Optical glass, light guide plate, image display device and optical element
Optical glass with enhanced spectral transmittance and refractive index characteristics addresses the challenge of wide viewing angles and clear images in light guide plates, particularly for augmented reality displays.
Patent Information
- Application Number
- JP2024016057
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-06
- Publication Date
- 2024-10-15
AI Technical Summary
Existing light guide plates made from optical glass with high refractive index struggle to provide a wide viewing angle and clear images due to limitations in spectral transmittance characteristics, particularly with a difference in wavelengths affecting light transmission.
Optical glass with a refractive index of 2.00000 or more, specific spectral transmittance properties (λ5 between 370 nm and 410 nm, and a difference of λ70-λ5 less than 70 nm) is developed, incorporating components like SiO2, B2O3, TiO2, Nb2O5, Y2O3, La2O3, and Gd2O3 to enhance light transmission and reduce surface devitrification.
The solution provides optical glass suitable for light guide plates, offering improved viewing angles and clear images by optimizing spectral transmittance and refractive index, suitable for applications like augmented reality displays.
Smart Images

Figure 2024146758000004 
Figure 2024146758000005 
Figure 2024146758000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical glass, a light guide plate, an image display device, and an optical element. [Background technology]
[0002] For example, Patent Document 1 discloses an optical glass having a high refractive index. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-116408 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, light guide plates, which are components of image display devices, have come to be made from optical glass. Optical glass with a high refractive index makes it possible to manufacture light guide plates with a wide viewing angle.
[0005] An object of one aspect of the present invention is to provide an optical glass having a high refractive index and suitable as a material for a light guide plate. [Means for solving the problem]
[0006] As a result of extensive investigations, the inventors have newly discovered that a light guide plate made of optical glass having a wavelength λ5 at which a spectral transmittance of 5% at a thickness of 10 mm is greater than 370 nm and less than 410 nm, a difference (λ70-λ5) between the wavelengths λ70 and λ5 at which a spectral transmittance of 70% at a thickness of 10 mm is 70 nm or less, and a refractive index nd of 2.00000 or more, makes it possible to widen the viewing angle and obtain a clear image.
[0007] One aspect of the present invention is as follows. [1] The wavelength λ5 at which the spectral transmittance is 5% at a thickness of 10 mm is greater than 370 nm and less than 410 nm, The difference between the wavelengths λ70 and λ5 at which the spectral transmittance is 70% at a thickness of 10 mm (λ70-λ5) is 70 nm or less, and Optical glass having a refractive index nd of 2.00000 or more (hereinafter simply referred to as "optical glass" or "glass"). [2] The optical glass according to [1], which contains B2O3. [3] The optical glass according to [1], comprising SiO2, B2O3, TiO2, Nb2O5, Y2O3, La2O3 and Gd2O3. [4] A light guide plate made of the optical glass according to any one of [1] to [3]. [5] An image display element; a light guide plate that guides light emitted from the image display element; Including, The image display device, wherein the light guide plate is the light guide plate according to [4]. [6] An optical element comprising the optical glass according to any one of [1] to [3]. Effect of the Invention
[0008] According to one aspect of the present invention, an optical glass having a high refractive index and suitable as a light guide plate material can be provided. According to another aspect of the present invention, there is provided a light guide plate made of the above-mentioned optical glass, and an image display device including this light guide plate. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic diagram illustrating an example of an image device (head mounted display) including an image display element and a light guide plate. [Diagram 2] 2 is a side view diagrammatically illustrating the configuration of the head mounted display 1 shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Optical glass] <Refractive index nd> From the viewpoint of widening the viewing angle, the refractive index nd of the optical glass is 2.00000 or more, preferably 2.01000 or more, more preferably 2.02000 or more, and more preferably 2.03000 or more, 2.04000 or more, 2.05000 or more, 2.06000 or more, 2.07000 or more, and 2.08000 or more in this order. The refractive index nd of the optical glass can be, for example, 2.20000 or less, 2.15000 or less, 2.14000 or less, 2.13000 or less, 2.12000 or less, 2.11000 or less t2.10000 or less. In the present invention and this specification, "refractive index" means "refractive index nd".
[0011] <λ5, λ70-λ5> "λ5" refers to the wavelength from the ultraviolet to the visible range at which the spectral transmittance (including surface reflection loss) of a 10 mm thick glass is 5%. "λ70" refers to the wavelength from the ultraviolet to the visible range at which the spectral transmittance (i.e., external transmittance) of a 10 mm thick glass, including surface reflection loss, is 70%. The spectral transmittances described below also include surface reflection loss. The λ5 and λ70 shown in the Examples section below are values measured in the wavelength range of 250 to 700 nm. More specifically, the spectral transmittance is the spectral transmittance obtained by using a glass sample having parallel flat surfaces polished to a thickness of 10.0±0.1 mm and illuminating light perpendicularly to the polished surfaces, that is, Iout / Iin, where Iin is the intensity of light incident on the glass sample and Iout is the intensity of light transmitted through the glass sample. If the thickness of the glass to be measured is not 10.0±0.1 mm, it is converted to a value at a thickness of 10 mm by a known method. For example, for glass with an internal transmittance (not including surface reflection loss) of τ (%), the following formula: logτ=(logT1-logT2) / Δd×10 The external transmittance (including surface reflection loss) at a thickness of 10 mm can be calculated using the formula: where T1 (%) is the transmittance (including surface reflection loss) obtained at a sample thickness of d1 (mm), T2 (%) is the transmittance (including surface reflection loss) obtained at a sample thickness of d2, and Δd is the difference in sample thickness (d2-d1). Optical glass in which the difference between λ70 and λ5 (λ70-λ5) is 70 nm or less is optical glass that exhibits high transmittance characteristics in a wide wavelength range. For example, a light guide plate of an image display device for AR (Augmented Reality) is required to have high transmittance characteristics in a wide wavelength range in order to grasp the surrounding environment through the light guide plate. In addition, high transmittance characteristics are required to reduce the loss of light propagating from the light source through the light guide plate. Therefore, optical glass in which the difference between λ70 and λ5 (λ70-λ5) is 70 nm or less is preferable as a light guide plate material. Optical glass with a wavelength λ5 of more than 370 nm and less than 410 nm is optical glass that blocks ultraviolet light and transmits visible light. When light on the short wavelength side is irradiated to the eyes, it may lead to the risk of cataracts, etc. Therefore, it is not preferable to have a transmittance characteristic that is higher than necessary on the short wavelength side. From this point of view, optical glass with a wavelength λ5 of more than 370 nm and less than 410 nm is preferable as a light guide plate material.
[0012] The difference between λ70 and λ5 of the optical glass (λ70-λ5) is 70 nm or less, preferably 68 nm or less, more preferably 66 nm or less, and further preferably 64 nm or less, 62 nm or less, 60 nm or less, 58 nm or less, 56 nm or less, 54 nm or less, 52 nm or less, and 50 nm or less in that order. The difference between 70 and λ5 (λ70-λ5) can be, for example, 10 nm or more, 20 nm or more, 30 nm or more, or 40 nm or more.
[0013] The λ5 of the optical glass is more than 370 nm, preferably 371 nm or more, more preferably 372 nm or more, more preferably 373 nm or more, 374 nm or more, and 375 nm or more in that order. The λ5 of the optical glass is less than 410 nm, preferably 408 nm or less, more preferably 405 nm or less, and further preferably 403 nm or less, 400 nm or less, 398 nm or less, 395 nm or less, 393 nm or less, 390 nm or less, 388 nm or less, 385 nm or less, and 380 nm or less in that order.
[0014] The λ70 of the optical glass is not particularly limited as long as the difference between λ70 and λ5 (λ70-λ5) is within the above range. In one embodiment, the λ70 of the optical glass can be more than 400 nm and less than 480 nm.
[0015] <Glass composition> In the present invention and this specification, the glass composition is expressed as a glass composition based on oxides. Here, "glass composition based on oxides" refers to a glass composition obtained by converting the glass raw materials into oxides that are present in the glass after being completely decomposed during melting. Furthermore, unless otherwise specified, the glass composition is expressed on a mass basis (mass %, mass ratio). The glass composition of the present invention and this specification can be determined by a method such as ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Quantitative analysis is performed for each element using ICP-AES. The analytical values are then converted into oxide notation. The analytical values obtained by ICP-AES may contain a measurement error of, for example, about ±5% of the analytical value. Therefore, the oxide notation values converted from the analytical values may also contain an error of about ±5%. In the present invention and this specification, the content of a component being 0%, 0.00%, 0.000%, or not being contained or not being introduced means that the component is substantially not contained, and the content of the component is at or below the level of impurities. At or below the level of impurities means, for example, less than 0.01%.
[0016] In one embodiment, the optical glass may be a borate-based glass and may include B2O3. Also, in one embodiment, the optical glass may include SiO2, B2O3, TiO2, Nb2O5, Y2O3, La2O3, and Gd2O3 as essential components.
[0017] The glass composition of the above optical glass will be described in more detail below, however, the optical glass is not limited to the optical glass having the glass composition described below as long as the refractive index nd, λ5, and the difference between λ70 and λ5 (λ70-λ5) are within the above ranges.
[0018] The mass ratio of the B2O3 content to the SiO2 content (B2O3 / SiO2) is preferably less than 3.000, more preferably 2.800 or less, and further preferably 2.600 or less, 2.400 or less, 2.200 or less, 2.000 or less, 1.800 or less, 1.600 or less, 1.400 or less, 1.200 or less, 1.000 or less, less than 1.000, 0.980 or less, 0.960 or less, 0.950 or less, 0.920 or less, and 0.900 or less in this order. The mass ratio (B2O3 / SiO2) can be, for example, 0.100 or more, 0.200 or more, 0.300 or more, 0.400 or more, 0.500 or more, or 0.600 or more.
[0019] The mass ratio of the Y2O3 content to the total content of Y2O3, La2O3, Gd2O3, and Yb2O3 (Y2O3 / (Y2O3+La2O3+Gd2O3+Yb2O3)) is preferably 0.010 or more, more preferably greater than 0.010, and further preferably 0.011 or more, 0.012 or more, 0.013 or more, 0.014 or more, 0.015 or more, 0.016 or more, 0.017 or more, 0.018 or more, 0.019 or more, 0.020 or more, 0.021 or more, 0.022 or more, 0.023 or more, 0.024 or more, and 0.025 or more in that order. The mass ratio (Y2O3 / (Y2O3+La2O3+Gd2O3+Yb2O3)) can be, for example, 0.100 or less, 0.090 or less, 0.080 or less, 0.070 or less, 0.060 or less, or 0.050 or less.
[0020] The optical glass may contain, as essential components, SiO2, B2O3, TiO2, Nb2O5, Y2O3, La2O3, and Gd2O3.
[0021] SiO2 is a network-forming oxide, and is a component that can contribute to maintaining glass stability, maintaining viscosity suitable for forming molten glass, and improving chemical durability. Increasing glass stability is preferable because it leads to suppressing surface devitrification of glass. The SiO2 content of the optical glass is preferably 0.10% or more, more preferably 0.50% or more, and further preferably 1.00% or more, 2.00% or more, 3.00% or more, 4.00% or more, and 5.00% or more in that order. From the viewpoint of suppressing the decrease in refractive index and maintaining glass meltability, the SiO2 content is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 10.00% or less, 8.00% or less, and 6.00% or less in that order.
[0022] B2O3 is a network-forming oxide, and is a component that can contribute to maintaining glass meltability and improving glass stability. The B2O3 content of the optical glass is preferably 0.10% or more, more preferably 0.50% or more, and further preferably 1.00% or more, 2.00% or more, 3.00% or more, 4.00% or more, and 5.00% or more in that order. From the viewpoint of suppressing the decrease in refractive index and the decrease in chemical durability, the B2O3 content is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 10.00% or less, 8.00% or less, and 6.00% or less in that order.
[0023] From the viewpoint of improving the stability of the glass, the total content of SiO2 and B2O3 (SiO2+B2O3) is preferably 1.00% or more, more preferably 3.00% or more, and further preferably 5.00% or more, 8.00% or more, and 10.00% or more. From the viewpoint of increasing the refractive index of the glass, the total content (SiO2+B2O3) is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 13.00% or less, and 12.00% or less.
[0024] TiO2 is a component that can increase the refractive index of glass and contribute to improving chemical durability. The TiO2 content of the optical glass is preferably 1.00% or more, more preferably 3.00% or more, and more preferably 5.00% or more, 8.00% or more, 10.00% or more, 13.00% or more, 15.00% or more, 18.00% or more, and 20.00% or more in this order. From the viewpoint of suppressing the deterioration of glass stability, the TiO2 content is preferably 50.00% or less, more preferably 45.00% or less, and more preferably 40.00% or less, 35.00% or less, 30.00% or less, 28.00% or less, and 26.00% or less in this order. In addition, it is preferable that the TiO2 content is in the above range from the viewpoint of controlling λ5 within the range described above.
[0025] The mass ratio of TiO2 content to the total content of SiO2 and B2O3 (TiO2 / (SiO2+B2O3)) is preferably 1.500 or more, more preferably 1.550 or more, and more preferably 1.600 or more, 1.650 or more, 1.700 or more, 1.750 or more, 1.800 or more, 1.850 or more, 1.900 or more, 1.950 or more, 1.960 or more, 1.970 or more, 1.980 or more, 1.990 or more, and 2.000 or more in this order from the viewpoint of increasing the refractive index of the glass. From the viewpoint of improving the stability of the glass, it is preferably 10.000 or less, more preferably 8.000 or less, and more preferably 5.000 or less, 3.000 or less, 2.800 or less, and 2.500 or less in this order.
[0026] Nb2O5 is a component that can increase the refractive index of glass and contribute to improving chemical durability. The Nb2O5 content of the optical glass is preferably 1.00% or more, more preferably 2.00% or more, and further preferably 3.00% or more, 4.00% or more, 5.00% or more, and 6.00% or more in that order. From the viewpoint of suppressing a decrease in glass stability, the Nb2O5 content is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 10.00% or less, and 8.00% or less in that order.
[0027] The WO3 content of the optical glass can be 0.00%, 0.00% or more, or more than 0.00%. WO3 is a component that can increase the refractive index of glass and contribute to improving chemical durability. The WO3 content can be, for example, 8.00% or less, 7.00% or less, 6.00% or less, or 5.00% or less.
[0028] From the viewpoint of increasing the refractive index of the glass and improving the chemical durability, the total content of TiO2, Nb2O5 and WO3 (TiO2+Nb2O5+WO3) is preferably 10.00% or more, more preferably 15.00% or more, and further preferably 20.00% or more, 25.00% or more, 28.00% or more, and 30.00% or more in that order. From the viewpoint of improving the glass stability, the total content (TiO2+Nb2O5+WO3) is preferably 60.00% or less, more preferably 55.00% or less, and further preferably 50.00% or less, 45.00% or less, 40.00% or less, 38.00% or less, and 35.00% or less in that order.
[0029] Y2O3 is a component that can contribute to increasing the refractive index of glass, maintaining low dispersion, and improving chemical durability. The Y2O3 content of the optical glass is preferably 0.10% or more, more preferably 0.30% or more, and further preferably 0.50% or more, 0.80% or more, and 1.00% or more in that order. From the viewpoint of suppressing the deterioration of glass stability and suppressing the increase of Tl, the Y2O3 content is preferably 10.00% or less, more preferably 8.00% or less, and further preferably 5.00% or less, and further preferably 3.00% or less in that order.
[0030] La2O3 is also a component that can contribute to increasing the refractive index of the glass, maintaining low dispersion, and improving chemical durability. The La2O3 content of the optical glass is preferably 10.00% or more, more preferably 15.00% or more, and further preferably 20.00% or more, 25.00% or more, 30.00% or more, and 35.00% or more in that order. From the viewpoint of suppressing the deterioration of glass stability and suppressing the increase of Tl, the La2O3 content is preferably 60.00% or less, more preferably 55.00% or less, and further preferably 50.00% or less, 45.00% or less, and 40.00% or less in that order.
[0031] Gd2O3 is also a component that can contribute to increasing the refractive index of the glass, maintaining low dispersion, and improving chemical durability. The Gd2O3 content of the optical glass is preferably 1.00% or more, more preferably 2.00% or more, and further preferably 3.00% or more, 4.00% or more, 5.00% or more, and 6.00% or more in that order. From the viewpoint of suppressing the deterioration of glass stability and suppressing the increase of Tl, the Gd2O3 content is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 10.00% or less, and 8.00% or less in that order.
[0032] The Yb2O3 content can be 0.00%, 0.00% or more, or more than 0.00%. Yb2O3 is also a component that can contribute to increasing the refractive index of the glass, maintaining low dispersion, and improving chemical durability. The Yb2O3 content of the optical glass can be, for example, 5.00% or less, 4.00% or less, 3.00% or less, 2.00% or less, 1.00% or less, 0.50% or less, or 0.10% or less.
[0033] The total content of Y2O3, La2O3, Gd2O3 and Yb2O3 (Y2O3+La2O3+Gd2O3+Yb2O3) is preferably 10.00% or more, more preferably 15.00% or more, and more preferably 20.00% or more, 25.00% or more, 30.00% or more, 35.00% or more, 40.00% or more, 43.00% or more, and 45.00% or more in this order, from the viewpoint of suppressing the deterioration of glass stability and suppressing the increase of Tl, the total content (Y2O3+La2O3+Gd2O3+Yb2O3) is preferably 70.00% or less, more preferably 65.00% or less, and more preferably 60.00% or less, 55.00% or less, 53.00% or less, and 50.00% or less in this order.
[0034] The content of each of Li2O, Na2O, K2O, and Cs2O can be 0.00%, 0.00% or more, more than 0.00%, 0.05% or more, or 0.10% or more. Also, the content of each of Li2O, Na2O, K2O, and Cs2O can be, for example, 5.00% or less, 4.00% or less, 3.00% or less, 2.00% or less, or 1.00% or less. Li2O, Na2O, K2O and Cs2O all have the function of improving the thermal stability of the glass, but when their contents increase, the refractive index and chemical durability tend to decrease. Therefore, the contents of Li2O, Na2O, K2O and Cs2O are preferably within the above ranges.
[0035] The content of each of MgO, CaO, SrO, and BaO may be 0.00%, 0.00% or more, more than 0.00%, 0.05% or more, or 0.10% or more. Also, the content of each of MgO, CaO, SrO, and BaO may be, for example, 5.00% or less, 4.00% or less, 3.00% or less, 2.00% or less, or 1.00% or less. Although MgO, CaO, SrO and BaO all have the function of improving the thermal stability of the glass, when the contents of these elements are high, the refractive index and chemical durability tend to decrease, so that the contents of MgO, CaO, SrO and BaO are preferably within the above ranges.
[0036] The ZnO content can be 0.00%, 0.00% or more, more than 0.00%, 0.10% or more, or 0.10% or more. The ZnO content can be, for example, 5.00% or less, 4.00% or less, 3.00% or less, or 2.00% or less. ZnO has the function of improving the thermal stability of the glass, but as the ZnO content increases, the specific gravity tends to increase, so the ZnO content is preferably within the above range.
[0037] The ZrO2 content can be 0.00%, 0.00% or more, more than 0.00%, 1.00% or more, 3.00% or more, or 5.00% or more. Also, the ZrO2 content can be, for example, 10.00% or less, or 8.00% or less. ZrO2 has the function of increasing the refractive index of the glass, but as the content of ZrO2 increases, the thermal stability of the glass tends to decrease, so the content of ZrO2 is preferably within the above range.
[0038] The Ta2O5 content can be 0.00%, 0.00% or more, more than 0.00%, 0.10% or more, or 0.10% or more. Also, the Ta2O5 content can be, for example, 5.00% or less, 4.00% or less, 3.00% or less, or 2.00% or less. Ta2O5 has the function of increasing the refractive index of the glass, but as the Ta2O5 content increases, the thermal stability of the glass tends to decrease, so the Ta2O5 content is preferably within the above range.
[0039] The optical glass may further contain one or more of P2O5, Al2O3, and the like in addition to the above components. The P2O5 content can be 0.00% or more, and is preferably 10.00% or less, and more preferably 8.00% or less, 6.00% or less, 4.00% or less, 2.00% or less, 1.00% or less, and 0.50% or less in that order. The Al2O3 content can be 0.00% or more, and is preferably 10.00% or less, and more preferably 8.00% or less, 6.00% or less, 4.00% or less, 2.00% or less, 1.00% or less, and 0.50% or less in that order.
[0040] In the optical glass, the platinum (Pt) content is preferably 10 ppm or less, more preferably 8 ppm or less, and further preferably 7 ppm or less, and 5 ppm or less. The lower limit of the platinum content is not particularly limited, and can be, for example, 0.001 ppm or more. By setting the Pt content within the above range, the coloring of the glass caused by Pt can be reduced. This is preferable in terms of reducing the difference between λ70 and λ5 (λ70-λ5). The platinum content is the mass-based content relative to the total mass of the glass, and can be quantified by inductively coupled plasma mass spectrometry (ICP-MS).
[0041] Pb, As, Cd, Tl, Be, and Se are each toxic, and therefore it is preferable not to include these elements, i.e., not to introduce these elements into the glass as glass components. U, Th, and Ra are all radioactive elements, and therefore it is preferable not to contain these elements, i.e., not to introduce these elements into the glass as glass components. V, Cr, Mn, Fe, Co, Ni, Cu, Pr, Nd, Pm, Sm, Eu, Tb, Dy, Ho, Er, Tm, and Ce are undesirable elements to be contained in glass for optical elements because they increase the coloring of the glass and are sources of fluorescence. Therefore, it is preferable not to contain these elements, i.e., not to introduce these elements into the glass as glass components.
[0042] Sb and Sn are elements that function as fining agents and can be added as desired. The amount of Sb added is, calculated as Sb2O3 and assuming the total content of glass components other than Sb2O3 to be 100 mass%, preferably in the range of 0.000 to 0.100 mass%, more preferably in the range of 0.000 to 0.020 mass%, even more preferably in the range of 0.000 to 0.010 mass%, and even more preferably in the range of 0.000 to 0.005 mass%. The amount of Sn added is, converted to SnO2, preferably in the range of 0.000 to 0.100 mass%, more preferably in the range of 0.000 to 0.020 mass%, even more preferably in the range of 0.000 to 0.010 mass%, and even more preferably in the range of 0.000 to 0.005 mass%, when the total content of glass components other than SnO2 is taken as 100 mass%.
[0043] <Glass properties>
[0044] (Abbe number νd) The Abbe number νd is a value that represents the property related to dispersion, and is expressed as νd=(nd-1) / (nF-nC) using the refractive indices nd, nF, and nC at the d-line, F-line, and C-line. From the viewpoint of usefulness as a material for optical elements and a material for light guide plates, the Abbe number νd of the optical glass is preferably 20.00 or more, more preferably 21.00 or more, and further preferably 22.00 or more and 23.00 or more in that order. From the same viewpoint, the Abbe number νd is preferably 30.00 or less, more preferably 28.00 or less, and further preferably 26.00 or less, 25.00 or less, and 24.00 or less in that order.
[0045] (glass transition temperature Tg) From the viewpoint of machinability, the glass transition temperature Tg of the optical glass is preferably 560°C or higher. Glass with a high glass transition temperature is preferred because it tends to be less likely to break during mechanical processing of the glass, such as cutting, milling, grinding, and polishing. From the viewpoint of machinability, the glass transition temperature Tg is more preferably 570°C or higher, and further preferably 580°C or higher, 590°C or higher, and 600°C or higher in that order. On the other hand, from the viewpoint of reducing the load on the annealing furnace and the molding die, the glass transition temperature Tg is preferably 800°C or lower, and more preferably 790°C or lower, 780°C or lower, 770°C or lower, 760°C or lower, and 750°C or lower in that order.
[0046] The glass transition temperature Tg is determined as follows. In differential scanning calorimetry, when a glass sample is heated, an endothermic behavior associated with a change in specific heat, i.e., an endothermic peak appears, and when the temperature is further increased, an exothermic peak appears. In differential scanning calorimetry analysis, a differential scanning calorimetry curve (DSC (Differential Scanning Calorimetry) curve) is obtained, in which the horizontal axis represents temperature and the vertical axis represents the amount corresponding to the heat generation and endothermic heat of the sample. The intersection of the tangent at the point where the slope of the curve becomes maximum when an endothermic peak appears from the baseline and the baseline is taken as the glass transition temperature Tg. The glass transition temperature Tg can be measured by using glass that has been thoroughly crushed in a mortar or the like as a sample and a differential scanning calorimeter at a heating rate of 10°C / min.
[0047] (Temperature Tl) The present inventors have newly discovered that glass with a low melt-switching temperature Tl in the above-mentioned differential scanning calorimetry is less likely to suffer from surface devitrification. When processing glass with a devitrified surface into a light guide plate or the like, the devitrified portion must be removed. Therefore, surface devitrification causes a decrease in yield. In addition, glass with a devitrified surface has a cloudy glass surface, making it difficult to inspect the quality of the inside of the glass. Therefore, glass that is less likely to suffer from surface devitrification is preferable. The Tl of the optical glass is preferably 1300°C or less, more preferably 1295°C or less, and more preferably 1290°C or less, 1285°C or less, 1280°C or less, 1275°C or less, 1270°C or less, 1265°C or less, 1260°C or less, 1255°C or less, 1250°C or less, 1247°C or less, 1246°C or less, 1245°C or less, 1244°C or less, 1243°C or less, 1242°C or less, 1241°C or less, and 1240°C or less in that order. The Tl of the optical glass can be, for example, 1200°C or more, 1210°C or more, or 1220°C or more. However, from the viewpoint of suppressing surface devitrification, the lower the Tl, the more preferable, so the Tl of the optical glass may be below the above range.
[0048] The temperature Tl is determined from the DSC curve as the temperature at the intersection between the tangent line at the point where the slope from the top of the endothermic peak due to melting to the baseline is maximum and the baseline. The temperature at the intersection is the temperature h in Figure 5 of "NEW GLASS, Vol.28, No.110 2013".
[0049] (specific gravity) The refractive power of the optical elements that make up an optical system is determined by the refractive index of the glass that makes up the optical element and the curvature of the optical functional surface of the optical element (the surface through which the light rays to be controlled enter and exit). If you try to increase the curvature of the optical functional surface, the thickness of the optical element also increases. As a result, the optical element becomes heavier. In contrast, if glass with a high refractive index is used, it is possible to obtain a large refractive power without increasing the curvature of the optical functional surface. From the above, if the refractive index can be increased while suppressing an increase in the specific gravity of the glass, it will be possible to reduce the weight of an optical element having a certain refractive power. Also, with regard to the glass constituting the light guide plate, a low specific gravity is preferable from the viewpoint of reducing the weight of the light guide plate and the image display device. From the above viewpoints, the specific gravity of the optical glass is preferably 5.30 or less, more preferably 5.20 or less, and even more preferably 5.10 or less. Since a lower specific gravity is more preferable from the viewpoint of reducing the weight of the optical element, the lower limit of the specific gravity of the optical glass is not particularly limited. In one embodiment, the specific gravity can be 4.00 or more, 4.40 or more, or 4.800 or more.
[0050] (T460) "T460" is the internal transmittance at a wavelength of 460 nm for a thickness of 10 mm, calculated using the respective spectral transmittances of a pair of samples with different thicknesses. As described above, the spectral transmittance includes surface reflection loss. The internal transmittance τ (%) is calculated using the following formula shown above: logτ=(logT1-logT2) / Δd×10 It can be calculated using: From the viewpoint of reducing the loss of blue wavelength light propagating through the light guide plate, T460 of the above optical glass is preferably 90.0% or more, more preferably 92.5% or more, more preferably 95.0% or more, even more preferably 96.0% or more, and even more preferably 97.0% or more.
[0051] (β-OH) β-OH calculated by the following formula (1) means the absorbance due to hydroxyl groups. Therefore, the content of water (and / or hydroxide ions, hereinafter simply referred to as "water") in glass can be evaluated by β-OH. In other words, a high β-OH in glass means a high water content in the glass. β-OH=-[ln(B / A)] / t…(1) In the above formula (1), t represents the thickness (mm) of the glass used to measure the spectral transmittance, A represents the spectral transmittance (%) at a wavelength of 2500 nm when light is incident on the glass parallel to its thickness direction, and B represents the spectral transmittance (%) at a wavelength of 2900 nm when light is incident on the glass parallel to its thickness direction. In formula (1), ln is the natural logarithm. The unit of β-OH is mm -1 Increasing the β-OH value of the glass is preferable because it leads to a smaller difference between λ70 and λ5 (λ70-λ5). The β-OH of the above optical glass is 0.50 mm -1 It is preferable that the thickness is 0.60 mm or more. -1 More preferably, it is 0.70 mm or more. -1 More preferably, it is 0.80 mm or more. -1 More preferably, it is 0.90 mm or more. -1 The β-OH of the optical glass is, for example, 1.50 mm or more. -1 Less than or equal to 1.25mm -1 It can be the following:
[0052] The optical glass described above is useful as a glass material for light guide plates, and is also useful as a glass material for optical elements.
[0053] <Glass manufacturing method> The optical glass can be obtained by the following method. Raw materials such as oxides, carbonates, sulfates, nitrates, and hydroxides are weighed, prepared, and thoroughly mixed to obtain the desired glass composition. This mixed batch is heated and melted in a melting vessel, degassed, and stirred to produce a homogeneous, bubble-free molten glass. Specifically, the molten glass can be produced by a known melting method. The molten glass thus obtained can be molded to obtain the optical glass.
[0054] For example, in the melting process, glass raw materials are prepared so as to obtain a target glass composition, and are thoroughly mixed to prepare a batch raw material, which is then roughly melted in a platinum crucible. In the melting process, a reducing agent can be added to the glass raw material. The reducing agent is not particularly limited, and examples thereof include substances exhibiting reducing properties, such as Al, Si, Ti, W, H2, CO, and C. More specifically, examples of substances exhibiting reducing properties include carbon compounds and activated carbon C. By adding a reducing agent to the glass raw material, oxygen with high reactivity, which is generated when the glass raw material is vitrified, reacts with the reducing agent, suppressing the oxidation reaction of platinum derived from the platinum crucible. As a result, the platinum content in the glass can be reduced. Reducing the platinum content is preferable because it leads to a reduction in the difference between λ70 and λ5 (λ70-λ5).
[0055] The melting atmosphere in the glass melting step is preferably a non-oxidizing atmosphere. By carrying out the melting step in a non-oxidizing atmosphere, the oxygen partial pressure in the melting atmosphere is reduced, and oxidation of platinum originating from the platinum crucible is suppressed, thereby making it possible to reduce the amount of platinum dissolved in the molten glass.
[0056] The non-oxidizing atmosphere is not particularly limited, and examples thereof include an inert gas atmosphere such as nitrogen, carbon dioxide, argon, helium, etc., and a water vapor-added atmosphere. In order to increase the β-OH of the final glass, a water vapor-added atmosphere is preferred.
[0057] Adding water vapor to the melting atmosphere can increase the β-OH of the final glass. Also, adding water vapor to the melting atmosphere can effectively prevent platinum and other metals from dissolving in the glass. Furthermore, adding water vapor to the melting atmosphere can supply sufficient dissolved gas to the glass, thereby improving the defoaming and clarification of the glass.
[0058] The method of adding water vapor to the melting atmosphere is not particularly limited, but may be, for example, a method of inserting a connecting pipe into the crucible from an opening provided in the melting apparatus and supplying water vapor to the space in the crucible through the pipe as necessary.
[0059] The melting process may be accompanied by bubbling in order to stir the molten material. The bubbling during melting may be continued even after the blended materials are melted. By stirring the molten material in the melting process, the oxidation of the glass components progresses. On the other hand, by stirring the molten material in the melting process, the oxidation of platinum derived from the platinum crucible is suppressed. This is because the glass components tend to be more easily oxidized than platinum. As a result, the reduction reaction of the glass components is suppressed and the reduction color is reduced. Furthermore, the dissolution of platinum into the molten material is suppressed and the coloring derived from platinum is also reduced. This point is preferable because it leads to a small difference between λ70 and λ5 (λ70-λ5).
[0060] The gas used for bubbling is not particularly limited, and any known gas can be used, such as inert gases such as nitrogen, carbon dioxide, argon, and helium, air, and gases obtained by adding water vapor to these gases.
[0061] By using a gas containing water vapor as the bubbling gas, the β-OH of the final glass can be increased. In addition, by using a gas containing water vapor as the bubbling gas, the dissolution of platinum into the glass can be effectively prevented. Furthermore, by using a gas containing water vapor as the bubbling gas, a sufficient amount of dissolved gas can be supplied to the glass, and as a result, the defoaming and clarification of the glass can be improved.
[0062] The content of water vapor in such a gas containing water vapor is preferably 10% by volume or more, more preferably 20% by volume or more, and further preferably 30% by volume or more, 40% by volume or more, 50% by volume or more, 60% by volume or more, 70% by volume or more, 80% by volume or more, and 90% by volume or more in that order. The higher the content of water vapor, the more preferable it is, and by setting it in the above range, the β-OH of the finally obtained glass can be increased.
[0063] For example, the molten material obtained by rough melting is quenched and pulverized to produce cullet. The cullet is then placed in a platinum crucible, heated, and remelted to produce molten glass, which is then clarified and homogenized, and then molded and slowly cooled to produce a molded glass body. A known method may be used to mold and slowly cool the molten glass.
[0064] In the melting, some of the components contained in the glass are reduced, and coloring of the glass molded body (hereinafter, referred to as "reduced color") may occur. When a reduced color occurs, the reduced color can be reduced by subjecting the glass molded body to a heat treatment. The heat treatment of the glass molded body can be performed in an oxidizing atmosphere, for example, at a temperature of about the glass transition temperature. If the heat treatment temperature is high, the heat treatment time can be shortened. In addition, the heat treatment time can be shortened by increasing the oxygen partial pressure in the oxidizing atmosphere. In this way, the heat treatment time varies depending on the heat treatment temperature and the oxygen partial pressure in the oxidizing atmosphere, so it is sufficient to set it so that the coloring of the glass can be sufficiently reduced. The heat treatment time can be, for example, about 0.1 hours to 100 hours. The oxidizing atmosphere may be any atmosphere containing oxygen, and may be, for example, an air atmosphere.
[0065] [Light guide plate, image display device] One aspect of the present invention is a light guide plate made of the optical glass; an image display device including an image display element and a light guide plate for guiding light emitted from the image display element, the light guide plate being made of any one of the optical glasses described above; A specific embodiment of the image display device will be described later.
[0066] [Glass material for press molding, optical element blanks, and their manufacturing methods] Another aspect of the present invention is a glass material for press molding comprising the optical glass; an optical element blank made of the optical glass; Regarding.
[0067] According to another aspect of the present invention, a method for producing a glass material for press molding, comprising a step of molding the optical glass into a glass material for press molding; a method for producing an optical element blank, comprising a step of press-molding the glass material for optical glass press molding using a press mold to produce an optical element blank; a method for producing an optical element blank, comprising the step of forming the optical glass into an optical element blank; will also be provided.
[0068] An optical element blank is an optical element base material that approximates the shape of a target optical element and has polishing margins (surface layers to be removed by polishing) and, if necessary, grinding margins (surface layers to be removed by grinding) added to the shape of the optical element. The optical element is finished by grinding and polishing the surface of the optical element blank. In one embodiment, the optical element blank can be produced by a method (called a direct press method) in which a molten glass obtained by melting an appropriate amount of the above glass is press-molded. In another embodiment, the optical element blank can also be produced by solidifying a molten glass obtained by melting an appropriate amount of the above glass.
[0069] In another embodiment, a glass material for press molding is prepared, and the prepared glass material for press molding is press molded to produce an optical element blank.
[0070] The press molding of the glass material for press molding can be carried out by a known method in which the glass material for press molding in a heated and softened state is pressed in a press mold. Both heating and press molding can be carried out in the atmosphere. By annealing after press molding to reduce distortion inside the glass, a homogeneous optical element blank can be obtained.
[0071] Glass materials for press molding include not only those called glass gobs for press molding, which are used for press molding as they are to produce optical element blanks, but also those that are mechanically processed such as by cutting, grinding, polishing, etc., and are used for press molding via glass gobs for press molding. Cutting methods include a method in which a groove is formed in the portion of the surface of the glass plate to be cut by a method called scribing, and local pressure is applied to the grooved portion from the back side of the surface on which the groove is formed, thereby breaking the glass plate at the grooved portion, and a method in which the glass plate is cut by a cutting blade. Grinding and polishing methods include barrel polishing, etc.
[0072] The glass material for press molding can be produced, for example, by casting molten glass into a mold to form a glass plate, and cutting this glass plate into a plurality of glass pieces. Alternatively, a suitable amount of molten glass can be molded to produce a glass gob for press molding. An optical element blank can also be produced by reheating, softening, and press-molding the glass gob for press molding. The method of producing an optical element blank by reheating, softening, and press-molding glass is called a reheat press method, as opposed to a direct press method.
[0073] [Optical elements and their manufacturing methods] Another aspect of the present invention is An optical element made of the above optical glass Regarding. The optical element is produced using the optical glass. In the optical element, the glass surface may be coated with one or more layers of coating, such as a multilayer film including an anti-reflection film.
[0074] According to another aspect of the present invention, A method for producing an optical element, comprising the step of producing an optical element by grinding and / or polishing the optical element blank described above; will also be provided.
[0075] In the above-mentioned method for producing an optical element, known methods may be used for grinding and polishing, and an optical element with high internal quality and surface quality can be obtained by thoroughly cleaning and drying the surface of the optical element after processing. In this manner, an optical element made of the above-mentioned glass can be obtained. Examples of optical elements include various lenses such as spherical lenses, aspherical lenses, and microlenses, and prisms.
[0076] In addition, the optical element made of the optical glass is also suitable as a lens constituting a cemented optical element. Examples of cemented optical elements include a cemented lens formed by cementing lenses together, and a lens and a prism. For example, a cemented optical element can be produced by precisely processing (for example, spherical polishing) the cemented surfaces of two optical elements to be cemented so that the shapes are inverted, applying an ultraviolet-curing adhesive used for bonding the cemented lens, bonding them together, and then irradiating ultraviolet light through the lens to cure the adhesive. In this way, the above glass is preferable for producing a cemented optical element. A plurality of optical elements to be cemented are produced using a plurality of types of glass having different Abbe numbers νd, and cemented together to produce an element suitable for correcting chromatic aberration. EXAMPLES
[0077] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the embodiments shown in the examples.
[0078] [Example 1, Comparative Example 1] First, oxides, hydroxides, carbonates, and nitrates corresponding to the components of glass were prepared as raw materials, and the raw materials were weighed and mixed so that the glass composition of the optical glass obtained would be each composition shown in the table below, and the raw materials were thoroughly mixed. The thus obtained mixed raw materials (batch raw materials) were charged into a platinum crucible together with a reducing agent in the amount (unit: mass %) shown in the table below relative to 100 mass % of the mixed raw materials, and melted to form molten glass by heating at 1250°C to 1400°C for 2 hours (melting process), and homogenized and refined by stirring at 1300°C to 1400°C for 1 to 2 hours (homogenization and clarification process). The molten glass was cast into a mold preheated to an appropriate temperature. The cast glass was heat-treated at the glass transition temperature Tg for 30 minutes and allowed to cool to room temperature in a furnace to obtain a glass molded body. The obtained molded body was heated to the glass transition temperature Tg in an air atmosphere and heat-treated by holding at this temperature for 48 hours. Thus, a glass sample was obtained. In the following tables, the unit of content is mass %. The Sb2O3 content is the content when the total content of glass components other than Sb2O3 is taken as 100 mass %.
[0079] The following operations were carried out in the melting process, homogenization and clarification process.
[0080] A platinum pipe was inserted from the outside of the melting furnace into a platinum crucible placed inside the furnace, and water vapor was supplied to the space inside the platinum crucible through the platinum pipe. The flow rate of the water vapor supplied was set to the flow rate shown in the table below.
[0081] Nitrogen was supplied to the space in the platinum crucible through the platinum pipe, and water vapor was bubbled into the melt from a tube installed at the bottom of the crucible. The flow rates of the supplied nitrogen and water vapor were 30 L / min for nitrogen and 5.0 cc / min for water vapor.
[0082] In this manner, glass samples of the optical glasses Nos. 1 to 10 of Example 1 and a glass sample of the optical glass of Comparative Example 1 were obtained.
[0083] [Comparative Examples 2 and 3] In the following table, Comparative Example 2 is TAFD55-W manufactured by HOYA Corporation, and Comparative Example 3 is E-FDS3-W manufactured by HOYA Corporation.
[0084] The physical properties of the optical glasses of the Examples and Comparative Examples are shown in the following table. The physical properties of the optical glasses were measured by the methods described below.
[0085] [Evaluation of physical properties of optical glass] (1) λ5, λ70, T460 A glass sample with a thickness of 10±0.1 mm and two optically polished flat surfaces facing each other was used, and a spectrophotometer was used to apply light with intensity Iin perpendicularly to the polished surfaces, and the intensity Iout of the light transmitted through the glass sample was measured. The spectral transmittance Iout / Iin was calculated, and the wavelength at which the spectral transmittance was 5% was defined as λ5, and the wavelength at which the spectral transmittance was 70% was defined as λ70. The difference between λ70 and λ5 (λ70-λ5) was calculated from the determined λ5 and λ70.
[0086] (2) T460 The internal transmittance T460 of a 10 mm thick sample at a wavelength of 460 nm was calculated using the respective spectral transmittances (including surface reflection losses) of a pair of samples with different thicknesses.
[0087] (3) Refractive index nd, Abbe number νd The glass obtained by cooling at a cooling rate of -30°C / hour was measured for refractive index nd and Abbe number vd by the refractive index measurement method specified by the Japan Optical Glass Industry Association.
[0088] (4) Glass transition temperature Tg, temperature Tl The glass was thoroughly crushed in a mortar and used as a sample, and a differential scanning calorimeter (DSC3300SA) manufactured by NETZSCH was used to perform DSC measurement at a heating rate of 10°C / min to obtain a DSC curve. From the obtained DSC curve, the glass transition temperature Tg and the temperature at which the glass changes to melt Tl were obtained as described above.
[0089] (4) Specific gravity Specific gravity was measured by Archimedes' method.
[0090] (5)β-OH The glass sample was processed into a plate-shaped glass specimen having a thickness of 1 mm and parallel optically polished flat surfaces. Light was irradiated perpendicularly to the polished surface of the plate-shaped glass specimen, and the spectral transmittance A at a wavelength of 2500 nm and the spectral transmittance B at a wavelength of 2900 nm were measured using a spectrophotometer, and β-OH was calculated using the formula (1) shown above.
[0091] The Pt content of each of the optical glasses No. 1 to 10 in Example 1 was quantitatively determined by inductively coupled plasma mass spectrometry (ICP-MS) and was found to be in the range of 0.001 ppm to 10 ppm.
[0092] Each of the optical glasses Nos. 1 to 10 of Example 1 was visually observed. As a result, no surface devitrification was observed in the glass blocks of each of the optical glasses of Example 1.
[0093] [Table 1]
[0094] [Table 2]
[0095] [Table 3]
[0096] Example 2 1 is a schematic diagram of a head mounted display, which is an example of an image device including an image display element and a light guide plate. A head mounted display 1 having the configuration shown in FIG. 1 was produced by the following method. Each of the optical glasses of Example 1 and Comparative Examples 1 to 3 was processed into a rectangular thin plate having a length of 50 mm, a width of 20 mm, and a thickness of 1.0 mm, to obtain a light guide plate 10. This light guide plate was attached to a head mounted display 1 (hereinafter, abbreviated as "HMD1") shown in FIG. 1. FIG. 1(a) is a front perspective view of the HMD1, and FIG. 1(b) is a rear perspective view of the HMD1. As shown in FIG. 1(a) and FIG. 1(b), a spectacle lens 3 is attached to the front part of a spectacle-type frame 2 worn on the head of a user. A backlight 4 for illuminating an image is attached to the mounting part 2a of the spectacle-type frame 2. A signal processing device 5 for projecting an image and a speaker 6 for reproducing sound are provided on the temple part of the spectacle-type frame 2. Flexible printed circuits (FPCs) 7 constituting wiring drawn from the circuit of the signal processing device 5 are wired along the spectacle-type frame 2. A display element unit (e.g., a liquid crystal display element) 20 is wired to the center position of both eyes of the user by the FPC 7, and is held so that the approximate center of the display element unit 20 is located on the optical axis of the backlight 4. The imager unit 20 is fixed relative to the light guide plate 10 so as to be located approximately at the center of the light guide plate 10. Holographic optical elements (HOEs) 32R and 32L (first optical elements) are fixed in close contact with the first surface 10a of the light guide plate 10 by adhesive or the like at locations in front of the user's eyes. HOEs 52R and 52L are laminated on the second surface 10b of the light guide plate 10 at positions facing the imager unit 20 across the light guide plate 10. 2 is a side view showing a schematic configuration of the HMD 1 shown in FIG. 2. In FIG. 2, in order to clarify the drawing, only the main parts are shown, and the eyeglass-type frame 2 and the like are omitted. As shown in FIG. 2, the HMD 1 has a bilaterally symmetrical structure with respect to a center line X connecting the center of the image display element 24 and the light guide plate 10. Furthermore, the light of each wavelength incident on the light guide plate 10 from the image display element 24 is divided into two and guided to the right eye and the left eye of the user, as described later. The optical paths of the light of each wavelength guided to each eye are also approximately bilaterally symmetrical with respect to the center line X. As shown in FIG. 2, the backlight 4 has a laser light source 21, a diffusion optical system 22, and a microlens array 23. The display element unit 20 is an image generating unit having an image display element 24, and is driven, for example, by a field sequential method. The laser light source 21 has laser light sources corresponding to the wavelengths of B (wavelength 436 nm), G (wavelength 546 nm), and R (wavelength 633 nm), and sequentially irradiates light of each wavelength at high speed. The light of each wavelength is incident on the diffusion optical system 22 and the microlens array 23, and is converted into a uniform, highly directional parallel light beam without unevenness in the amount of light, and is incident perpendicularly on the display panel surface of the image display element 24. The image display element 24 is, for example, a transmissive liquid crystal (LCDT-LCOS) panel driven by a field sequential method. The image display element 24 modulates the light of each wavelength according to an image signal generated by an image engine (not shown) of the signal processing device 5. The light of each wavelength modulated by the pixels in the effective area of the image display element 24 is incident on the light guide plate 10 with a predetermined light beam cross section (approximately the same shape as the effective area). The image display element 24 can also be replaced with other types of display elements, such as a DMD (Digital Mirror Device), a reflective liquid crystal (LCOS) panel, a MEMS (Micro Electro Mechanical Systems), an organic EL (Electro-Luminescence), or an inorganic EL. The image generating unit of the image display element 20 is not limited to a field sequential type image display element, but may be a simultaneous type image display element (a display element having a predetermined arrangement of RGB color filters in front of the emission surface). In this case, for example, a white light source is used as the light source. As shown in Fig. 2, the light of each wavelength modulated by the image display element 24 is sequentially incident on the inside of the light guide plate 10 from the first surface 10a. HOEs 52R and 52L (second optical elements) are laminated on the second surface 10b of the light guide plate 10. The HOEs 52R and 52L are, for example, reflective volume phase HOEs having a rectangular shape, and are configured by laminating three photopolymer sheets on which interference fringes corresponding to the light of each wavelength of R, G, and B are recorded. In other words, the HOEs 52R and 52L are configured to have a wavelength selection function that diffracts the light of each wavelength of R, G, and B and transmits light of other wavelengths. The HOEs 32R and 32L are also reflective volume phase type HOEs and have the same layer structure as the HOEs 52R and 52L. The HOEs 32R and 32L and the HOEs 52R and 52L may have, for example, approximately the same pitch of the interference fringe patterns. The HOEs 52R and 52L are stacked with their centers aligned and with their interference fringe patterns inverted by 180 degrees. They are then fixed in close contact with the second surface 10b of the light guide plate 10 by adhesive or the like so that their centers in the stacked state are aligned with the center line X. Light of each wavelength modulated by the image display element 24 is sequentially incident on the HOEs 52R and 52L via the light guide plate 10. The HOEs 52R and 52L each diffract the light of each wavelength incident sequentially at a predetermined angle to guide it to the right eye and the left eye. The light of each wavelength diffracted by the HOEs 52R and 52L is repeatedly totally reflected at the interface between the light guide plate 10 and the air, propagates inside the light guide plate 10, and is incident on the HOEs 32R and 32L. Here, the HOEs 52R and 52L give the same diffraction angle to the light of each wavelength. Therefore, all the light of wavelengths that are incident at approximately the same position on the light guide plate 10 (or, in other words, emitted from approximately the same coordinates within the effective area of the image display element 24) propagate through approximately the same optical path inside the light guide plate 10 and are incident on approximately the same position on the HOEs 32R and 32L. From another perspective, the HOEs 52R and 52L diffract the light of each wavelength of RGB so that the pixel positional relationship within the effective area of the image displayed in the effective area of the image display element 24 is faithfully reproduced on the HOEs 32R and 32L. Thus, in this embodiment, HOEs 52R and 52L each diffract light of all wavelengths emitted from approximately the same coordinates within the effective area of image display element 24 so that it is incident on approximately the same position on HOEs 32R and 32L. Alternatively, HOEs 52R and 52L may be configured to diffract light of all wavelengths that originally constitute the same pixel but are relatively shifted within the effective area of image display element 24 so that it is incident on approximately the same position on HOEs 32R and 32L. The light of each wavelength incident on the HOEs 32R and 32L is diffracted by the HOEs 32R and 32L and sequentially emitted from the second surface 10b of the light guide plate 10 in a substantially perpendicular direction to the outside. The light of each wavelength emitted as substantially parallel light in this manner is imaged on the right and left retina of the user as a virtual image I of the image generated by the image display element 24. In addition, a condenser effect may be given to the HOEs 32R and 32L so that the user can observe the virtual image I of the enlarged image. That is, the light incident on the peripheral area of the HOEs 32R and 32L may be emitted at an angle closer to the center of the pupil and imaged on the user's retina. Alternatively, in order to allow the user to observe the virtual image I of the enlarged image, the HOEs 52R and 52L may diffract the light of each wavelength of RGB so that the pixel positional relationship on the HOEs 32R and 32L forms an enlarged similar shape to the pixel positional relationship within the effective area of the image displayed in the effective area of the image display element 24. Since the air-equivalent optical path length of light traveling inside the light guide plate 10 becomes shorter as the refractive index increases, by using each of the above optical glasses having a high refractive index, it is possible to increase the apparent viewing angle relative to the width of the image display element 24. Furthermore, since the specific gravity of a glass having a high refractive index is kept low, it is possible to provide a light guide plate that is lightweight yet provides the above effects. The light guide plate 10 thus obtained was incorporated into the HMD 1, and the image was evaluated at the eye point position. With the HMD 1 incorporating the light guide plate made of each of the optical glasses of the Examples, it was possible to observe high brightness and high contrast images at a wide viewing angle. With the HMD 1 incorporating the light guide plate made of each of the optical glasses of the Examples, a clearer image was obtained compared to the HMD 1 incorporating the light guide plate made of each of the optical glasses of Comparative Examples 1 to 3. The light guide plate made of each of the optical glasses of the Examples can be used in see-through transmissive head mounted displays and non-transmissive head mounted displays. These head mounted displays have a light guide plate made of high refractive index glass, which provides a wide viewing angle and a sense of immersion, making them ideal as image display devices for use in combination with information terminals, for providing AR (Augmented Reality), and for providing movies, games, VR (Virtual Reality), etc. In this embodiment, a head mounted display has been taken as an example for explanation, but the light guide plate may be attached to other image display devices.
[0097] Example 3 Glass gobs for press molding (glass gobs) were prepared using the various glasses obtained in Example 1. The glass gobs were heated and softened in the atmosphere, and press molded in a press mold to prepare lens blanks (optical element blanks). The prepared lens blanks were removed from the press mold, annealed, and machined, including polishing, to prepare spherical lenses made of the optical glasses of Example 1.
[0098] Example 4 A desired amount of the molten glass produced in Example 1 was press molded in a press mold to produce a lens blank (optical element blank). The produced lens blank was removed from the press mold, annealed, and subjected to mechanical processing including polishing to produce a spherical lens made of each optical glass of Example 1.
[0099] Example 5 The molten glass produced in Example 1 was solidified to produce a glass lump (optical element blank), which was then annealed and machined, including polishing, to produce a spherical lens made of each of the optical glasses in Example 1.
[0100] Example 6 The spherical lenses produced in Examples 3 to 5 were bonded to spherical lenses made of other types of glass to produce cemented lenses.
[0101] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. For example, by subjecting the glass compositions exemplified above to compositional adjustments as described in the specification, an optical glass according to one aspect of the present invention can be obtained. Furthermore, it is of course possible to arbitrarily combine two or more of the items described in the specification as examples or preferred ranges.
Claims
1. The wavelength λ5 at which the spectral transmittance is 5% at a thickness of 10 mm is greater than 370 nm and less than 410 nm; The difference between the wavelengths λ70 and λ5 at which the spectral transmittance is 70% at a thickness of 10 mm (λ70-λ5) is 70 nm or less, and An optical glass having a refractive index nd of 2.00000 or more.
2. B 2 O 3 The optical glass of claim 1 , comprising:
3. SiO 2 , B 2 O 3 , TiO 2 , Nb 2 O 5 , Y 2 O 3 , La 2 O 3 and Gd 2 O 3 The optical glass of claim 1 , comprising:
4. A light guide plate comprising the optical glass according to any one of claims 1 to 3.
5. An image display element; a light guide plate for guiding light emitted from the image display element; Including, An image display device, wherein the light guide plate is the light guide plate according to claim 4.
6. An optical element comprising the optical glass according to any one of claims 1 to 3.
Citation Information
Patent Citations
Optical glass, preform and optical element
JP2019116408A