner as in Example 1, except that copolymer E was used.

[0116] (Fabrication of lithium half-cells) A lithium half-cell was produced in the same manner as in Example 1, except that a thin film obtained using copolymer E was used. Then, an electrolyte solution was poured into the produced cell, and the cell was allowed to stand at 25°C for 18 hours, and the ionic conductivity and coulombic efficiency were measured in the same manner as in Example 1.

[0117] [Example 6] (Polymerization of Copolymer F) Polymerization was carried out in the same manner as in Example 1, except that a mixture of propylene oxide and 4-hydroxybutyl acrylate glycidyl ether in a molar ratio of 98:2 was used as the epoxide monomer. The structure of the obtained copolymer F was determined in the same manner as in Example 1. 1 When confirmed by H-NMR, the molar ratio of structural unit (1), structural unit (2), structural unit (3), and structural unit (4) in copolymer F was structural unit (1):structural unit (2):structural unit (3):structural unit (4)=95.0:2.1:2.8:0.1 (see FIG. 5). The number average molecular weight Mn of the obtained copolymer F was 38,000, and the molecular weight distribution Mw / Mn was 1.2.

[0118] (thin film preparation) A thin film having a thickness of 10 μm was obtained in the same manner as in Example 1, except that copolymer F was used.

[0119] (Fabrication of lithium half-cells) A lithium half-cell was produced in the same manner as in Example 1, except that a thin film obtained using copolymer F was used. Then, ionic conductivity and Coulomb efficiency were measured in the same manner as in Example 1.

[0120] [Example 7] (Polymerization of Copolymer G) Polymerization was carried out in the same manner as in Example 1, except that a mixture of propylene oxide and 4-hydroxybutyl acrylate glycidyl ether in a molar ratio of 95:5 was used as the epoxide monomer. The structure of the obtained copolymer G was determined in the same manner as in Example 1. 1 When confirmed by H-NMR, the molar ratio of structural unit (1), structural unit (2), structural unit (3), and structural unit (4) in copolymer G was structural unit (1):structural unit (2):structural unit (3):structural unit (4)=92.3:5.1:2.5:0.1. The number average molecular weight Mn of the resulting copolymer G was 41,000, and the molecular weight distribution Mw / Mn was 1.1.

[0121] (thin film preparation) A thin film having a thickness of 10 μm was obtained in the same manner as in Example 1, except that copolymer G was used.

[0122] (Fabrication of lithium half-cells) A lithium half-cell was produced in the same manner as in Example 1, except that a thin film obtained using copolymer G was used. Then, ionic conductivity and Coulomb efficiency were measured in the same manner as in Example 1.

[0123] [Comparative Example 1] (Fabrication of lithium half-cells) Except for not using a thin film as the negative electrode protective film, a lithium half-cell was produced in the same manner as in Example 1. Then, ionic conductivity and Coulomb efficiency were measured in the same manner as in Example 1.

[0124] Comparative Example 2 (thin film preparation) Polyethylene carbonate (product name "QPAC25", manufactured by Empower Materials) was diluted with chloroform to prepare a solution with a solids concentration of 30% by mass. The prepared solution was applied to the release-treated surface of a release film (manufactured by Lintec Corporation, product name "SP-PET381031") and dried at 90°C for 1 minute to obtain a thin film with a thickness of 10 μm.

[0125] (Fabrication of lithium half-cells) Except for using the thin film obtained as described above, a lithium half-cell was produced in the same manner as in Example 1. Then, ionic conductivity and Coulomb efficiency were measured in the same manner as in Example 1.

[0126] Comparative Example 3 (thin film preparation) Polypropylene carbonate (product name "QPAC40", manufactured by Empower Materials) was diluted with ethyl acetate to prepare a solution with a solids concentration of 30% by mass. The prepared solution was applied to the release-treated surface of a release film (manufactured by Lintec Corporation, product name "SP-PET381031") and dried at a temperature of 120°C for 1 minute to obtain a thin film with a thickness of 10 μm.

[0127] (Fabrication of lithium half-cells) Except for using the thin film obtained as described above, a lithium half-cell was produced in the same manner as in Example 1. Then, ionic conductivity and Coulomb efficiency were measured in the same manner as in Example 1.

[0128] [Table 1]

[0129] [Table 2]

[0130] The results shown in Table 2 demonstrate that the ionic conductivity and Coulombic efficiency can be improved by the anode protective films obtained in Examples 1 to 8. Furthermore, it is inferred from these results that the anode protective films obtained in Examples 1 to 8 can suppress the generation of dendrites. [Explanation of symbols]

[0131] 10...negative electrode with negative electrode protective film, 11...negative electrode protective film, 13...negative electrode, 15...negative electrode current collector, 20...positive electrode layer, 25...positive electrode current collector, 30...electrolyte layer, 31...separator, 33...electrolyte solution, 100...battery, 111...first main surface of negative electrode protective film, 112...second main surface of negative electrode protective film, 131...first main surface of negative electrode, 132...second main surface of negative electrode.

Claims

1. A negative electrode protective film that covers at least a part of the negative electrode, The copolymer includes a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2) in an amount of 0.3 mol % or more and 20.0 mol % or less: Negative electrode protective film. 【Chemistry 1】 (In the general formula (1) and the general formula (2), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; L 1 and L 2 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 3 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 1 is any one of the reactive groups represented by the following structural formula (2-1), the following structural formula (2-2), and the following structural formula (2-3). 【Chemistry 2】

2. The anode protective film according to claim 1 , -L in the general formula (2) 3 -X 1 is any one of reactive groups represented by the following structural formula (2-4), the following structural formula (2-5), and the following structural formula (2-6), Negative electrode protective film. 【Chemistry 3】

3. The anode protective film according to claim 1 or 2, The copolymer further contains at least one structural unit selected from the group consisting of a structural unit represented by the following general formula (3) and a structural unit represented by the following general formula (4), in an amount of 0.1 mol % to 30.0 mol %: Negative electrode protective film. 【Chemistry 4】 (In the general formula (3) and the general formula (4), R 2 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; L 4 and L 5 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 6 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 2 is any one of the reactive groups represented by the following structural formula (4-1), the following structural formula (4-2), and the following structural formula (4-3). 【Chemistry 5】

4. The anode protective film according to claim 1 or 2, the amount of the copolymer eluted in ethyl acetate is 10% or less; The degree of swelling of the copolymer in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is 100% or more. Negative electrode protective film.

5. The anode protective film according to claim 1 or 2, the negative electrode protective film further contains an electrolyte, the electrolyte solution contains a carbonate-based solvent and a lithium salt; a molar ratio of the lithium salt to the carbonate-based solvent (lithium salt / carbonate-based solvent) is 1 / 6 or more and 1 / 1 or less; Negative electrode protective film.

6. The anode protective film according to claim 1 or 2, The negative electrode is a lithium negative electrode. Negative electrode protective film.

7. The negative electrode protective film according to claim 1 or 2, battery.

Citation Information

Patent Citations

  • JP1974081498A

  • Collector and lithium ion secondary battery using it

    JP2007035297A

  • Polymer electrolyte composition

    JP2015173017A

  • Secondary battery electrode and secondary battery

    JP2015179595A

  • Semi-interpenetrating polymer networks as separators for alkali metal batteries.

    JP2023502319A

Cited By

  • Resin composition, binder resin, polymer thin film and battery

    JP7644875B2

  • Resin composition, binder resin, polymer thin film and battery

    JPWO2024203399A1