Manufacturing method of imprint mold, and, imprint mold
The method addresses the issue of rounded cross-sectional shapes in imprint molds by using controlled etching and resin parts to achieve uniform curvature and precise height variations in convex structures, enhancing nanoimprint lithography precision.
Patent Information
- Application Number
- JP2023062414
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
Smart Images

Figure 2024148880000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing an imprint mold and an imprint mold. More particularly, the present disclosure relates to a method for manufacturing an imprint mold having convex structures with different heights and an imprint mold having convex structures with different heights. [Background technology]
[0002] Nanoimprint lithography is known as a technique for transferring and forming fine patterns in the manufacture of semiconductor devices and the like. The above-mentioned nanoimprint lithography is a technology in which an imprint mold (also called a template, stamper, or plate) having a transfer pattern of fine concave-convex shapes formed on its surface is brought into close contact with a resin formed on a transfer substrate such as a semiconductor wafer, the shape of the surface side of the resin is molded to the concave-convex shape of the transfer pattern of the template, the template is then released, and excess resin parts (residual film parts) are then removed by dry etching or the like, thereby transferring the concave-convex shape (more specifically, the inverted concave-convex shape) of the transfer pattern of the imprint mold to the resin on the transfer substrate (for example, Patent Documents 1 and 2).
[0003] The transfer pattern of the concave-convex shape formed on the imprint mold (hereinafter also simply referred to as the imprint mold) used in the above-mentioned nanoimprint lithography has conventionally been a line pattern or pillar pattern with a rectangular cross section, and these line patterns (hereinafter also referred to as the line structure) and pillar patterns (hereinafter also referred to as the pillar structure) have been made to the same height.
[0004] On the other hand, if an imprint mold having pillar structures or line structures of different heights is used as the transfer pattern, complex three-dimensional shapes can be obtained in fewer steps. Therefore, there is a demand for imprint molds having pillar structures or line structures of different heights not only in the manufacture of semiconductor devices, but also in the manufacture of, for example, optical elements, wiring circuits, recording devices, display panels, medical testing chips, microchannels, and the like. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2004-504718 [Patent Document 2] JP 2002-93748 A Summary of the Invention [Problem to be solved by the invention]
[0006] When manufacturing an imprint mold having multiple convex structures of different heights (e.g., pillar structures or line structures) as a transfer pattern, a conceivable method is to use an intermediate product from a conventional imprint mold manufacturing method and sequentially remove the hard mask from the convex structures with lower heights during dry etching (called a virtual imprint mold manufacturing method). The conventional method for manufacturing an imprint mold and the virtual method for manufacturing an imprint mold will be described below.
[0007] (Conventional manufacturing method for imprint molds) 20 to 24 are schematic process diagrams showing an example of a conventional method for producing an imprint mold.
[0008] To manufacture a conventional imprint mold, that is, an imprint mold having a plurality of convex structures with the same height, a laminate having a hard mask layer 120 provided on a first surface of a light-transmitting substrate 110 is first prepared, as shown in FIG. 20. The light-transmitting substrate 110 is, for example, a synthetic quartz substrate. Alternatively, the substrate may be made of various known materials used in the manufacture of imprint molds. The hard mask layer 120 is, for example, a layer containing chromium. Alternatively, the hard mask layer 120 may be a layer made of various known materials (e.g., aluminum, silicon, etc.) used in the manufacture of imprint molds.
[0009] 21, resist patterns 131, 132, and 133 are formed on the hard mask layer 120. For example, electron beam lithography can be used as a method for forming the resist patterns 131, 132, and 133. In addition, various known methods used for forming fine resist patterns may be used.
[0010] Next, the hard mask layer 120 exposed from the resist patterns 131, 132, and 133 is etched to form hard mask patterns 121, 122, and 123, as shown in Fig. 22. Note that in Fig. 22, the resist patterns 131, 132, and 133 remaining after etching have been removed. For example, when the hard mask layer 120 is a layer containing chromium, a dry etching method using a mixed gas of chlorine and oxygen can be used for the above etching. In addition, various known methods used in the manufacture of imprint molds may be used. For example, when the material constituting the hard mask layer 120 is other than chromium, a dry etching method using boron trichloride gas or hydrogen chloride gas can be used.
[0011] Next, the light-transmitting substrate 110 exposed from the hard mask patterns 121, 122, and 123 is etched to obtain an imprint mold 100A with a hard mask pattern, which is an intermediate product, as shown in FIG. For example, when the light-transmitting substrate 110 is a synthetic quartz substrate, the above etching can be performed by dry etching using an etching gas containing fluorine. In addition, various known methods used in the manufacture of imprint molds can be used.
[0012] Thereafter, the hard mask patterns 121, 122, and 123 are removed to obtain the imprint mold 100 having the first convex structure 101, the second convex structure 102, and the third convex structure 103, as shown in FIG. For example, a dry etching technique using a mixed gas of chlorine and oxygen can be used as a method for removing the hard mask patterns 121, 122, and 123. In addition, various known techniques used in manufacturing imprint molds may also be used.
[0013] (Virtual imprint mold manufacturing method) As a method for manufacturing an imprint mold having a plurality of convex structures with different heights using an intermediate product in a conventional imprint mold manufacturing method, for example, the following method for manufacturing a virtual imprint mold can be mentioned.
[0014] First, as shown in Fig. 25, an imprint mold with a hard mask pattern that can be produced by the conventional imprint mold manufacturing method described above is prepared as a mold material 110A. The mold material 110A shown in Fig. 25 may be the same as the imprint mold with a hard mask pattern 100A shown in Fig. 23. For example, the mold material 110A is made of a synthetic quartz substrate, and the hard mask patterns 121, 122, and 123 are made of a material containing chromium.
[0015] Next, the hard mask pattern 121 on the upper surface of the first convex structure 101 of the molding material 110A is removed to produce an intermediate product 110B as shown in Fig. 26, and the first surface 10f side of this intermediate product 110B is subjected to dry etching using an etching gas containing fluorine. As a result, the parts exposed from the hard mask patterns 122 and 123 are etched, and it is considered that in the obtained intermediate product 110C, as shown in Fig. 27, the height (H0) of the first convex structure 101 is maintained, while the height (H1) of the second convex structure 102 and the third convex structure 103 is higher than the height (H0) of the first convex structure 101.
[0016] Next, the hard mask pattern 122 on the upper surface of the second convex structure 102 of the intermediate product 110C is removed to produce an intermediate product 110D as shown in Fig. 28, and the first surface 10f side of this intermediate product 110D is subjected to dry etching using an etching gas containing fluorine. As a result, the parts exposed from the hard mask pattern 123 are etched, and the resulting intermediate product 110E may have a form having a first convex structure 101, a second convex structure 102, and a third convex structure 103, each of which has a different height, as shown in Fig. 29.
[0017] It is also possible to subsequently remove the hard mask pattern 123 on the upper surface of the third convex structure 103 of the intermediate product 110E to produce an imprint mold 200 having a first convex structure 101, a second convex structure 102, and a third convex structure 103, each of which has a different height, as shown in FIG. 30. In the imprint mold 200 shown in FIG. 30, the relationship between the height (H0) of the first convex structure 101, the height (H1) of the second convex structure 102, and the height (H2) of the third convex structure 103 is as follows: H0 It is also possible that this could be the case.
[0018] However, when attempting to manufacture an imprint mold having multiple convex structures of different heights (e.g., pillar structures or line structures) using a manufacturing method such as that shown in Figures 25 to 30, in reality, the convex structure from which the hard mask pattern has been removed is prone to having a rounded cross-sectional shape due to the corners of the upper surface of the convex structure being etched by side etching, and there was a problem that the desired cross-sectional shape could not be obtained.
[0019] For example, the resulting imprint mold 200 did not actually have the desired cross-sectional shape (shown by the dashed line in the figure) as shown in FIG. 31, but rather had a rounded cross-sectional shape (shown by the solid line in the figure) in which the corners of the upper surface of the convex structure were etched.
[0020] In fact, as shown in Figure 31, the resulting imprint mold 200 is such that a shorter convex structure is more likely to have a cross-sectional shape with a rounded upper surface than a taller convex structure (for example, in Figure 31, the first convex structure 101 is more likely to have a cross-sectional shape with a rounded upper surface than the second convex structure 102), and it has been difficult to manufacture an imprint mold having a convex structure in which the cross-sectional shape of the corners on the upper surface of each convex structure is uniform (more specifically, the magnitude of the radius of curvature in cross-section of the corners on the upper surface of each convex structure is within a certain numerical range) even if the heights of multiple convex structures are different.
[0021] The present disclosure has been made in consideration of the above-mentioned situation, and has as its main object to provide an imprint mold having a plurality of convex structures, in which even if the heights of the plurality of convex structures are different, the radius of curvature in cross-section of the corners on the upper surface of each convex structure is small and the cross-sectional shape of the corners on the upper surface of each convex structure is uniform (more specifically, the radius of curvature in cross-section of the corners on the upper surface of each convex structure falls within a certain numerical range), and to provide a method for manufacturing such an imprint mold. [Means for solving the problem]
[0022] The manufacturing method of the imprint mold of the present disclosure includes a molding material preparation step of preparing a molding material having a first convex structure and a second convex structure on a first surface, and a resin part having a first convex structure top surface resin part covering an upper surface of the first convex structure, a first convex structure side surface resin part covering a side surface of the first convex structure, a second convex structure top surface resin part covering an upper surface of the second convex structure, and a second convex structure side surface resin part covering a side surface of the second convex structure, wherein the thickness of the first convex structure top surface resin part is smaller than the thickness of the second convex structure top surface resin part. The method includes, in order, a resin portion forming process, forming a resin portion on the first surface side of the molding material; a first convex structure top surface exposing process, etching the resin portion to remove the first convex structure top surface resin portion while leaving the first convex structure side surface resin portion, the second convex structure top surface resin portion, and the second convex structure side surface resin portion, thereby exposing the top surface of the first convex structure from the resin portion; and a first convex structure etching process, etching the top surface of the first convex structure exposed from the resin portion, thereby lowering the height of the first convex structure.
[0023] In the manufacturing method of the imprint mold disclosed herein, after the first convex structure top surface exposing step, the method may sequentially include a second convex structure top surface exposing step of further etching the resin part to remove the second convex structure top surface resin part while leaving the first convex structure side surface resin part and the second convex structure side surface resin part, thereby exposing the top surface of the second convex structure from the resin part, and a second convex structure etching step of etching the top surface of the second convex structure exposed from the resin part, thereby lowering the height of the second convex structure.
[0024] In the method for manufacturing an imprint mold according to the present disclosure, the etching gas in the first convex structure upper surface exposing step and the etching gas in the first convex structure etching step may be an etching gas made of the same material.
[0025] In the method for manufacturing an imprint mold according to the present disclosure, the etching gas in the second convex structure upper surface exposing step and the etching gas in the second convex structure etching step may be an etching gas made of the same material.
[0026] In the manufacturing method of the imprint mold disclosed herein, the etching gas in the first convex structure upper surface exposing step, the etching gas in the first convex structure etching step, the etching gas in the second convex structure upper surface exposing step, and the etching gas in the second convex structure etching step may all be etching gases composed of the same material.
[0027] In the manufacturing method of the imprint mold disclosed herein, the resin portion may also be etched in the first convex structure etching step, and an etching rate of the resin portion in the first convex structure etching step may be the same as an etching rate of the first convex structure.
[0028] In the manufacturing method of the imprint mold disclosed herein, in the second convex structure etching step, the resin portion and the first convex structure may also be etched, and the etching rate of the resin portion and the first convex structure in the second convex structure etching step may be the same as the etching rate of the second convex structure.
[0029] In the manufacturing method of the imprint mold disclosed herein, in the first convex structure etching step, the resin part is also etched, and an etching rate of the resin part in the first convex structure etching step is the same as an etching rate of the first convex structure, and in the second convex structure etching step, the resin part and the first convex structure are also etched, and an etching rate of the resin part and the first convex structure in the second convex structure etching step is the same as an etching rate of the second convex structure, and the etching rate of the resin part in the first convex structure etching step may be the same as an etching rate of the resin part in the second convex structure etching step.
[0030] In the manufacturing method of the imprint mold of the present disclosure, a height of the first convex structure after the second convex structure etching step is completed is defined as H1A, a height of the second convex structure after the second convex structure etching step is completed is defined as H2A, and a thickness of the first convex structure upper surface resin portion in the resin portion forming step is defined as T1, When the thickness of the second convex structure upper surface resin portion in the resin portion forming step is T2, H2A-H1A=T2-T1 It may be:
[0031] In the manufacturing method of the imprint mold disclosed herein, the resin portion may also be etched in the first convex structure etching step, and an etching rate of the resin portion in the first convex structure etching step may be slower than an etching rate of the first convex structure.
[0032] In the manufacturing method of the imprint mold disclosed herein, in the second convex structure etching step, the resin portion and the first convex structure are also etched, and the etching rate of the resin portion in the second convex structure etching step is slower than the etching rate of the second convex structure, and the etching rate of the first convex structure in the second convex structure etching step may be the same as the etching rate of the second convex structure.
[0033] In the manufacturing method of an imprint mold disclosed herein, in the first convex structure etching step, the resin part is also etched, and the etching rate of the resin part in the first convex structure etching step is slower than the etching rate of the first convex structure, in the second convex structure etching step, the resin part and the first convex structure are also etched, and the etching rate of the resin part in the second convex structure etching step is slower than the etching rate of the second convex structure, the etching rate of the first convex structure in the second convex structure etching step is the same as the etching rate of the second convex structure, and the etching rate of the resin part in the first convex structure etching step may be the same as the etching rate of the resin part in the second convex structure etching step.
[0034] In the method for manufacturing an imprint mold disclosed herein, when a height of the first convex structure after completion of the second convex structure etching step is H1B, a height of the second convex structure after completion of the second convex structure etching step is H2B, a thickness of the resin portion on the upper surface of the first convex structure in the resin portion forming step is T1, a thickness of the resin portion on the upper surface of the second convex structure in the resin portion forming step is T2, an etching rate of the resin portion in the second convex structure etching step is Ej, and an etching rate of the first convex structure and an etching rate of the second convex structure in the second convex structure etching step are Et, H2B-H1B=(T2-T1)×(Et / Ej) It may be:
[0035] In the method for manufacturing an imprint mold of the present disclosure, the first convex structure may be a pillar structure.
[0036] In the method for manufacturing an imprint mold of the present disclosure, the second convex structure may be a pillar structure.
[0037] In the method for manufacturing an imprint mold of the present disclosure, the first convex structure may be a line structure.
[0038] In the method for manufacturing an imprint mold of the present disclosure, the second convex structure may be a line structure.
[0039] The imprint mold of the present disclosure has on a first surface a first convex structure and a second convex structure taller than the first convex structure, and the radius of curvature in cross-sectional view of a corner formed by an upper surface and a side surface of the first convex structure and the radius of curvature in cross-sectional view of a corner formed by an upper surface and a side surface of the second convex structure are both 15 nm or less.
[0040] In the imprint mold of the present disclosure, the first convex structure may be a pillar structure.
[0041] In the imprint mold of the present disclosure, the second convex structure may be a pillar structure.
[0042] In the imprint mold of the present disclosure, the first convex structure may be a line structure.
[0043] In the imprint mold of the present disclosure, the second convex structure may be a line structure. Effect of the Invention
[0044] According to the present disclosure, it is possible to provide an imprint mold having a plurality of convex structures, in which even if the heights of the plurality of convex structures are different, the radius of curvature in cross-section of the corners on the upper surface of each convex structure is small and the cross-sectional shape of the corners on the upper surface of each convex structure is uniform (more specifically, the radius of curvature in cross-section of the corners on the upper surface of each convex structure falls within a certain numerical range), and a method for manufacturing the imprint mold. [Brief description of the drawings]
[0045] [Figure 1] FIG. 1 is a schematic process diagram showing an example of a first embodiment of a method for producing an imprint mold according to the present disclosure. [Diagram 2] 1 is a schematic process diagram showing an example of the first embodiment of the method for producing an imprint mold according to the present disclosure; [Diagram 3] 3 is a schematic process diagram showing an example of the first embodiment of the method for producing an imprint mold according to the present disclosure, which follows FIG. [Figure 4] 4 is a schematic process diagram showing an example of the first embodiment of the manufacturing method of the imprint mold of the present disclosure, following FIG. 3. [Diagram 5] 5 is a schematic process diagram showing an example of the first embodiment of the method for producing an imprint mold according to the present disclosure, which follows FIG. [Figure 6] 5 is a schematic process diagram showing an example of the first embodiment of the manufacturing method of the imprint mold of the present disclosure. [Figure 7] FIG. 3 is a schematic process diagram showing an example of a method for forming the resin portion 20 shown in FIG. [Figure 8] FIG. 8 is a schematic process diagram showing an example of a method for forming the resin portion 20, which follows FIG. [Figure 9] FIG. 9 is a schematic process diagram showing an example of a method for forming the resin portion 20, which follows FIG. 8. [Figure 10] FIG. 10 is a schematic process diagram showing an example of a method for forming the resin portion 20, which follows FIG. [Figure 11] FIG. 2 is a schematic process diagram showing an example of a second embodiment of a method for producing an imprint mold according to the present disclosure. [Figure 12] 12 is a schematic process diagram showing an example of the second embodiment of the method for producing an imprint mold according to the present disclosure, which follows FIG. [Figure 13] FIG. 13 is a schematic process diagram showing an example of the second embodiment of the method for producing an imprint mold according to the present disclosure, which follows FIG. [Figure 14] FIG. 14 is a schematic process diagram showing an example of the second embodiment of the method for producing an imprint mold according to the present disclosure, which follows FIG. [Figure 15] 15 is a schematic process diagram showing an example of the second embodiment of the method for producing an imprint mold according to the present disclosure, which follows FIG. [Figure 16] 15 is a schematic process diagram showing an example of the second embodiment of the method for producing an imprint mold according to the present disclosure; [Figure 17] FIG. 1 is a schematic cross-sectional view showing an example of an imprint mold according to the present disclosure. [Figure 18] SEM image showing an example of a convex structure of an imprint mold according to the present disclosure. [Figure 19] A diagram explaining how to measure the radius of curvature [Figure 20] Schematic process diagram showing an example of a conventional imprint mold manufacturing method [Figure 21] A schematic process diagram showing an example of a conventional imprint mold manufacturing method, continued from FIG. 20. [Figure 22] A schematic process diagram showing an example of a conventional imprint mold manufacturing method, continued from FIG. 21. [Figure 23] A schematic process diagram showing an example of a conventional imprint mold manufacturing method, continued from FIG. 22. [Figure 24]A schematic process diagram showing an example of a conventional imprint mold manufacturing method, continued from FIG. 23. [Diagram 25] A schematic diagram showing an example of a method for manufacturing a virtual imprint mold. [Figure 26] A schematic process diagram showing an example of a manufacturing method for a virtual imprint mold, which follows FIG. [Figure 27] A schematic process diagram showing an example of a manufacturing method for a virtual imprint mold, which follows FIG. [Figure 28] A schematic process diagram showing an example of a manufacturing method for a virtual imprint mold, which follows FIG. [Figure 29] A schematic process diagram showing an example of a manufacturing method for a virtual imprint mold, which follows FIG. [Diagram 30] A schematic process diagram showing an example of a manufacturing method for a virtual imprint mold, which follows FIG. [Diagram 31] Schematic cross-sectional view showing an example of an actual imprint mold. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0046] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. However, the present disclosure can be implemented in many different forms, and should not be interpreted as being limited to the description of the embodiments exemplified below. In addition, in order to make the explanation clearer, the drawings may be schematic in terms of the width, thickness, shape, etc. of each part compared to the actual form, but these are merely examples and do not limit the interpretation of the present disclosure. In addition, in this specification and each figure, elements similar to those described above with respect to the previous figures may be given the same reference numerals, and detailed explanations may be omitted as appropriate.
[0047] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" is intended to include both a case in which another component is disposed directly above or below a certain component so as to be in contact with the component, and a case in which another component is disposed above or below a certain component with another component interposed therebetween, unless otherwise specified. Also, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface" is intended to include both a case in which another component is disposed directly above or below a certain component so as to be in contact with the component, and a case in which another component is disposed above or below a certain component with another component interposed therebetween, unless otherwise specified.
[0048] The imprint mold manufacturing method and the imprint mold of the present disclosure will be described in detail below.
[0049] <Manufacturing method of imprint mold> First, a method for producing the imprint mold of the present disclosure will be described. The manufacturing method of the imprint mold of the present disclosure includes a molding material preparation step of preparing a molding material having a first convex structure and a second convex structure on a first surface, and a resin part having a first convex structure top surface resin part covering an upper surface of the first convex structure, a first convex structure side surface resin part covering a side surface of the first convex structure, a second convex structure top surface resin part covering an upper surface of the second convex structure, and a second convex structure side surface resin part covering a side surface of the second convex structure, wherein the thickness of the first convex structure top surface resin part is smaller than the thickness of the second convex structure top surface resin part. The method includes, in order, a resin portion forming process for forming a resin portion on the first surface side of the molding material; a first convex structure top surface exposing process for etching the resin portion to remove the first convex structure top surface resin portion while leaving the first convex structure side surface resin portion, the second convex structure top surface resin portion, and the second convex structure side surface resin portion, thereby exposing the top surface of the first convex structure from the resin portion; and a first convex structure etching process for etching the top surface of the first convex structure exposed from the resin portion to reduce the height of the first convex structure.
[0050] Furthermore, the manufacturing method for an imprint mold disclosed herein sequentially includes, after the first convex structure top surface exposing step, a second convex structure top surface exposing step of further etching the resin part to remove the second convex structure top surface resin part while leaving the first convex structure side surface resin part and the second convex structure side surface resin part, thereby exposing the top surface of the second convex structure from the resin part, and a second convex structure etching step of etching the top surface of the second convex structure exposed from the resin part, thereby lowering the height of the second convex structure.
[0051] The method for producing an imprint mold according to the present disclosure will be described in detail below with reference to the drawings. Note that, for matters common to the method for producing an imprint mold according to the prior art, the same techniques as those used in the prior art can be used, and therefore detailed description thereof will be omitted.
[0052] [First embodiment] First, a first embodiment of the method for producing an imprint mold according to the present disclosure will be described. Figures 1 to 6 are schematic process diagrams showing an example of the first embodiment of the method for producing an imprint mold according to the present disclosure.
[0053] (Molding material preparation process) To manufacture an imprint mold according to the first embodiment of the manufacturing method for an imprint mold of the present disclosure, for example, first, a molding material having at least two convex structures (a first convex structure and a second convex structure) on a first surface is prepared as shown in Fig. 1. Note that the molding material 10A shown in Fig. 1 has a first convex structure 11, a second convex structure 12, and a third convex structure 13 on a first surface 10f.
[0054] A conventional imprint mold (an imprint mold in which the height of the protruding structures is the same) can be used for the molding material 10A. The mold material 10A can be manufactured by using a substrate (typically a synthetic quartz substrate) used in conventional imprint molds, and by various manufacturing methods used in conventional imprint mold manufacturing methods. For example, the molding material 10A can be manufactured by the method described above with reference to FIGS.
[0055] The first convex structure 11, the second convex structure 12, and the third convex structure 13 of the molding material 10A may all be a line structure or may all be a pillar structure. Also, any one of the first convex structure 11, the second convex structure 12, and the third convex structure 13 may be a line structure and the others may be pillar structures.
[0056] The first convex structure 11, the second convex structure 12, and the third convex structure 13 usually have the same height. However, the first convex structure 11, the second convex structure 12, and the third convex structure 13 may have different heights. Even if the heights are different, as long as the heights of the respective convex structures are known in advance, a desired imprint mold can be obtained by the manufacturing method for an imprint mold of the present disclosure.
[0057] However, as described above, in conventional imprint molds, the convex structures of the line structure and pillar structure are usually made to have the same height. In other words, it is difficult to manufacture an imprint mold having convex structures of different heights. For example, when attempting to manufacture an imprint mold having convex structures of different heights, as shown in FIG. 31, the corners of the upper surface of the convex structure are easily etched by side etching to form a rounded cross-sectional shape, and there is a problem that the desired cross-sectional shape cannot be obtained.
[0058] Therefore, the convex structures of the prepared molding material usually have the same height. In the molding material 10A shown in Fig. 1, the first convex structure 11, the second convex structure 12, and the third convex structure 13 all have a height H0.
[0059] Note that the term "same height" as used herein refers to the fact that in conventional imprint mold manufacturing methods, convex structures of the same height are manufactured by etching the first surface side of a substrate (typically a synthetic quartz substrate) that will become the imprint mold to the same depth by design. For example, the term "same height" as used herein also includes the distribution of heights of the convex structures due to the influence of the in-plane distribution of etching when manufacturing the convex structures of the mold material.
[0060] (Resin part forming process) Next, as shown in Figure 2, a resin part 20 having a first convex structure top surface resin part 21u covering the top surface of the first convex structure 11, a first convex structure side surface resin part 21s covering the side surface of the first convex structure 11, a second convex structure top surface resin part 22u covering the top surface of the second convex structure 12, and a second convex structure side surface resin part 22s covering the side surface of the second convex structure 12, wherein the thickness (T1) of the first convex structure top surface resin part 21u is smaller than the thickness (T2) of the second convex structure top surface resin part 22u, is formed on the first surface 10f side of the molding material 10A to produce the intermediate product 10B.
[0061] In the intermediate product 10B illustrated in Figure 2, the resin part 20 further has a third convex structure upper surface resin part 23u covering the upper surface of the third convex structure 13, and a third convex structure side surface resin part 23s covering the side surface of the third convex structure 13, and the thickness (T2) of the second convex structure upper surface resin part 22u is smaller than the thickness (T3) of the third convex structure upper surface resin part 23u.
[0062] A method for forming the intermediate product 10B having the resin portion 20 will be described in detail later with reference to FIGS.
[0063] (First convex structure upper surface exposing step and first convex structure etching step) Next, as shown in Figure 3, the resin part 20 is etched to remove the first convex structure top surface resin part 21u while leaving the first convex structure side surface resin part 21s, the second convex structure top surface resin part 22u, and the second convex structure side surface resin part 22s, and to expose the top surface of the first convex structure 11 from the resin part 20. Next, as shown in FIG. 4, the upper surface of the first convex structure 11 exposed from the resin portion 20 is etched to reduce the height of the first convex structure 11.
[0064] (Second convex structure upper surface exposing step and second convex structure etching step) Furthermore, in the manufacturing method of the imprint mold disclosed herein, after the above-mentioned first convex structure top surface exposing step, the resin part 20 is further etched in the same step as the above-mentioned first convex structure etching step, so that the second convex structure top surface resin part 22u disappears while leaving the first convex structure side surface resin part 21s and the second convex structure side surface resin part 22s, as shown in Figure 4, and the top surface of the second convex structure 12 is exposed from the resin part 20. Next, as shown in FIG. 5, the upper surface of the second convex structure 12 exposed from the resin portion 20 is etched to reduce the height of the second convex structure 12.
[0065] In the example shown in FIGS. 1 to 6, the etching steps (that is, the first convex structure etching step and the second convex structure etching step) are terminated when the third convex structure upper surface resin portion 23u disappears as shown in FIG.
[0066] Then, the remaining resin portion 20 (in the example shown in Figure 5, the first convex structure side resin portion 21s, the second convex structure side resin portion 22s, and the third convex structure side resin portion 23s) is removed to obtain an imprint mold 1A having multiple convex structures of different heights (the first convex structure 11A, the second convex structure 12A, and the third convex structure 13A), as shown in Figure 6. The relationship between the height (H1A) of the first convex structure 11A, the height (H2A) of the second convex structure 12A, and the height (H3A) of the third convex structure 13A is as follows: H1A <H2A<H3A It is.
[0067] The remaining first convex structure side surface resin portion 21s, second convex structure side surface resin portion 22s, and third convex structure side surface resin portion 23s can be removed by, for example, dry etching using oxygen gas, argon gas, helium gas, or a mixture of these gases. In addition, various known methods used in the manufacture of imprint molds may be used.
[0068] The above-mentioned resin part 20 and molding material 10A (more specifically, the first convex structure 11 and the second convex structure 12 of the molding material 10A) can be etched using a dry etching technique similar to that used in processing imprint molds for conventional nanoimprint lithography. Here, the dry etching may be performed using one type of etching gas or multiple types of etching gases. Also, an etching gas having a characteristic of mainly etching the molding material 10A and an etching gas having a characteristic of mainly etching the resin portion 20 may be mixed and used.
[0069] For example, in this embodiment, a gas containing fluorine (F) (e.g., a gas containing CF4 or CHF3) can be used as an etching gas having a characteristic of mainly etching the molding material 10A. Also, a gas containing oxygen (O) (e.g., O2) can be used as an etching gas having a characteristic of mainly etching the resin part 20.
[0070] In this embodiment, the etching gas in the first convex structure upper surface exposing step (see FIG. 3) and the etching gas in the first convex structure etching step (see FIG. 4) may be an etching gas composed of the same material.
[0071] If the etching gas in the first convex structure upper surface exposing process (see Figure 3) and the etching gas in the first convex structure etching process (see Figure 4) are made of the same material, the first convex structure upper surface exposing process (see Figure 3) and the first convex structure etching process (see Figure 4) can be carried out consecutively using the same etching gas, thereby further improving productivity.
[0072] In this embodiment, the etching gas in the first convex structure upper surface exposing step (see FIG. 3) and the etching gas in the first convex structure etching step (see FIG. 4) may be etching gases composed of different materials.
[0073] In this embodiment, the etching gas in the second convex structure upper surface exposing step (see FIG. 4) and the etching gas in the second convex structure etching step (see FIG. 5) may be an etching gas made of the same material.
[0074] If the etching gas in the second convex structure upper surface exposing process (see Figure 4) and the etching gas in the second convex structure etching process (see Figure 5) are made of the same material, the second convex structure upper surface exposing process (see Figure 4) and the second convex structure etching process (see Figure 5) can be carried out consecutively using the same etching gas, thereby further improving productivity.
[0075] In this embodiment, the etching gas in the second convex structure upper surface exposing step (see FIG. 4) and the etching gas in the second convex structure etching step (see FIG. 5) may be etching gases composed of different materials.
[0076] In this embodiment, the etching gas in the first convex structure upper surface exposing process (see FIG. 3), the etching gas in the first convex structure etching process (see FIG. 4), the etching gas in the second convex structure upper surface exposing process (see FIG. 4), and the etching gas in the second convex structure etching process (see FIG. 5) may all be etching gases composed of the same material.
[0077] If the etching gas in the first convex structure upper surface exposing process (see Figure 3), the etching gas in the first convex structure etching process (see Figure 4), the etching gas in the second convex structure upper surface exposing process (see Figure 4), and the etching gas in the second convex structure etching process (see Figure 5) are all etching gases composed of the same material, the processes from the first convex structure upper surface exposing process (see Figure 3) to the second convex structure etching process (see Figure 5) can be carried out continuously using the same etching gas, thereby further improving productivity.
[0078] In this embodiment, as shown in FIG. 4, the resin part 20 is also etched in the first convex structure etching step, and the etching rate of the resin part 20 in the first convex structure etching step is the same as the etching rate of the first convex structure 11.
[0079] In this embodiment, as shown in FIG. 5, the resin portion 20 is also etched in the second convex structure etching step, and the etching rate of the resin portion 20 in the second convex structure etching step is the same as the etching rate of the second convex structure 12.
[0080] In addition, in this embodiment, as shown in Figure 5, the first convex structure 11 is also etched in the second convex structure etching process, and the etching rate of the first convex structure 11 in the second convex structure etching process is the same as the etching rate of the second convex structure 12.
[0081] That is, in this embodiment, in the first convex structure etching process, the resin part 20 is also etched, and the etching rate of the resin part 20 in the first convex structure etching process is the same as the etching rate of the first convex structure 11; in the second convex structure etching process, the resin part 20 and the first convex structure 11 are also etched, and the etching rate of the resin part 20 and the first convex structure 11 in the second convex structure etching process is the same as the etching rate of the second convex structure 12; and the etching rate of the resin part 20 in the first convex structure etching process is the same as the etching rate of the resin part 20 in the second convex structure etching process.
[0082] In this embodiment, the etching gas material and mixture ratio, and dry etching conditions are adjusted to satisfy the etching rate conditions for the resin portion 20, the first convex structure 11, and the second convex structure 12.
[0083] In this embodiment, as described above, the etching rate of the resin part 20 in the first convex structure etching process is the same as the etching rate of the first convex structure 11, the etching rate of the resin part 20 in the second convex structure etching process is the same as the etching rate of the second convex structure 12, and the etching rate of the resin part 20 in the first convex structure etching process is the same as the etching rate of the resin part 20 in the second convex structure etching process.
[0084] Therefore, the difference between the height (H2A) of the second convex structure 12A and the height (H1A) of the first convex structure 11A in the imprint mold 1A shown in Figure 6 is equal to the difference between the thickness (T2) of the second convex structure upper surface resin portion 22u and the thickness (T1) of the first convex structure upper surface resin portion 21u.
[0085] More specifically, assuming that the height of the first convex structure 11A after completion of the second convex structure etching step is H1A, the height of the second convex structure 12A after completion of the second convex structure etching step is H2A, the thickness of the first convex structure upper surface resin portion 21u in the resin portion forming step is T1, and the thickness of the second convex structure upper surface resin portion 22u in the resin portion forming step is T2, H2A-H1A=T2-T1 This results in the following relationship.
[0086] In the example shown in FIGS. 1 to 6, the etching process (that is, the first convex structure etching process and the second convex structure etching process) is completed when the third convex structure upper surface resin portion 23u disappears. Therefore, the height (H1A) of the first convex structure 11A in the imprint mold 1A shown in Figure 6 is calculated to be the height (H0) of the first convex structure 11 in the molding material 10A shown in Figure 1 minus the difference between the thickness (T3) of the third convex structure upper surface resin portion 23u in the resin portion 20 shown in Figure 2 and the thickness (T1) of the first convex structure upper surface resin portion 21u. That is, H1A=H0-(T3-T1) It becomes.
[0087] Similarly, the height (H2A) of the second convex structure 12A in the imprint mold 1A shown in Figure 6 is calculated to be the height (H0) of the second convex structure 12 in the molding material 10A shown in Figure 1 minus the difference between the thickness (T3) of the third convex structure upper surface resin portion 23u in the resin portion 20 shown in Figure 2 and the thickness (T2) of the second convex structure upper surface resin portion 22u. That is, H2A=H0-(T3-T2) It becomes.
[0088] Note that the height (H3A) of the third convex structure 13A in the imprint mold 1A shown in FIG. 6 is theoretically the same as the height (H0) of the third convex structure 13 in the molding material 10A shown in FIG. That is, H3A=H0 It becomes.
[0089] Furthermore, in the manufacturing method of the imprint mold of this embodiment described above, while the upper surface of the convex structure is being etched, the resin portion is present on the side surface of the convex structure, and therefore the side surface is not subjected to side etching. Therefore, in the imprint mold 1A (Figure 6) manufactured using the imprint mold manufacturing method of this embodiment, even if the heights of the multiple convex structures are different, the radius of curvature in cross-section of the corners on the upper surface of each convex structure is small, and the cross-sectional shape of the corners on the upper surface of each convex structure is uniform (more specifically, the radius of curvature in cross-section of the corners on the upper surface of each convex structure falls within a certain numerical range).
[0090] More specifically, in the above-mentioned first convex structure etching process (see Figure 4), while etching is being performed on the upper surface of the first convex structure 11, the first convex structure side surface resin part 21s is present on the side surface of the first convex structure 11, and therefore the first convex structure 11 does not undergo side etching.
[0091] Furthermore, in the above-mentioned second convex structure etching process (see FIG. 5), while etching is being performed on the upper surface of the second convex structure 12, the second convex structure side surface resin part 22s is present on the side surface of the second convex structure 12, and therefore the second convex structure 12 does not undergo side etching.
[0092] In the above-mentioned first convex structure etching process (see FIG. 4) and second convex structure etching process (see FIG. 5), since the third convex structure upper surface resin part 23u is present on the upper surface of the third convex structure 13 and the third convex structure side surface resin part 23s is present on the side surface of the third convex structure 13, the third convex structure 13 does not undergo etching.
[0093] Therefore, in the imprint mold 1A manufactured using the imprint mold manufacturing method of this embodiment, the radius of curvature in cross-sectional view of the corners on the upper surface of each of the first convex structure 11A, the second convex structure 12A, and the third convex structure 13A is small, and the cross-sectional shapes of the corners on the upper surface of each of the first convex structure 11A, the second convex structure 12A, and the third convex structure 13A are uniform (more specifically, the radius of curvature in cross-sectional view of the corners on the upper surface of each of the first convex structure 11A, the second convex structure 12A, and the third convex structure 13A falls within a certain numerical range).
[0094] (Method of forming intermediate product 10B) Next, a method for forming an intermediate product 10B having a resin portion 20 whose thickness varies depending on the position as shown in FIG. 2 will be described. As a method for forming the resin portion 20 of the intermediate product 10B, for example, as shown in FIGS. 7 to 10, there can be mentioned a method of imprinting using an imprint mold having a stepped structure with different depths depending on the position.
[0095] For example, first, as shown in FIG. 7, a resin layer 20A is formed on the first surface 10f side of the molding material 10A shown in FIG. 1 to produce an intermediate product 10S.
[0096] The resin layer 20A is subjected to a process of shaping by imprinting and curing to become the resin part 20 shown in FIG. The resin layer 20A may be made of a resin that is used in conventional nanoimprint lithography. For example, a photocurable resin may be suitably used as the material of the resin layer 20A. Alternatively, a thermosetting resin may be used as the material of the resin layer 20A. An example of a method for forming the resin layer 20A is to apply the resin layer 20A onto the first surface 10f side of the molding material 10A.
[0097] In the intermediate product 10S, the resin layer 20A has a thickness sufficient to cover the upper surfaces of the first convex structure 11, the second convex structure 12, and the third convex structure 13. 7, the surface of the resin layer 20A (the resin layer first surface 20Af shown in FIG. 7) has a flat shape, but is not limited thereto and may have another shape as long as it has a thickness sufficient to cover the upper surfaces of the first convex structure 11, the second convex structure 12, and the third convex structure 13. For example, the surface may have periodic peaks and valleys according to the convex structure of the molding material 10A.
[0098] Next, as shown in FIGS. 8 and 9, imprinting is performed using an imprint mold 30 having a step structure (hereinafter also simply referred to as the imprint mold 30). That is, the surface of the imprint mold 30 on which the step structure is provided is pressed against the surface (resin layer first surface 20Af) of the resin layer 20A of the intermediate product 10S to form a shape, and if the resin layer 20A is a photocurable resin, the resin layer 20A is cured by irradiation with light to form the resin part 20. If the resin layer 20A is a thermosetting resin, the resin layer 20A is cured by heating to form the resin part 20.
[0099] Thereafter, the imprint mold 30 is released to obtain an intermediate product 10B having a resin portion 20 whose thickness varies depending on the position, as shown in Fig. 10. In this manner, the intermediate product 10B shown in Fig. 2 can be produced.
[0100] In addition, the step D1 in the imprint mold 30 corresponds to the step (T2-T1) between the second convex structure upper surface resin part 22u and the first convex structure upper surface resin part 21u in the resin part 20 of the intermediate product 10B, and the step D2 in the imprint mold 30 corresponds to the step (T3-T2) between the third convex structure upper surface resin part 23u and the second convex structure upper surface resin part 22u in the resin part 20 of the intermediate product 10B.
[0101] The imprint mold 30 having a stepped structure can also be manufactured using a substrate (typically a synthetic quartz substrate) used for conventional imprint molds, by various manufacturing methods used for manufacturing conventional imprint molds. When the imprint mold 30 has optical transparency, in the state shown in FIG. 9, the resin layer 20A can be cured by irradiating the imprint mold 30 with light from the side opposite to the surface on which the step structure is provided.
[0102] In addition, when the imprint mold 30 does not have optical transparency, the resin layer 20A can be hardened by irradiating light from the side opposite to the side on which the convex structures (first convex structures 11, etc.) of the molding material 10A are provided in the state shown in Figure 9.
[0103] In addition, the method of forming the intermediate product 10B having the resin part 20 whose thickness varies depending on the position as shown in Fig. 2 may be a method other than the above. For example, the gradation exposure method disclosed in JP 2022-142294 A may be used.
[0104] Gradient exposure refers to an exposure method in which, for a negative or positive resist composition, energy for hardening is supplied in a gradational manner in the case of a negative resist composition, and energy for facilitating dissolution is supplied in a gradational manner in the case of a positive resist composition. As the method of gradation exposure, a known method can be appropriately selected and used. For example, exposure through a gradation mask having a predetermined pattern shape can be performed using an exposure device such as an electron beam lithography device or an EUV exposure device, or gradation exposure can be selectively performed by lithography by direct irradiation with an electron beam without using a gradation mask.
[0105] The gradation mask may be appropriately selected from known gradation masks, such as a halftone mask and a slit mask (graytone mask). In addition, as a method for selectively performing gradation exposure by drawing using direct irradiation of an electron beam without using a gradation mask, for example, gradation exposure can be performed by changing the acceleration voltage or the exposure amount by using focus adjustment of the exposure or the gradation exposure function of a drawing exposure machine. For example, by performing gradational exposure on a negative resist film, a curing reaction of the resist composition in the resist film can be progressed according to the amount of exposure, and then by performing development, a form in which the thickness varies depending on the position can be obtained. Also, by performing gradational exposure on a positive resist film, the resist composition in the resist film can be easily dissolved according to the amount of exposure, and then by performing development, a form in which the thickness varies depending on the position can be obtained.
[0106] The exposure light source is not particularly limited, and can be an ArF excimer laser, a KrF excimer laser, an F2 excimer laser, EUV (Extreme Ultraviolet), an electron beam, an X-ray, an ion beam of helium, hydrogen, or the like, or the like.
[0107] [Second embodiment] Next, a second embodiment of the method for producing an imprint mold according to the present disclosure will be described. Figures 11 to 16 are schematic process diagrams showing an example of the second embodiment of the method for producing an imprint mold according to the present disclosure.
[0108] (Molding material preparation process) To manufacture an imprint mold according to the second embodiment of the manufacturing method of the imprint mold of the present disclosure, a molding material having at least two convex structures (a first convex structure and a second convex structure) on a first surface is prepared, as in the above-described first embodiment. The molding material 10F shown in Fig. 11 has a first convex structure 11, a second convex structure 12, and a third convex structure 13 on a first surface 10f. The molding material 10F shown in FIG. 11 may be the same as the molding material 10A shown in FIG.
[0109] (Resin part forming process) Next, as in the first embodiment described above, as shown in Figure 12, a resin part 20 having a first convex structure top surface resin part 21u covering the top surface of the first convex structure 11, a first convex structure side surface resin part 21s covering the side surface of the first convex structure 11, a second convex structure top surface resin part 22u covering the top surface of the second convex structure 12, and a second convex structure side surface resin part 22s covering the side surface of the second convex structure 12, wherein the thickness (T1) of the first convex structure top surface resin part 21u is smaller than the thickness (T2) of the second convex structure top surface resin part 22u, is formed on the first surface 10f side of the molding material 10F to produce an intermediate product 10G.
[0110] In the intermediate product 10G illustrated in Figure 12, the resin part 20 further has a third convex structure upper surface resin part 23u covering the upper surface of the third convex structure 13, and a third convex structure side surface resin part 23s covering the side surface of the third convex structure 13, and the thickness (T2) of the second convex structure upper surface resin part 22u is smaller than the thickness (T3) of the third convex structure upper surface resin part 23u.
[0111] The intermediate product 10G shown in Fig. 12 may be the same as the intermediate product 10B shown in Fig. 2. The intermediate product 10G shown in Fig. 12 can be produced in the same manner as the intermediate product 10B shown in Fig. 2.
[0112] (First convex structure upper surface exposing step and first convex structure etching step) Next, as shown in Figure 13, the resin part 20 is etched to remove the first convex structure top surface resin part 21u while leaving the first convex structure side surface resin part 21s, the second convex structure top surface resin part 22u, and the second convex structure side surface resin part 22s, and to expose the top surface of the first convex structure 11 from the resin part 20. Next, as shown in FIG. 14, the upper surface of the first convex structure 11 exposed from the resin portion 20 is etched to reduce the height of the first convex structure 11.
[0113] (Second convex structure upper surface exposing step and second convex structure etching step) Furthermore, in the manufacturing method of the imprint mold disclosed herein, after the above-mentioned first convex structure top surface exposing step, the resin part 20 is further etched in the same step as the above-mentioned first convex structure etching step, so that the second convex structure top surface resin part 22u is eliminated while leaving the first convex structure side surface resin part 21s and the second convex structure side surface resin part 22s, as shown in Figure 14, and the top surface of the second convex structure 12 is exposed from the resin part 20. Next, as shown in FIG. 15, the upper surface of the second convex structure 12 exposed from the resin portion 20 is etched to reduce the height of the second convex structure 12.
[0114] In the example shown in FIGS. 11 to 16, the etching steps (that is, the first convex structure etching step and the second convex structure etching step) are terminated when the third convex structure upper surface resin portion 23u disappears as shown in FIG.
[0115] Then, the remaining resin portion 20 (in the example shown in Figure 15, the first convex structure side surface resin portion 21s, the second convex structure side surface resin portion 22s, and the third convex structure side surface resin portion 23s) is removed to obtain an imprint mold 1B having multiple convex structures of different heights (first convex structure 11B, second convex structure 12B, and third convex structure 13B), as shown in Figure 16. The relationship between the height (H1B) of the first convex structure 11B, the height (H2B) of the second convex structure 12B, and the height (H3B) of the third convex structure 13B is as follows: H1B <H2B<H3B It is.
[0116] The remaining first convex structure side surface resin portion 21s, second convex structure side surface resin portion 22s, and third convex structure side surface resin portion 23s can be removed by, for example, dry etching using oxygen gas, argon gas, helium gas, or a mixture of these gases. In addition, various known methods used in the manufacture of imprint molds may be used.
[0117] The above-mentioned resin part 20 and molding material 10F (more specifically, the first convex structure 11 and the second convex structure 12 of the molding material 10F) can be etched using a dry etching technique similar to that used in processing imprint molds for conventional nanoimprint lithography. Here, the dry etching may be performed using one type of etching gas or multiple types of etching gases. Also, an etching gas having a characteristic of mainly etching the molding material 10F and an etching gas having a characteristic of mainly etching the resin portion 20 may be mixed and used.
[0118] For example, in this embodiment, a gas containing fluorine (F) (e.g., a gas containing CF4 or CHF3) can be used as an etching gas having a characteristic of mainly etching the molding material 10F. Also, a gas containing oxygen (O) (e.g., O2) can be used as an etching gas having a characteristic of mainly etching the resin part 20.
[0119] In this embodiment as well, the etching gas in the first convex structure upper surface exposing step (see FIG. 13) and the etching gas in the first convex structure etching step (see FIG. 14) may be an etching gas made of the same material.
[0120] If the etching gas in the first convex structure upper surface exposing process (see FIG. 13) and the etching gas in the first convex structure etching process (see FIG. 14) are made of the same material, the first convex structure upper surface exposing process (see FIG. 13) and the first convex structure etching process (see FIG. 14) can be carried out consecutively using the same etching gas, thereby further improving productivity.
[0121] Also in this embodiment, the etching gas in the first convex structure upper surface exposing step (see FIG. 13) and the etching gas in the first convex structure etching step (see FIG. 14) may be etching gases composed of different materials.
[0122] Also in this embodiment, the etching gas in the second convex structure upper surface exposing step (see FIG. 14) and the etching gas in the second convex structure etching step (see FIG. 15) may be an etching gas made of the same material.
[0123] If the etching gas in the second convex structure upper surface exposing process (see FIG. 14) and the etching gas in the second convex structure etching process (see FIG. 15) are made of the same material, the second convex structure upper surface exposing process (see FIG. 14) and the second convex structure etching process (see FIG. 15) can be carried out consecutively using the same etching gas, thereby further improving productivity.
[0124] Also in this embodiment, the etching gas in the second convex structure upper surface exposing step (see FIG. 14) and the etching gas in the second convex structure etching step (see FIG. 15) may be etching gases composed of different materials.
[0125] In this embodiment, too, the etching gas in the first convex structure upper surface exposing process (see FIG. 13), the etching gas in the first convex structure etching process (see FIG. 14), the etching gas in the second convex structure upper surface exposing process (see FIG. 14), and the etching gas in the second convex structure etching process (see FIG. 15) may all be etching gases composed of the same material.
[0126] If the etching gas in the first convex structure upper surface exposing process (see Figure 13), the etching gas in the first convex structure etching process (see Figure 14), the etching gas in the second convex structure upper surface exposing process (see Figure 14), and the etching gas in the second convex structure etching process (see Figure 15) are all etching gases composed of the same material, the processes from the first convex structure upper surface exposing process (see Figure 13) to the second convex structure etching process (see Figure 15) can be carried out continuously using the same etching gas, thereby further improving productivity.
[0127] In this embodiment, as shown in FIG. 14, the resin part 20 is also etched in the first convex structure etching step, and the etching rate of the resin part 20 in the first convex structure etching step is slower than the etching rate of the first convex structure 11.
[0128] In this embodiment, as shown in FIG. 15, the resin portion 20 is also etched in the second convex structure etching step, and the etching rate of the resin portion 20 in the second convex structure etching step is slower than the etching rate of the second convex structure 12.
[0129] In addition, in this embodiment, as shown in Figure 15, the first convex structure 11 is also etched in the second convex structure etching process, and the etching rate of the first convex structure 11 in the second convex structure etching process is the same as the etching rate of the second convex structure 12.
[0130] That is, in this embodiment, in the first convex structure etching process, the resin part 20 is also etched, and in the second convex structure etching process, the resin part 20 is also etched, the etching rate of the resin part 20 in the first convex structure etching process is slower than the etching rate of the first convex structure 11, and in the second convex structure etching process, the resin part 20 and the first convex structure 11 are also etched, the etching rate of the resin part 20 in the second convex structure etching process is slower than the etching rate of the second convex structure 12, the etching rate of the first convex structure 11 in the second convex structure etching process is the same as the etching rate of the second convex structure 12, and the etching rate of the resin part 20 in the first convex structure etching process is the same as the etching rate of the resin part 20 in the second convex structure etching process.
[0131] In this embodiment, the etching gas material, mixing ratio, and dry etching conditions are adjusted to satisfy the etching rate conditions for the resin part 20, the first convex structure 11, and the second convex structure 12.
[0132] In this embodiment, as described above, the etching rate of the resin part 20 in the first convex structure etching process is slower than the etching rate of the first convex structure 11, the etching rate of the resin part 20 in the second convex structure etching process is slower than the etching rate of the second convex structure 12, the etching rate of the first convex structure 11 in the second convex structure etching process is the same as the etching rate of the second convex structure 12, and the etching rate of the resin part 20 in the first convex structure etching process is the same as the etching rate of the resin part 20 in the second convex structure etching process.
[0133] Therefore, the etching rate of the resin portion 20 in the second convex structure etching step is defined as Ej, If the etching rate of the first convex structure 11 and the etching rate of the second convex structure 12 in the second convex structure etching process are Et, the difference between the height (H2B) of the second convex structure 12B and the height (H1B) of the first convex structure 11B in the imprint mold 1B shown in Figure 16 is calculated by multiplying the difference between the thickness (T2) of the second convex structure upper surface resin part 22u and the thickness (T1) of the first convex structure upper surface resin part 21u by the above-mentioned etching rate ratio (Et / Ej).
[0134] For more information, The height of the first convex structure 11B after the second convex structure etching step is H1B. The height of the second convex structure 12B after the second convex structure etching step is H2B. The thickness of the first convex structure upper surface resin portion 21u in the resin portion forming step is T1, The thickness of the second convex structure upper surface resin portion 22u in the resin portion forming step is T2, The etching rate of the resin portion 20 in the second convex structure etching step is Ej, In the second convex structure etching step, the etching rate of the first convex structure 11B and the etching rate of the second convex structure 12B are Et, H2B-H1B=(T2-T1)×(Et / Ej) This results in the following relationship.
[0135] Furthermore, in the manufacturing method of the imprint mold of this embodiment, as in the manufacturing method of the imprint mold of the first embodiment described above, while etching is being performed on the upper surface of the convex structure, a resin portion is present on the side surface of the convex structure, and therefore side etching is not performed. Therefore, in the imprint mold 1B (Figure 16) manufactured using the imprint mold manufacturing method of this embodiment, even if the heights of the multiple convex structures are different, the radius of curvature in cross-section of the corners on the upper surface of each convex structure is small, and the cross-sectional shape of the corners on the upper surface of each convex structure is uniform (more specifically, the radius of curvature in cross-section of the corners on the upper surface of each convex structure falls within a certain numerical range).
[0136] More specifically, in the above-mentioned first convex structure etching process (see Figure 14), while etching is being performed on the upper surface of the first convex structure 11, the first convex structure side surface resin part 21s is present on the side surface of the first convex structure 11, and therefore the first convex structure 11 does not undergo side etching.
[0137] Furthermore, in the above-mentioned second convex structure etching process (see FIG. 15), while etching is being performed on the upper surface of the second convex structure 12, the second convex structure side surface resin part 22s is present on the side surface of the second convex structure 12, and therefore the second convex structure 12 does not undergo side etching.
[0138] In the above-mentioned first convex structure etching process (see FIG. 14) and second convex structure etching process (see FIG. 15), since the third convex structure upper surface resin part 23u is present on the upper surface of the third convex structure 13 and the third convex structure side surface resin part 23s is present on the side surface of the third convex structure 13, the third convex structure 13 does not undergo etching.
[0139] Therefore, in the imprint mold 1B manufactured using the imprint mold manufacturing method of this embodiment, the radius of curvature in cross-sectional view of the corners on the upper surface of each of the first convex structure 11B, the second convex structure 12B, and the third convex structure 13B is small, and the cross-sectional shapes of the corners on the upper surface of each of the first convex structure 11B, the second convex structure 12B, and the third convex structure 13B are uniform (more specifically, the radius of curvature in cross-sectional view of the corners on the upper surface of each of the first convex structure 11B, the second convex structure 12B, and the third convex structure 13B falls within a certain numerical range).
[0140] <Imprint mold> Next, the imprint mold of the present disclosure will be described. The imprint mold of the present disclosure can be manufactured by the above-mentioned manufacturing method of the imprint mold of the present disclosure.
[0141] FIG. 17 is a schematic cross-sectional view showing an example of the imprint mold of the present disclosure. An imprint mold 1C shown in FIG. 17 has, on the first surface 10f, a first convex structure 11C and a second convex structure 12C that is taller than the first convex structure 11C. 17 further has a third convex structure 13C on the first surface 10f. The third convex structure 13C is taller than the second convex structure 12C.
[0142] The first convex structure 11C, the second convex structure 12C, and the third convex structure 13C of the imprint mold 1C may all be a line structure or may all be a pillar structure. Also, any one of the first convex structure 11C, the second convex structure 12C, and the third convex structure 13C may be a line structure and the others may be pillar structures.
[0143] The imprint mold 1C shown in FIG. 17 can be manufactured by the above-described method for manufacturing an imprint mold according to the first embodiment of the present disclosure, or the method for manufacturing an imprint mold according to the second embodiment of the present disclosure.
[0144] Therefore, in the imprint mold 1C, the radius of curvature in cross-sectional view of the corners on the upper surface of each of the first convex structure 11C, the second convex structure 12C, and the third convex structure 13C is small, and the cross-sectional shapes of the corners on the upper surface of each of the first convex structure 11C, the second convex structure 12C, and the third convex structure 13C are uniform (more specifically, the radius of curvature in cross-sectional view of the corners on the upper surface of each of the first convex structure 11C, the second convex structure 12C, and the third convex structure 13C falls within a certain numerical range).
[0145] For example, in the imprint mold 1C shown in Figure 17, the radius of curvature R1 in cross-sectional view of the corner formed by the upper surface and side surface of the first convex structure 11C, and the radius of curvature R2 in cross-sectional view of the corner formed by the upper surface and side surface of the second convex structure 12C can both be 15 nm or less.
[0146] Fig. 18 is an SEM image showing an example of a convex structure of the imprint mold of the present disclosure, and Fig. 19 is a diagram for explaining a method for measuring the radius of curvature. Hereinafter, a method for measuring the radius of curvature (corner R) in a cross-sectional view of a corner portion defined by the upper surface and side surface of a convex structure will be described.
[0147] (How to measure the radius of curvature) A method for measuring the radius of curvature in a cross-sectional view of a corner portion defined by the upper surface and side surface of the above-mentioned convex structure will be described with reference to FIG.
[0148] First, the image data acquired by SEM observation (Figure 18) is converted into a numerical representation of 256 levels for each pixel, and a histogram of the gray distribution is created.
[0149] Next, a threshold is set, and the data converted into a numerical representation of 256 gradations for each pixel is subjected to a binarization process of less than the threshold and more than the threshold. In the example shown in Fig. 19, the threshold is set to 50. As a result, in the example shown in Fig. 19, the area is visually divided into areas with light and dark shades and areas with light and dark shades. From the data that has been subjected to this binarization process, a straight line (line segment Lu) that is recognized as the top surface of the convex structure, a straight line (line segment Ls) that is recognized as the side surface of the convex structure, and a curve (Lc) that is recognized as the contour line of the corner of the convex structure are determined.
[0150] Next, calculate the area (S) of the region enclosed by the line extending from the straight line (line segment Lu) recognized as the top surface of the convex structure, the line extending from the straight line (line segment Ls) recognized as the side surface of the convex structure, and the curve (Lc) recognized as the contour line of the corner of the convex structure. For example, calculate the area of the region to be determined by measuring the number of pixels in the enclosed region and multiplying this number of pixels by the unit area of one pixel.
[0151] Next, the radius of curvature (corner R) is calculated from the calculated area according to the description disclosed in Japanese Patent No. 4139664 using the following formula 1 (corresponding to formula 7 in Japanese Patent No. 4139664). Note that θ in the following formula 1 is the angle on the side of the desired area, which is formed by an extension of a straight line (segment Lu) recognized as the upper surface of the above-mentioned convex structure and an extension of a straight line (segment Ls) recognized as the side surface of the convex structure. In the example shown in FIG. 19, it was 88°.
[0152]
number
[0153] As described above, the radius of curvature (corner R) in a cross-sectional view of the corner formed by the upper surface and side surface of the convex structure of the example shown in FIG. 18 was found to be 12.9 nm.
[0154] Although the manufacturing method of the imprint mold and the imprint mold according to the present disclosure have been described above, the present disclosure is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure in any case. [Explanation of symbols]
[0155] 1, 1A, 1B, 1C Imprint mold 10A, 10F Molding material 10f 1st page 10B, 10C, 10D, 10E intermediate products 10G, 10H, 10I, 10J intermediate products 10S intermediate products 11, 11A, 11B, 11C 1st convex structure 12, 12A, 12B, 12C 2nd convex structure 13, 13A, 13B, 13C third convex structure 20 Resin part 20A Resin layer 20Af Resin layer first side 21s 1st convex structure side resin part 21u 1st convex structure top resin part 22s 2nd convex structure side resin part 22u 2nd convex structure top resin part 23s Third convex structure side resin part 23u 3rd convex structure top resin part 30 Imprint Mold 100 Imprint Mold Imprint mold with 100A hard mask pattern 110A Molding material 110B, 110C, 110D, 110E intermediate products 101 First convex structure 102 Second convex structure 103 Third convex structure 110 Light-transparent substrate 120 Hard Mask Layer 121, 122, 123 Hard mask pattern 131, 132, 133 Resist pattern 200 Imprint Mold
Claims
1. a molding material preparation step of preparing a molding material having a first convex structure and a second convex structure on a first surface; a first convex structure upper surface resin portion covering an upper surface of the first convex structure; a first convex structure side surface resin portion covering a side surface of the first convex structure; a second convex structure upper surface resin portion covering an upper surface of the second convex structure; a second convex structure side surface resin portion covering a side surface of the second convex structure; having The thickness of the first convex structure upper surface resin portion is A resin portion having a shape smaller than the thickness of the second convex structure upper surface resin portion, a resin portion forming step of forming a resin portion on the first surface side of the molding material; The resin portion is etched, While leaving the first convex structure side surface resin portion, the second convex structure upper surface resin portion, and the second convex structure side surface resin portion, The first convex structure upper surface resin portion is eliminated, a first convex structure upper surface exposing step of exposing an upper surface of the first convex structure from the resin portion; a first convex structure etching step of etching an upper surface of the first convex structure exposed from the resin portion to reduce a height of the first convex structure; A method for manufacturing an imprint mold comprising, in order:
2. After the first convex structure upper surface exposing step, The resin portion is further etched, While leaving the first convex structure side surface resin portion and the second convex structure side surface resin portion, The second convex structure upper surface resin portion is eliminated, a second convex structure upper surface exposing step of exposing an upper surface of the second convex structure from the resin portion; a second convex structure etching step of etching an upper surface of the second convex structure exposed from the resin portion to reduce a height of the second convex structure; The method of claim 1 , further comprising, in order:
3. 3 . The method for manufacturing an imprint mold according to claim 1 , wherein an etching gas used in the first convex structure upper surface exposing step and an etching gas used in the first convex structure etching step are etching gases made of the same material.
4. The method for manufacturing an imprint mold according to claim 2 , wherein an etching gas used in the second convex structure upper surface exposing step and an etching gas used in the second convex structure etching step are made of the same material.
5. 3. The method for manufacturing an imprint mold according to claim 2, wherein the etching gas in the first convex structure upper surface exposing step, the etching gas in the first convex structure etching step, the etching gas in the second convex structure upper surface exposing step, and the etching gas in the second convex structure etching step are all etching gases composed of the same material.
6. In the first convex structure etching step, the resin portion is also etched, an etching rate of the resin portion in the first convex structure etching step is The method for manufacturing an imprint mold according to claim 1 or 2, wherein the etching rate is the same as that of the first convex structure.
7. In the second convex structure etching step, the resin portion and the first convex structure are also etched, an etching rate of the resin portion and the first convex structure in the second convex structure etching step is the etching rate of the second convex structure is equal to the etching rate of the second convex structure; A method for producing the imprint mold according to claim 2.
8. In the first convex structure etching step, the resin portion is also etched, an etching rate of the resin portion in the first convex structure etching step is the etching rate is equal to that of the first convex structure, In the second convex structure etching step, the resin portion and the first convex structure are also etched, an etching rate of the resin portion and the first convex structure in the second convex structure etching step is the etching rate is equal to that of the second convex structure, The method for manufacturing an imprint mold according to claim 2 , wherein an etching rate of the resin portion in the first convex structure etching step is the same as an etching rate of the resin portion in the second convex structure etching step.
9. The height of the first convex structure after the second convex structure etching step is H1A, The height of the second convex structure after the second convex structure etching step is H2A, A thickness of the first convex structure upper surface resin portion in the resin portion forming step is defined as T1, When the thickness of the second convex structure upper surface resin portion in the resin portion forming step is T2, H2A-H1A=T2-T1 The method for producing an imprint mold according to claim 2 ,
10. In the first convex structure etching step, the resin portion is also etched, an etching rate of the resin portion in the first convex structure etching step is The method for manufacturing an imprint mold according to claim 1 or 2, wherein the etching rate of the first convex structure is slower than that of the first convex structure.
11. In the second convex structure etching step, the resin portion and the first convex structure are also etched, an etching rate of the resin portion in the second convex structure etching step is an etching rate slower than the etching rate of the second convex structure, an etching rate of the first convex structure in the second convex structure etching step is the etching rate of the second convex structure is equal to the etching rate of the second convex structure; A method for producing the imprint mold according to claim 2.
12. In the first convex structure etching step, the resin portion is also etched, an etching rate of the resin portion in the first convex structure etching step is an etching rate slower than the etching rate of the first convex structure, In the second convex structure etching step, the resin portion and the first convex structure are also etched, an etching rate of the resin portion in the second convex structure etching step is an etching rate slower than the etching rate of the second convex structure, an etching rate of the first convex structure in the second convex structure etching step is the etching rate is equal to that of the second convex structure, The method for manufacturing an imprint mold according to claim 2 , wherein an etching rate of the resin portion in the first convex structure etching step is the same as an etching rate of the resin portion in the second convex structure etching step.
13. The height of the first convex structure after the second convex structure etching step is H1B, The height of the second convex structure after the second convex structure etching step is H2B, A thickness of the first convex structure upper surface resin portion in the resin portion forming step is defined as T1, A thickness of the second convex structure upper surface resin portion in the resin portion forming step is T2, an etching rate of the resin portion in the second convex structure etching step is defined as Ej; When the etching rate of the first convex structure and the etching rate of the second convex structure in the second convex structure etching step are Et, H2B-H1B=(T2-T1)×(Et / Ej) The method for producing an imprint mold according to claim 2 ,
14. The method for manufacturing an imprint mold according to claim 1 or 2, wherein the first convex structure is a pillar structure.
15. The method for manufacturing an imprint mold according to claim 1 or 2, wherein the second convex structure is a pillar structure.
16. The method for manufacturing an imprint mold according to claim 1 or 2, wherein the first convex structure is a line structure.
17. The method for manufacturing an imprint mold according to claim 1 or 2, wherein the second convex structure is a line structure.
18. A first surface has a first convex structure and a second convex structure that is taller than the first convex structure, An imprint mold, wherein the radius of curvature in cross-sectional view of a corner formed by the upper surface and side surface of the first convex structure and the radius of curvature in cross-sectional view of a corner formed by the upper surface and side surface of the second convex structure are both 15 nm or less.
19. The imprint mold of claim 18 , wherein the first raised structure is a pillar structure.
20. The imprint mold of claim 18 , wherein the second raised structure is a pillar structure.
21. The imprint mold according to claim 18 , wherein the first raised structure is a line structure.
22. The imprint mold according to claim 18 , wherein the second raised structure is a line structure.
Citation Information
Patent Citations
Imprinting apparatus and imprinting method
JP2002093748A
fluid pressure imprint lithography
JP2004504718A