Niobium-titanium composite oxide for electrodes, electrode using the same, and power storage device

Optimized synthesis of niobium-titanium composite oxide powders addresses the challenges of high-rate charge/discharge, cycle stability, and low-temperature performance in power storage devices by controlling peak ratios and zeta potential, enhancing lithium ion insertion and desorption.

JP2024146389APending Publication Date: 2024-10-15UBE CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023059255
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing niobium-titanium composite oxides used in power storage devices, such as lithium-ion batteries, face challenges in achieving high-rate charge and discharge characteristics, cycle stability, and low-temperature performance, particularly when used as negative electrode materials in all-solid-state batteries.

Method used

The synthesis of niobium-titanium composite oxide powders is optimized by controlling firing temperature and crushing conditions to achieve specific peak intensity ratios in X-ray diffraction and Raman spectroscopy, along with targeted zeta potential and particle size distributions, enhancing the material's ability to insert and desorb lithium ions effectively.

Benefits of technology

The optimized niobium-titanium composite oxide powders improve rate characteristics, cycle stability, and low-temperature performance in both liquid-based non-aqueous electrolyte batteries and all-solid-state batteries, maintaining initial capacity and charge/discharge efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146389000001_ABST
    Figure 2024146389000001_ABST
Patent Text Reader

Abstract

To provide a liquid-based non-aqueous electrolyte battery and a niobium-titanium composite oxide powder for all-solid battery electrodes.SOLUTION: In a niobium-titanium composite oxide powder for non-aqueous electrolyte power storage device electrodes, in a diffraction diagram of powder X-ray diffraction using a Cu-Kα ray source, an intensity ratio of two peaks represented in the following formula (I) is 1.0 or more and in a spectrum obtained by microscopic Raman spectroscopy, an intensity ratio of two peaks represented by the formula (II) is 0.2 or less. The formula (I) is I (24 deg) / I (26 deg)≥1.0 which is a peak intensity value of a strongest intensity appearing in the range of I(24deg):2θ=24±0.2° and a peak intensity value of a strongest intensity appearing in the range of I(26deg):2θ=26±0.2°. The formula (II) is I(A) / I(C)≤0.2 in which I(A): is an intensity value of a peak A appearing in 430 to 460 cm-1 and I(C) is an intensity value of a peak C appearing in 260 to 280 cm-1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a niobium-titanium composite oxide powder for electrodes, an electrode using the same, and an electricity storage device. [Background technology]

[0002] Electrical storage devices for electric vehicles require high energy density in order to improve fuel efficiency or power consumption, and lithium-ion batteries in particular are widely used as power sources for electric vehicles and power storage. Various materials have been researched as electrode materials for lithium-ion batteries, and although lithium titanate has excellent input / output characteristics, its energy density remains at 175mAh / g, and there remain challenges in achieving even higher energy. Therefore, as an alternative candidate, there is a movement to use niobium-titanium composite oxides, mainly niobium titanate, which has a high energy density of 380mAh / g in theoretical capacity, as negative electrode materials.

[0003] In addition, lithium-ion batteries currently on the market use electrolytes containing flammable organic solvents, so measures to prevent leakage, installation of safety devices to suppress temperature rise in the event of a short circuit, and a structure to prevent short circuits are necessary. Under these circumstances, all-solid-state secondary batteries using inorganic solid electrolytes instead of organic electrolytes are attracting attention. Since the positive electrode, negative electrode, and electrolyte of all-solid-state secondary batteries are all solid, there is a possibility that the safety and reliability issues that are problems with batteries using organic electrolytes can be greatly improved, and since the safety devices can be simplified, high energy density can be achieved, so applications to electric vehicles and large storage batteries are expected. However, issues regarding battery characteristics such as improvement of charge and discharge rate characteristics remain.

[0004] Patent Document 1 discloses a battery active material that contains a monoclinic complex oxide represented by TiNb2O7, and in a powder X-ray diffraction pattern obtained using a Cu-Kα radiation source, the most intense peak appears at 2θ=26°±0.5° and two peaks appear at 2θ=44°±1°, and the intensity ratio of the two peaks (IH / IL) is 1.37 or less, where IH is the high-angle peak and IL is the low-angle peak. According to Patent Document 1, the growth of crystallites on a specific lattice plane improves the insertion and desorption of lithium ions, and the space for insertion and desorption of lithium ions is effectively increased, thereby providing a battery active material with excellent rapid charge and discharge performance and higher energy density, and a nonaqueous electrolyte battery using the active material.

[0005] Patent Document 2 discloses an active material for non-aqueous electrolyte batteries, which is characterized by containing monoclinic niobium-titanium composite oxide particles containing rutile oxide, in which the peak intensity corresponding to a specific Raman band falls within a certain range. According to Patent Document 2, the contained rutile oxide absorbs lithium at the beginning of charging and discharging, thereby contributing to improving the electronic conductivity of the monoclinic niobium-titanium composite oxide particles, and as a result, an active material for non-aqueous electrolyte batteries with excellent input / output characteristics and cycle characteristics, and a non-aqueous electrolyte battery using the active material, can be obtained. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2012-99287 A [Patent Document 2] International Publication No. 2015 / 140936 Summary of the Invention [Problem to be solved by the invention]

[0007] However, for an energy storage device that uses the monoclinic complex oxide represented by TiNb2O7 in Patent Document 1 as the negative electrode active material, only the discharge characteristics equivalent to a 1C rate have been studied. For example, no study has been done on the charge / discharge characteristics at even faster rates such as a 5C rate or a 10C rate. In fact, there has been a problem in that it is not possible to improve the charge / discharge characteristics at rapid rates while maintaining the initial capacity (battery capacity) and cycle characteristics of the battery.

[0008] For the active material in Patent Document 2, high-rate discharge characteristics and cycle characteristics are examined, but no findings are given on improvements in the initial capacity (battery capacity) of the battery, the charging characteristics at a high rate of 5C, or the low-temperature characteristics. In fact, the inclusion of a rutile-type oxide tends to decrease the initial capacity (battery capacity) of the battery, the charging characteristics at a high rate, and the low-temperature characteristics, and in addition, there is no description whatsoever on the performance when a niobium-titanium composite oxide is applied to an all-solid-state secondary battery.

[0009] For the reasons described above, the power storage devices using the negative electrode active materials and electrodes of Patent Documents 1 and 2 cannot simultaneously achieve improved energy density and improved input / output characteristics at high rates, as well as improved battery performance in low temperature regions and improved performance in all-solid-state batteries.

[0010] Therefore, an object of the present invention is to provide a niobium-titanium-containing oxide powder that can be used as an electrode material for a nonaqueous electrolyte electricity storage device and can improve the rate characteristics, cycle characteristics, and low-temperature characteristics in a liquid nonaqueous electrolyte battery, and further the rate characteristics in an all-solid-state battery, as well as an electrode and an electricity storage device using the same. [Means for solving the problem]

[0011] In order to achieve the above object, the present inventors have investigated various synthesis conditions for niobium-titanium composite oxide powder, and as a result, by carrying out the calcination temperature and crushing conditions during synthesis within specific ranges in accordance with the raw materials, it has been possible to obtain a niobium-titanium composite oxide powder in which the intensity ratio of two specific peaks in a powder X-ray diffraction pattern is 1.0 or more and the intensity ratio of two specific peaks in a spectrum obtained by microscopic Raman spectroscopy is controlled to 0.2 or less. Furthermore, it has been found that when this niobium-titanium composite oxide powder is used as a negative electrode active material, the rate characteristics, cycle characteristics, and low-temperature characteristics in a liquid nonaqueous electrolyte battery, and further the rate characteristics in an all-solid-state battery, can be improved, and the present invention has been completed. That is, the present invention relates to the following items.

[0012] [1] A niobium-titanium composite oxide powder for use in an electrode of a nonaqueous electrolyte electricity storage device, characterized in that in a powder X-ray diffraction pattern obtained using a Cu-Kα radiation source, the intensity ratio of two peaks represented by the following formula (I) is 1.0 or more, and in a spectrum obtained by micro-Raman spectroscopy, the intensity ratio of two peaks represented by the following formula (II) is 0.2 or less. I(24deg) / I(26deg)≧1.0 (I) I(24deg): The highest peak intensity value that appears in the range of 2θ=24±0.2° I(26deg): The highest peak intensity value that appears in the range of 2θ=26±0.2° I(A) / I(C)≦0.2 (II) I(A):430~460cm -1 Intensity value of peak A appearing in I(C):260~280cm -1 Intensity value of peak C appearing in [2] General formula Ti 1-x / 2 NbO 7-x The niobium-titanium composite oxide powder for an electrode of a nonaqueous electrolyte electricity storage device according to [1], characterized in that it has a composition represented by (0≦x<2). [3] The niobium-titanium composite oxide powder for an electrode of a nonaqueous electrolyte electricity storage device according to [1] or [2], characterized in that the zeta potential of the niobium-titanium composite oxide powder at 25°C, as measured by electrophoresis, is -65 mV or more and -25 mV or less. [4] The niobium-titanium composite oxide powder for an electrode of a nonaqueous electrolyte electricity storage device according to any one of [1] to [3], characterized in that, when D50 is the particle size at a point where the cumulative volume distribution of particle sizes of primary particles in a particle size distribution is 50% and DBET is the diameter equivalent to the specific surface area calculated from the specific surface area determined by a BET method, D50 is 1 μm or more and the ratio of D50 to DBET, D50 / DBET (μm / μm), is 2.1 or less. [5] The niobium-titanium composite oxide powder for an electrode of a nonaqueous electrolyte electricity storage device according to any one of [1] to [4], characterized in that, when the particle size D50 is defined as a particle size at a point where a cumulative volume distribution of particle sizes of primary particles is 50% in a particle size distribution, the particle size D50 is less than 1 μm, and the area ratio of two peaks represented by the following formula (III) in a spectrum obtained by micro-Raman spectroscopy is 0.5 or more: I(538cm -1 ) / I(650cm -1 ) ≧0.5 (III) I(538cm -1 ):560~520cm -1 The area value of the peaks obtained by separating the spectra that appear in I(650cm -1 ):620~680cm -1 The area value of the peaks obtained by separating the spectra that appear in [6] The niobium-titanium composite oxide powder for an electrode of a nonaqueous electrolyte electricity storage device according to any one of [1] to [5], characterized in that in the niobium-titanium composite oxide powder for an electrode, element M1 (M1 includes any one or more selected from the group consisting of Al, Mg, Mo, and Ce) is localized and present on the surface of the niobium-titanium composite oxide particle. [7] An electrode comprising the niobium-titanium composite oxide powder according to any one of [1] to [6]. [8] A negative electrode active material composition comprising the niobium-titanium composite oxide powder according to any one of [1] to [7] and an inorganic solid electrolyte. [9] A non-aqueous electrolyte electricity storage device comprising the electrode according to [7].

[10] An all-solid-state secondary battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer, the negative electrode layer being a layer containing the negative electrode active material composition according to [8]. Effect of the Invention

[0013] According to the present invention, it is possible to provide a niobium-titanium composite oxide powder capable of improving the rate characteristics, cycle characteristics, and low-temperature characteristics in liquid nonaqueous electrolyte batteries, and further the rate characteristics in all-solid-state batteries, and an electrode and an electricity storage device using the same. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a diagram showing a Raman spectrum of the titanium-niobium composite oxide powder of Example 2-1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] [Niobium-titanium composite oxide for electrodes of the present invention] The niobium-titanium composite oxide for electrodes of the present invention is a niobium-titanium composite oxide powder for electrodes of nonaqueous electrolyte electricity storage devices, characterized in that in a powder X-ray diffraction pattern obtained using a Cu-Kα radiation source, the intensity ratio of two peaks represented by the following formula (I) is 1.0 or more, and in a spectrum obtained by micro-Raman spectroscopy, the intensity ratio of two peaks represented by the following formula (II) is 0.2 or less. I(24deg) / I(26deg)≧1.0 (I) I(24deg): The highest peak intensity value that appears in the range of 2θ=24±0.2° I(26deg): The highest peak intensity value that appears in the range of 2θ=26±0.2° I(A) / I(C)≦0.2 (II) I(A):430~460cm -1 Intensity value of peak A appearing in I(C):260~280cm -1 Intensity value of peak C appearing in The niobium-titanium composite oxide powder of the present invention is used for electrodes of nonaqueous electrolyte storage devices. That is, the niobium-titanium composite oxide powder of the present invention is a niobium-titanium composite oxide powder for electrodes of nonaqueous electrolyte storage devices. The nonaqueous electrolyte may be any electrolyte other than an aqueous electrolyte, and is not particularly limited, but examples thereof include nonaqueous electrolyte solutions and solid electrolytes.

[0016] <General formula Ti 1-x / 2 NbO 7-x Niobium-titanium composite oxide represented by (0≦x<2) The niobium-titanium composite oxide of the present invention is represented by the general formula Ti 1-x / 2 NbO 7-x (0≦x<2). Specific examples of the compound include niobium-titanium composite oxides, such as TiNb2O7 and Ti2Nb 14 O 39 , TiNb 14 O 37 , Ti2Nb6O 19 , etc. Niobium-titanium composite oxide may contain a titanium oxide phase (e.g., rutile-type TiO2, TiO, etc.) derived from the synthesis raw material. In the case of niobium-titanium composite oxide, the ratio of the number of moles of Nb to the number of moles of Ti (Nb / Ti ratio) is preferably in the range of 1.5 to 14, more preferably in the range of 1.8 to 7.0. Within this range, the electronic conductivity of the composite oxide is improved, and the rate characteristics are excellent.

[0017] The niobium-titanium composite oxide of the present invention is not limited in crystal system, but is generally monoclinic. It may also have a crystal structure belonging to the ReO3 space group A / 2m. In the case of monoclinic, the aspect ratio tends to be large, but from the viewpoint of electrode density, the aspect ratio is preferably in the range of 1.0 to 4.0.

[0018] <Powder X-ray diffraction> The powder X-ray diffraction measurement of the niobium-titanium composite oxide powder of the present invention is carried out as follows. A glass plate filled with a sample specimen is placed in a powder X-ray diffractometer, and a diffraction pattern is obtained using Cu-Kα radiation. In the obtained diffraction pattern, the intensity ratio of the two peaks represented by the following formula (I) is 1.0 or more. If the intensity ratio is within the above range, the rate characteristics, cycle characteristics, and low-temperature characteristics in a liquid-based nonaqueous electrolyte battery, and further the rate characteristics in an all-solid-state battery can be improved. The intensity ratio is preferably 1.01 or more and 2.0 or less, more preferably 1.02 or more and 2.0 or less, even more preferably 1.04 or more and 1.9 or less, and particularly preferably 1.05 or more and 1.2 or less. The peak appearing at 2θ=24°±0.2° is considered to be mainly a peak of the (1 1 0) plane, and the peak appearing at 2θ=26°±0.5° is considered to be mainly a peak of the (0 0 3) plane. Although this is merely speculation, it is presumed that the change in the intensity ratio of these two peaks indicates a change in the balance of the crystallite sizes of each crystal plane, which is thought to affect the insertion and desorption properties of lithium ions into the crystal structure of the niobium-titanium composite oxide. The raw materials and sintering temperature used affect the growth of specific crystal planes, and it is presumed that the intensity ratio of the two peaks can be controlled by keeping the sintering temperature and crushing conditions during synthesis within specific ranges in accordance with the raw materials. I(24deg) / I(26deg)≧1.0 (I) I(24deg): The highest peak intensity value that appears in the range of 2θ=24±0.2° I(26deg): The highest peak intensity value that appears in the range of 2θ=26±0.2°

[0019] <Microscopic Raman spectroscopy> In the microscopic Raman spectroscopy measurement of the niobium-titanium composite oxide powder of the present invention, an appropriate amount of sample is placed on a slide glass, and a Raman spectrum is obtained using a laser Raman spectrometer. In the spectrum obtained, the intensity ratio of two peaks represented by the following formula (II) is 0.2 or less. If the intensity ratio is within the above range, the rate characteristics, cycle characteristics, and low-temperature characteristics in a liquid nonaqueous electrolyte battery, as well as the rate characteristics in an all-solid-state battery, can be improved. It is preferably 0 or more and 0.15 or less, and more preferably 0 or more and 0.1 or less. When the niobium-titanium composite oxide is contained, the Raman spectrum has an intensity ratio of 260 to 280 cm -1 On the other hand, when rutile-type TiO2, TiO, etc. are contained, a peak appears at 430 to 460 cm in the Raman spectrum, although it depends on the Ti and Nb contents. -1 Since a peak appears at this temperature, the initial capacity (battery capacity), high-rate charging characteristics, and low-temperature characteristics of the battery decrease. The content of rutile-type TiO2 and other substances is affected by the raw materials and firing temperature used, and it is possible to control the content of rutile-type TiO2 and other substances by setting the firing temperature and crushing conditions during synthesis within a specific range in accordance with the raw materials. I(A) / I(C)≦0.2 (II) I(A):430~460cm -1 Intensity value of peak A appearing in I(C):260~280cm -1 Intensity value of peak C appearing in

[0020] Regarding the microscopic Raman spectroscopy of the niobium-titanium composite oxide powder of the present invention, the Raman spectrum is measured using a laser Raman splitter under the following measurement conditions: laser wavelength 532 nm, beam diameter 4 μm, laser intensity 0.8 mW. The peak separation method is the wavenumber range of 520 to 800 cm of the baseline-corrected Raman spectrum. -1 The peaks are separated using the Lorentzian function as a fitting function. The wavenumber range of the Raman spectrum is 520-800 cm. -1 When the extract is extracted and subjected to peak separation, it is preferable that the area ratio of the two peaks represented by the following formula (III) is 0.5 or more.-1 The peak at 620-680 cm reflects the Ti-O bond. -1 The peaks appearing in reflect the Nb-O bond, and the areas of the two peaks are presumed to represent the strength of each bond in the crystal structure. The change in the area ratio of these two peaks is presumed to be due to a change in the insertion and desorption properties of lithium ions in the crystal structure. It is believed that the insertion and desorption of lithium ions can be controlled by setting the firing temperature and crushing conditions during synthesis within a specific range in accordance with the raw materials, which is why the area ratio of the two peaks has changed. If the intensity ratio is within the above range, the rate characteristics, cycle characteristics, and low-temperature characteristics in liquid nonaqueous electrolyte batteries, as well as the rate characteristics in all-solid-state batteries, can be improved. I(538cm -1 ) / I(650cm -1 ) ≧ 0.5 (III) I(538cm -1 ):520~560cm -1 The area value of the peaks obtained by separating the spectra that appear in I(650cm -1 ):620~680cm -1 The area value of the peaks obtained by separating the spectra that appear in

[0021] <Zeta potential by electrophoresis> In the niobium-titanium composite oxide powder of the present invention, the lower limit of the zeta potential of the niobium-titanium composite oxide powder at 25°C measured by electrophoresis is preferably -65 mV or more, more preferably -55 mV or more, and even more preferably -45 mV or more. The upper limit of the zeta potential is preferably -25 mV or less, more preferably -30 mV or less, and even more preferably -35 mV or less. The zeta potential represents the potential difference between the slip surface in the electric double layer and a portion sufficiently distant from the interface, and this potential difference is the Li + It is presumed that this affects the permeability. The measurement method will be explained in the examples described later.

[0022] <Specific surface area> The specific surface area of ​​the niobium-titanium composite oxide powder of the present invention is the surface area per unit mass when nitrogen is used as the adsorption gas. The measuring method will be explained in the examples described later.

[0023] The niobium-titanium composite oxide powder of the present invention has a specific surface area of ​​8 m 2 / g or less, and it is possible to obtain an electricity storage device with improved rate characteristics in a liquid nonaqueous electrolyte battery and an all-solid-state battery. 2 / g or less is more preferable, and 3.5m 2 The lower limit of the specific surface area is preferably 1 m / g or less, but is not particularly limited. 2 / g or more.

[0024] <d50> D50 of the niobium-titanium composite oxide powder of the present invention is an index of the volume median particle size. It means the particle size at which the cumulative volume frequency calculated from the volume fraction determined by laser diffraction / scattering particle size distribution measurement is 50% when calculated from the smallest particle size. The measurement method will be explained in the examples described later.

[0025] The niobium-titanium composite oxide powder of the present invention may be in the form of primary particles or secondary particles formed by agglomeration of primary particles. When the powder contains secondary particles formed by agglomeration of primary particles made of niobium-titanium composite oxide particles, some of the particles may not form secondary particles and may be in the form of primary particles themselves.

[0026] When the niobium-titanium composite oxide powder of the present invention is a secondary particle, the lower limit of the D50 of the secondary particle is preferably 11 μm or more, more preferably 12 μm or more, and even more preferably 13 μm or more, from the viewpoint of improving the electrode density. Furthermore, the upper limit of the D50 of the secondary particle is preferably 20 μm or less, more preferably 18 μm or less, and even more preferably 14 μm or less. Note that the D50 of the secondary particle represents the D50 before the crushing treatment (ultrasonic application with an ultrasonic device).

[0027] From the viewpoint of improving the rate characteristics in liquid nonaqueous electrolyte batteries and all-solid-state batteries, the lower limit of D50 of the primary particles of the niobium-titanium composite oxide powder of the present invention is preferably 0.4 μm or more, more preferably 0.7 μm or more. The upper limit of D50 of the primary particles is preferably 3 μm or less, more preferably 2.1 μm or less, and even more preferably less than 1 μm. Note that D50 of the primary particles represents D50 after crushing treatment (ultrasonication with an ultrasonic device). The niobium-titanium composite oxide powder may contain primary particles having a primary particle diameter of less than 0.4 μm in the range of 15% to 30%, and may contain primary particles having a primary particle diameter of less than 0.7 μm in the range of 15% to 45%. In addition, the primary particles having a primary particle diameter exceeding 3 μm may be contained in the range of 45% to 75%, the primary particles having a primary particle diameter exceeding 2.1 μm may be contained in the range of 25% to 75%, and the primary particles having a primary particle diameter exceeding 1 μm may be contained in the range of 25% to 80%.

[0028] <dbet> The DBET of the niobium-titanium composite oxide powder of the present invention is a specific surface area equivalent diameter calculated from the specific surface area determined by the BET method. From the viewpoint of achieving high electrode density and improving volumetric energy density, the DBET of the niobium-titanium composite oxide powder of the present invention may be 0.2 μm or more, preferably 0.3 μm or more, and more preferably 0.4 μm or more. The upper limit of the DBET of the niobium-titanium composite oxide powder may be 3 μm or less, preferably 2 μm or less, and more preferably 1.2 μm or less. The DBET of the niobium-titanium composite oxide powder can be determined by the method described in the examples below.

[0029] <d50 dbet> The ratio of D50 to DBET of the primary particles of the niobium-titanium composite oxide powder of the present invention (D50 / DBET (μm / μm)) is 2.1 or less, preferably 2.06 or less, more preferably 2.0 or less, and the lower limit is preferably 1 or more, more preferably 1.3 or more, and even more preferably 1.5 or more, from the viewpoint of improving the rate characteristics in liquid nonaqueous electrolyte batteries and all-solid-state batteries. The D50 / DBET of the niobium-titanium composite oxide powder can be determined by the method described in the examples below.

[0030] <Presence of element M1 on the particle surface> The niobium-titanium composite oxide powder of the present invention may have element M1 (including any one or more selected from the group of elements consisting of aluminum (Al), magnesium (Mg), cerium (Ce), and molybdenum (Mo)) present on the particle surface. Two or more of these elements may be contained. The presence of element M1 means that element M1 is detected in inductively coupled plasma atomic emission spectrometry (ICP-AES) or X-ray fluorescence spectrometry (XRF) of the niobium oxide powder of the present invention. The lower limit of the amount detectable by inductively coupled plasma atomic emission spectrometry is usually 0.001 mass%.

[0031] <Content of element M1> When the niobium-titanium composite oxide powder of the present invention contains element M1, its content (mass%) is preferably 0.01 to 0.8. If the content of element M1 is within this range, the rate characteristics and cycle characteristics in a liquid nonaqueous electrolyte battery, and the rate characteristics in an all-solid-state battery can be improved. It is more preferably 0.05 to 0.5, and from the viewpoint of further improving the discharge rate characteristics and further enhancing the low-temperature characteristics, it is even more preferably 0.2 to 0.5, and even more preferably 0.3 to 0.4.

[0032] In addition, when the niobium-titanium composite oxide powder of the present invention contains the element M1, the element M1 is localized and exists more in the surface region than in the internal region of the niobium-titanium composite oxide particles constituting the powder. That is, the element M1 is present on the surface of the niobium-titanium composite oxide particles, and more specifically, the element M1 is localized and exists more in the surface region than in the internal region of the niobium-titanium composite oxide particles. As an example, in a cross-sectional analysis of the niobium-titanium composite oxide particles using a scanning transmission electron microscope, it is sufficient that the element M1 is contained in a large amount in the so-called near-surface region from the surface of the niobium oxide particles to a depth of about 20 nm measured by energy dispersive X-ray spectroscopy, and it is preferable that the element M1 is not detected at a depth position of 100 nm from the surface. That is, when measured by energy dispersive X-ray spectroscopy, it means that it is below the amount detected by the measurement, and the lower limit of the detection amount in the measurement by energy dispersive X-ray spectroscopy is usually 0.5 atm%, although the value varies depending on the element and state to be measured. Other surface analysis techniques include X-ray photoelectron spectroscopy (XPS) and Auger electron spectroscopy (AES).

[0033] <Inclusion of further heterogeneous elements> The niobium-titanium composite oxide powder of the present invention may contain at least one element selected from the group consisting of B, Mo, W, and S as a further different element other than the element M1. Of these, S is particularly preferred. It is presumed that the niobium-titanium composite oxide powder of the present invention contains such a different element together with the element M1, thereby improving the electronic conductivity of the surface of the niobium-titanium composite oxide powder compared to when the niobium-titanium composite oxide powder contains only the element M1.

[0034] [Method of producing niobium-titanium composite oxide powder of the present invention] An example of the method for producing the niobium-titanium composite oxide powder of the present invention will be described below, divided into a raw material preparation step, a firing step, and a surface treatment step; however, the method for producing the niobium-titanium composite oxide powder of the present invention is not limited thereto.

[0035] <Raw material preparation process> First, the starting materials are mixed. As the starting material, an oxide or salt containing Ti and Nb is used. Here, as the oxide containing Nb, it is preferable to use orthorhombic Nb2O5. In addition, when other additive elements of the niobium-titanium composite oxide are included, an oxide or salt containing at least one element selected from the group consisting of Zr, Si, Sn, V, Ta, Bi, Mo, and W is used as the starting material in addition to the oxide containing Ti and Nb, and mixed in a stoichiometric ratio to obtain the target composition of the present invention. The salt used as the starting material is preferably a salt that decomposes at a relatively low melting point to produce an oxide, such as a hydroxide salt, carbonate salt, or nitrate salt. In addition, in order to reduce the primary particle size, it is preferable to use a powder having an average primary particle size of 2 μm or less, preferably an average primary particle size of 0.5 μm or less, as the starting material. In some cases, a compound containing the element M1 is added before the firing step described below.

[0036] The method for mixing the raw materials is not particularly limited, and either wet mixing or dry mixing may be used. For example, a Henschel mixer, an ultrasonic dispersing device, a homomixer, a mortar, a ball mill, a centrifugal ball mill, a planetary ball mill, a vibration ball mill, an attritor type high speed ball mill, a bead mill, a roll mill, etc. may be used.

[0037] <Firing process> Next, the mixture obtained above is fired. The firing is performed in a temperature range of 500 to 1200°C, more preferably in a temperature range of 700 to 1150°C, even more preferably in a temperature range of 1100 to 1150°C or less, and even more preferably in a temperature range of 1120 to 1150°C or less, depending on the raw material used. By performing the firing at a temperature of 1150°C or less, general-purpose equipment can be used. When the mixture is fired in a short time, it is preferable to prepare the mixed powder constituting the mixture before firing so that D95 in the particle size distribution curve measured by a laser diffraction / scattering type particle size distribution measuring device is 5 μm or less. Here, D95 refers to the particle size at which the cumulative volume frequency calculated by volume fraction is 95% when integrated from the smallest particle size.

[0038] The calcination method is not particularly limited as long as it can be performed under the above conditions. Examples of calcination methods that can be used include a fixed bed calcination furnace, a roller hearth calcination furnace, a mesh belt calcination furnace, a fluidized bed calcination furnace, and a rotary kiln calcination furnace. However, in the case of performing efficient calcination in a short time, a roller hearth calcination furnace, a mesh belt calcination furnace, and a rotary kiln calcination furnace are preferred. In particular, a rotary kiln calcination furnace is a particularly preferred calcination furnace for producing the niobium-titanium composite oxide powder of the present invention, since it does not require a container for storing the mixture, it is possible to calcinate while continuously feeding the mixture, the thermal history of the calcined material is uniform, and a homogeneous oxide can be obtained.

[0039] <Crushing process> The niobium-titanium composite oxide powder after calcination may be subjected to a crushing treatment to obtain the desired particle size. Methods for crushing the calcined product recovered from the calcined product recovery side include a hammer mill, a ball mill, a jet mill, a vibration mill, a bead mill, etc., and a bead mill is particularly preferred. As a crushing method when a bead mill is used, any of the following methods can be adopted: circulation treatment of wet crushing, batch treatment of wet crushing or circulation treatment of dry crushing, and batch treatment of dry crushing. However, it is preferable to perform the crushing uniformly, and in this respect, circulation treatment of wet crushing is preferred. The circulation conditions may be determined in consideration of the calcination temperature in the calcination step, and for example, the particle size of the niobium-titanium composite oxide powder can be suitably controlled by adjusting the circulation conditions. For wet crushing, the calcined lithium titanate powder is put into water or an alcohol solvent and mixed in a slurry state. As the alcohol solvent, those with a boiling point of 100°C or less, such as methanol, ethanol, and isopropyl alcohol, are preferred in that they are easy to remove the solvent. Moreover, from an industrial perspective, a water solvent is preferred because of the ease of recovery and disposal.

[0040] <Surface treatment process> The niobium-titanium composite oxide obtained above may be subjected to a surface treatment. The niobium-titanium composite oxide of the present invention may have element M1 (M1 includes at least one selected from the group of elements consisting of aluminum (Al), magnesium (Mg), cerium (Ce), and molybdenum (Mo)) present on the surface of the particles, and when used as a negative electrode material for a battery, a dense negative electrode layer can be formed and excellent charge rate characteristics can be imparted. In the firing step, a compound containing the element M1 (hereinafter, sometimes referred to as a treatment agent) can be added to produce the niobium-titanium composite oxide powder of the present invention, but more preferably, the niobium-titanium composite oxide powder of the present invention can be produced by the following surface treatment step or the like. In particular, by adopting the following surface treatment step, the element M1 can be present on the surface of the niobium-titanium composite oxide particles appropriately and relatively easily.

[0041] There is no particular limitation on the method for mixing the niobium-titanium composite oxide powder as the base material with the compound containing the element M1, and either wet mixing or dry mixing can be used. However, it is preferable to uniformly disperse the compound containing the element M1 on the surfaces of the particles constituting the niobium-titanium composite oxide powder as the base material, and in this respect, wet mixing is preferred.

[0042] In the wet mixing, the treatment agent 2 and the niobium-titanium composite oxide powder of the substrate are put into a water or alcohol solvent and mixed in a slurry state. As the alcohol solvent, those with a boiling point of 100°C or less, such as methanol, ethanol, and isopropyl alcohol, are preferred because they are easy to remove. Also, from an industrial perspective, water solvents are preferred because they are easy to recover and dispose of.

[0043] Compounds (treatment agents) containing element M1 (M1 includes at least one selected from the group of elements consisting of aluminum (Al), magnesium (Mg), cerium (Ce), and molybdenum (Mo)) are not particularly limited, and examples thereof include oxides, phosphoric oxides, hydroxides, sulfate compounds, nitrate compounds, fluorides, chlorides, organic compounds, and metal salt compounds such as ammonium salts and phosphates. Specifically, when the element M1 is Al, examples thereof include aluminum oxide, aluminum phosphate, aluminum hydroxide, aluminum sulfate, aluminum nitrate, aluminum fluoride, aluminum chloride, aluminum acetate, ammonium aluminum sulfate, and aluminum alkoxides, and among these, aluminum sulfate and its hydrates are preferred. When the element M1 is Mg, examples thereof include magnesium oxide, magnesium phosphate, magnesium hydroxide, magnesium sulfate, magnesium nitrate, magnesium fluoride, magnesium chloride, magnesium acetate, ammonium magnesium phosphate, and magnesium alkoxides, and among these, magnesium sulfate and its hydrates are preferred. When the element M1 is Ce, examples of the cerium oxide include cerium oxide, cerium hydroxide, cerium fluoride, cerium sulfate, cerium nitrate, cerium carbonate, cerium acetate, cerium oxalate, cerium chloride, cerium boride, and cerium phosphate. Of these, cerium sulfate and its hydrates are preferred. When the element M1 is Mo, examples of the compound include molybdenum oxide, molybdenum trioxide, molybdenum trioxide hydrate, molybdenum boride, molybdic phosphomolybdic acid, molybdenum disilicide, molybdenum chloride, molybdenum sulfide, molybdic silicic acid hydrate, sodium molybdenum oxide, molybdenum carbide, molybdenum acetate dimer, lithium molybdate, sodium molybdate, potassium molybdate, calcium molybdate, magnesium molybdate, manganese molybdate, and ammonium molybdate. Of these, molybdenum trioxide, molybdenum trioxide hydrate, molybdenum chloride, molybdenum sulfide, and lithium molybdate are preferred.

[0044] The amount of the compound containing the element M1 added may be any amount as long as the amount of the metal element M1 in the niobium-titanium composite oxide falls within the range of the present invention, but it may be added in a proportion of 0.1 mass% or more relative to the niobium-titanium composite oxide powder substrate. Also, it is preferably added in a proportion of 12 mass% or less relative to the niobium-titanium composite oxide powder substrate, more preferably 10 mass% or less, and even more preferably 8 mass% or less.

[0045] <Heat treatment process> It is preferable to perform heat treatment on the niobium-titanium composite oxide powder of the present invention after synthesis. The heat treatment temperature is preferably a temperature at which the niobium-titanium composite oxide of the base material is sintered and thus the particle size growth and the specific surface area are not significantly reduced. The upper limit of the heat treatment temperature is preferably 700°C or less, more preferably 650°C or less. The lower limit of the heat treatment temperature is preferably 300°C or more, more preferably 400°C or more. The heat treatment time is preferably 0.1 to 8 hours, more preferably 0.5 to 5 hours. In addition, when the above surface treatment is performed using a compound containing a metal element M1, the temperature and time at which the metal element diffuses into at least the surface region of the niobium-titanium composite oxide powder of the base material should be appropriately set because the reactivity differs depending on the compound containing the metal element. In addition, the heating method in the heat treatment is not particularly limited. Examples of heat treatment furnaces that can be used include fixed bed type firing furnaces, roller hearth type firing furnaces, mesh belt type firing furnaces, fluidized bed type firing furnaces, and rotary kiln type firing furnaces. The atmosphere during the heat treatment may be either an air atmosphere or an inert atmosphere such as a nitrogen atmosphere. In particular, when a metal salt compound is used for the surface treatment, an air atmosphere is preferred in which anion species are easily removed from the particle surface.

[0046] The niobium-titanium composite oxide powder obtained after the heat treatment as described above has slight agglomerations, but does not need to be pulverized to destroy the particles. Therefore, after the heat treatment, it is sufficient to carry out disintegration or classification to the extent that agglomerations are broken down, if necessary.

[0047] The niobium-titanium composite powder of the present invention may be mixed with a treatment agent in a surface treatment step, granulated, and heat-treated to form a powder containing secondary particles formed by aggregation of primary particles. Any method for granulation may be used as long as secondary particles can be produced, but a spray dryer is preferred because it can process large quantities.

[0048] In order to reduce the amount of moisture contained in the niobium-titanium composite oxide powder of the present invention, dew point control may be performed in the heat treatment process. If the heat-treated powder is exposed to the air as it is, moisture in the air will be adsorbed by the powder, so it is preferable to handle the powder in a dew point controlled environment during cooling in the heat treatment furnace and after the heat treatment. The heat-treated powder may be classified as necessary to make the particles within the desired maximum particle size range. When dew point control is performed in the heat treatment process, it is preferable to seal the niobium-titanium composite oxide powder of the present invention in an aluminum laminate bag or the like and then place it in an environment outside of dew point control. Even under dew point control, if the heat-treated niobium-titanium composite oxide powder is pulverized, moisture will be easily absorbed from the crushed surface, and the amount of moisture contained in the powder will increase, so it is preferable not to pulverize the powder after heat treatment. As for the heat treatment conditions, the temperature and holding time in a specific range greatly affect the secondary particle morphology and the surface treatment process. The heat treatment temperature is preferably 450°C or higher, and preferably less than 550°C. This is because the specific surface area decreases significantly when the heat treatment temperature exceeds 550°C, and the battery performance, especially the rate characteristics, decreases significantly. Also, the holding time is preferably 1 hour or more, because if the holding time is short, the amount of moisture contained in the powder increases and it is thought that it also affects the particle surface state.

[0049] [Active material] The active material of the present invention contains the niobium-titanium composite oxide powder of the present invention. It may contain one or more substances other than the niobium-titanium composite oxide powder of the present invention. Examples of other substances include carbon materials (pyrolytic carbons, cokes, graphites (artificial graphite, natural graphite, etc.), organic polymer compound combustion bodies, carbon fibers), tin and tin compounds, silicon and silicon compounds, and metal oxides containing lithium. In particular, Li4Ti5O 12 Lithium titanate having the main component is exemplified.

[0050] [Electricity storage device] The electricity storage device of the present invention is a device that includes an electrode containing the active substance material of the present invention and stores and releases energy by utilizing the intercalation and deintercalation of lithium ions into such an electrode, and examples of such a device include a hybrid capacitor and a lithium battery.

[0051] [Lithium battery] The lithium battery of the present invention is a general term for lithium primary batteries and lithium secondary batteries. In this specification, the term lithium secondary battery is used as a concept including so-called lithium ion secondary batteries and all-solid-state lithium ion secondary batteries.

[0052] The lithium battery is composed of a positive electrode, a negative electrode, and a non-aqueous electrolyte in which an electrolyte salt is dissolved in a non-aqueous solvent, or a solid electrolyte, and the active material of the present invention can be used as an electrode material. The active material of the present invention is usually used in the form of an electrode sheet for the lithium battery. This active material may be used as either a positive electrode active material or a negative electrode active material, but the following description will be given of the case where it is used as a negative electrode active material.

[0053] <Negative electrode> The negative electrode has a negative electrode layer containing a negative electrode active material (the active material of the present invention), a conductive agent, and a binder on one or both sides of a negative electrode current collector. This negative electrode layer is usually in the form of an electrode sheet. In the case of a negative electrode current collector having pores such as a porous body, the negative electrode layer contains a negative electrode active material (the active material of the present invention), a conductive agent, and a binder in the pores.

[0054] The conductive agent for the negative electrode is not particularly limited as long as it is an electron conductive material that does not undergo chemical changes. For example, graphites such as natural graphite (e.g., flake graphite) and artificial graphite, carbon blacks such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, carbon nanotubes such as single-phase carbon nanotubes, multi-walled carbon nanotubes (graphite layers are multi-layered concentric cylinders) (non-fishbone-shaped), cup-stacked carbon nanotubes (fishbone-shaped), nodular carbon nanofibers (non-fishbone structure), and platelet-type carbon nanofibers (playing cards), etc. may be used in combination with graphites, carbon blacks, and carbon nanotubes. Although not particularly limited, the specific surface area of ​​the carbon blacks is preferably 30 m 2 / g~3000m 2 / g, and more preferably 50m 2 / g~2000m 2 The specific surface area of ​​the graphite is preferably 30 m 2 / g~600m 2 / g, and more preferably 50m 2 / g~500m 2 The aspect ratio of the carbon nanotubes is 2-150, preferably 2-100, and more preferably 2-50.

[0055] The amount of conductive agent added should be optimized because it varies depending on the specific surface area of ​​the active material and the type and combination of conductive agents. It is preferably 0.1% by mass to 10% by mass, more preferably 0.5% by mass to 5% by mass in the negative electrode layer. If it is less than 0.1% by mass, the conductivity of the negative electrode layer cannot be ensured, and if it exceeds 10% by mass, the active material ratio decreases, and the discharge capacity of the power storage device per unit mass and unit volume of the negative electrode layer becomes insufficient, so it is not suitable for increasing the capacity. The conductive agent may be added when the electrode is prepared, or may be coated on the active material itself. This is because the conductivity of the negative electrode layer can be further improved by coating with a conductive agent such as carbon fiber.

[0056] Examples of the binder for the negative electrode include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylpyrrolidone (PVP), styrene-butadiene copolymer (SBR), acrylonitrile-butadiene copolymer (NBR), and carboxymethyl cellulose (CMC). Although not particularly limited, the molecular weight of polyvinylidene fluoride is preferably 20,000 to 1,000,000. From the viewpoint of ensuring the binding property of the negative electrode layer, it is preferably 25,000 or more, more preferably 30,000 or more, and even more preferably 50,000 or more. From the viewpoint of ensuring conductivity without interfering with the contact between the active material and the conductive agent, it is preferably 500,000 or less. In particular, when the specific surface area of ​​the active material is 10 m 2 In the case where the molecular weight is 1 / g or more, the molecular weight is preferably 100,000 or more.

[0057] The amount of binder added should be optimized since it varies depending on the specific surface area of ​​the active material and the type and combination of the conductive agent, but is preferably 0.2% by mass to 15% by mass in the negative electrode layer. From the viewpoint of increasing the binding property and ensuring the strength of the negative electrode layer, it is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more. From the viewpoint of preventing a decrease in the active material ratio and a decrease in the discharge capacity of the power storage device per unit mass and unit volume of the negative electrode layer, it is preferably 10% by mass or less, and more preferably 5% by mass or less.

[0058] Examples of the negative electrode current collector include aluminum, stainless steel, nickel, copper, titanium, baked carbon, or those coated with carbon, nickel, titanium, or silver. The surface of these materials may be oxidized, or the surface of the negative electrode current collector may be roughened by surface treatment. Examples of the form of the negative electrode current collector include a sheet, net, foil, film, punched, lath, porous body, foam, fiber group, and nonwoven fabric molded body. Porous aluminum is preferred as the form of the negative electrode current collector. The porosity of the porous aluminum is 80% or more and 95% or less, and preferably 85% or more.

[0059] The negative electrode can be produced by uniformly mixing the negative electrode active material (including the active material of the present invention), the conductive agent, and the binder in a solvent to prepare a paint, which is then applied to the negative electrode current collector, dried, and compressed. In the case of a negative electrode current collector having pores, such as a porous body, the paint is pressed into the pores of the current collector to fill the pores, or the current collector having pores is immersed in the paint to diffuse the pores, and then dried and compressed.

[0060] As a method for uniformly mixing the negative electrode active material (the active material of the present invention), the conductive agent, and the binder in a solvent to prepare a paint, for example, a kneader of the type in which a stirring rod revolves while rotating in a kneading vessel such as a planetary mixer, a twin-screw extrusion type kneader, a planetary stirring defoamer, a bead mill, a high-speed rotating type mixer, a powder suction continuous dissolution and dispersion device, etc. Also, as a manufacturing process, the process may be divided according to the solid content concentration, and these devices may be used separately.

[0061] In order to mix the negative electrode active material (the active material of the present invention), the conductive agent and the binder uniformly in the solvent, the mixing should be optimized because it depends on the specific surface area of ​​the active material, the type of conductive agent, the type of binder and the combination of these. However, when using a kneader in which the stirring rod revolves while rotating in a kneading container such as a planetary mixer, a twin-screw extrusion type kneader, a planetary stirring degassing device, etc., it is preferable to divide the steps according to the solid content concentration in the manufacturing process, knead the mixture in a state where the solid content concentration is high, and then gradually reduce the solid content concentration to adjust the viscosity of the paint. The high solid content concentration is preferably 60% by mass to 90% by mass, more preferably 60% by mass to 80% by mass. If it is 60% by mass or more, it is preferable because shear force can be obtained, if it is 90% by mass or less, it is preferable because the load on the device is reduced, and if it is 80% by mass or less, it is more preferable.

[0062] The mixing procedure is not particularly limited, but examples thereof include a method of simultaneously mixing the negative electrode active material, the conductive agent, and the binder in a solvent, a method of previously mixing the conductive agent and the binder in a solvent and then adding and mixing the negative electrode active material, a method of previously preparing a negative electrode active material slurry, a conductive agent slurry, and a binder solution, and then mixing each of them, etc. Among these, in order to disperse them uniformly, a method of previously mixing the conductive agent and the binder in a solvent and then adding and mixing the negative electrode active material, and a method of previously preparing a negative electrode active material slurry, a conductive agent slurry, and a binder solution, and then mixing each of them are preferred.

[0063] As the solvent, an organic solvent can be used. Examples of the organic solvent include aprotic organic solvents such as 1-methyl-2-pyrrolidone, dimethylacetamide, and dimethylformamide, which may be used alone or in combination of two or more kinds, and preferably 1-methyl-2-pyrrolidone.

[0064] When an organic solvent is used as the solvent, it is preferable to dissolve the binder in the organic solvent before use.

[0065] <Positive electrode> The positive electrode has a positive electrode layer containing a positive electrode active material, a conductive agent, and a binder on one or both sides of a positive electrode current collector.

[0066] As the positive electrode active material, a material capable of absorbing and releasing lithium is used. For example, the active material may be a composite metal oxide containing lithium and containing cobalt, manganese, or nickel, or a lithium-containing olivine-type phosphate. These positive electrode active materials may be used alone or in combination of two or more. Examples of such composite metal oxides include LiCoO2, LiMn2O4, LiNiO2, LiCo 1-x Ni x O2(0.01 <x<1)、LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, LiNi 1 / 2 Mn 3 / 2 O4, etc., and these lithium composite oxides may be partially substituted with other elements, and a portion of the cobalt, manganese, and nickel may be partially substituted with at least one element such as B, Nb, Sn, Mg, Fe, Ti, Al, Zr, Cr, V, Ga, Zn, Cu, Bi, Mo, and La, a portion of the O may be substituted with S or F, or a compound containing these other elements may be coated. Examples of lithium-containing olivine-type phosphates include LiFePO4, LiCoPO4, LiNiPO4, LiMnPO4, LiFe 1-x MxPO4 (M is at least one selected from Co, Ni, Mn, Cu, Zn, and Cd, and x is 0≦x≦0.5).

[0067] The conductive agent and binder for the positive electrode may be the same as those for the negative electrode. The positive electrode current collector may be, for example, aluminum, stainless steel, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, or silver. The surface of these materials may be oxidized, or the positive electrode current collector surface may be unevenly formed by surface treatment. The form of the current collector may be, for example, a sheet, a net, a foil, a film, a punched one, a lath body, a porous body, a foam, a fiber group, or a molded body of a nonwoven fabric.

[0068] <Nonaqueous electrolyte> The non-aqueous electrolyte is a non-aqueous solvent having an electrolyte salt dissolved therein. There are no particular limitations on the type of non-aqueous electrolyte, and various types can be used.

[0069] The electrolyte salt used is one that dissolves in a non-aqueous electrolyte, and examples of the electrolyte salt include inorganic lithium salts such as LiPF6, LiBF4, LiPO2F2, LiN(SO2F)2, and LiClO4; lithium salts containing a chain-like fluorinated alkyl group such as LiN(SO2CF3)2, LiN(SO2C2F5)2, LiCF3SO3, LiC(SO2CF3)3, LiPF4(CF3)2, LiPF3(C2F5)3, LiPF3(CF3)3, LiPF3(iso-C3F7)3, and LiPF5(iso-C3F7); lithium salts containing a cyclic fluorinated alkylene chain such as (CF2)2(SO2)2NLi and (CF2)3(SO2)2NLi; and lithium salts having an oxalate complex as the anion, such as lithium bis[oxalate-O,O']borate and lithium difluoro[oxalate-O,O']borate. Among these, particularly preferred electrolyte salts are LiPF6, LiBF4, LiPO2F2, and LiN(SO2F)2, and the most preferred electrolyte salt is LiPF6. These electrolyte salts can be used alone or in combination of two or more. In addition, a suitable combination of these electrolyte salts is preferably a combination containing LiPF6 and at least one lithium salt selected from LiBF4, LiPO2F2, and LiN(SO2F)2 in the non-aqueous electrolyte solution.

[0070] The concentration of all of these electrolyte salts dissolved in the nonaqueous solvent is usually preferably 0.3 M or more, more preferably 0.5 M or more, and even more preferably 0.7 M or more. The upper limit is preferably 2.5 M or less, more preferably 2.0 M or less, and even more preferably 1.5 M or less.

[0071] On the other hand, the non-aqueous solvent may be a cyclic carbonate, a chain carbonate, a chain ester, an ether, an amide, a phosphoric acid ester, a sulfone, a lactone, a nitrile, an S=O bond-containing compound, etc., and preferably contains a cyclic carbonate. The term "chain ester" is used as a concept including a chain carbonate and a chain carboxylate ester.

[0072] Examples of the cyclic carbonate include one or more selected from ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 4-fluoro-1,3-dioxolan-2-one (FEC), trans- or cis-4,5-difluoro-1,3-dioxolan-2-one (hereinafter, both are collectively referred to as "DFEC"), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), and 4-ethynyl-1,3-dioxolan-2-one (EEC). More preferred are at least one selected from ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, 4-fluoro-1,3-dioxolan-2-one and 4-ethynyl-1,3-dioxolan-2-one (EEC) from the viewpoints of improving the charge rate characteristics of the power storage device and suppressing the amount of gas generated during high-temperature operation, and even more preferred are at least one cyclic carbonate having an alkylene chain selected from propylene carbonate, 1,2-butylene carbonate and 2,3-butylene carbonate. The proportion of the cyclic carbonate having an alkylene chain in all the cyclic carbonates is preferably 55% by volume to 100% by volume, and even more preferably 60% by volume to 90% by volume.

[0073] Therefore, the non-aqueous electrolyte is preferably prepared by dissolving an electrolyte salt containing at least one lithium salt selected from LiPF6, LiBF4, LiPO2F2, and LiN(SO2F)2 in a non-aqueous solvent containing one or more cyclic carbonates selected from ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, 4-fluoro-1,3-dioxolan-2-one, and 4-ethynyl-1,3-dioxolan-2-one. The cyclic carbonate is more preferably one or more cyclic carbonates having an alkylene chain selected from propylene carbonate, 1,2-butylene carbonate, and 2,3-butylene carbonate.

[0074] In particular, it is preferable to use a non-aqueous electrolyte solution in which the concentration of the total electrolyte salt is 0.5M to 2.0M, the electrolyte salt contains at least LiPF6, and further contains at least one lithium salt selected from LiBF4, LiPO2F2, and LiN(SO2F)2 at 0.001M to 1M. If the ratio of lithium salts other than LiPF6 in the non-aqueous solvent is 0.001M or more, the effect of improving the charge rate characteristics of the power storage device and suppressing the amount of gas generation during high-temperature operation is easily exhibited, and if it is 1.0M or less, there is little concern that the effect of improving the charge rate characteristics of the power storage device and suppressing the amount of gas generation during high-temperature operation will decrease, which is preferable. The ratio of lithium salts other than LiPF6 in the non-aqueous solvent is preferably 0.01M or more, particularly preferably 0.03M or more, and most preferably 0.04M or more. The upper limit is preferably 0.8M or less, more preferably 0.6M or less, and particularly preferably 0.4M or less.

[0075] In addition, the non-aqueous solvent is preferably used in a mixed state in order to achieve appropriate physical properties. Examples of the combination include a combination of a cyclic carbonate and a chain carbonate, a combination of a cyclic carbonate, a chain carbonate and a lactone, a combination of a cyclic carbonate, a chain carbonate and an ether, a combination of a cyclic carbonate, a chain carbonate and a chain ester, a combination of a cyclic carbonate, a chain carbonate and a nitrile, and a combination of a cyclic carbonate, a chain carbonate and a compound containing an S=O bond.

[0076] Suitable examples of the chain ester include one or more asymmetric chain carbonates selected from methyl ethyl carbonate (MEC), methyl propyl carbonate (MPC), methyl isopropyl carbonate (MIPC), methyl butyl carbonate, and ethyl propyl carbonate; one or more symmetric chain carbonates selected from dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, and dibutyl carbonate; pivalic acid esters such as methyl pivalate, ethyl pivalate, and propyl pivalate; and one or more chain carboxylate esters selected from methyl propionate, ethyl propionate, propyl propionate, methyl acetate, and ethyl acetate (EA).

[0077] Among the chain esters, chain esters having a methyl group selected from dimethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, methyl butyl carbonate, methyl propionate, methyl acetate, and ethyl acetate (EA) are preferred, and chain carbonates having a methyl group are particularly preferred.

[0078] In addition, when chain carbonates are used, it is preferable to use two or more kinds. It is more preferable that both symmetric chain carbonates and asymmetric chain carbonates are contained, and it is even more preferable that the content of the symmetric chain carbonate is higher than that of the asymmetric chain carbonate.

[0079] The content of the chain ester is not particularly limited, but is preferably in the range of 60% by volume to 90% by volume relative to the total volume of the nonaqueous solvent. If the content is 60% by volume or more, the viscosity of the nonaqueous electrolyte does not become too high, and if the content is 90% by volume or less, the electrical conductivity of the nonaqueous electrolyte decreases, which reduces the improvement of the charge rate characteristics of the electricity storage device and the effect of suppressing the amount of gas generation during high-temperature operation, so the above range is preferable.

[0080] The volume ratio of the symmetric chain carbonate in the chain carbonate is preferably 51% by volume or more, more preferably 55% by volume or more. The upper limit is more preferably 95% by volume or less, and even more preferably 85% by volume or less. It is particularly preferable that the symmetric chain carbonate contains dimethyl carbonate. It is more preferable that the asymmetric chain carbonate has a methyl group, and methyl ethyl carbonate is particularly preferable. In the above case, the charging rate characteristic of the power storage device is improved and the effect of suppressing the amount of gas generation during high-temperature operation is improved, which is preferable.

[0081] From the viewpoint of improving the charge rate characteristics of the electricity storage device and increasing the effect of suppressing the amount of gas generated during high-temperature operation, the ratio of cyclic carbonate to chain ester (volume ratio) is preferably 10:90 to 45:55, more preferably 15:85 to 40:60, and particularly preferably 20:80 to 35:65.

[0082] <The structure of a lithium battery> The structure of the lithium battery of the present invention is not particularly limited, and examples include a coin battery having a positive electrode, a negative electrode, and a single-layer or multi-layer separator, and further, a cylindrical battery or a square battery having a positive electrode, a negative electrode, and a roll-shaped separator.

[0083] As the separator, an insulating thin film having a large ion permeability and a predetermined mechanical strength is used. Examples include polyethylene, polypropylene, cellulose paper, glass fiber paper, polyethylene terephthalate, and polyimide microporous membranes, and a multilayer film formed by combining two or more of them can also be used. In addition, the surface of these separators can be coated with resins such as PVDF, silicone resins, and rubber-based resins, or particles of metal oxides such as aluminum oxide, silicon dioxide, and magnesium oxide. The pore size of the separator may be within a range that is generally useful for batteries, for example, 0.01 μm to 10 μm. The thickness of the separator may be within a range that is generally useful for batteries, for example, 5 μm to 300 μm.

[0084] <Solid electrolyte> A solid electrolyte is a solid electrolyte that can move ions inside. In particular, inorganic solid electrolytes are solid in a stationary state, and therefore are not usually dissociated or liberated into cations and anions. There are no particular limitations on the inorganic solid electrolyte as long as it has the conductivity of metal ions belonging to Group 1 of the periodic table, and it is common for inorganic solid electrolytes to have almost no electronic conductivity. Representative examples of inorganic solid electrolytes include (A) sulfide inorganic solid electrolytes and (B) oxide inorganic solid electrolytes. In particular, sulfide solid electrolytes are preferably used because they have high ionic conductivity and can be formed into a dense molded body with few grain boundaries by simply applying pressure at room temperature. The periodic table referred to here refers to the long-period type periodic table.

[0085] The sulfide inorganic solid electrolyte may be a non-crystalline glass, a crystallized glass, or a crystalline material. Specific examples of the sulfide inorganic solid electrolyte include, but are not limited to, the following combinations. Li2S-P2S5, Li2S-P2S5-Al2S3, Li2S-GeS2, Li2S-Ga2S3, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S -GeS2-Sb2S5, Li2S-GeS2-Al2S3, Li2S-SiS2, Li2S-Al2S3, Li2S-SiS2-Al2S3, Li2S-SiS2-P2S5, Li 10 GeP2S 12 .

[0086] Among the above combinations, LPS glass and LPS glass ceramics produced by combining Li2S-P2S5 are preferred. In addition, other sulfide inorganic solid electrolytes such as argerodite-type solid electrolytes such as Li6PS5Cl and Li6PS5Br are also suitable.

[0087] The oxide inorganic solid electrolyte contains oxygen atoms and is a metal iridium that belongs to Group 1 of the periodic table. It is preferable that the material has both on-conductivity and electronic insulation properties.

[0088] As the oxide inorganic solid electrolyte, for example, Li having a LISICON (Lithium super ionic conductor) type crystal structure is used. 3.5 Zinc 0.25 GeO4, La with perovskite crystal structure 0.55 Li 0.35 TiO3, LiTi2P3O with NASICON (sodium super ionic conductor) type crystal structure 12 , Li7La3Zr2O with garnet-type crystal structure 12 (LLZ), lithium phosphate (Li3PO4), lithium phosphate in which some of the oxygen has been replaced with nitrogen, Li3BO3-Li2SO4, Li2O-B2O3-P2O5, Li2O-SiO2, and Li6BaLa2Ta2O 12 etc. are preferred.

[0089] The volume average particle diameter of the inorganic solid electrolyte is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.1 μm or more, and is preferably 100 μm or less, more preferably 50 μm or less. EXAMPLES

[0090] Next, the present invention will be described in more detail with reference to examples and comparative examples. However, the present invention is not limited to the following examples and includes various combinations that can be easily inferred from the gist of the invention.

[0091] (Lithium-ion secondary battery: coin battery) [Example 1-1] The niobium raw material was orthorhombic Nb2O5 (average particle size 0.2 μm), and the titanium raw material was anatase type TiO2 (specific surface area 10 m 2 / g, Zr content 238 ppm) were weighed out in a molar ratio of 1:1 and mixed. This mixed powder was subjected to a calcination treatment at 1,150°C for 5 hours. Powder X-ray diffraction measurement was performed on the obtained calcined powder sample under conditions of a sampling interval of 0.01° and a scan speed of 2° / min. From the results of crystal structure analysis by the Rietveld method, it was confirmed that the synthesized sample was the desired titanium-niobium composite oxide (TiNb2O7: Titanium niobium oxide, PDF card 01-077-1374 of ICDD (PDF2010)). The obtained calcined powder sample was used as the titanium-niobium composite oxide powder according to Example 1-1.

[0092] [Examples 1-2 to 1-3] The titanium-niobium composite oxide powder according to Example 1-2 or 1-3 was synthesized in the same manner as in Example 1-1, except that the niobium raw material was changed to orthorhombic+monoclinic or amorphous as shown in Table 1.

[0093] [Examples 1-4] The calcined powder sample obtained in Example 1-1 was subjected to a surface treatment process and a heat treatment process. Specifically, the calcined powder sample obtained in Example 1-1 was used, and ion-exchanged water was added and stirred to disintegrate the slurry so that the solid content concentration was 30 mass%, and aluminum sulfate 16-hydrate (Al2(SO4)3·16H2O) was added as a treatment agent at 1.6 mass% per 100 g of the disintegrated calcined powder to prepare a mixed slurry. After mixing, the mixed slurry was dried at a temperature of 60°C, and then heat-treated in a muffle furnace at 550°C for 1 hour to synthesize the titanium-niobium composite oxide powder according to Example 1-4.

[0094] [Examples 1-5] The titanium-niobium composite oxide powder was synthesized in the same manner as in Example 1-1, except that the firing temperature was changed to 1,125°C, and then a crushing process (using zirconia beads (φ2.0 mm) in a paint shaker device at a motor rotation frequency of 60 Hz for 60 minutes) was carried out. Thereafter, as a heat treatment process, a heat treatment was carried out at 650°C for 1 hour in a muffle furnace, thereby synthesizing the titanium-niobium composite oxide powder according to Example 1-5.

[0095] [Examples 1-6 to 1-7] The titanium-niobium composite oxide powders of Examples 1-6 and 1-7 were synthesized in the same manner as in Example 1-5, except that a surface treatment step was carried out as shown in Table 1, aluminum sulfate hexadecahydrate (Al2(SO4)3·16H2O) or magnesium sulfate heptahydrate (MgSO4·7H2O) was added as a treatment agent in an amount of 1.6 mass% per 100 g of the crushed fired powder, and a heat treatment step was carried out at 550°C.

[0096] [Examples 1-8] As shown in Table 1, the procedure was the same as in Example 1-1 except that the firing temperature was changed to 1,125°C and a crushing process (using zirconia beads (φ2.0 mm) in a bead mill for 40 minutes) was carried out, to synthesize the titanium-niobium composite oxide powder of Example 1-8.

[0097] [Examples 1-9] As shown in Table 1, the procedure was the same as in Example 1-1 except that the firing temperature was changed to 1,125°C and a crushing process (using zirconia beads (φ2.0 mm) in a bead mill for 120 minutes) was carried out, to synthesize the titanium-niobium composite oxide powder of Example 1-9.

[0098] [Examples 1-10 to 1-11] As shown in Table 1, the titanium-niobium composite oxide powder of Example 1-10 or Example 1-11 was synthesized in the same manner as in Example 1-8 or Example 1-9, except that after the crushing step, a heat treatment was added as a heat treatment step at 650°C for 1 hour using a muffle furnace.

[0099] [Examples 1-12] Nb2O5 and anatase type TiO2 were weighed and mixed in a molar ratio of 7:18. The mixed powder was sintered at 1,050℃ for 12 hours to obtain the desired titanium-niobium composite oxide (Ti2Nb 10 O 29 ) was obtained, and thus the resulting powder was designated as titanium-niobium composite oxide powder according to Example 1-12.

[0100] [Examples 1-13] Nb2O5 and anatase type TiO2 were weighed and mixed in a molar ratio of 1:7. The mixed powder was sintered at 1,100℃ for 12 hours to obtain the desired titanium-niobium composite oxide (TiNb 14 O 37 ) was obtained, and thus the resulting powder was designated as titanium-niobium composite oxide powder according to Example 1-13.

[0101] [Examples 1-14] Nb2O5 and anatase type TiO2 were weighed and mixed in a molar ratio of 2:3. This mixed powder was calcined at 1,100°C for 12 hours to obtain the desired titanium-niobium composite oxide (Ti2Nb6O 19 ) was obtained, and thus the resulting powder was designated as titanium-niobium composite oxide powder according to Example 1-14.

[0102] [Comparative Example 1-1] Nb2O5 and anatase type TiO2 were weighed and mixed in a molar ratio of 1:1. This mixed powder was subjected to a firing treatment at 1000°C for 5 hours, and a crushing process (using zirconia beads (φ2.0 mm) in a bead mill for 40 minutes) was carried out to synthesize a titanium-niobium composite oxide powder according to Comparative Example 1-1.

[0103] [Comparative Example 1-2] The surface treatment process and the heat treatment process were carried out on the calcined powder sample obtained in Comparative Example 1-1. Specifically, the calcined powder sample obtained in Comparative Example 1-1 was used, and ion-exchanged water was added and stirred to disintegrate the slurry so that the solid content concentration was 30 mass%, and magnesium sulfate heptahydrate (MgSO4·7H2O) was added at 1.6 mass% to 100 g of the disintegrated calcined powder to prepare a mixed slurry. After mixing and processing, this mixed slurry was dried at a temperature of 60°C, and then heat-treated at 550°C for 1 hour in a muffle furnace to synthesize the titanium-niobium composite oxide powder according to Comparative Example 1-2.

[0104] [Comparative Example 1-3] As shown in Table 1, except that the firing temperature was changed to 1,000° C., the same procedure as in Example 1-2 was carried out to synthesize a titanium-niobium composite oxide powder according to Comparative Example 1-3.

[0105] [Comparative Example 1-4] As shown in Table 1, except that the firing temperature was changed to 1,000° C., the same procedure as in Example 1-3 was carried out to synthesize a titanium-niobium composite oxide powder according to Comparative Example 1-4.

[0106] [Comparative Example 1-5] In the raw material preparation process, orthorhombic Nb2O5 (average particle size 0.2 μm) and anatase type TiO2 (specific surface area 10 m 2 Further, 1.4 mass% of aluminum oxide (Al2O3) was mixed in. This powder was subjected to a calcination treatment at 1,150°C for 5 hours to synthesize a titanium-niobium composite oxide powder according to Comparative Example 1-5.

[0107] [Measurement of powder properties] Various physical properties of the titanium-niobium composite oxide powders of the respective Examples and Comparative Examples were measured as follows.

[0108] <Measurement of specific surface area (BET)> The specific surface area (BET) (m 2 The specific surface area (g) was measured using a fully automatic BET specific surface area measuring device (manufactured by Mountec Co., Ltd., product name "Macsorb HM model-1208") and nitrogen gas was used as the adsorption gas. 0.5 g of the measurement sample powder was weighed out and placed in a φ12 standard cell (HM1201-031), and after degassing for 0.5 hours under vacuum at 100°C, it was measured by the BET single point method. The results are shown in Tables 1 and 4.

[0109] <dbet> The DBET of the titanium-niobium composite oxide powders in each example and comparative example was determined from the following formula on the assumption that all the particles constituting the powder were spheres of the same diameter. The results are shown in Tables 1 and 4. DBET = 6 / (ρ × S) Here, ρ is the true density (g / cc) of each titanium-niobium composite oxide powder, and S is the BET specific surface area (m 2 / g).

[0110] <Calculation of D50: Dry laser diffraction scattering method> The D50 of the titanium-niobium composite oxide powders in each example and comparative example was calculated from the particle size distribution curve measured using a laser diffraction / scattering type particle size distribution analyzer (Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd.). 50 mg of the sample was put into a container containing 50 ml of ion-exchanged water as the measurement solvent, and the measurement solvent was added until the transmittance of the slurry was within the appropriate range (the range indicated by the green bar of the apparatus) to perform the particle size distribution measurement. The D50 of the powder was calculated from the obtained particle size distribution curve.

[0111] <Calculation of D50 / DBET> Using the values of D50 and DBET obtained in the above measurement, D50 / DBET was calculated. The results are shown in Tables 1 and 4.

[0112] <Calculation of peak intensity ratio I(24deg) / I(26deg) in powder X-ray diffraction measurement> For the titanium-niobium composite oxide powders in each example and comparative example, powder X-ray diffraction measurement was carried out using a multi-purpose powder X-ray diffractometer (MiniFlex600 manufactured by Rigaku Corporation) under the conditions of a sampling interval of 0.01° and a scan rate of 2° / min. The peak intensities appearing within the range of 2θ of 24.0° ± 0.1° or 26.0 ± 0.2° were taken as I(24deg) or I(26deg), respectively, and the results of calculating the respective intensity ratios as I(24deg) / I(26deg) are shown in Tables 1, 3, and 4.

[0113] <Calculation of spectral peak intensity ratio in microscopic Raman spectroscopy measurement> For the titanium-niobium composite oxide powder of each Example and Comparative Example, Raman spectrum was measured using a laser Raman analyzer (manufactured by JASCO Corporation, NRS-3300) under conditions of a laser wavelength of 532 nm, a beam diameter of 4 μm, and a laser intensity of 0.8 mW. -1 The intensity of peak A appearing at 260-280 cm is I(A), -1 The intensity ratio of the two peaks, I(A) / I(C), was calculated using the intensity of peak C appearing in the figure as I(C), and the results are shown in Tables 1, 3, and 4.

[0114] <Zeta potential results by electrophoresis> The zeta potential of the titanium-niobium composite oxide powder of each Example and Comparative Example was measured by electrophoresis using a zeta potential measuring device (manufactured by Malvern, device name "Zetasizer Nano ZS"). 0.02 g of the titanium-niobium composite oxide powder was weighed out and placed in 200 mL of ion-exchanged water, and the results of measurement in an environment of 25°C are shown in Tables 1 and 4.

[0115] [Evaluation of battery characteristics] Coin-type batteries were fabricated using the titanium-niobium composite oxide powders of each of the Examples and Comparative Examples, and their battery characteristics were evaluated. The evaluation results are shown in Tables 2 and 3.

[0116] <Preparation of negative electrode sheet> The negative electrode sheet was prepared as follows in a room controlled at a room temperature of 25°C and a dew point of -20°C or less. A paint was prepared by mixing 85% by mass of the titanium-niobium composite oxide powder of each Example and Comparative Example as an active material, 10% by mass of acetylene black as a conductive agent, and 5% by mass of polyvinylidene fluoride as a binder. The obtained paint was applied to an aluminum foil and dried to prepare a negative electrode sheet to be used in a coin battery described later.

[0117] <Preparation of electrolyte> The electrolyte used in the battery for characteristic evaluation was prepared by preparing a non-aqueous solvent of ethylene carbonate (EC): dimethyl carbonate (DMC) = 1: 2 (volume ratio), and dissolving LiPF6 as an electrolyte salt in this to a concentration of 1 M to prepare the electrolyte for the coin battery described below. Similarly, a non-aqueous solvent of propylene carbonate (PC): diethyl carbonate (DEC) = 1: 2 (volume ratio) was prepared, and dissolving LiPF6 as an electrolyte salt in this to a concentration of 1.3 M to prepare the electrolyte for the laminate battery described below.

[0118] <Preparation of a coin monopolar battery> The negative electrode sheet prepared by the above method was punched into a circle with a diameter of 14 mm and a thickness of 2 t / cm 2 The electrode was pressed at a pressure of 1000 MPa and then vacuum dried at 120° C. for 5 hours to prepare an evaluation electrode. The evaluation electrode and metallic lithium (formed into a circle with a thickness of 0.5 mm and a diameter of 16 mm) were placed opposite each other via glass filters (one each of ADVANTEC GA-100 and Whatman GF / C), and the nonaqueous electrolyte prepared by the method described above in <Preparation of electrolyte> was added and sealed to prepare a 2032-type coin single-electrode battery.

[0119] <Initial characteristics of coin single-electrode batteries: Measurement of initial efficiency, initial discharge capacity, 10C discharge rate characteristics, and 5C-CC charge rate characteristics> The coin-type battery prepared by the method described above in <Preparation of a Coin Single-Electrode Battery> was placed in a thermostatic chamber at 25°C and charged at 0.2 mA / cm in the direction in which Li was absorbed into the evaluation electrode. 2 The battery was charged to 1 V at a current density of 0.05 mA / cm at 1 V. 2 After constant current and constant voltage charging, the battery was charged to a current density of 0.2 mA / cm 2 A constant current discharge was performed for three cycles, discharging to 2V at a current density of 10 ... If titanium-niobium composite oxide powder has high charge / discharge characteristics at high rates, it is expected that when it is used as an electrode material for an electricity storage device, it will improve the charge / discharge rate characteristics of the device. Note that the "C" in 1C represents the current value when charging / discharging. For example, 1C refers to the current value at which the theoretical capacity can be fully discharged (or fully charged) in 1 / 1 hour, and 0.1C refers to the current value at which the theoretical capacity can be fully discharged (or fully charged) in 1 / 0.1 hour.

[0120] <Coin cell single-electrode battery cycle characteristics: Measurement of cycle capacity retention rate> A cycle characteristic test was carried out using the coin battery prepared by the method described in the above <Preparation of Coin Battery>. In a thermostatic chamber at 25°C, charging was performed in the direction in which Li was absorbed in the electrode, and charging was performed to 0.8V at a current value corresponding to 0.5C of the initial discharge capacity, and then discharging was performed to 2.0V at a current value corresponding to 0.5C of the initial discharge capacity. This charge and discharge was repeated for 20 cycles, and the discharge capacity at the 20th cycle was calculated, and then divided by the initial discharge capacity to obtain the cycle capacity retention rate. The results calculated as relative values ​​for each Example and Comparative Example when the cycle capacity retention rate of Comparative Example 1-1 was set to 100 are shown in Table 2.

[0121] [Table 1]

[0122] [Table 2]

[0123] <Evaluation Results> It was found that the electrodes using the titanium-niobium composite oxide powders of Examples 1-1 to 1-14 maintain a high initial discharge capacity, leading to improved energy density, and also excellent charge / discharge rate characteristics at high rates. In other words, by implementing the synthesis conditions of the niobium-titanium composite oxide powder within a specific range, such as the calcination temperature and crushing conditions during synthesis in accordance with the raw materials, it was possible to obtain a niobium-titanium composite oxide powder in which the intensity ratio of two specific peaks in the powder X-ray diffraction diffraction pattern is 1.0 or more, and the intensity ratio of two specific peaks in the spectrum obtained by microscopic Raman spectroscopy is controlled to 0.2 or less, leading to improved battery performance. In particular, it was found that the electrodes using the niobium-titanium composite oxide powders of Examples 1-5, 1-8, 1-11, 1-12, and 1-14 in which the intensity ratio (I(24deg) / I(26deg)) of two specific peaks in the powder X-ray diffraction diffraction pattern is 1.05 or more and 2.00 or less, show a large improvement in charge / discharge rate characteristics. As mentioned above, although it is only a guess, the change in the intensity ratio of these two peaks is inferred to mean that the balance of the crystallite sizes of the crystal planes has changed, and this is thought to affect the insertion and desorption of lithium ions into the crystal structure of the niobium-titanium composite oxide. Furthermore, the niobium-titanium composite oxide powders of Examples 1-5, 1-8, 1-11, 1-12, and 1-14 showed a zeta potential of -65 mV or more and -30 mV or less at 25°C measured by electrophoresis. The zeta potential represents the potential difference between the slip surface in the electric double layer and a portion sufficiently distant from the interface, and is inferred to affect the Li+ permeability at the surface of the niobium-titanium composite oxide powder. On the other hand, the niobium-titanium composite oxide powders of Comparative Examples 1-1 to 1-5 did not show a significant improvement in the initial discharge capacity, charge / discharge rate characteristics, or cycle characteristics, and did not lead to an improvement in the battery characteristics.

[0124] (Lithium-ion secondary battery: Laminated battery) [Example 2-1] The titanium-niobium composite oxide powder synthesized in Example 1-10 was used as the negative electrode active material to prepare a laminate battery described below, and the battery characteristics were evaluated. The evaluation results are shown in Table 3. The Raman spectrum was also measured as shown in Figure 1. Wave number range: 520 to 800 cm -1 Extract the peak and separate it. I (538cm -1 ) / I(650cm -1 ) was 0.57.

[0125] [Example 2-2] The titanium-niobium composite oxide powder synthesized in Example 1-11 was used as the negative electrode active material to fabricate a laminate battery described below, and the battery characteristics were evaluated. The evaluation results are shown in Table 3.

[0126] [Example 2-3] The titanium-niobium composite oxide powder synthesized in Example 1-8 was used as the negative electrode active material to fabricate a laminate battery described below, and the battery characteristics were evaluated. The evaluation results are shown in Table 3.

[0127] [Example 2-4] The titanium-niobium composite oxide powder synthesized in Example 1-9 was used as the negative electrode active material to fabricate a laminate battery described below, and the battery characteristics were evaluated. The evaluation results are shown in Table 3.

[0128] [Example 2-5] Nb2O5 and anatase type TiO2 were weighed and mixed in a molar ratio of 7:18. The mixed powder was sintered at 900°C for 12 hours to obtain the desired titanium-niobium composite oxide (Ti2Nb 10 O 29 ) was obtained, and therefore it was designated as the titanium-niobium composite oxide powder according to Example 2-4. A laminate battery described below was produced using this titanium-niobium composite oxide powder as the negative electrode active material, and the battery characteristics were evaluated. The evaluation results are shown in Table 3.

[0129] [Comparative Example 2-1] The titanium-niobium composite oxide powder synthesized in Comparative Example 1-1 was used as the negative electrode active material to fabricate a laminate battery described below, and the battery characteristics were evaluated. The evaluation results are shown in Table 3.

[0130] [Comparative Example 2-2] As shown in Table 3, the titanium-niobium composite oxide powder according to Comparative Example 2-2 was synthesized in the same manner as in Comparative Example 1-1, except that the bead mill device in the crushing step was changed to a paint shaker device (using zirconia beads (φ1.0 mm) at a motor rotation frequency of 60 Hz for 60 minutes). A laminate battery described below was produced using this titanium-niobium composite oxide powder as the negative electrode active material, and the battery characteristics were evaluated. The evaluation results are shown in Table 3.

[0131] [Comparative Example 2-3] As shown in Table 3, the titanium-niobium composite oxide powder according to Comparative Example 2-3 was synthesized in the same manner as in Comparative Example 1-1, except that the bead mill processing time in the crushing step was changed (to 120 minutes) and the heat treatment step was performed (heat treatment at 650°C for 1 hour using a muffle furnace). A laminate battery described below was produced using this titanium-niobium composite oxide powder as the negative electrode active material, and the battery characteristics were evaluated. The evaluation results are shown in Table 3.

[0132] [Comparative Example 2-4] As shown in Table 3, the titanium raw material was TiO2 of rutile type (specific surface area 20 m 2 The titanium-niobium composite oxide powder according to Comparative Example 2-4 was synthesized in the same manner as in Comparative Example 2-3, except that the titanium-niobium composite oxide powder was changed to 1.0 ppm (Zr content 190 ppm) and 1.0 ppm (Cu content 190 ppm). A laminate battery described below was produced using this titanium-niobium composite oxide powder as the negative electrode active material, and the battery characteristics were evaluated. The evaluation results are shown in Table 3.

[0133] <Calculation of spectral peak area ratio in microscopic Raman spectroscopy> For the titanium-niobium composite oxide powders of each Example and Comparative Example, Raman spectroscopy was performed under the conditions described above, and then the Raman spectroscopy was performed at 560 to 520 cm -1 The area value of the peak (I(538 cm)) obtained by peak separation of the spectrum appearing in -1 )) and 620~680cm -1 The area value of the peak (I(650cm)) obtained by separating the spectrum appearing in -1 Specifically, the wavenumber range of the baseline-corrected Raman spectrum from 520 to 800 cm was calculated. -1 The peaks were separated using a Lorentzian function as a fitting function. As an example of peak separation, the analysis results for the titanium-niobium composite oxide powder of Example 2-1 are shown in FIG. 1. In addition, the two peak area ratios I (538 cm) of each Example and Comparative Example were -1 ) / I(650cm -1 ) are shown in Table 3.

[0134] <Preparation of laminated battery> The laminated battery was fabricated in a room controlled at a room temperature of 25°C and a dew point of -40°C or less as follows. The negative electrode double-sided sheet fabricated by the above method was placed on a 2t / cm 2 After pressing at a pressure of 1000 MPa, a negative electrode with a lead wire connection was fabricated. Next, LiCo was used as the positive electrode active material. 1 / 3 Ni 1 / 3 Mn 1 / 3 A positive electrode sheet using O2 was applied on one side at 2t / cm 2 After pressing at a pressure of 1000 kPa, a positive electrode with a lead wire connection was produced. The produced negative and positive electrodes were vacuum dried at 150°C for 12 hours. The vacuum dried positive and negative electrodes were laminated facing each other with a separator (UPZ210, manufactured by Ube Maxell) between them, and aluminum foil lead wires were connected to the positive and negative electrodes, respectively. The laminated battery electrolyte prepared by the method described above in <Preparation of electrolyte> was added, and the laminated battery was vacuum sealed with aluminum laminate to produce a laminated battery for evaluation. The capacity of the battery was 30 mAh, and the ratio of the negative and positive electrode capacities (negative electrode capacity / positive electrode capacity) was 1.2. Next, as an aging step, the laminated battery prepared by the method described above in <Preparation of Laminated Battery> was charged to 2.75 V at a current of 0.2 C in a thermostatic chamber at 60° C., and further charged at 2.75 V until the charging current became 0.05 C. This was followed by two cycles of constant current discharge at a current of 0.2 C to 1.4 V. The discharge capacity in the second cycle was taken as the initial discharge capacity.

[0135] <Laminated battery characteristics: 5C discharge rate characteristics, -10℃ discharge rate characteristics, cycle capacity retention rate> Using the laminated battery prepared by the method described above in <Preparation of Laminated Battery>, the battery was charged at a constant current and constant voltage up to 2.75 V at a current equivalent to 0.2 C of the initial discharge capacity in a thermostatic bath environment of 25 ° C, and then discharged at a current of 5 C to 1.4 V to obtain the 5 C discharge capacity. The 5 C discharge capacity was divided by the initial discharge capacity to calculate the 5 C rate discharge rate characteristic (%). Next, the battery was charged at a constant current and constant voltage up to 2.75 V at a current equivalent to 0.2 C of the initial discharge capacity in a thermostatic bath environment of 25 ° C, and then changed to a thermostatic bath environment of -10 ° C, and then discharged at a constant current of 0.2 C to 1.4 V to obtain the -10 ° C discharge capacity. The -10 ° C discharge capacity was divided by the initial discharge capacity to calculate the -10 ° C discharge rate characteristic (%). Furthermore, in a thermostatic chamber at 55°C, the battery was charged to 2.75V at a current of 2C, and then charged at 2.75V until the charging current became 0.05C. This was followed by 100 cycles of constant current discharge at a current of 2C to 1.4V. The cycle capacity retention rate (%) was calculated by dividing the discharge capacity at the 100th cycle by the initial discharge capacity. The evaluation results are shown in Table 3.

[0136] [Table 3]

[0137] <Evaluation Results> It was found that the electrodes using the titanium-niobium composite oxide powders of Examples 2-1 to 2-5 were excellent in discharge rate characteristics, low-temperature characteristics (-10°C discharge rate characteristics), and high-temperature cycle characteristics. In other words, by carrying out the synthesis conditions of the niobium-titanium composite oxide powder within a specific range, such as the calcination temperature and crushing conditions during synthesis in accordance with the raw materials, it was possible to obtain a niobium-titanium composite oxide powder in which the intensity ratio of two specific peaks in the diffraction pattern of powder X-ray diffraction is 1.0 or more and the intensity ratio of two peaks in a specific spectrum obtained by microscopic Raman spectroscopy is controlled to 0.2 or less, which led to improvement in battery performance. In addition, it was also found that the titanium-niobium composite oxide powders of Examples 2-1 to 2-5 have an area ratio of two specific peaks in the spectrum obtained by microscopic Raman spectroscopy of 0.5 or more. As described above, the change in the area ratio of these two peaks reflects the strength relationship between the Ti-O bond and the Nb-O bond in the crystal structure, and as a result, it is presumed that the insertion and desorption property of lithium ions in the crystal structure has changed. On the other hand, the niobium-titanium composite oxide powders of Comparative Examples 2-1 to 2-4 did not achieve a balance between discharge rate characteristics, low-temperature characteristics (-10° C. discharge rate characteristics), and high-temperature cycle characteristics, and did not lead to improvement in battery characteristics.

[0138] (All-solid-state secondary battery) [Example 3-1] In a glove box under an argon atmosphere, the niobium-titanium composite oxide powder of Example 1-1 and the sulfide solid electrolyte Li6PS5Cl powder (volume average particle size: 6 μm obtained using a laser diffraction / scattering type particle size distribution analyzer) and the conductive agent were weighed out to a mass ratio of niobium-titanium composite oxide: Li6PS5Cl: conductive agent = 60: 40: 6, and mixed in an agate mortar and a planetary ball mill to obtain the negative electrode active material composition of Example 3-1. The obtained negative electrode active material composition was pressed (360 MPa) at room temperature for 10 minutes to produce a pellet (molded body) with a diameter of 10 mm and a thickness of about 0.7 mm. A pellet-shaped electrode containing this negative electrode active material composition, a pellet-shaped solid electrolyte layer (LPS glass with a molar ratio of Li2S:P2S5=75:25) as a separator layer, and a lithium-indium alloy foil as a counter electrode were laminated in this order, and the laminate was sandwiched between stainless steel current collectors to prepare an all-solid-state secondary battery, and the battery characteristics were evaluated. The evaluation results are shown in Table 4.

[0139] [Example 3-2] As shown in Table 4, the titanium-niobium composite oxide powder according to Example 3-2 was synthesized in the same manner as in Example 1-1, except that a heat treatment step (heat treatment at 550°C for 1 hour using a muffle furnace) was additionally performed, and the negative electrode active material composition of Example 3-2 was obtained in the same manner as in Example 3-1, except that this was used, and then an all-solid-state secondary battery was produced and the battery characteristics were evaluated. The evaluation results are shown in Table 4.

[0140] [Example 3-3] As shown in Table 4, the surface treatment step was carried out, lithium molybdate (Li2MоO4) was added as a treatment agent at 1.0 mass% per 100 g of crushed fired powder, and a heat treatment step was carried out at 550 ° C. The titanium-niobium composite oxide powder according to Example 3-3 was synthesized in the same manner as in Example 1-1, except that it was used to obtain the negative electrode active material composition of Example 3-3. An all-solid-state secondary battery was then produced and the battery characteristics were evaluated. The evaluation results are shown in Table 4.

[0141] [Example 3-4] As shown in Table 4, except that the niobium-titanium composite oxide powder of Example 1-5 was used, the negative electrode active material composition of Example 3-4 was obtained in the same manner as in Example 3-1, and then an all-solid-state secondary battery was produced and the battery characteristics were evaluated. The evaluation results are shown in Table 4.

[0142] [Examples 3-5] As shown in Table 4, the treatment agent for the surface treatment step was added in an amount of 1.6 mass% and 0.5 mass% relative to 100 g of sintered powder obtained by crushing aluminum sulfate 16-hydrate (Al2(SO4)3·16H2O) and lithium molybdate (Li2MоO4), and the heat treatment step was carried out at 550°C. The titanium-niobium composite oxide powder according to Example 3-5 was synthesized in the same manner as in Example 1-7, and the negative electrode active material composition of Example 3-5 was obtained, except that this was used. An all-solid-state secondary battery was fabricated and the battery characteristics were evaluated. The evaluation results are shown in Table 4.

[0143] [Comparative Example 3-1] As shown in Table 4, except that the niobium-titanium composite oxide powder of Comparative Example 1-1 was used, an all-solid-state secondary battery was produced after obtaining the negative electrode active material composition of Comparative Example 3-1 in the same manner as in Example 3-1, and the battery characteristics were evaluated. The evaluation results are shown in Table 4.

[0144] [Comparative Example 3-2] As shown in Table 4, the same procedure as in Comparative Example 1-1 was carried out except that the bead mill treatment step in the crushing step was not carried out, and the titanium-niobium composite oxide powder according to Comparative Example 3-2 was synthesized and used. Except for this, an all-solid-state secondary battery was produced after obtaining the negative electrode active material composition of Comparative Example 3-2 in the same manner as in Example 3-1, and the battery characteristics were evaluated. The evaluation results are shown in Table 4.

[0145] [Comparative Example 3-3] As shown in Table 4, the surface treatment step was carried out, lithium molybdate (Li2MоO4) was added as a treatment agent at 1.0 mass% per 100 g of crushed fired powder, and a heat treatment step was carried out at 550 ° C. The titanium-niobium composite oxide powder according to Comparative Example 3-3 was synthesized in the same manner as in Comparative Example 3-2, except that it was used to obtain the negative electrode active material composition of Comparative Example 3-3. An all-solid-state secondary battery was then produced and the battery characteristics were evaluated. The evaluation results are shown in Table 4.

[0146] <Measurement of 1C charge / discharge rate characteristics> In a thermostatic chamber at 25°C, the all-solid-state secondary battery prepared by the above method was charged to 0.5V with a current equivalent to 0.05C of the theoretical capacity of the niobium-titanium composite oxide, with the direction of Li absorption in the evaluation electrode being the charging direction, and further constant current constant voltage charging was performed in which charging was performed at 0.5V until the charging current reached a current equivalent to 0.01C, and the charging capacity (mAh) was divided by the mass of the niobium-titanium composite oxide to obtain the initial charging capacity (mAh / g). Then, constant current discharging was performed to 2V with a current equivalent to 0.05C. The discharge capacity (mAh) was divided by the mass of the niobium-titanium composite oxide to obtain the initial discharging capacity (mAh / g). Next, the battery was charged to 0.5V with a current equivalent to 1C of the theoretical capacity of the niobium-titanium composite oxide, and the 1C charging capacity was obtained. The 1C charging capacity was divided by the initial charging capacity to calculate the 1C charging rate characteristic (%). Thereafter, the battery was discharged to 2 V at a current equivalent to 1 C, the theoretical capacity of the niobium-titanium composite oxide, and the 1 C discharge capacity was then calculated. The 1 C discharge capacity was divided by the initial discharge capacity to calculate the 1 C discharge rate characteristic (%). The evaluation results are shown in Table 4.

[0147] [Table 4]

[0148] <Evaluation Results> It was found that the negative electrode active material compositions using the niobium-titanium composite oxide powders of Examples 3-1 to 3-5 had excellent battery performance in all-solid-state secondary batteries, whereas the negative electrode active material compositions using the niobium-titanium composite oxide powders of Comparative Examples 3-1 to 3-3 did not show any improvement in battery performance in all-solid-state secondary batteries. [Industrial Applicability]

[0149] The niobium-titanium composite oxide powder obtained by the present invention can improve the energy density, improve the charge / discharge rate characteristics, and improve the battery performance in the low temperature region, so it is useful as an electrode active material for lithium-ion batteries, and furthermore, since it shows performance improvement in all-solid-state batteries, it is also useful as an electrode active material for all-solid-state secondary batteries. The power storage device using this niobium-titanium composite oxide powder as an electrode active material is useful as a secondary battery for driving or backing up various devices such as automobiles and electronic devices, and for storing power at night in homes and offices. By providing electrode materials for lithium-ion batteries, such as non-aqueous electrolyte secondary batteries, to society, it can contribute to the achievement of Goal 12 (ensure sustainable consumption and production patterns), Goal 3 (ensure healthy lives and promote well-being for all at all ages), Goal 7 (ensure access to affordable, reliable, sustainable and modern energy for all), and Goal 11 (make cities and human settlements inclusive, safe, resilient and sustainable) out of the 17 goals of the Sustainable Development Goals (SDGs) established by the United Nations.< / dbet> < / dbet>

Claims

1. A niobium-titanium composite oxide powder for an electrode of a nonaqueous electrolyte electricity storage device, characterized in that in a powder X-ray diffraction pattern obtained using a Cu-Kα radiation source, the intensity ratio of two peaks represented by the following formula (I) is 1.0 or more, and in a spectrum obtained by microscopic Raman spectroscopy, the intensity ratio of two peaks represented by the following formula (II) is 0.2 or less. I(24deg) / I(26deg)≧1.0 (I) I (24 deg): The highest peak intensity value appearing in the range of 2θ = 24 ± 0.2° I (26 deg): The highest peak intensity value appearing in the range of 2θ = 26 ± 0.2° I(A) / I(C)≦0.2 (II) I(A): 430-460cm -1 The intensity value of peak A appearing in I(C): 260-280cm -1 The intensity value of peak C appearing in

2. General formula Ti 1-x/2 Nb 2 O 7-x 2. The niobium-titanium composite oxide powder for use in an electrode of a nonaqueous electrolyte electricity storage device according to claim 1, characterized in that the powder has a composition expressed by (0≦x<2).

3. The niobium-titanium composite oxide powder for an electrode of a nonaqueous electrolyte electricity storage device according to claim 1 or 2, characterized in that the zeta potential of the niobium-titanium composite oxide powder at 25° C., as measured by electrophoresis, is −65 mV or more and −25 mV or less.

4. 3. The niobium-titanium composite oxide powder for electrodes of nonaqueous electrolyte electricity storage devices according to claim 1 or 2, wherein, in the niobium-titanium composite oxide powder for electrodes, when D50 is the particle size at a point where the cumulative volume distribution of primary particle sizes is 50% and DBET is the diameter equivalent to the specific surface area calculated from the specific surface area obtained by the BET method, D50 is 1 μm or more and the ratio of D50 to DBET, D50 / DBET (μm / μm), is 2.1 or less.

5. 3. The niobium-titanium composite oxide powder for electrodes of nonaqueous electrolyte electricity storage devices according to claim 1 or 2, characterized in that, when the particle size D50 is defined as a particle size at a point where a cumulative volume distribution of particle sizes of primary particles is 50% in a particle size distribution, D50 is less than 1 μm, and in a spectrum obtained by micro-Raman spectroscopy, the area ratio of two peaks represented by the following formula (III) is 0.5 or more: I(538cm -1 ) / I(650cm -1 )≧0.5 (III) I (538 cm -1 ): 520-560cm -1 The area value of the peaks obtained by separating the spectra that appear in I (650 cm -1 ): 620-680cm -1 The area value of the peaks obtained by separating the spectra that appear in

6. 3. The niobium-titanium composite oxide powder for an electrode of a nonaqueous electrolyte electricity storage device according to claim 1 or 2, characterized in that in the niobium-titanium composite oxide powder for an electrode, element M1 (M1 includes any one or more selected from the group consisting of Al, Mg, Mo, and Ce) is localized and present on the surface of the niobium-titanium composite oxide particle.

7. 3. An electrode comprising the niobium-titanium composite oxide powder according to claim 1.

8. 3. A negative electrode active material composition comprising the niobium-titanium composite oxide powder according to claim 1 or 2, and an inorganic solid electrolyte.

9. A non-aqueous electrolyte electricity storage device comprising the electrode according to claim 7.

10. 9. An all-solid-state secondary battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer, the negative electrode layer being a layer containing the negative electrode active material composition according to claim 8.

Citation Information

Patent Citations

  • Active material for battery, nonaqueous electrolyte battery, and battery pack

    JP2012099287A

  • Active material for battery use, nonaqueous electrolyte battery and battery pack

    JP2014209445A

  • Active material, non-aqueous electrolyte battery and battery pack

    JP2015035420A

  • Negative electrode and nonaqueous electrolyte battery

    JP2015135770A

  • Negative electrode active material for power storage element, negative electrode for power storage element, storage element, and usage of power storage element