Optical laminate and manufacturing method of the same

The optical laminate with a functional layer of pigments and resin achieves high infrared transmittance and color matching, addressing visibility and design issues in applications like driver monitoring systems.

JP2024146762AInactive Publication Date: 2024-10-15TOYO INK MFG CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024019369
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-13
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing optical laminates struggle to achieve high infrared transmittance while maintaining a black appearance and matching the color of transmitted visible light with the irradiated light, leading to reduced visibility and design issues in applications like driver monitoring systems.

Method used

An optical laminate with an optical functional layer containing multiple types of pigments and a binder resin, achieving specific spectral transmittance ratios and a black appearance by absorbing visible light without impairing infrared transmission.

Benefits of technology

The laminate provides excellent infrared transmittance with a black appearance and matching visible light colors, enhancing visibility and design integration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146762000001_ABST
    Figure 2024146762000001_ABST
Patent Text Reader

Abstract

To provide an optical laminate which is excellent in transmissivity in near-infrared region of wavelength 850 nm to 2500 nm, is black, and is emitted light of which is same in color as transmitted light in visible light region.SOLUTION: The optical laminate includes an optical functional layer on at least one surface of a base material. The optical functional layer includes colorant containing plural types of pigments and binder resin. The optical laminate has an average spectral transmission factor of 25% or less in a wavelength 350 nm to 750 nm and an average spectral transmission factor of 85% or more in a wavelength 850 nm to 2500 nm. When a maximum spectral transmission factor in a wavelength 350 nm or more and less than 460 nm is denoted by T1, a maximum spectral transmission factor in wavelength 460 nm or more and less than 570 nm is denoted by T2, and a maximum spectral transmission factor in wavelength 570 nm or more and 750 nm or less is denoted by T3, the following expressions (1) and (2) are satisfied. 1≤T1 / T2≤10...(1) and 2≤T3 / T2≤20...(2).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical laminate and a method for producing the same. [Background technology]

[0002] In various optical devices, there is a demand for technology to control optical properties such as selectively transmitting or blocking light of specific wavelengths. This technology is used in laminates such as dichroic mirrors, bandpass filters, AR coatings, UV cut filters, IR cut filters, and UVIR cut filters. Infrared wavelengths are often used as light sources for infrared sensors, and LEDs with maximum wavelengths of 850 nm, 905 nm, and 940 nm are used. LED light with a maximum wavelength of 850 nm contains some visible light, so in order to improve sensor accuracy, there is a demand for laminate technology that blocks the visible light and transmits only infrared light.

[0003] One example of the use of laminates for sensors is a driver monitoring system that uses infrared rays to detect the driver's movements. This is a system that detects the driver's condition by irradiating the driver with infrared rays from LEDs built into the automobile panel (Patent Document 1). In recent years, it is expected that the design of automobile panels will be improved by incorporating LEDs of various colors that serve as indicator lights for the automobile panel in addition to infrared sensors and lighting the LED indicator lights as backlights from behind the laminate.

[0004] On the other hand, from the viewpoint of the appearance of the optical member, it is preferable that the sensor sensing portion of the laminate is a laminate having a color that matches the black color of the surrounding members. That is, this laminate needs to be infrared-transmissive and have a black appearance. In addition, in order to match the color of the surrounding members, the appearance of the optical laminate is black, but as described above, it is necessary to see the indicator lights of the automobile panel through the optical laminate. However, for example, when a white LED indicator light is turned on as a backlight from behind the laminate and the driver sees the indication, it is ideally preferable that it is seen as white, but the transmitted light of the laminate including the infrared-transmitting layer is often colored, which causes a problem of significantly reducing visibility and design (design).

[0005] For this reason, there has been a strong demand for the development of an optical laminate that is excellent in transmittance in the infrared region and in which the irradiated light and the transmitted light in the visible light region are the same color. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2022-170958 A Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide an optical laminate which has excellent infrared transmittance, is black in color, and in which irradiated light and transmitted light in the visible light region have the same color. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that the above problems can be solved by the following optical laminate, and have thus completed the present invention.

[0009] The present invention provides an optical laminate having an optical functional layer on at least one surface of a substrate, The optical functional layer includes a colorant including a plurality of pigments and a binder resin, The laminate is The average spectral transmittance at wavelengths of 350 nm to 750 nm is 25% or less. The average spectral transmittance at wavelengths of 850 nm to 2500 nm is 85% or more, The present invention relates to an optical laminate, which satisfies the following formulas (1) and (2), where T1 is the maximum spectral transmittance at a wavelength of 350 nm or more and less than 460 nm, T2 is the maximum spectral transmittance at a wavelength of 460 nm or more and less than 570 nm, and T3 is the maximum spectral transmittance at a wavelength of 570 nm or more and less than 750 nm. 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2)

[0010] The present invention also relates to the optical laminate, wherein the colorant containing multiple types of pigments contains a yellow pigment, a red pigment, and a cyan pigment, or a red pigment, a cyan pigment, and a green pigment, or a yellow pigment, a cyan pigment, and a violet pigment.

[0011] The present invention also relates to the optical laminate, wherein the colorant containing multiple types of pigments contains a yellow pigment, a red pigment, and a cyan pigment.

[0012] The present invention also relates to the optical laminate, which is for see-through viewing.

[0013] The present invention also relates to the optical laminate, wherein the optical functional layer contains a dispersant.

[0014] The present invention also relates to the optical laminate, wherein the binder resin contains at least one resin selected from the group consisting of an acrylic resin, a polyester resin, and an epoxy resin.

[0015] A method for producing an optical laminate, comprising a step of applying a colorant containing a plurality of types of pigments and a black ink containing a binder resin onto a substrate to form an optical functional layer, The optical laminate is The average spectral transmittance at wavelengths of 350 nm to 750 nm is 25% or less. The average spectral transmittance at wavelengths of 850 nm to 2500 nm is 85% or more, The present invention relates to a method for producing an optical laminate, which satisfies the following formulas (1) and (2), where T1 is the maximum spectral transmittance at a wavelength of 350 nm or more and less than 460 nm, T2 is the maximum spectral transmittance at a wavelength of 460 nm or more and less than 570 nm, and T3 is the maximum spectral transmittance at a wavelength of 570 nm or more and less than 750 nm. 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2) Effect of the Invention

[0016] According to the present invention, it is possible to provide an optical laminate that has excellent infrared transmittance, is black in color, and in which irradiated light and transmitted light in the visible light region have the same color. [Brief description of the drawings]

[0017] [Figure 1] 1 shows a transmission spectrum of the optical laminate of Example 1 at wavelengths of 320 nm to 800 nm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be described in detail below.

[0019] The following describes in detail the embodiments of the present invention. However, the description of the components described below is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to these contents as long as it does not go beyond the gist of the present invention.

[0020] The present invention provides an optical laminate having an optical functional layer on at least one surface of a substrate, the optical functional layer contains a colorant containing a plurality of types of pigments and a binder resin; The optical laminate is The average spectral transmittance at wavelengths of 350 nm to 750 nm is 25% or less, The average spectral transmittance at wavelengths of 850 nm to 2500 nm is 85% or more, The present invention relates to an optical laminate, which satisfies the following formulas (1) and (2), where T1 is the maximum spectral transmittance at a wavelength of 350 nm or more and less than 460 nm, T2 is the maximum spectral transmittance at a wavelength of 460 nm or more and less than 570 nm, and T3 is the maximum spectral transmittance at a wavelength of 570 nm or more and less than 750 nm. 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2)

[0021] By including multiple types of pigments in the optical functional layer, the visible light that cannot be absorbed by a single pigment can be absorbed while complementing each other, and by setting the average spectral transmittance at wavelengths of 350 nm to 750 nm to 25% or less, a laminate with high blackness can be obtained, and the color can be made to match the color of the peripheral components using the optical laminate (seamless). Furthermore, by satisfying the formulas (1) and (2), it becomes possible for the transmitted light to reproduce the color of the light source as it is (when white light is used as the light source, the transmitted light is visually recognized as white, and when a green light source is used, the transmitted light is visually recognized as green). Furthermore, by setting the average spectral transmittance at wavelengths of 850 nm to 2500 nm to 85% or more, it is possible to achieve color matching covering the infrared light source and the receiving unit without impairing the infrared sensor sensitivity.

[0022] In this specification, the optical laminate may be abbreviated to simply "laminate", but this has the same meaning. In addition, "CI" in this specification means color index (CI).

[0023] <Optical laminate> The optical laminate of the present invention has at least a substrate and an optical functional layer. The optical laminate of the present invention has an average spectral transmittance of 25% or less at wavelengths of 350 nm to 750 nm, preferably 20% or less, and more preferably 15% or less. By having the average spectral transmittance of 25% or less, the OD value (optical density) of the optical laminate is increased, and a black appearance is obtained. In addition, the average spectral transmittance at wavelengths of 850 nm to 2500 nm is 85% or more, preferably 87% or more, and more preferably 90% or more. By having the average spectral transmittance be 85% or more, when the material is used as a decorative member for an infrared sensor, the inhibition of infrared transmission and reception can be minimized, leading to improved sensor sensitivity.

[0024] In the optical laminate of the present invention, when the maximum spectral transmittance of 350 nm or more and less than 460 nm is T1, the maximum spectral transmittance of 460 nm or more and less than 570 nm is T2, and the maximum spectral transmittance of 570 nm or more and less than 750 nm is T3, The following formulas (1) and (2) are satisfied. 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2) When T1, T2, and T3 satisfy the above ranges, blue, green, and red light can be transmitted in a suitable balance, and the irradiated light and the transmitted light in the visible light region have the same color. 1.2≦T1 / T2≦7 2.5≦T3 / T2≦15 It is preferred that 1.5≦T1 / T2≦5 3≦T3 / T2≦10 It is more preferable that:

[0025] <Optical functional layer> The optical functional layer is preferably formed from a colorant containing multiple pigments and a black ink containing a binder resin. For example, the optical functional layer is obtained by applying the colorant containing multiple pigments and the black ink containing a binder resin to a substrate and drying the applied layer, and the resulting printed matter becomes an optical laminate. The thickness of the optical functional layer can be appropriately adjusted depending on the purpose and application, but in one embodiment, it is preferably 3 to 20 μm, more preferably 5 to 15 μm, and even more preferably 5 to 10 μm, because this improves the light blocking property in the visible light region and provides a blacker appearance.

[0026] (Black ink) The black ink contains a colorant including multiple types of pigments, and a binder resin.

[0027] <Coloring agent> Examples of the colorant used in the present invention include various organic pigments, inorganic pigments, dyes, etc. Pigments that have high color development and high heat resistance are preferred, and organic pigments are preferred. Among organic pigments, combinations of yellow pigments, red pigments, and indigo pigments, combinations of red pigments, indigo pigments, and green pigments, and combinations of yellow pigments, indigo pigments, and purple pigments can be mentioned. From the viewpoint of uniform shielding properties in the visible light region, it is preferable to include yellow pigments, red pigments, and indigo pigments. In addition, orange pigments, green pigments, purple pigments, etc. may be used within a range that does not interfere with the effects of the present invention. The above pigments are used in a mixture of multiple types. By including multiple types of pigments, the blackness of the appearance is ensured, making it possible to achieve seamlessness by designing the same color as the surrounding components, and providing designability.

[0028] Specific examples of organic pigments that can be used as colorants are shown below by color index numbers.

[0029] Yellow pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 12, 13, 14, 15, 16, 17, 18, 20, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 86, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 117, 118, 119, 120, 123, 125, 126, 127, 128, 129, 130, 131, 132, 133, 134, 135, 136, 137, 138, 139, 140, 141, 142, 143, 144, 145, 146, 147, 148, 149, 150, 151, 152, 153, 154, 155, 156, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 171, 1 No. 6, 127, 128, 129, 137, 138, 139, 147, 148, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 185, 187, 188, 193, 194, 198, 199, 213, 214, 218, 219, 220, 221, 231, etc. can be suitably used.

[0030] Red pigments include CI Pigment Red 7, 9, 14, 41, 48:1, 48:2, 48:3, 48:4, 57:1, 81, 81:1, 81:2, 81:3, 81:4, 97, 122, 123, 146, 149, 150, 168, 169, 176, 177, 178, 180, 184, 185, 187, 192, 200, 202, 208, 209, 210, 215, 216, 217, 220, 223, 224, 226, 227, 228, 240, 242, 246, 254, 255, 264, 268, 270, 272, 273, 274, 276, 277, 278, 279, 280, 281, 282, 283, 284, 285, 286, 287, etc. can be suitably used.

[0031] As the indigo pigment, CI Pigment Blue 1, 1:2, 1:3, 2, 2:1, 2:2, 3, 8, 9, 10, 10:1, 11, 12, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 18, 19, 22, 24, 24:1, 53, 56, 56:1, 57, 58, 59, 60, 61, 62, 64, etc. can be suitably used.

[0032] As the orange pigment, CI Pigment Orange 36, 38, 43, 51, 55, 59, 61, 71, 73, etc. can be suitably used.

[0033] Green pigments include CI Pigment Green 7, 10, 36, 37, 58, 62, 63 and the like can be suitably used.

[0034] As the purple pigment, CI Pigment Violet 1, 19, 27, 29, 30, 32, 37, 40, 42, 50, etc. can be suitably used.

[0035] Examples of inorganic pigments include titanium oxide, carbon black, aluminum paste, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, iron oxide red, yellow iron oxide, iron black, etc. Examples of extender pigments include silica, alumina, talc, calcium carbonate, precipitated barium, etc. In order to ensure good coatability, sensitivity, developability, etc. while maintaining a balance between saturation and brightness, it is also preferable to use inorganic pigments in combination with organic pigments.

[0036] In the optical functional layer of the present invention, the content of the colorant is preferably 10 to 45% by mass, more preferably 15 to 40% by mass, and even more preferably 20 to 35% by mass. By being in the above range, the light-shielding property is improved and a blacker appearance is obtained.

[0037] In order to satisfy the above transmittance in the optical laminate of the present invention, in the case of a combination of a yellow pigment, a red pigment and a cyan pigment, the total mass of the optical functional layer preferably contains 0.1 to 10 mass% yellow pigment, 0.1 to 10 mass% red pigment, and 0.1 to 10 mass% cyan pigment, more preferably 0.1 to 4 mass% yellow pigment, 0.1 to 8 mass% red pigment, and 0.1 to 8 mass% cyan pigment, and even more preferably 0.1 to 3 mass% yellow pigment, 0.1 to 6 mass% red pigment, and 0.1 to 6 mass% cyan pigment. The blending ratio of the pigments is preferably yellow pigment / red pigment / indigo pigment=5-40 / 5-60 / 5-60, more preferably 10-30 / 10-50 / 10-50, and further preferably 10-30 / 25-50 / 25-50 by mass relative to the total amount of pigments. It is preferable to use CI Pigment Yellow 139 as the yellow pigment, CI Pigment Red 264 as the red pigment, and CI Pigment Blue 15:6 as the indigo pigment, since these pigments can exhibit excellent shielding properties in the visible light region.

[0038] In the case of a combination of red pigment, indigo pigment, and green pigment, the optical functional layer preferably contains 0.1 to 10 mass% red pigment, 0.1 to 10 mass% indigo pigment, and 0.1 to 10 mass% green pigment, more preferably 0.1 to 8 mass% red pigment, 0.1 to 4 mass% indigo pigment, and 0.1 to 8 mass% green pigment, and even more preferably 0.1 to 6 mass% red pigment, 0.1 to 3 mass% indigo pigment, and 0.1 to 6 mass% green pigment. The blending ratio of the pigments is preferably red pigment / indigo pigment / green pigment=5-60 / 5-40 / 5-60, more preferably 10-50 / 10-30 / 10-50, and further preferably 30-50 / 20-30 / 30-50, in terms of mass ratio relative to the total amount of pigments. It is preferred to use CI Pigment Red 264 as the red pigment, CI Pigment Blue 15:6 as the indigo pigment, and CI Pigment Green 7 as the green pigment.

[0039] In the case of a combination of a yellow pigment, an indigo pigment, and a violet pigment, the total mass of the optical functional layer is 0.1 to 10 mass% of the yellow pigment, 0.1 to 10 mass% of the indigo pigment, and 0.1 to 10 mass% of the violet pigment. It is preferable that the pigment contains 0.1 to 8 mass% of a yellow pigment, 0.1 to 4 mass% of an indigo pigment, and 0.1 to 8 mass% of a violet pigment, and it is even more preferable that the pigment contains 0.1 to 6 mass% of a yellow pigment, 0.1 to 3 mass% of an indigo pigment, and 0.1 to 6 mass% of a violet pigment. The blending ratio of the pigments is preferably yellow pigment / indigo pigment / violet pigment=5-60 / 5-40 / 5-60, more preferably 10-50 / 10-30 / 10-50, and further preferably 30-50 / 20-30 / 30-50, in terms of mass ratio relative to the total amount of pigments. The yellow pigment is CI Pigment Yellow 139, the indigo pigment is CI Pigment Blue 15:6, and the purple pigment is CI Pigment Violet 23. It is preferable to use

[0040] Furthermore, in the case of a combination of a yellow pigment, a red pigment, and a violet pigment, the optical functional layer preferably contains 0.1 to 10 mass% of the yellow pigment, 0.1 to 10 mass% of the red pigment, and 0.1 to 10 mass% of the violet pigment, more preferably 0.1 to 8 mass% of the yellow pigment, 0.1 to 4 mass% of the red pigment, and 0.1 to 8 mass% of the violet pigment, and even more preferably 0.1 to 6 mass% of the yellow pigment, 0.1 to 3 mass% of the red pigment, and 0.1 to 6 mass% of the violet pigment. The blending ratio of the pigments is preferably yellow pigment / red pigment / violet pigment=5-60 / 5-40 / 5-60, more preferably 10-50 / 10-30 / 10-50, and further preferably 30-50 / 20-30 / 30-50, in terms of mass ratio relative to the total amount of pigments. The yellow pigment is CI Pigment Yellow 139, the red pigment is CI Pigment Red 264, and the purple pigment is CI Pigment Violet 23. It is preferable that

[0041] <Binder resin> The optical functional layer of the present invention contains a binder resin. In the present invention, the binder resin refers to a resin that can function as a binding agent in a colored ink, and is preferably a thermoplastic resin. Examples of the thermoplastic resin include acrylic resin, polyester resin, epoxy resin, styrene-based resin, rosin-based resin, styrene-maleic acid resin, dammar resin, polycarbonate resin, rosin-modified maleic acid resin, rosin ester resin, terpene resin, and urethane resin, and these resins may be used in combination within a range that does not impair the effects of the present invention.

[0042] From the viewpoint of adhesion to the substrate, the optical functional layer of the present invention preferably contains at least one thermoplastic resin selected from the group consisting of acrylic resin, polyester resin, and epoxy resin, and more preferably contains an acrylic resin.

[0043] When the optical functional layer of the present invention contains an acrylic resin, the acid value of the acrylic resin is preferably 20 mgKOH / g or less, more preferably 15 mgKOH / g or less, even more preferably 10 mgKOH / g or less, still more preferably 5 mgKOH / g or less, and particularly preferably 1 mgKOH / g or less.

[0044] Furthermore, when the optical functional layer of the present invention contains an acrylic resin, the hydroxyl value of the acrylic resin is preferably 1 mgKOH / g or more, more preferably 10 mgKOH / g or more, even more preferably 20 mgKOH / g or more, and particularly preferably 25 mgKOH / g or more.

[0045] In addition, when the optical functional layer of the present invention contains an acrylic resin, the reactive functional group value (the sum of the acid value and the hydroxyl value) of the acrylic resin is preferably 1 to 50 mgKOH / g, and more preferably 5 to 60 mgKOH / g. It is more preferably 40 mgKOH / g, and further preferably 10 to 35 mgKOH / g.

[0046] The weight average molecular weight of the binder resin is preferably from 5,000 to 120,000, more preferably from 20,000 to 100,000, and even more preferably from 30,000 to 80,000, in order to improve printability.

[0047] The content of the binder resin in the optical functional layer is preferably 40 to 80% by mass, more preferably 45 to 75% by mass, and even more preferably 50 to 70% by mass, because this improves dispersion stability.

[0048] In the optical functional layer, the mass ratio of the total amount of colorants to the binder resin is preferably 85 / 15 to 60 / 40, more preferably 80 / 20 to 65 / 35. The above ratio provides good light blocking properties and a blacker appearance.

[0049] <Dispersant> The optical functional layer in the present invention preferably contains a dispersant. The dispersant has the effect of suppressing pigment aggregation and improving dispersion stability in the black ink forming the optical functional layer, and more preferably has a comb structure. In the present invention, the "comb structure" refers to a (co)polymer structure in which repeating units are bonded as side chains to the main chain. The dispersant having a comb structure improves dispersion stability.

[0050] The dispersant preferably has an acidic group, and more preferably has an acid value of 0.1 to 100 mgKOH / g. When the dispersant has an acidic group, it is possible to prevent light in the visible region from being transmitted and to exhibit excellent shielding properties.

[0051] The content of the dispersant in the optical functional layer (solid content of the black ink) is preferably 1 to 25% by mass, more preferably 2 to 20% by mass, and even more preferably 3 to 15% by mass. By being in the above range, compatibility with the binder resin can be maintained, and the coating film can be prevented from becoming cloudy and the coating film transparency can be maintained.

[0052] The weight average molecular weight of the dispersant is preferably 10,000 to 100,000, more preferably 10,000 to 50,000, and even more preferably 10,000 to 30,000. When the weight average molecular weight is 10,000 or more, steric repulsion that contributes to dispersion stability can be obtained, and aggregation of the pigment can be prevented. When the weight average molecular weight is 100,000 or less, compatibility with the solvent can be maintained, and dispersion stability of the pigment can be maintained.

[0053] (Organic solvent) The black ink may contain an organic solvent, such as glycol ether organic solvents, ester organic solvents, aliphatic organic solvents, aromatic organic solvents, alcohol organic solvents, and cyclic ketone organic solvents. Among these, cyclic ketone organic solvents are preferred because of their good printability.

[0054] (Antifoaming agent) The black ink preferably contains an antifoaming agent. The content of the antifoaming agent is preferably 0.1 to 5 mass %, and more preferably 0.3 to 4 mass %, relative to the total mass of the black ink.

[0055] <Formation of optical functional layer> The optical functional layer of the present invention is formed by applying the black ink to a substrate by a method such as screen printing, roll coating, dispenser coating, dip coating, brush coating, etc. Among these, any of screen printing, dispenser coating, and dip coating is preferred. It is preferable to use a cylinder press printing machine or a semi-automatic printing machine as the printing machine, and to use a resin material such as nylon or polyester, or a resin material such as stainless steel as the printing plate.

[0056] <Base material> In the present invention, the substrate used to form the optical laminate is not particularly limited, and a transparent substrate is preferred. For example, inorganic substrates such as glass, polyester substrates such as polyethylene terephthalate, polyethylene, polypropylene, ethylene-vinyl acetate and other polyolefin substrates, nylon substrates such as polyamide, acrylic substrates such as polymethyl methacrylate, polyvinyl chloride substrates, polycarbonate substrates, polyurethane substrates, epoxy substrates, cyclic olefin substrates such as cycloolefin polymer (COP) and cycloolefin copolymer (COC), and other resin substrates may be used. A deposition substrate in which an inorganic compound such as silica, alumina, or aluminum is deposited on the substrate may also be used, and the deposition surface may be further coated with polyvinyl alcohol or the like. Corona treatment, frame treatment, or stretching treatment may also be performed. Among the above, inorganic material substrates such as glass, polyester substrates such as polyethylene terephthalate, acrylic substrates such as polymethyl methacrylate (PMMA), and polycarbonate substrates are preferred.

[0057] <Screen printing> Screen printing is a technique that uses a screen made of chemical fibers such as polyester or nylon or stainless steel as a plate, and uses a photosensitive emulsion on the plate to pattern areas through which the ink passes and areas through which it does not pass, and then transfers the ink to the substrate by applying pressure and moving the ink on the inner surface of the screen with a spatula-shaped rubber plate called a squeegee. The thickness of the ink film printed can be adjusted by the thickness of the photosensitive emulsion applied to the substrate surface. After printing, the ink can be fixed to the substrate by evaporating the solvent in the ink using a hot air oven.

[0058] <Method of manufacturing optical laminate> The optical laminate of the present invention is produced by a production method including a step of forming an optical functional layer by applying a colorant containing multiple pigments and a black ink containing a binder resin on a substrate. The optical laminate has an average spectral transmittance of 25% or less at wavelengths of 350 nm to 750 nm and an average spectral transmittance of 85% or more at wavelengths of 850 nm to 2500 nm, and satisfies the following formulas (1) and (2) when the maximum spectral transmittance at wavelengths of 350 nm to less than 460 nm is T1, the maximum spectral transmittance at wavelengths of 460 nm to less than 570 nm is T2, and the maximum spectral transmittance at wavelengths of 570 nm to 750 nm is T3. 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2)

[0059] An example of a method for producing the black ink includes a method in which a colorant, a binder resin, and an organic solvent are uniformly stirred with a stirrer, then dispersed in a bead mill, and filtered with a filter. Preferred methods for applying the black ink include screen printing, dispenser coating, and dip coating, and preferred printing conditions are those using a cylinder press printing machine or a semi-automatic printing machine as the printing machine and a printing plate made of a resin material such as nylon or polyester, or a resin material such as stainless steel.

[0060] <Use forms of optical laminate> The use of the optical laminate of the present invention is not particularly limited as long as it is an optical device, and examples thereof include interior parts for automobiles, parts for home appliances, etc. In addition, optical laminates used in infrared sensors of smartphones, etc. The optical laminate is also suitable as a filter. In particular, the optical laminate can be suitably used as a member for transmission viewing, and in this specification, transmission viewing means viewing the light irradiated onto the optical laminate from the side opposite to the light source with the optical laminate sandwiched therebetween.

[0061] (light source) The light source for irradiating the optical laminate of the present invention is not particularly limited, but it is preferable to use an incandescent lamp, an EL lamp such as an organic EL lamp, or a light emitting diode (LED). EXAMPLES

[0062] The present invention will be specifically described below using examples, but the present invention is not limited to the following examples. In the present invention, unless otherwise specified, "parts" and "%" represent "mass parts" and "mass %", respectively.

[0063] <Synthesis Example> (Synthesis Example 1) [Synthesis of Acrylic Resin 1] 300g of methyl ethyl ketone (MEK) was placed in a four-neck flask equipped with a stirrer, reflux condenser, nitrogen inlet tube, inlet tube, and thermometer, and heated to 80°C while injecting nitrogen gas into the container. At the same temperature, a mixture of 38g of methyl methacrylate (MMA), 53g of butyl methacrylate (BMA), 16g of 2-hydroxyethyl methacrylate (HEMA), 13g of styrene (St), and 0.8g of 2,2'-azobisisobutyronitrile (AIBN) was added dropwise over 1 hour to carry out a polymerization reaction. After the addition was completed, the reaction was continued for another 3 hours at 80°C, and then the 2,2'-azobis A solution of 1.2 parts of isobutyronitrile in 100 g of isophorone was added and reacted at 80° C. for 1 hour to obtain acrylic resin 1 (weight average molecular weight 40,000, acid value 0.3 mg KOH / g, hydroxyl value 30 mg KOH / g).

[0064] <Preparation of black ink> <Adjustment Example 1> (Black Ink S1) The following finely divided pigments, dispersing resin, and isophorone were mixed and stirred until uniform, and then dispersed in an Eiger mill (Eiger Japan, "Mini Model M-250 MKII") using zirconia beads with a diameter of 0.5 mm for 5 hours. The mixture was then filtered through a 5 μm filter to obtain a mixed-color pigment dispersion. Yellow fine pigment CI Pigment Yellow 139 (LIONOGEN YELLOW 1090) 2 parts Red fine pigment CI Pigment Red 264 (Cinilex DPP Rubine SR6T) 4 parts Indigo blue fine pigment CI Pigment Blue 15:6 (LIONOGEN BLUE 7703) 4 parts Dispersants (NOF Corporation "Marialim SC-1015F", comb structure, weight average molecular weight 20,000) 5 parts Isophorone 35 parts

[0065] To the mixed pigment dispersion obtained above, 49 parts of acrylic resin 1 solution (resin / isophorone=24 / 25) and 1 part of defoamer (BYK-054 manufactured by BYK Japan) were added, and mixed uniformly using a mixer rotary stirrer to prepare black ink S1.

[0066] <Preparation Examples 2 to 14, Comparative Preparation Examples 1 to 7> (Preparation of Black Inks S2 to S14, T1 to T7) In the same manner as in Preparation Example 1, black inks were prepared using the raw materials and mixing ratios shown in Tables 1 and 2.

[0067] [Table 1] [Table 2]

[0068] The abbreviations in Tables 1 and 2 are shown below. Unless otherwise noted, the numbers in the tables represent "parts" and blanks indicate that no numbers are used.

[0069] (Pigments) CI Pigment Yellow 139 (Product name: LIONOGEN YELLOW 1090, manufactured by Toyo Color Co., Ltd.) CI Pigment Red 264 (Kikuchi Color Co., Ltd. Product name: Cinilex DPP Rubine SR6T) CI Pigment Blue 15:6 (Product name: LIONOGEN BLUE 7703, manufactured by Toyo Color Co., Ltd.) CI Pigment Violet 23 (Product name: LIONOGEN VIOLET FG-6240, manufactured by Toyo Color Co., Ltd.) CI Pigment Green 7 (Product name: LIONOGEN GREEN 8944, manufactured by Toyo Color Co., Ltd.) CI Pigment Black 10 (Mitsubishi Chemical Corporation product name: Mitsubishi Carbon Black MA8)

[0070] (binder resin) Polyester resin: VYLON GK250 (manufactured by Toyobo Co., Ltd., number average molecular weight 10,000, acid value <2 mg KOH / g, hydroxyl value 11 mg KOH / g). Epoxy resin: JER1010 (manufactured by Mitsubishi Chemical Corporation, number average molecular weight 5000, acid value <2 mgKOH / g) Urethane resin: Polylite OD-X-2523 (DIC Corporation, molecular weight 3500, acid value 0.5 mg KOH / g, hydroxyl value 32 mg KOH / g)

[0071] Example 1 (Preparation of Optical Laminate SS1) MICRO SLIDE GLASS (large slide glass S9213, manufactured by Matsunami Glass Co., Ltd.) was used as the substrate, and the above black ink S1 was screen-printed onto this substrate in a pattern using a screen printing plate (L-SCREEN, 250-015 / 255PW, manufactured by NBC Meshtec Co., Ltd.) to form an optical functional layer with a thickness of 7 μm, thereby producing the optical laminate SS1.

[0072] <Examples 2 to 14 and Comparative Examples 1 to 7> (Preparation of optical laminates SS2 to SS14 and TT1 to TT7) An optical laminate was produced in the same manner as in Example 1, except that the black ink S1 used in Example 1 was changed to the black inks shown in Tables 1 and 2.

[0073] <Spectral transmittance of optical laminate> The spectral transmittance was measured using a UV3600 ultraviolet, visible and near infrared spectrophotometer manufactured by Shimadzu Corporation, and is shown in Tables 1 and 2. The values ​​in the tables are as follows. (Average spectral transmittance at wavelengths of 350nm to 750nm) 3|Less than 10% 2|More than 10% and less than 25% 1|More than 25% (Average spectral transmittance from 850nm to 2500nm) 3|Over 90% 2 | 85% or more, less than 90% 1|Less than 85% (Value of T1 / T2) 3|1.5≦T1 / T2≦5 2|1≦T1 / T2<1.5, 5 <T1 / T2≦10 1|T1 / T2<1, 10 <T1 / T2 (T3 / T2 value) 3|3≦T3 / T2≦10 2|2≦T3 / T2<3, 10 <T3 / T2≦20 1|T3 / T2<2, 20 <T3 / T2

[0074] <Evaluation of optical laminate> The following evaluations were performed on the optical laminates obtained in the above Examples and Comparative Examples. The evaluation results are shown in Tables 1 and 2.

[0075] <OD value (optical density)> Using a transmission densitometer Gretag Macbeth TD-931, the OD value in the visible light region was measured. The evaluation criteria are shown below. Note that the higher the OD value, the darker the black color, and if it is 2 or more, it is at a practical level. 3 | OD value of 1.4 or more 2 | OD value of 1 or more and less than 1.4 1 | OD value less than 1

[0076] <Color of transmitted light> The laminate was irradiated with white light or green light, and the color of the transmitted light was visually evaluated. The evaluation criteria are shown below. Note that if it is 2 or more, it is at a practical level. 3 | The same color as the irradiated light (no color change) 2 | Slightly different color from the irradiated light (slight color change) 1 | Different color from the irradiated light (color change)

[0077] According to the present invention, it has become possible to provide an optical laminate that is black with a high OD value, excellent in infrared region permeability, and has the same color for the irradiated light and the transmitted light in the visible light region (the transmitted light is white when irradiated with white light).

[0078] In Comparative Example 1 where the average spectral transmittance at wavelengths of 350 nm to 750 nm exceeded 25%, the OD value was low. In Comparative Examples 2 to 6 where T1 / T2 and T3 / T2 were outside the scope of the present invention, the color of the irradiated light and the transmitted light in the visible light region did not become the same color, resulting in poor visibility. In Comparative Example 7 using carbon black, visible light hardly transmitted and the color of the transmitted light could not be confirmed, and furthermore, the infrared permeability was poor.

Claims

1. An optical laminate having an optical functional layer on at least one surface of a substrate, the optical functional layer contains a colorant containing a plurality of types of pigments and a binder resin; The optical laminate is The average spectral transmittance at wavelengths of 350 nm to 750 nm is 25% or less; The average spectral transmittance at wavelengths of 850 nm to 2500 nm is 85% or more; An optical laminate that satisfies the following formulas (1) and (2), where T1 is the maximum spectral transmittance at a wavelength of 350 nm or more and less than 460 nm, T2 is the maximum spectral transmittance at a wavelength of 460 nm or more and less than 570 nm, and T3 is the maximum spectral transmittance at a wavelength of 570 nm or more and less than 750 nm. 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2)

2. The optical laminate according to claim 1, wherein the colorant containing a plurality of pigments contains a yellow pigment, a red pigment, and a cyan pigment, or a red pigment, a cyan pigment, and a green pigment, or a yellow pigment, a cyan pigment, and a violet pigment.

3. The optical laminate according to claim 1 or 2, wherein the colorant containing a plurality of types of pigments contains a yellow pigment, a red pigment, and a cyan pigment.

4. The optical laminate according to claim 1 or 2, which is for transmission viewing.

5. The optical laminate according to claim 1 or 2, wherein the optical functional layer contains a dispersant.

6. 3. The optical laminate according to claim 1, wherein the binder resin comprises at least one resin selected from the group consisting of an acrylic resin, a polyester resin, and an epoxy resin.

7. A method for producing an optical laminate, comprising a step of applying a colorant containing a plurality of types of pigments and a black ink containing a binder resin onto a substrate to form an optical functional layer, The optical laminate is The average spectral transmittance at wavelengths of 350 nm to 750 nm is 25% or less; The average spectral transmittance at wavelengths of 850 nm to 2500 nm is 85% or more; A method for producing an optical laminate, which satisfies the following formulas (1) and (2), where T1 is a maximum spectral transmittance at a wavelength of 350 nm or more and less than 460 nm, T2 is a maximum spectral transmittance at a wavelength of 460 nm or more and less than 570 nm, and T3 is a maximum spectral transmittance at a wavelength of 570 nm or more and less than 750 nm. 1≦T1 / T2≦10 (1) 2≦T3 / T2≦20 (2)