Expanded microspheres with excellent barrier properties

Halogen-free thermoplastic microspheres with specific monomer compositions and propellants provide lower expansion temperatures and improved storage stability, addressing sustainability and safety concerns while maintaining excellent barrier properties.

JP2024159640AActive Publication Date: 2024-11-08AKZO NOBEL CHEMICALS INTERNATIONAL BV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024071029
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-25
Publication Date
2024-11-08
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

Existing thermally expandable microspheres containing halogenated monomers, such as PVDC, face sustainability and health, safety, and environmental concerns due to high halogen content, and halogen-free alternatives require higher expansion temperatures and suffer from poor storage stability, especially when stored in wet conditions.

Method used

Developing thermoplastic microspheres with a polymer shell composed of specific ratios of acrylonitrile, methacrylonitrile, and methyl acrylate or methacrylate monomers, combined with a propellant like isobutane, that are essentially halogen-free, allowing for lower expansion temperatures and excellent storage stability, even in wet conditions.

Benefits of technology

The new microspheres achieve high expandability with excellent barrier properties and long-term storage stability, suitable for applications requiring ease of handling and reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159640000006
    Figure 2024159640000006
  • Figure 2024159640000007
    Figure 2024159640000007
  • Figure 2024159640000001
    Figure 2024159640000001
Patent Text Reader

Abstract

To provide thermoplastic thermally expandable microspheres with excellent barrier properties and thermal stability, wherein the thermoplastic thermally expandable microspheres comprise a polymer shell and a propellant.SOLUTION: A polymer shell is formed from ethylenically unsaturated monomers and encapsulates a propellant, wherein the ethylenically unsaturated monomers comprise acrylonitrile in an amount from 45 to 80 weight %, methacrylonitrile in an amount of from 10 to 45 weight %, and methyl acrylate and / or methyl methacrylate in an amount of 5 to 35 weight %, each based on the total weight of ethylenically unsaturated monomers, and wherein the thermoplastic thermally expandable microspheres comprise the propellant in an amount of 5 to 17 weight %, based on the total weight of the thermoplastic thermally expandable microspheres. The disclosure further relates to a process for preparing such thermoplastic thermally expandable microspheres and an aqueous slurry comprising such thermoplastic thermally expandable microspheres.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to thermoplastic heat-expandable microspheres and expandable microspheres made from thermoplastic heat-expandable microspheres having excellent barrier properties and thermal stability. The present invention further relates to a method for preparing such thermoplastic heat-expandable microspheres and an aqueous slurry comprising such thermoplastic heat-expandable microspheres. [Background technology]

[0002] Thermally expandable microspheres are known in the art and are described, for example, in U.S. Pat. No. 3,615,972, International Patent Publication No. WO 00 / 37547, and International Patent Publication No. WO 2007 / 091960. Some examples are sold under the trade name Expancel®. They can be expanded to form extremely low weight and low density fillers and can find use in applications such as foamed or low density resins, paints and coatings, cements, inks, and crack fillers. Consumer products that often contain expandable microspheres include lightweight shoe soles (e.g., for running shoes), textured coverings such as wallpaper, solar reflective and thermal insulation coatings, food package sealants, wine corks, artificial leather, foam for protective helmet liners, and weather stripping for automobiles.

[0003] Thermally expandable polymeric microspheres typically comprise a thermoplastic polymer shell and a hollow core containing a propellant (or sometimes referred to as a blowing agent) that expands upon heating. Examples of propellants include low boiling point hydrocarbons or halogenated hydrocarbons that are either condensed or liquid at room temperature that vaporize upon heating. To produce expandable microspheres, the expandable microspheres are heated such that the thermoplastic polymer shell softens, and the propellant vaporizes and expands, thereby expanding the microspheres. Typically, the diameter of the microspheres may increase between 1.5 and 8 times during expansion. Expandable microspheres are commercially available in various forms, for example, as dry free-flowing particles, as aqueous slurries, or as partially dewatered wet cakes. Heating of expandable microspheres may be performed using various techniques. One commonly used technique is the so-called wet expansion technique, where the microspheres are expanded in water that is heated to the boiling point. If higher temperatures are required for expansion, the expansion may be performed using, for example, high energy steam techniques.

[0004] Expandable microspheres may be produced by polymerizing ethylenically unsaturated monomers in the presence of a propellant, for example, using a suspension polymerization method. Typical monomers include acrylates, acrylonitrile, acrylamide, halogen-containing monomers such as vinylidene dichloride (VDC), and those based on styrene. Usually, mixtures of such monomers are used to produce expandable microspheres with a copolymer shell.

[0005] Expandable microspheres with a copolymer shell based on either VDC and acrylonitrile (AN) or AN and methacrylonitrile (MAN) are often used in the manufacture of wet heat expandable microspheres. These microspheres are distinguished in that the polymer shell has excellent barrier properties against the encapsulated propellant even in the wet state, even though water can act as a plasticizer in the microsphere shell. If the polymer shell is plasticized, the propellant is lost by diffusion and the properties of the microsphere are reduced. This can be seen already during expansion in an aqueous environment or during storage of wet expandable heat expandable microspheres.

[0006] Halogen-containing microspheres, especially VDC-containing microspheres, have been found to have excellent barrier properties due to the crystalline polyvinylidene chloride (PVDC) moieties in the polymer shell, which also limits the plasticizing effect of water due to the hydrophobic nature of PVDC. Another advantage of these expandable VDC-containing microspheres is their expansion at relatively low temperatures due to the low glass transition temperature (Tg), i.e., the low softening point of the polymer shell, which allows the expansion of these expandable VDC-containing microspheres in boiling water. However, the main drawback of these microspheres is the high halogen content due to PVDC, which makes the microspheres unsustainable. Furthermore, there are health, safety, and environmental (HSE) concerns regarding these VDC-containing microspheres due to the significant amount of residual VDC, since it is often difficult to polymerize VDC to a high conversion to PVDC.

[0007] There are attempts to overcome these sustainability and HSE issues with halogen-free AN-co-MAN polymer shells. However, these microspheres typically require temperatures above 150°C for efficient expansion, which creates other challenges since boiling water cannot be used. Instead, steam is usually used as the energy source during expansion. This makes the use of these microspheres less flexible, as it places higher demands on the expansion equipment, and also creates HSE issues when working with high-energy steam. Furthermore, it has been found that there are some drawbacks, especially with regard to the storage stability of expandable microspheres made from such halogen-free expandable microspheres, for example as described in WO 2007 / 091960 A1. In particular, it has been found that the storage stability of such halogen-free expandable microspheres that are wet expanded and stored wet after expansion is not satisfactory. Storage stability is a very relevant issue commercially because for logistical and economic reasons, customers tend to order larger batches of expandable microspheres, which are then used for a certain period of time, for example, at least 3 weeks, preferably at least 4 weeks, more preferably at least 6 weeks. Also, the time of transporting the expandable microspheres from the manufacturing site to the customer must be taken into account. Furthermore, there are many applications of expandable microspheres where the expandable microspheres are not completely embedded in a solid matrix. In such applications, the long-term storage stability of the expandable microspheres is important.

[0008] Wet storage of expandable microspheres is preferred because handling of wet microspheres is much easier than handling of completely dry microspheres, which are dusty powders. However, as already mentioned above, water acts as a plasticizer for the polymer shell, thus impairing the barrier properties of the polymer shell and resulting in reduced storage stability.

[0009] Therefore, there is still a need for thermoplastic heat-expandable microspheres that are essentially free of halogen-containing monomers, particularly free of VDC, and still have excellent barrier stability after expansion and very good storage stability.Furthermore, it is desirable that such thermoplastic heat-expandable microspheres can be expanded at lower temperatures, preferably by using aqueous wet expansion.In particular, it is desirable to provide such heat-expandable microspheres that are essentially free of halogen-containing monomers, particularly free of VDC, can be wet expanded, and have excellent barrier stability after expansion and very good storage stability even when stored in a wet state after wet expansion.

[0010] The present invention is therefore directed to finding such expandable polymeric microspheres, the polymeric shell of which is essentially free of halogen-containing monomers, and in particular essentially free of VDC, and yet has excellent barrier stability and very good storage stability after expansion, can be expanded at preferably lower temperatures, such as by using aqueous wet expansion, and has very good storage stability even when stored in a wet state after wet expansion. Surprisingly, it has been found that these objectives can be achieved by a specific combination of specific ranges of amounts of monomers in the polymeric shell of the expandable microspheres, further combined with specific ranges of amounts of propellants contained in the expandable microspheres. Summary of the Invention

[0011] In a first aspect, the present invention is directed to a thermoplastic heat-expandable microsphere comprising a polymer shell and a propellant, the polymer shell being made from ethylenically unsaturated monomers and encapsulating the propellant, the ethylenically unsaturated monomers comprising acrylonitrile in an amount of 45-80% by weight, methacrylonitrile in an amount of 10-45% by weight, and methyl acrylate and / or methyl methacrylate in an amount of 5-35% by weight, each based on the total weight of the ethylenically unsaturated monomers, and the thermoplastic heat-expandable microsphere comprising the propellant in an amount of 5-17% by weight, based on the total weight of the thermoplastic heat-expandable microsphere.

[0012] In a second aspect, the present invention is further directed to a method for preparing thermoplastic thermally expandable microspheres comprising a polymer shell and a propellant, the method comprising the step of polymerizing ethylenically unsaturated monomers in the presence of a propellant in a polymerization mixture, the ethylenically unsaturated monomers comprising acrylonitrile in an amount of 45-80 wt%, methacrylonitrile in an amount of 10-45 wt%, and methyl acrylate and / or methyl methacrylate in an amount of 5-35 wt%, each based on the total weight of the ethylenically unsaturated monomers, and the propellant comprises at least one of propane, isobutane, and n-butane and is present in an amount of 5-30 wt%, based on the total weight of the ethylenically unsaturated monomers and the propellant.

[0013] In a third aspect, the present invention is further directed to an aqueous slurry comprising the thermoplastic thermally expandable microspheres as described above according to the first aspect, or the aqueous slurry obtained from the above process as described above according to the second aspect. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 illustrates the difference between single-core (FIG. 1A) and multi-core (FIG. 1B) microspheres. [Diagram 2] FIG. 2 shows the storage stability of expandable microspheres from the examples over periods up to 42 days. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In a first aspect, the present invention is directed to a thermoplastic heat-expandable microsphere comprising a polymer shell and a propellant, the polymer shell being made from ethylenically unsaturated monomers and encapsulating the propellant, the ethylenically unsaturated monomers comprising acrylonitrile in an amount of 45-80% by weight, methacrylonitrile in an amount of 10-45% by weight, and methyl acrylate and / or methyl methacrylate in an amount of 5-35% by weight, each based on the total weight of the ethylenically unsaturated monomers, and the thermoplastic heat-expandable microsphere comprising the propellant in an amount of 5-17% by weight, based on the total weight of the thermoplastic heat-expandable microsphere.

[0016] The ethylenically unsaturated monomers preferably comprise acrylonitrile in an amount of 50 to 75% by weight, more preferably 53 to 70% by weight, most preferably 55 to 65% by weight, for example 57 to 61% by weight, each based on the total weight of the ethylenically unsaturated monomers.

[0017] The ethylenically unsaturated monomers preferably include methacrylonitrile in an amount of 15 to 40% by weight, more preferably 20 to 35% by weight, for example, 21 to 33% by weight, and most preferably 22 to 30% by weight, for example, 23 to 28% by weight, each based on the total weight of the ethylenically unsaturated monomers.

[0018] The ethylenically unsaturated monomers preferably comprise methyl acrylate and / or methyl methacrylate in an amount of 6 to 34 wt%, for example, 7 to 33 wt%, 8 to 32 wt%, or 10 to 30 wt%, preferably 12 to 25 wt%, and most preferably 13 to 23 wt%, for example, 14 to 20 wt%, each based on the total weight of the ethylenically unsaturated monomers.

[0019] The total weight of ethylenically unsaturated monomers in the polymer shell of the thermoplastic heat-expandable microspheres is 100% by weight.

[0020] Thus, according to a preferred embodiment, the polymer shell of the thermoplastic heat-expandable microspheres of the present invention is made from ethylenically unsaturated monomers including acrylonitrile in an amount of 50-75 wt.%, methacrylonitrile in an amount of 15-40 wt.%, and methyl acrylate and / or methyl methacrylate in an amount of 10-30 wt.%, each based on the total weight of the ethylenically unsaturated monomers.

[0021] According to a more preferred embodiment, the polymer shell of the thermoplastic heat-expandable microspheres of the present invention is made from ethylenically unsaturated monomers including acrylonitrile in an amount of 53-70% by weight, methacrylonitrile in an amount of 20-35% by weight, and methyl acrylate and / or methyl methacrylate in an amount of 12-25% by weight, each based on the total weight of the ethylenically unsaturated monomers.

[0022] According to an even more preferred embodiment, the polymer shell of the thermoplastic heat-expandable microspheres of the present invention is made from ethylenically unsaturated monomers including acrylonitrile in an amount of 55-65% by weight, methacrylonitrile in an amount of 22-30% by weight, and methyl acrylate and / or methyl methacrylate in an amount of 13-23% by weight, each based on the total weight of the ethylenically unsaturated monomers.

[0023] According to a particularly preferred embodiment, the polymer shell of the thermoplastic heat-expandable microspheres of the present invention is made from ethylenically unsaturated monomers including acrylonitrile in an amount of 57-61 wt.%, methacrylonitrile in an amount of 23-28 wt.%, and methyl acrylate and / or methyl methacrylate in an amount of 14-20 wt.%, each based on the total weight of the ethylenically unsaturated monomers.

[0024] Surprisingly, it has been found that this particular combination of specific monomers and ranges of amounts thereof provides a polymer mixture for the polymer shell suitable for providing desirable properties such as low expansion temperature and at the same time excellent barrier properties and good long term stability of the expandable microspheres obtained from the expandable microspheres having a polymer shell comprising this particular polymer mixture.

[0025] In a further preferred embodiment, the polymer shell of the thermoplastic heat-expandable microspheres of the present invention is made from ethylenically unsaturated monomers, including methyl acrylate, either in the amounts in the ranges specified above for methyl acrylate and / or methyl methacrylate.

[0026] In a further preferred embodiment, the ethylenically unsaturated monomer is substantially free of VDC. If included, the amount of VDC is less than 5% by weight, most preferably less than 2% by weight, or even less than 1% by weight of the ethylenically unsaturated monomer, such as less than 0.5% by weight, or even less than 0.1% by weight of the ethylenically unsaturated monomer. It is further preferred that the ethylenically unsaturated monomer is substantially free of halogen-containing monomer. If included, the amount of halogen-containing monomer is preferably less than 5% by weight, most preferably less than 2% by weight, or even less than 1% by weight of the ethylenically unsaturated monomer, such as less than 0.5% by weight, or even less than 0.1% by weight of the ethylenically unsaturated monomer. In some embodiments, the ethylenically unsaturated monomer is completely free of any VDC and / or halogen-containing monomer.

[0027] In a further preferred embodiment, the ethylenically unsaturated monomer comprises more methacrylonitrile than methyl acrylate and / or methyl methacrylate by weight. Particularly preferably, the ethylenically unsaturated monomer comprises more methacrylonitrile than methyl acrylate by weight. For example, the ethylenically unsaturated monomer comprises at least 1% by weight more methacrylonitrile than methyl acrylate and / or methyl methacrylate by weight, preferably at least 2% by weight more, more preferably at least 3% by weight more, most preferably at least 5% by weight more methacrylonitrile. It has been found that such an excess weight of methacrylonitrile compared to methyl acrylate further improves the storage stability of the expanded microspheres.

[0028] The ethylenically unsaturated monomer may include additional monomers, for example, in an amount of up to 20% by weight, for example 0-15% by weight, or 0.1-12% by weight, preferably up to 10% by weight, for example 0.2-8% by weight, and more preferably up to 5% by weight, for example up to 2% by weight, each based on the total weight of the ethylenically unsaturated monomers. Suitable additional monomers include, for example, (meth)acrylates, vinyl esters, styrenes (such as styrene and α-methylstyrene), nitrile-containing monomers, (meth)acrylamides, vinyl ethers (such as methyl vinyl ether and ethyl vinyl ether), N-substituted maleimides, dienes (such as butadiene and isoprene), vinylpyridines, and any combination thereof.

[0029] In a further embodiment, the ethylenically unsaturated monomers may include, as an additional monomer, a lactone according to formula (1): [ka] In the formula, R1, R2, R3, and R4 are each independently selected from the group consisting of H and an alkyl group. The alkyl group preferably contains 1 to 4 carbon atoms. Particularly preferred alkyl groups are methyl and ethyl. More preferably, R1, R2, R3, and R4 are each independently selected from the group consisting of H and CH3.

[0030] In a preferred embodiment, R1, R2, R3, and R4 in formula (1) are selected as follows: R1 = H, R2 = H, R3 = CH3, R4 = H (same as α-methylene-γ-valerolactone (MVL) and γ-methyl-α-methylene-γ-butyrolactone), R1 = H, R2 = H, R3 = H, R4 = H (α-methylene-γ-butyrolactone (MBL)), R1=CH3, R2=H, R3=H, R4=H (β-methyl-α-methylene-γ-butyrolactone (MMBL)), or R1 = H, R2 = H, R3 = CH3, R4 = CH3 (γ,γ-dimethyl-α-methylene-γ-butyrolactone).

[0031] When the ethylenically unsaturated monomer comprises a lactone according to formula (1), the lactone is most preferably either MVL or MBL.

[0032] In a further embodiment, the ethylenically unsaturated monomers may include, as an additional monomer, an itaconate dialkyl ester according to formula (2): [ka] In the formula, each of R1 and R2 is preferably an alkyl group having 1 to 4 carbon atoms, independently of each other. Suitable alkyl groups include methyl, ethyl, n-propyl, isopropyl, and butyl. In particular, the itaconate dialkyl ester is preferably selected from the group consisting of dimethyl itaconate (DMI), diethyl itaconate (DEI), di(n-propyl) itaconate, diisopropyl itaconate, and dibutyl itaconate (DBI).

[0033] In a further embodiment, the ethylenically unsaturated monomers may include, as an additional monomer, a monomer of formula (3). [ka] In the formula, A 1 ~A 12 each is independently selected from H and C1-C4 alkyl; 1~4 The alkyl group is optionally selected from halogen, hydroxyl and C 1~4 and alkoxy, X is a bridging group selected from -O-, -NR"-, -S-, -OC(O)-, -NR"C(O)-, -SC(O)-, -C(O)O-, -C(O)NR"-, and -C(O)S-, the group C(O) representing a carbonyl group C=O, R" is H or C(O) optionally substituted with one or more substituents selected from halogen and hydroxy. 1-2 It is an alkyl. When the ethylenically unsaturated monomer comprises a monomer of formula (3), in a preferred embodiment, A 12 is H. In another preferred embodiment, A 12 is optionally selected from halogen, hydroxy, and C 1~4 alkoxy, C 1~ It is selected from C4 alkyl, preferably methyl. Most preferably, when the ethylenically unsaturated monomer comprises a monomer of formula (3), the monomer of formula (3) is tetrahydrofuryl (meth)acrylate or tetrahydrofuryl acrylate.

[0034] In a further preferred embodiment, the ethylenically unsaturated monomers include small amounts of one or more crosslinking multifunctional monomers, such as divinylbenzene, ethylene glycol di(meth)acrylate, di(ethylene glycol) di(meth)acrylate, triethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, glycerol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, and the like. acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, triallyl formal tri(meth)acrylate, allyl methacrylate, trimethylolpropane tri(meth)acrylate, tributanediol di(meth)acrylate, PEG#200 di(meth)acrylate, PEG#400 di(meth)acrylate, PEG#600 di(meth)acrylate, 3-acryloyloxyglycol monoacrylate, triacrylformal, triallyl isocyanate, and triallyl isocyanurate. Particularly preferred are crosslinking monomers that are at least trifunctional, examples of which include pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tolylformal tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, triacrylformal, tolyl isocyanate, and tolyl isocyanurate. The amount of crosslinking functional monomer may be, for example, 0.1 to 6% by weight, or 0.1 to 1% by weight, or 1 to 3% by weight of the ethylenically unsaturated monomer, and when one or more polyfunctional monomers are at least trifunctional, 0.1 to 1% by weight is particularly preferred, and when one or more polyfunctional monomers are bifunctional, 1 to 3% by weight is particularly preferred.When ethylenically unsaturated monomers other than acrylonitrile, methacrylonitrile, methyl acrylate and / or methyl methacrylate, and mixtures thereof, and one or more crosslinking polyfunctional monomers are included, the amount is preferably 0-6% by weight, most preferably 0-5% by weight. Examples of such other types of monomers that may be included include nitrile-containing monomers (such as α-ethoxyacrylonitrile, fumaronitrile, or crotonitrile), vinylpyridines, vinyl esters (such as vinyl acetate), styrenes (such as styrene, halogenated styrene, or α-methylstyrene), dienes (such as butadiene, isoprene, and chloroprene), unsaturated carboxylic acid compounds (such as acrylic acid, methacrylic acid, and salts thereof), or other unsaturated monomers (such as acrylamide, methacrylamide, or N-substituted maleimide).

[0035] In some embodiments, the ethylenically unsaturated monomers used to prepare the thermoplastic heat-expandable microspheres of the present invention comprise less than 5% by weight, preferably less than 2% by weight, and even more preferably less than 1% by weight of halogen-containing monomers, the weight percentage being based on the total weight of the ethylenically unsaturated monomers. In some embodiments, the ethylenically unsaturated monomers are substantially free of halogen-containing monomers.

[0036] In a more preferred embodiment, the ethylenically unsaturated monomers consist essentially of acrylonitrile, methacrylonitrile, methyl acrylate and / or methyl methacrylate, and mixtures thereof, and optionally one or more crosslinking multifunctional monomers, each in the respective amounts specified above. In a particular embodiment, the ethylenically unsaturated monomers consist essentially of acrylonitrile, methacrylonitrile, methyl acrylate and / or methyl methacrylate, and mixtures thereof, and one or more crosslinking multifunctional monomers, each in the respective amounts specified above. In a further particular embodiment, the ethylenically unsaturated monomers consist essentially of acrylonitrile, methacrylonitrile, methyl acrylate, and one or more crosslinking multifunctional monomers, each in the respective amounts specified above.

[0037] Thermoplastic heat expandable microspheres are hollow, the shell comprises a polymer made from the ethylenically unsaturated monomers described above, and the hollow center or core comprises one or more propellants. For expandable microspheres, the density is typically less than 1 g / cm. 3 and preferably 0.005 to 0.8 g / cm 3 , or 0.01 to 0.6 g / cm 3 In a preferred embodiment, the density of the expandable microspheres is in the range of 0.01 to 0.4 g / cm 3 At higher densities, especially at 1 g / cm 3 A density above this generally means that the microsphere sample is not suitable for use.

[0038] The propellant is preferably a hydrocarbon or mixture of hydrocarbons having a boiling point below the softening point of the thermoplastic polymer shell. The boiling point at atmospheric pressure is preferably in the range of -50 to 100°C, most preferably -20 to 50°C, and most preferably -20 to 30°C. The propellant may consist essentially of at least one of methane, ethane, propane, isobutane, n-butane, and neopentane, and may further comprise one or more additional hydrocarbons, for example in an amount of 0 to 50% by weight of the propellant. Examples of such hydrocarbons include n-pentane, isopentane, cyclopentane, hexane, isohexane, neo-hexane, cyclohexane, heptane, isoheptane, octane, and isooctane. Alternatively, other hydrocarbon types such as petroleum ether, or chlorinated or fluorinated hydrocarbons such as methyl chloride, methylene chloride, dichloroethane, dichloroethylene, trichloroethane, trichloroethylene, trichlorofluoromethane, perfluorinated hydrocarbons, fluorine-containing ethers, etc. may be used. In a preferred embodiment, the propellant comprises at least one of propane, isobutane, and n-butane, alone or in a mixture with one or more other hydrocarbons. More preferably, the propellant consists of at least one of propane, isobutane, and n-butane. Even more preferably, the propellant comprises isobutane. Most preferably, the propellant consists of isobutane. The amount of isobutane in the propellant is preferably 50-100% by weight, most preferably 75-100% by weight, for example 75-99% by weight.

[0039] The thermoplastic heat-expandable microspheres include a propellant in an amount of 5-17% by weight based on the total weight of the thermoplastic heat-expandable microspheres. Preferably, the thermoplastic heat-expandable microspheres include a propellant in an amount of 7-16% by weight, such as 9-15% by weight, and most preferably 10-14% by weight, based on the total weight of the thermoplastic heat-expandable microspheres.

[0040] Surprisingly, by using such extremely low amounts of propellant in the unexpanded expandable microspheres, relative to the total weight of the thermoplastic heat expandable microspheres, in combination with the specific combination of ethylenically unsaturated monomers in the amounts specified above for the microsphere shell, it is possible to obtain expanded microspheres that, on the one hand, have excellent barrier properties, and good storage stability, while at the same time, are still expandable to meet the commercial requirements for expandable microspheres.

[0041] Determining the weight of the propellant in the microsphere can be accomplished by measuring the volatile content of the microsphere (i.e., the weight of the volatile material, i.e., the propellant, encapsulated in the microsphere). Thus, when used herein in the context of microspheres, the terms "weight of the propellant" or "weight percentage of the propellant" are considered equivalent and are used interchangeably. Determining the volatile content of a microsphere is well known to those skilled in the art, and in principle, any suitable method for determining the volatile content of a microsphere can be used.

[0042] For example, the propellant content of the microspheres can be determined using gas chromatography techniques, in which the microspheres are placed in a sealed gas-tight vial and heated to release the encapsulated propellant, and a gas phase sample is introduced into a gas chromatograph, which quantifies the content of specific hydrocarbons.

[0043] In the present invention, the temperature at which the thermally expandable microspheres begin to expand, T Start For example, the thermally expandable microspheres can be expanded at a temperature of 50°C to less than 150°C, T Start However, it is preferred that the microspheres be expanded using an aqueous wetting method. Start The temperature at which the expansion starts is preferably 60 to 120° C., for example, 70 to 110° C., or 80 to 105° C.Start The temperature at which maximum expansion is reached is called T max It is called. Start and T Max may be determined using standard measurement techniques commonly known by those skilled in the art. For example, T Start and T Max can be determined in a heating experiment, for example, using a Mettler-Toledo thermomechanical analyzer, such as a Mettler-Toledo TMA / SDTA 841e, using a heating rate of 20° C. / min and a load (net) of 0.06 N. In such a heating experiment, a sample of known weight of thermally expandable microspheres is heated at a constant heating rate of 20° C. / min under a load (net) of 0.06 N. As the thermally expandable microspheres begin to expand, the volume of the sample increases and the load moves upward. From such measurements, an expansion thermogram is obtained, where the vertical axis represents the height to which the load is moved upward and the horizontal axis represents the temperature. T Start and T Max can be determined from this expansion thermogram using, for example, STARe software from Mettler-Toledo.

[0044] In a further preferred embodiment, the thermoplastic heat-expandable microspheres have an average particle size of 5 to 30 μm, preferably 7 to 28 μm, more preferably 8 to 25 μm, and most preferably 10 to 20 μm. When using certain combinations of monomers and their amounts relative to the amount of polymer shell and propellant, it has been found that such very low average particle sizes are particularly suitable for obtaining expandable microspheres that expand easily, have excellent barrier properties, and have good storage stability after expansion.

[0045] In further embodiments, the polymer shell may include particles to improve the mechanical properties and gas barrier of the polymer shell, thus acting as polymer shell enhancers. Examples of such particles include various types of clays, such as talc, montmorillonite, nanocrystalline cellulose, and bentonite.

[0046] Apart from the polymer shell and the propellant, the microspheres may contain further substances, which are usually added during their manufacture in an amount of 0-20% by weight, preferably 1-10% by weight. Examples of such substances include solid suspending agents, such as one or more of starch, cross-linked polymers, gum agar, derivatized celluloses, such as methylcellulose, hydroxypropylmethylcellulose, hydroxyethylcellulose, and carboxymethylcellulose, silica, colloidal clays, such as chalk and bentonite, and / or one or more salts, oxides, or hydroxides of metals, such as Al, Ca, Mg, Ba, Fe, Zn, Ni, and Mn, such as one or more of calcium phosphate, calcium carbonate, magnesium hydroxide, barium sulfate, calcium oxalate, and hydroxides of aluminum, iron, zinc, nickel, or manganese. If present, these solid suspending agents are usually mainly located on the outer surface of the polymer shell. However, even if a suspending agent is added during the manufacture of the microspheres, it is washed out at a later stage and therefore may be substantially absent from the final product.

[0047] A number of factors can result in high density. For example, high density can be the result of insufficient microsphere yield, i.e., the proportion of microspheres in the polymeric material is too low to reduce the overall density to an acceptable level. Another problem is insufficient expansion properties, which can result in many microspheres containing insufficient propellant to allow adequate expansion. This can result from the polymer shell being too permeable to the propellant, or from the formation of so-called "multicore" microspheres, i.e., instead of a single propellant-containing core, there are multiple propellant-containing cores within the shell (e.g., like a microsphere, foam, or sponge). In such multicore microspheres, the concentration of propellant is typically too low to adequately reduce the density. Another cause is polymer agglomeration or aggregation, resulting in poorly manufactured microspheres and higher density materials. Microspheres with too high agglomerated material or that do not expand sufficiently can also result in large inhomogeneities in the expansion properties of the resulting microsphere product. This is particularly undesirable for surface sensitive applications such as coatings where a smooth finish is desired.

[0048] Exemplary cross-sections of single-core and multicore microspheres are provided in Figures 1A and 1B, respectively, where polymeric regions 1 are represented by cross-hatched areas and propellant-containing regions 2 are represented by blank areas.

[0049] In a second aspect, the present invention provides a process for preparing thermoplastic heat-expandable microspheres comprising a polymer shell and a propellant, the process comprising polymerizing ethylenically unsaturated monomers in the presence of a propellant in a polymerization mixture, the ethylenically unsaturated monomers comprising acrylonitrile in an amount of 45-80 wt%, methacrylonitrile in an amount of 10-45 wt%, methyl acrylate and / or methyl methacrylate in an amount of 5-35 wt%, and the propellant comprises at least one of propane, isobutane, and n-butane and is present in an amount of 5-30 wt%, based on the total weight of the ethylenically unsaturated monomers and the propellant. The process according to the second aspect of the present invention can be used to prepare thermoplastic heat-expandable microspheres according to the first aspect of the present invention.

[0050] The method comprises polymerizing, preferably in aqueous suspension, an ethylenically unsaturated monomer as described above in the presence of a propellant as described above to obtain microspheres comprising a polymeric shell encapsulating the propellant. The above description of the expandable microspheres with respect to the type and amount of monomer, as well as any further additives as described above, such as crosslinkers, equally applies to the method of this second aspect of the invention.

[0051] In the method according to the second aspect of the invention, the propellant comprises at least one of propane, isobutane, and n-butane, for example in an amount of 50-100% by weight, or 50-99% by weight, of the total propellant amount. In some embodiments, the propellant consists of propane, isobutane, n-butane, and mixtures thereof. In preferred embodiments, the propellant comprises isobutane, for example in an amount of 50-100% by weight, or 50-99% by weight, of the total propellant amount. In particularly preferred embodiments, the propellant consists of isobutane.

[0052] In the process according to the second aspect of the present invention, the propellant is present in the polymerization mixture in an amount of from 5 to 30% by weight, for example, from 7 to 27% by weight, or from 10 to 25% by weight, or from 12 to 22% by weight, preferably from 15 to 20% by weight, based on the total weight of the ethylenically unsaturated monomer and the propellant.

[0053] In principle, any known common method for preparing expandable microspheres can be used.Suitable methods include, for example, suspension polymerization.For example, the method may follow the method described in US Pat. No. 3,615,972 or International Patent Publication No. 2019 / 043235 A1.

[0054] In one embodiment of the present invention, the microspheres are produced in a batch process, and the polymerization may then be carried out in a reaction vessel as described below. 100 parts by weight of a monomer phase (preferably comprising monomer and propellant, in a ratio that determines the proportion of monomer in the polymer shell and the amount of propellant in the final product), preferably one or more polymerization initiators in an amount of 0.1-5 parts by weight, preferably an aqueous phase in an amount of 100-800 parts by weight, and preferably one or more solid colloidal suspending agents in an amount of 1-20 parts by weight are mixed and homogenized. The size of the resulting droplets of the monomer phase determines the size of the final expandable microspheres. The temperature is preferably maintained at 40-90°C, preferably 50-80°C, while the preferred pH depends on the suspending agent used. For example, a high pH, ​​preferably 5-12, most preferably 6-10, is suitable when the suspending agent is selected from one or more of the salts, oxides, or hydroxides of metals such as Ca, Mg, Ba, Zn, Ni, and Mn, e.g., calcium phosphate, calcium carbonate, magnesium hydroxide, magnesium oxide, barium sulfate, calcium oxalate, and hydroxides of zinc, nickel, or manganese. A low pH, preferably 1-6, most preferably 3-5, is suitable when the suspending agent is selected from the group consisting of starch, methylcellulose, hydroxypropylmethylcellulose, hydroxypropylmethylcellulose, carboxymethylcellulose, gum agar, silica, colloidal clay, or oxides or hydroxides of aluminum or iron. Each of the above agents has a different optimum pH, depending, for example, on solubility data.

[0055] The suspending agent serves to stabilize droplets of the ethylenically unsaturated monomer containing organic phase in the aqueous phase and, in embodiments, assists in forming an emulsion of the organic phase (i.e., an oil-in-water emulsion) in the aqueous phase.

[0056] Stabilization of the droplets or emulsion droplets is preferred for several reasons. Without stabilization, coalescence of droplets containing ethylenically unsaturated monomers and propellants can occur. Coalescence can have adverse effects, such as non-uniform droplet size, poor microsphere yield, and can increase microsphere agglomeration.

[0057] The suspending agent is typically present in the aqueous phase in an amount of 0 to 20% by weight, for example 0.01 to 20% by weight, 0.05 to 10% by weight, 0.1 to 5% by weight, in a further embodiment the suspending agent is present in the aqueous phase in an amount of 0.1 to 1% by weight.

[0058] The choice of suspending agent is not particularly limited, but may be selected from inorganic or organic suspending agents.

[0059] Examples of inorganic materials that may act as suspending agents include silica, particularly colloidal silica, which may be used in an unmodified "bare" form or, optionally, surface modified to adjust its hydrophobic / hydrophilic properties, for example, using organosilane-modified silica or colloidal silica.

[0060] In embodiments, the “organic” group in the organosilane is C 1~20 Alkyl, C 1~20 Alkenyl, C 5~6 Aryl and C having one or more (e.g., 1 to 3) heteroatoms selected from O, S, and N 5-6 Each of these groups may be optionally selected from halide, hydroxy, epoxy, thiol, amino, C 1~20 Alkylamino, Di-C 1~20 Alkylamino, Hydroxyamino, Hydroxy-C 1~20 Alkylamino, (hydroxy-C 1~20 Alkyl)(C 1~20 Alkyl)amino, di(hydroxy-C 1~20 Alkyl)amino C 1-20 Alkoxy, C 1~20 Amide, C 1~20 Ureid, C1~20 Mercapto, C 3~20 Epoxyalkoxy, C 1~20 It may be substituted with one or more groups selected from alkyl acrylates, ethylene glycol or its oligomers having 1 to 20 ethylene glycol groups, and propylene glycol or its oligomers having 1 to 20 propylene glycol groups. Any aliphatic groups may be linear, branched, or cyclic.

[0061] Organosilane-modified silica or colloidal silica is prepared by dissolving silica (or colloidal silica) in a solvent, typically represented by the formula: n Six 4-n where R is one of the organic groups identified above and X is a halide, hydroxy, or C 1~6 alkoxy, where n is an integer in the range of 1 to 3, typically 1 or 2.

[0062] Suitable silane compounds include tris-(trimethoxy)silane, octyltriethoxysilane, methyltriethoxysilane, methyltrimethoxysilane, gamma-mercaptopropyltrimethoxysilane, beta-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, epoxy groups (epoxy silanes), glycidoxy groups, and / or glycidoxypropyl groups, such as gamma-glycidoxypropyltrimethoxysilane, gamma-glycidoxypropylmethyldiethoxysilane, (3-glycidoxypropyl)trimethoxysilane, (3-glycidoxypropyl)hexyltrimethoxysilane, beta-(3,4-epoxycyclohexyl)-ethyltriethoxysilane, silanes containing glycidoxypropyl groups, vinyl groups, such as vinyltriethoxysilane, vinyltrimethoxysilane, vinyltris-(2-methoxyethoxy)silane, vinylmethyldi ... Examples of suitable silanes include silanes containing vinyl groups, such as silanes of ...

[0063] Examples of silica that can be used include silica sold under the trade names Levasil®, Bindzil®, and Ludox®, which are related to colloidal silica.Solid forms of silica include fumed silica, and precipitated silica may also be used, which can be dispersed in water to form a fine suspension.Sources of fumed silica include silica sold under the trade names Cab-o-Sil®, and Aerosil®.

[0064] Other inorganic suspending agents include colloidal clays (e.g., chalk and bentonite), and salts, oxides, and hydroxides of Al, Ca, Mg, Ba, Fe, Zn, Ti, Ni, and Mn (e.g., calcium phosphate, calcium carbonate, magnesium hydroxide, barium sulfate, calcium oxalate, titanium dioxide, and hydroxides of aluminum, iron, zinc, nickel, or manganese).

[0065] When solid inorganic suspending agents are used, they can produce so-called "Pickering" emulsions, in which the solid inorganic particles are at the interface between the aqueous and organic phases. One or more suspending agents may be used. Mixtures of organic and inorganic suspending agents may also be used.

[0066] To enhance the effect of the suspending agent, a small amount, for example, 0.001 to 1% by weight, of one or more promoters may be added. Typically, such promoters are organic substances, and may be selected from one or more of water-soluble sulfonated polystyrene, alginate, carboxymethylcellulose, tetramethylammonium hydroxide or tetramethylammonium chloride, or water-soluble complex resinous amine condensates (e.g., water-soluble condensates of diethanolamine and adipic acid, water-soluble condensates of ethylene oxide, etc.), urea and formaldehyde, polyethyleneimine, polyvinyl alcohol, polyvinylpyrrolidone, polyvinylamine, amphoteric substances such as proteinaceous substances (e.g., gelatin, glue, casein, albumin, glutin, and the like), nonionic substances such as methoxycellulose, ionic substances usually classified as suspending agents (e.g., soaps, alkyl sulfates, and sulfonates, etc.), and long-chain quaternary ammonium compounds.

[0067] Conventional radical polymerization initiators are selected from one or more of organic peroxides, such as dialkyl peroxides, diacyl peroxides, peroxide esters, dicarbonate peroxides, or azo compounds. Suitable initiators include dicetyl peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, dioctanyl peroxide, dibenzoyl peroxide, dilauroyl peroxide, didecanoyl peroxide, tert-butyl peracetate, tert-butyl perlaurate, tert-butyl perbenzoate, tert-butyl hydroperoxide, cumene hydroperoxide, cumene ethyl peroxide, diisopropyl hydroxydicarboxylate, 2,2'-azo-bis(2,4-dimethylvaleronitrile), 2,2'-azobis(isobutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2' <1> -Azobis(2-methylpropionate, 2,2' <1> -azobis[2-methyl-N-(2-hydroxyethyl)propionamide], and the like. Polymerization can also be initiated using radiation, such as high-energy ionizing radiation.

[0068] Where appropriate, the microspheres may be treated at any stage to reduce the amount of residual unreacted monomer, for example by any of the procedures described in WO 2004 / 072160, or U.S. Pat. No. 4,287,308.

[0069] In a further aspect, the present invention is also directed to thermoplastic heat-expandable microspheres obtainable by the method according to the second aspect of the invention described above.

[0070] In a further aspect, the present invention is also directed to an aqueous slurry comprising expandable thermoplastic microspheres, preferably in an amount of 5-55% by weight, most preferably 20-55% by weight, based on the total weight of the slurry, obtained by the process according to the first aspect of the invention described above or according to the second aspect of the invention described above. Such a slurry is useful for various applications of expandable microspheres, including for example papermaking. The slurry also preferably comprises at least one thickening agent, preferably compatible with papermaking. Examples of such thickening agents include at least partially water soluble polymers selected from the group consisting of starches, gums, celluloses, chitins, chitosans, glycans, galactans, pectins, mannans, dextrins, copolymers made from monomers containing acrylic acid or salts thereof (preferably up to 50 mole %, most preferably up to 20 mole %, of acrylic acid or salts thereof), homopolymers and copolymers made from monomers containing esters or amides of acrylic acid, homopolymers and copolymers made from monomers containing methacrylic acid, its esters or its amides, rubber latexes and copolymers, polyvinyl esters and copolymers (e.g., containing ethylene), polyvinyl alcohols, polyamines, polyethyleneimines, polyethylene / polypropylene oxides, polyurethanes, and precondensates of aminoplasts and phenoplasts, such as urea / formaldehyde, urea / melamine / formaldehyde, or phenol / formaldehyde, and polyamidoamine epichlorohydrin resins. Examples of suitable gums include guar gum, tamarind gum, locust bean gum, tara gum, karaya, okra, acacia, xanthan gum, etc., and mixtures thereof, of which guar gum is particularly preferred. Examples of suitable celluloses include derivatives, such as optionally chemically modified CMC (carboxymethylcellulose), and cellulose ethers, such as EHEC (ethyl hydroxyethyl cellulose), and HEC (hydroxyethyl cellulose), and mixtures thereof.Chemically modified cellulose derivatives include those modified with a variety of functional groups, such as, for example, quaternary amines, other amines, sulfates, sulfonates, phosphates, phosphonates, polyethylene oxide, and polypropylene oxide.

[0071] The at least partially water-soluble polymer may be linear, branched, or crosslinked. The average molecular weight may vary within wide limits, depending on the type of polymer. In most cases, the preferred average molecular weight is at least 500, more preferably at least 2000, and most preferably at least 5000. The upper limit is not critical, and in most cases the average molecular weight is preferably at most 50,000,000, more preferably at most 10,000,000, and most preferably at most 1,000,000.

[0072] Particularly preferred polymers include starch, CMC, EHEC, guar gum, polyamidoamine epichlorohydrin resins, copolymers of acrylic acid with other monomers (e.g., with acrylamide), and homopolymers or copolymers of polyacrylamide, polyamines, polyvinyl alcohol, and polyethylene / polypropylene oxide.

[0073] The one or more at least partially water-soluble polymers effective as thickeners are preferably present in an amount that stabilizes the slurry against substantial sedimentation or suspension of the microspheres to the extent that they cannot be redispersed. In many cases, this can be achieved by adding sufficient polymer to obtain a preferred viscosity of the slurry (measured using an Anton Paar DV-1P viscometer with spindle L3) of about 150 to about 1000 mPas at 25°C, most preferably about 200 to about 600 mPas at 25°C. The amount required to stabilize the slurry depends on the polymer and other circumstances such as pH. In many cases, the preferred content of the at least partially water-soluble polymer in the slurry is about 0.1 to about 15% by weight, most preferably about 0.1 to about 10% by weight, and most preferably about 0.5 to about 10% by weight. EXAMPLES

[0074] The following examples are intended to illustrate the invention.

[0075] The propellant content in the microspheres was determined using headspace gas chromatography (HS-GC) using an Agilent 7697A static headspace connected to an Agilent 7890B gas chromatograph. 8-10 mg of sample is placed in a sealed gas-tight vial and heated to 170 °C. The sample in the gas phase is introduced by a gas-tight syringe into the gas chromatograph equipped with a CP-Sil 19cb column (30 m long, 0.32 mm inner diameter, 1 μm film thickness, Agilent). Isooctane is used as a reference and the evaluation is carried out using Chromeleon software from Thermo.

[0076] Expansion properties were evaluated using a Mettler TMA / SDTA 841e thermomechanical analyzer interfaced to a PC running STARe software. The samples to be analyzed were prepared from 0.5 mg (+ / - 0.02 mg) of thermally expandable microspheres contained in an aluminum oxide crucible with a diameter of 6.8 mm and a depth of 4.0 mm. The crucible was sealed using an aluminum oxide lid with a diameter of 6.1 mm. Using a TMA expansion probe type, the temperature of the sample was increased at 20°C / min while applying a load (net) of 0.06 N on the probe. -1 The temperature was increased from about 30°C to 240°C at a heating rate of 100°C. The vertical displacement of the probe was measured to analyze the expansion characteristics. The initial temperature of expansion (T start ): The temperature (℃) when the probe begins to displace. Maximum expansion temperature (T max ) is the temperature (°C) at which the probe displacement reaches its maximum. TMA density is calculated by multiplying the sample weight (d) by the sample volume increase (dm 3 )

[0077] Particle sizes were determined on wet samples by laser light scattering on a Malvern Mastersizer Hydro 2000 SM instrument. Median particle sizes are presented as volume median diameter d(0.5).

[0078] [Example 1] The microspheres were prepared using the following procedure. A reaction mixture containing Mg(OH)2-stabilized organic droplets in water was produced by mixing the phases and vigorously stirring until a suitable droplet size was achieved. The water dispersion contained 1.8 parts by weight of Mg(OH)2, 0.02 parts by weight of sodium 2-ethylhexyl sulfate, and 283 parts by weight of water. The organic droplets contained 2.0 parts by weight of dilauryl peroxide, 22.0 parts by weight of isobutane, 55.0 parts by weight of acrylonitrile, 30.0 parts by weight of methacrylonitrile, 15.0 parts by weight of methyl acrylate, and 0.3 parts by weight of trimethylolpropane trimethacrylate. The polymerization was carried out in a sealed reactor under stirring and at 62°C. After cooling to room temperature, a sample of the resulting microsphere slurry was removed, filtered, dehydrated, and dried before analysis by TMA and headspace gas chromatography. The microspheres contained about 14% by weight isobutane, based on the total weight of the microspheres, and had an average particle size of about 38 μm. The TMA results can be found in Table 1 below.

[0079] [Example 2] 329 parts by weight of water, 22.7 parts by weight of 50% by weight surface-modified colloidal silica (Bindzil, 80 ml) 2A dispersion containing 1.6 parts by weight of dilauryl peroxide, 38.0 parts by weight of isobutane, 55.0 parts by weight of acrylonitrile, 30.0 parts by weight of methacrylonitrile, 15.0 parts by weight of methyl acrylate, and 0.3 parts by weight of trimethylolpropane trimethacrylate was prepared and maintained at a pH of about 4.5. The aqueous dispersion was mixed with an organic phase containing 1.6 parts by weight of dilauryl peroxide, 38.0 parts by weight of isobutane, 55.0 parts by weight of acrylonitrile, 30.0 parts by weight of methacrylonitrile, 15.0 parts by weight of methyl acrylate, and 0.3 parts by weight of trimethylolpropane trimethacrylate. The polymerization was carried out in a sealed reactor under stirring and at 62° C. After cooling to room temperature, a sample of the resulting microsphere slurry was removed, filtered, dehydrated, and dried before analysis by TMA and headspace gas chromatography. The microspheres contained about 20% by weight of isobutane based on the total weight of the microspheres, isobutane, and had an average particle size of about 14 μm. The TMA results can be found in Table 1 below.

[0080] [Examples 3 to 7] Further microspheres were prepared in additional polymerization examples carried out in the same manner as Example 2. However, in these further examples, the monomers and propellants were used in the amounts specified in Table 1 below. In Example 7, 0.5 parts by weight of acetyl peroxydicarbonate was used as the initiator. Analytical results can be found in Table 1.

[0081] [Table 1]

[0082] [Storage stability test] The storage stability test was carried out as follows. Expandable microspheres were obtained from the expandable microsphere slurries obtained in Examples 1-7 by expanding in boiling water, as described, for example, in International Patent Publication No. 2014 / 198532A1. The expandable microspheres were stored in a sealed container at 40°C for at least 28 days. The initial amount of propellant contained in each expandable microsphere was determined after drying and set to 100(%). Furthermore, the amount of propellant contained in each expandable microsphere was determined after 1, 3, 7, 14, 28, and 42 days, and the relative percentage of the propellant content compared to the initial amount of propellant was calculated (in %). The results are shown in Table 2 below. As further comparative microspheres, two commercially available microspheres were used, namely, the VDC-containing benchmark expandable microsphere Expancel 461 WE 40 (Comparative Example 8) and the commercially available unexpanded VDC-free microsphere Expancel 051 DU 40 (Comparative Example 9), which were investigated after wet expansion using the same procedures as in Examples 1-7.

[0083] [Table 2]

[0084] The results of Table 2 are shown in Figure 2. Figure 2 shows that the expandable microspheres according to the invention (i.e., the microspheres from Examples 1, 3, 4, and 6) have improved storage stability properties, even when stored as wet microspheres, compared to other non-halogen-containing expandable microspheres (i.e., the microspheres of Comparative Examples 2, 5, 7, and 9), particularly after at least 28 days of storage, and even approaching or exceeding the storage stability properties of commercially available VDC-containing expandable microspheres (i.e., the microspheres of Comparative Example 8).

Claims

1. 1. A thermoplastic heat-expandable microsphere comprising a polymer shell and a propellant, the polymer shell being made from ethylenically unsaturated monomers and encapsulating the propellant, the ethylenically unsaturated monomers comprising acrylonitrile in an amount of 45-80% by weight, methacrylonitrile in an amount of 10-45% by weight, and methyl acrylate and / or methyl methacrylate in an amount of 5-35% by weight, each based on the total weight of the ethylenically unsaturated monomers, and the thermoplastic heat-expandable microspheres comprising the propellant in an amount of 5-17% by weight, based on the total weight of the thermoplastic heat-expandable microspheres.

2. 2. The thermoplastic heat-expandable microsphere according to claim 1, wherein the ethylenically unsaturated monomers each comprise acrylonitrile in an amount of 50-75% by weight, preferably 53-70% by weight, most preferably 55-65% by weight, based on the total weight of the ethylenically unsaturated monomers.

3. The thermoplastic heat expandable microsphere according to claim 1 or 2, wherein the ethylenically unsaturated monomers each comprise methacrylonitrile in an amount of 15-40% by weight, preferably 20-35% by weight, most preferably 22-30% by weight, based on the total weight of the ethylenically unsaturated monomers.

4. The thermoplastic heat-expandable microspheres according to any one of claims 1 to 3, wherein the ethylenically unsaturated monomers comprise methyl acrylate and / or methyl methacrylate in an amount of 6 to 34 wt%, for example 7 to 33 wt%, 8 to 32 wt%, or 10 to 30 wt%, preferably 12 to 25 wt%, and most preferably 13 to 23 wt%, each based on the total weight of the ethylenically unsaturated monomers.

5. The thermoplastic heat-expandable microspheres according to any one of claims 1 to 4, wherein the ethylenically unsaturated monomer comprises more methacrylonitrile than methyl acrylate and / or methyl methacrylate, by weight, preferably at least 1% by weight more methacrylonitrile than methyl acrylate and / or methyl methacrylate, by weight, and even more preferably at least 1% by weight more methacrylonitrile than methyl acrylate and / or methyl methacrylate, by weight.

6. The thermoplastic thermoexpandable microsphere according to any one of claims 1 to 5, wherein the thermoplastic thermoexpandable microsphere comprises the propellant in an amount of 7 to 16 wt%, preferably 9 to 15 wt%, most preferably 10 to 14 wt%, based on the total weight of the thermoplastic thermoexpandable microsphere.

7. The thermoplastic heat-expandable microsphere according to any one of claims 1 to 6, wherein the ethylenically unsaturated monomer comprises methyl acrylate.

8. Thermoplastic heat-expandable microspheres according to any one of claims 1 to 7, wherein the ethylenically unsaturated monomers comprise less than 5% by weight, preferably less than 2% by weight, and even more preferably less than 1% by weight of halogen-containing monomers.

9. The thermoplastic heat-expandable microsphere according to any one of claims 1 to 8, wherein the propellant comprises at least one of propane, isobutane, and n-butane, preferably isobutane.

10. The thermoplastic heat expandable microsphere according to any one of claims 1 to 9, wherein the propellant comprises 50 to 100% by weight of isobutane.

11. Thermoplastic heat expandable microspheres according to any one of claims 1 to 10, having an average particle size of 5 to 30 μm, preferably 7 to 28 μm, more preferably 8 to 25 μm, most preferably 10 to 20 μm.

12. The thermoplastic heat-expandable microsphere according to any one of claims 1 to 11, wherein the ethylenically unsaturated monomers further comprise 0.1 to 6.0 wt.% of one or more crosslinking agents, preferably 0.2 to 1.0 wt.%, each based on the total weight of the ethylenically unsaturated monomers.

13. 1. A process for preparing thermoplastic, thermally expandable microspheres comprising a polymeric shell and a propellant, comprising polymerizing ethylenically unsaturated monomers in the presence of a propellant in a polymerization mixture, the ethylenically unsaturated monomers comprising acrylonitrile in an amount of 45 to 80 weight percent, methacrylonitrile in an amount of 10 to 45 weight percent, and methyl acrylate and / or methyl methacrylate in an amount of 5 to 35 weight percent, each based on the total weight of the ethylenically unsaturated monomers, and the propellant comprises at least one of propane, isobutane, and n-butane, and is present in an amount of 5 to 30 weight percent, based on the total weight of the ethylenically unsaturated monomers and the propellant.

14. 14. The process of claim 13, wherein the polymerization mixture comprises inorganic particles, preferably magnesium hydroxide or colloidal silica, more preferably colloidal silica.

15. An aqueous slurry comprising said thermoplastic heat expandable microspheres according to any one of claims 1 to 12 or obtained from the method according to any one of claims 13 and 14.

Citation Information

Patent Citations

  • Thermally expandable microcapsule excellent in heat and solvent resistance

    JP1997019635A

  • microsphere

    JP2009526117A

  • THERMALLY EXPANSIVE THERMOPLASTIC MICROSPHERES AND METHOD FOR THEIR PREPARATION - Patent application

    JP2019528158A

  • Method for producing thermally expandable microspheres

    WO2015029916A1

  • Hollow resin particles and use of same

    WO2018025575A1