Toner for electrostatic charge image development, method for manufacturing toner for electrostatic charge image development, and image forming method

The toner composition with a binder resin and release agent addresses the challenge of low-temperature fixability and heat-resistant storage properties by enhancing dispersion and plasticization, resulting in improved image quality and stability.

JP2024162021AInactive Publication Date: 2024-11-21KONICA MINOLTA INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023077159
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing toners do not adequately address the need for improved low-temperature fixability while maintaining heat-resistant storage properties, as evidenced by the limitations in existing technologies.

Method used

A toner composition comprising a binder resin with specific structural units, including a first polymer with a branched alkyl group and a release agent, which enhances low-temperature fixability by allowing the release agent to disperse finely within the binder resin, thereby improving plasticization during heating and fixing, while maintaining the glass transition temperature to prevent extreme deterioration in heat-resistant storage properties.

Benefits of technology

The toner achieves significant improvements in low-temperature fixability while effectively suppressing the deterioration of heat-resistant storage properties, ensuring high-quality image formation and stability under varying thermal conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162021000001_ABST
    Figure 2024162021000001_ABST
Patent Text Reader

Abstract

To provide a toner for electrostatic charge image development that can sufficiently increase low temperature fixability and can prevent an excessive reduction in heat storage properties, a method for manufacturing the toner for electrostatic charge image development, and an image forming method using the toner for electrostatic charge image development.SOLUTION: A toner for electrostatic charge image development includes toner base particles including a binder resin and a mold release agent. The binder resin includes a first polymer having a first structural unit represented by the following formula (1). (In formula (1), R1 is a hydrogen atom or an alkyl group having 1 or more and 3 or less carbon atoms, and R2 is an alkyl group having 3 or more and 5 or less carbon atoms and having a branched chain.)SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner for developing electrostatic images, a method for producing a toner for developing electrostatic images, and a method for forming an image. [Background technology]

[0002] In the thermal fixing method, which is widely used as one of the toner fixing methods, in recent years, there has been a demand for reducing the thermal energy used when fixing a toner image in order to increase print speed, save energy, etc. In order to reduce the thermal energy used when fixing a toner image, there has been a demand for improving the low-temperature fixability of the toner, and methods for achieving this have been investigated.

[0003] For example, Patent Document 1 discloses a toner containing a colorant and a release agent, in which the release agent melts at a temperature of 65° C. to 90° C. and precipitates from the inside of the toner to the outside, and the colored toner particles and the release agent form a sea-island structure. Patent Document 1 claims that the above toner has improved low-temperature fixability, etc.

[0004] Patent Document 2 also describes a hybrid resin (A) of a polyester resin and a vinyl resin, and a polyolefin resin (a) having an SP value of 10.0 to 12.6 (cal / cm 3 ) 1 / 2 The toner binder contains a resin (B) having a structure in which the vinyl resin (b) is grafted, and has a crushing rate of 60% or more. Patent Document 2 states that the toner containing the toner binder has improved low-temperature fixing properties.

[0005] Patent Document 3 discloses a toner binder resin obtained by melt-kneading an amorphous resin (X) containing a specific amount of a specific monomer and having a molecular weight of 20,000 or more, an amorphous resin (Y) containing a specific amount of a specific monomer and having a molecular weight of 10,000 or more, and a crystalline resin (Z). Patent Document 3 states that a toner containing the toner binder resin achieves both low-temperature fixability and offset resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2007-279714 A [Patent Document 2] JP 2008-287229 A [Patent Document 3] JP 2010-015159 A Summary of the Invention [Problem to be solved by the invention]

[0007] Although toners having improved low-temperature fixability are known, such as those disclosed in Patent Documents 1 to 3, there is a demand for a toner with sufficiently improved low-temperature fixability.

[0008] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a toner for developing electrostatic images that can sufficiently improve low-temperature fixing property, a method for producing the toner for developing electrostatic images, and a method for forming an image using the toner for developing electrostatic images. [Means for solving the problem]

[0009] In order to achieve the above object, one aspect of the present invention relates to a toner for developing electrostatic images as set forth in the following items [1] to

[12] . [1] A toner for developing an electrostatic image, the toner comprising a binder resin and a release agent in a toner base particle, The binder resin contains a first polymer having a first structural unit represented by general formula (1), Toner for developing electrostatic images. (In the general formula (1), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and R 2 is a branched alkyl group having 3 to 5 carbon atoms. [ka] [2] In the general formula (1), R2 The toner for developing electrostatic images according to [1], wherein [3] In the general formula (1), R 1 The toner for developing electrostatic images according to [1] or [2], wherein [4] The toner for developing electrostatic images according to any one of [1] to [3], wherein the release agent is a hydrocarbon wax or a fatty acid ester wax. [5] The first polymer further has a second structural unit represented by general formula (2), or The binder resin further contains a second polymer having a second structural unit represented by general formula (2) and not having the first structural unit. The toner for developing electrostatic images according to any one of [1] to [4]. [ka] (In the general formula (2), R 3 is a hydrogen atom or an alkoxy group having 1 to 3 carbon atoms. [6] In the general formula (2), R 3 The toner for developing electrostatic images according to [5], wherein [7] The toner for developing electrostatic images according to [5] or [6], wherein in the binder resin, a content of the first structural unit is 10% by mass or more and 90% by mass or less with respect to a total mass of a content of the first structural unit and a content of the second structural unit. [8] The toner for developing electrostatic images according to any one of [5] to [7], wherein in the binder resin, a content of the first structural unit is 25% by mass or more and 80% by mass or less with respect to a total mass of a content of the first structural unit and a content of the second structural unit. [9] The electrostatic image developing toner according to any one of [5] to [8], wherein the first polymer is a copolymer further having a second structural unit represented by general formula (2).

[10] The electrostatic image developing toner according to [9], wherein the first polymer further has a third structural unit different from the first structural unit and the second structural unit.

[11] The toner for developing electrostatic images according to

[10] , wherein the third structural unit is a structural unit derived from (meth)acrylic acid or a (meth)acrylic acid ester.

[12] The toner for developing electrostatic images according to

[10] or

[11] , wherein the third structural unit is at least one structural unit derived from a compound selected from the group consisting of (meth)acrylic acid, (meth)methacrylic acid, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.

[0010] In order to achieve the above object, another aspect of the present invention relates to a method for producing a toner for developing electrostatic images as described below in

[13] .

[13] A method for producing a toner for developing an electrostatic image, the toner base particles containing a binder resin and a release agent, comprising the steps of: Providing a monomer represented by general formula (1a); and polymerizing the prepared monomer in an aqueous medium to prepare a particle dispersion of the binder resin containing a first polymer having a first structural unit. A method for producing a toner for developing electrostatic images. [ka] (In the general formula (1a), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and R 2 is a branched alkyl group having 3 to 5 carbon atoms.

[0011] In order to achieve the above object, another aspect of the present invention relates to an image forming method as described below in

[14] .

[14] A step of adhering the toner for developing electrostatic images according to any one of [1] to

[12] to a recording medium; a step of fixing the electrostatic image developing toner adhered to the recording medium; The image forming method according to claim 1, Effect of the Invention

[0012] According to the present invention, there are provided a toner for developing electrostatic images capable of sufficiently improving low-temperature fixing property, a method for producing the toner for developing electrostatic images, and a method for forming an image using the toner for developing electrostatic images. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram showing an example of an image forming apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] 1. Toner for developing electrostatic images One embodiment of the present invention relates to a toner for developing an electrostatic image (electrostatic latent image) formed on an image carrier such as a photoconductor. The toner may be a one-component developer or a two-component developer having toner base particles and carrier particles.

[0015] The electrostatic image developing toner according to this embodiment is a toner containing a binder resin and a release agent in toner base particles, and the binder resin contains a first polymer having a first structural unit represented by general formula (1).

[0016] [ka]

[0017] In the general formula (1), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and R 2 is a branched alkyl group having 3 to 5 carbon atoms.

[0018] The present inventors have discovered that by incorporating a binder resin containing the above-mentioned first polymer and a release agent into the toner base particles, it is possible to sufficiently improve low-temperature fixing ability while suppressing an extreme decrease in heat-resistant storage stability.

[0019] The first structural unit is a branched alkyl group having a side chain branched from the main chain of the first polymer and having 3 to 5 carbon atoms (R 2 ). Therefore, the first polymer has a bulky structure as a whole molecule. It is considered that this bulky structure forms minute voids in the binder resin containing the first polymer, which makes it easier for the release agent to disperse in the binder resin. Furthermore, the release agent dispersed in the binder resin exists in a finer state than when the release agent is aggregated, and therefore, when the toner is heated and fixed, the toner base particles can be sufficiently plasticized, and therefore, the toner can be fixed to the recording medium with low thermal energy.

[0020] In addition, since the first structural unit has a bulky structure having an alkyl group with a branched chain as described above, the glass transition temperature of the binder resin can be prevented from excessively decreasing compared to when the side chain branched from the main chain of the first polymer is linear, and therefore the heat-resistant storage stability of the toner can be prevented from excessively decreasing.

[0021] The toner of the present invention based on the above findings will be described in more detail below.

[0022] 1-1. Toner base particles As described above, the toner base particles contain a binder resin and a release agent.

[0023] The volume-based median diameter of the toner base particles (D 50 ) is preferably 4.0 μm or more and 10.0 μm or less, and more preferably 5.0 μm or more and 9.0 μm or less. When the volume median diameter is 4.0 μm or more, the transfer efficiency of the toner can be increased, and the image quality of halftone images can be improved. Also, when the volume average particle diameter is 10.0 μm or less, the image quality of images including thin lines and dots can be improved.

[0024] The volume average particle size of the toner base particles can be measured using a measuring device that is a particle size distribution measuring device (Coulter Multisizer 3, manufactured by Beckman Coulter, Inc.) connected to a computer system equipped with data processing software Software V3.51. Specifically, 0.02 g of a sample (toner base particles) is added to 20 mL of a surfactant solution (a surfactant solution obtained by diluting, for example, a neutral detergent containing a surfactant component 10 times with pure water in order to disperse the toner base particles), and then ultrasonic dispersion treatment is performed for 1 minute to prepare a dispersion liquid of the toner base particles. This dispersion liquid is injected with a pipette into a beaker containing an electrolyte (ISOTON II, manufactured by Beckman Coulter, Inc.) in a sample stand until the concentration displayed on the measuring device is 8%. By adjusting the concentration to this level, reproducible measurement values ​​can be obtained. In the measurement device, the number of measured particles is set to 25,000, the aperture diameter is set to 100 μm, the measurement range of 2 to 60 μm is divided into 256 parts to calculate frequency values, and the volume-based average particle diameter is calculated based on this.

[0025] 1-1-1. Binder resin In this embodiment, the binder resin includes a first polymer having the above-mentioned first structural unit.

[0026] In the general formula (1), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. From the viewpoint of making the first structural unit have a more rigid structure and increasing the glass transition temperature Tg of the first polymer, R 1 is preferably an alkyl group having 1 to 3 carbon atoms, and more preferably a methyl group. This can further improve the heat-resistant storage stability of the toner containing the first polymer. 1 When is an alkyl group having from 1 to 3 carbon atoms, the alkyl group may have a branched chain.

[0027] In the general formula (1), R 2 is a branched alkyl group having 3 to 5 carbon atoms. From the viewpoint of increasing the glass transition temperature of the first polymer and the binder resin containing the first polymer, R 2The number of carbon atoms in R is preferably 4 or more and 5 or less, and is preferably 4 (R 2 is an isobutyl group).

[0028] In addition, in the general formula (1), R 1 is a methyl group, and R 2 It is particularly preferred that is an isobutyl group.

[0029] The first polymer can be synthesized by carrying out a polymerization reaction using a monomer represented by general formula (1a). 1 and R 2 is the same as in general formula (1).

[0030] [ka]

[0031] The binder resin preferably has a second structural unit represented by general formula (2). Specifically, the first polymer is preferably a copolymer further having a second structural unit represented by general formula (2), or the binder resin preferably has the second structural unit represented by general formula (2) and further contains a second polymer having no first structural unit, and more preferably the first polymer is a copolymer further having a second structural unit represented by general formula (2). The second structure has a rigid cyclic structure, which reduces the mobility of the molecular chain of the polymer having the second structural unit. Therefore, the glass transition temperature Tg of the binder resin having the second structural unit can be increased. This can further improve the heat-resistant storage stability of the toner.

[0032] [ka]

[0033] In the general formula (2), R 3is a hydrogen atom or an alkoxy group having 1 to 3 carbon atoms. From the viewpoint of further reducing the mobility of the molecular chain of the polymer having the second structural unit and further suppressing the decrease in the glass transition temperature Tg of the binder resin, R 3 is preferably a hydrogen atom or a methoxy group, and more preferably a hydrogen atom.

[0034] The polymer having the second structural unit can be synthesized by carrying out a polymerization reaction using a monomer represented by general formula (2a). 3 is the same as in general formula (2).

[0035] [ka]

[0036] In the binder resin, the content of the first structural unit is preferably 10% by mass or more and 90% by mass or less, more preferably 25% by mass or more and 80% by mass or less, and even more preferably 30% by mass or more and 75% by mass or less, based on the total mass of the content of the first structural unit and the content of the second structural unit. It is considered that the content of the first structural unit is 10% by mass or more, so that more minute voids derived from the first structural unit are formed in the binder resin, and the release agent is more easily dispersed in the binder resin. This allows the toner base particles to be more sufficiently plasticized, and the low-temperature fixability of the toner can be more sufficiently improved. In addition, the content of the first structural unit is 90% by mass or less, so that the content of the second structural unit is more increased, the glass transition temperature of the binder resin is more increased, and the deterioration of the heat-resistant storage stability of the toner can be more suppressed.

[0037] The content of the first structural unit relative to the total mass of the content of the first structural unit and the content of the second structural unit can be calculated from the charge ratio of the monomer represented by general formula (1a) and the monomer represented by general formula (2a) used when preparing the binder resin, or can be measured by an NMR method.

[0038] Hereinafter, a case where the first polymer is a copolymer containing a first structural unit and a second structural unit, and a case where the binder resin contains a first polymer and a second polymer will be separately described.

[0039] (When the first polymer is a copolymer containing a first structural unit and a second structural unit) When the first polymer has the first structural unit and the second structural unit, the first polymer may further have a third structural unit different from the first structural unit and the second structural unit. The first polymer having the third structural unit can be synthesized by carrying out a polymerization reaction using a monomer different from the monomer represented by general formula (1a) and the monomer represented by general formula (2a).

[0040] Examples of the other monomers include styrene monomers including α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, o-acetoxystyrene, m-acetoxystyrene, and p-acetoxystyrene; Monomers having an ionically dissociable group (preferably a carboxyl group), including (meth)acrylic acid (acrylic acid and methacrylic acid), maleic acid, itaconic acid, fumaric acid, and the like; (Meth)acrylic acid esters including methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, and phenyl (meth)acrylate are included.

[0041] Among these, monomers having an ionically dissociable group and (meth)acrylic acid esters are preferred, (meth)acrylic acid and (meth)acrylic acid esters are more preferred, and (meth)acrylic acid, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are particularly preferred.

[0042] That is, the third structural unit is preferably a structural unit derived from (meth)acrylic acid or a (meth)acrylic acid ester, and particularly preferably at least one structural unit derived from a compound selected from the group consisting of (meth)acrylic acid, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.

[0043] From the viewpoint of preventing a decrease in the glass transition temperature Tg of the binder resin and further suppressing a decrease in the heat-resistant storage stability of the toner, it is preferable that the content of the structural unit derived from 2-ethylhexyl acrylate among the third structural units is 10 mass % or less with respect to the total mass of the binder resin.

[0044] When the third structural unit contains a structural unit derived from a monomer having an ionic dissociative group, the content of the structural unit derived from the monomer having an ionic dissociative group is preferably 3 mass% or more and 8 mass% or less with respect to the total mass of the content of the first structural unit, the content of the second structural unit, and the content of the third structural unit.

[0045] When the third structural unit contains a structural unit derived from a (meth)acrylic acid ester, the content of the structural unit derived from the (meth)acrylic acid ester is preferably 5% by mass or more and 50% by mass or less, more preferably 10% by mass or more and 40% by mass or less, based on the total mass of the content of the first structural unit, the content of the second structural unit, and the content of the third structural unit. The content of these structural units can be calculated from the charge ratio of the above-mentioned other monomers or measured by NMR.

[0046] The weight average molecular weight Mw of the first polymer is preferably 3500 or more and 35000 or less, more preferably 10000 or more and 30000 or less. When it is 3500 or more, the glass transition temperature Tg of the first polymer and the binder resin containing it can be further increased, and the deterioration of heat-resistant storage stability can be further suppressed. Also, when it is 35000 or less, the melt viscosity of the toner can be appropriately lowered, and the fixing property can be improved.

[0047] The method for measuring the weight-average molecular weight Mw is as follows. Using an apparatus "HLC-8220" (manufactured by Tosoh Corporation) and a column "TSKguard column + TSKgel Super HZM-M triple column" (manufactured by Tosoh Corporation), tetrahydrofuran (THF) is passed as a carrier solvent at a flow rate of 0.2 ml / min while maintaining the column temperature at 40°C, and the measurement sample is dissolved in tetrahydrofuran to a concentration of 1 mg / ml under dissolution conditions in which the measurement sample is treated for 5 minutes at room temperature (25°C) using an ultrasonic disperser. Then, the measurement sample is treated with a membrane filter having a pore size of 0.2 μm. 10 μl of the treated sample solution is injected into the apparatus together with the above carrier solvent, and the molecular weight distribution of the measurement sample is detected using a refractive index detector (RI detector). The peak molecular weight is measured from the detected molecular weight distribution.

[0048] The content of the first polymer is preferably 60% by mass or more and 100% by mass or less, and more preferably 70% by mass or more and 100% by mass or less, based on the total mass of the binder resin.

[0049] (When the binder resin contains a first polymer and a second polymer) The content of the first polymer is preferably 10% by mass or more and 90% by mass or less, and more preferably 25% by mass or more and 80% by mass or less, based on the total mass of the binder resin. By being 10% by mass or more, more voids derived from the first structural unit are formed in the binder resin, and the release agent is more dispersed in the binder resin, so that the toner can be more plasticized during fixing. This can further improve the low-temperature fixability. By being 90% by mass or less, the content of the second polymer can be increased, and the glass transition temperature of the binder resin can be further increased, thereby improving the heat-resistant storage stability.

[0050] The content of the second polymer is preferably 10% by mass or more and 90% by mass or less, and more preferably 20% by mass or more and 75% by mass or less, based on the total mass of the binder resin. By making it 10% by mass or more, the binder resin can contain more of the second structural unit, and the glass transition temperature of the binder resin can be further increased. This can further improve the heat-resistant storage stability of the toner. By making it 90% by mass or less, the content of the first polymer can be increased, and the low-temperature fixability can be further improved.

[0051] (others) The glass transition temperature Tg of the binder resin is preferably 25° C. or higher and 65° C. or lower, and more preferably 35° C. or higher and 55° C. or lower. When the glass transition temperature Tg is 25° C. or higher, the deterioration of the heat-resistant storage stability of the toner can be further suppressed. Also, when the glass transition temperature Tg is 65° C. or lower, the low-temperature fixability of the toner can be further improved.

[0052] The glass transition temperature Tg can be measured using a differential scanning calorimeter "Diamond DSC" (manufactured by PerkinElmer) under heating and cooling conditions with a temperature increase and decrease rate of 10°C / min and a temperature increase range of 0°C to 150°C.

[0053] The binder resin may contain other known resins in addition to the first polymer (and the second polymer).

[0054] The other resin may be a thermoplastic resin or a thermosetting resin, but is preferably a thermoplastic resin.

[0055] Examples of the thermoplastic resin include vinyl resins other than the first polymer and the second polymer, polyester resins, silicone resins, olefin resins, polyamide resins, and epoxy resins.

[0056] The other resin may be an amorphous resin, a crystalline resin, or a composite resin in which a crystalline resin and an amorphous resin are hybridized. Among these, the crystalline resin is preferred from the viewpoint of further improving low-temperature fixability.

[0057] In this specification, the term "crystalline resin" refers to a resin whose melting point is observed in a measurement by differential scanning calorimetry (DSC). In addition, the term "amorphous resin" refers to a resin whose melting point is not observed in a measurement by DSC. In addition, in this specification, "a resin whose melting point is observed" refers to a peak whose half-width of the endothermic peak is within 15°C when measured by DSC at a heating rate of 10°C / min.

[0058] As the crystalline resin, a known crystalline resin can be used. Examples of the crystalline resin include a crystalline polyester resin, a crystalline polyurethane resin, a crystalline polyurea resin, a crystalline polyamide resin, and a crystalline polyether resin. Among these, a crystalline polyester resin is preferred.

[0059] The crystalline polyester resin is obtained by a dehydration condensation reaction between a polycarboxylic acid and a polyhydric alcohol.

[0060] The polycarboxylic acid may be a divalent or higher carboxylic acid, and may be a trivalent or higher carboxylic acid such as trimellitic acid or pyromellitic acid. Among these, dicarboxylic acids are preferred from the viewpoint of increasing the crystallinity of the crystalline polyester. Examples of dicarboxylic acids include aliphatic carboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid (dodecanedioic acid), 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid, as well as aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, t-butylisophthalic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-biphenyldicarboxylic acid.

[0061] The polyhydric alcohol may be a dihydric or higher alcohol, and may be a trihydric or higher alcohol such as glycerin, pentaerythritol, trimethylolpropane, sorbitol, etc. Among these, dihydric alcohols are preferred from the viewpoint of increasing the crystallinity of the crystalline polyester. Examples of the dihydric alcohol include aliphatic diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,20-eicosanediol, diols having an unsaturated double bond such as 2-butene-1,4-diol, 3-hexene-1,6-diol, and 4-octene-1,8-diol, and diols having a sulfonic acid group.

[0062] The weight average molecular weight (Mw) of the crystalline polyester is preferably 5000 or more and 50000 or less. The number average molecular weight (Mn) of the crystalline polyester is preferably 2000 or more and 10000 or less. When the weight average molecular weight (Mw) and number average molecular weight (Mn) of the crystalline polyester are within the above ranges, the low temperature fixability is improved.

[0063] The content of the other resins is preferably from 0% by mass to 50% by mass, and more preferably from 0% by mass to 25% by mass, based on the total mass of the binder resin.

[0064] 1-1-2. Release agent The release agent can enhance the releasability of the toner from the fixing member, etc. As described above, in this embodiment, the release agent is dispersed in the binder resin and can sufficiently plasticize the toner when the toner is heat-fixed. The release agent is preferably a wax.

[0065] Examples of wax release agents include hydrocarbon waxes, including polyethylene waxes, paraffin waxes, microcrystalline waxes, and Fischer-Tropsch waxes; Dialkyl ketone waxes, including distearyl ketone, fatty acid ester waxes including carnauba wax, montan wax, behenic acid behenate, behenyl behenate, trimethylolpropane tribehenate, pentaerythritol tetramyristate, pentaerythritol tetrastearate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18-octadecanediol distearate, tristearyl trimellitate, and distearyl maleate; amide waxes, including ethylenediamine dibehenylamide, and trimellitic acid tristearylamide, and the like.

[0066] Among these, from the viewpoint of further improving low-temperature fixability, the release agent is preferably a hydrocarbon wax or a fatty acid ester wax, and more preferably a fatty acid ester wax, which allows the release agent to be more finely dispersed in the binder resin, thereby more sufficiently plasticizing the toner base particles and further improving low-temperature fixability.

[0067] The content of the release agent is preferably 1% by mass or more and 25% by mass or less, more preferably 5% by mass or more and 20% by mass or less, based on the total mass of the toner base particles. When the content of the release agent is 1% by mass or more, the toner can be more plasticized during heat fixing of the toner, so that the low-temperature fixability can be more sufficiently improved. When the content of the release agent is 25% by mass or less, a sufficient amount of binder resin can be contained in the toner base particles, so that the fixability of the image is sufficiently improved.

[0068] 1-1-3.Other ingredients The toner base particles may contain a colorant, a charge control agent, and the like.

[0069] The colorant may be a dye or a pigment. When the toner is a color toner that imparts a predetermined color tone to an image, the toner base particles may contain a colorant such as yellow, magenta, cyan, or black, depending on the color tone to be presented by the color toner. The toner base particles may contain only one type of colorant, or may contain a combination of multiple types of colorants.

[0070] Examples of yellow colorants include yellow dyes, including CI Solvent Yellow 19, 44, 77, 79, 81, 82, 93, 98, 103, 104, 112, and 162, and the like; and yellow pigments, including CI Pigment Yellow 14, 17, 74, 93, 94, 138, 155, 180, and 185, and the like.

[0071] Examples of magenta colorants include magenta dyes, including CI Solvent Red 1, 49, 52, 58, 63, 111, and 122, and the like; and magenta pigments, such as CI Pigment Red 5, 48:1, 53:1, 57:1, 122, 139, 144, 149, 166, 177, 178, and 222.

[0072] Examples of cyan colorants include cyan dyes, such as CI Solvent Blue 25, 36, 60, 70, 93, and 95, and cyan pigments, such as CI Pigment Blue 1, 7, 15, 15:3, 60, 62, 66, and 76.

[0073] Examples of black colorants include carbon blacks, including channel black, furnace black, acetylene black, thermal black, and lamp black; magnetic materials, including ferrite and magnetite; and iron-titanium composite oxides.

[0074] The content of the colorant is preferably 0.5% by mass or more and 20% by mass or less, more preferably 2% by mass or more and 10% by mass or less, based on the total mass of the toner base particles. When the toner is a clear toner, it is preferable that the toner base particles do not substantially contain a colorant, and the content of the colorant is preferably 0.1% by mass or less based on the total mass of the toner base particles.

[0075] The charge control agent can adjust the chargeability of the toner base particles.

[0076] Examples of the charge control agent include nigrosine dyes, metal salts of naphthenic acid or higher fatty acids, alkoxylated amines, quaternary ammonium salt compounds, azo metal complexes, metal salicylates or metal complexes thereof, and the like.

[0077] The content of the charge control agent is preferably 0.1% by mass to 10% by mass, more preferably 0.5% by mass to 5% by mass, based on the total mass of the binder resin. If an attempt is made to control the chargeability of the toner by adding an excessive amount of the charge control agent, other properties of the toner base particles may change significantly. In contrast, in this embodiment, the chargeability of the toner is adjusted by strontium titanate, so that the chargeability of the toner can be adjusted to a desired level while satisfying other required properties.

[0078] 1-2.External additives The toner base particles may contain an external additive that is added to the surface of the toner base particles as a post-treatment agent in order to enhance the fluidity, chargeability and cleanability of the toner.

[0079] The external additive preferably contains inorganic particles such as silica particles, alumina particles, zirconia particles, titanium oxide particles, strontium titanate particles, zinc oxide particles, chromium oxide particles, cerium oxide particles, antimony oxide particles, tungsten oxide particles, tin oxide particles, tellurium oxide particles, manganese oxide particles, and boron oxide particles. If necessary, these inorganic particles may be hydrophobized with a surface treatment agent such as a silane coupling agent or silicone oil.

[0080] The particle diameter of the inorganic particles is preferably 20 nm to 200 nm, more preferably 30 nm to 150 nm. The number average primary particle diameter of the external additive can be determined by binarizing image data of strontium titanate captured by a scanning electron microscope (SEM) using an image processing analyzer (LUZEX AP, manufactured by Nireco Corporation) and averaging the horizontal Feret diameters measured for 100 particles.

[0081] The external additive may also contain organic particles containing homopolymers such as styrene and methyl methacrylate, or copolymers thereof. The particle size of the organic particles is preferably 10 nm or more and 1000 nm or less in terms of the peak top particle size measured by the same method as for strontium titanate.

[0082] The external additive may also contain a lubricant such as a metal salt of a higher fatty acid. The higher fatty acid salts include stearic acid, oleic acid, palmitic acid, linoleic acid, and ricinoleic acid. Examples of metals constituting the metal salts include zinc, manganese, aluminum, iron, copper, magnesium, and calcium.

[0083] The content of the external additive is preferably from 0.05% by mass to 5.00% by mass, and more preferably from 0.10% by mass to 3.00% by mass, based on the total mass of the toner.

[0084] 1-3. Toner manufacturing method The toner can be produced by a method such as a pulverization method, an emulsion polymerization aggregation method, an emulsion aggregation method, a suspension polymerization method, a dissolution suspension method, etc. Among these, the pulverization method, the emulsion polymerization aggregation method, and the suspension polymerization method are preferred, and from the viewpoints of uniformity of particle size and controllability of shape, the emulsion polymerization aggregation method is more preferred.

[0085] The emulsion polymerization aggregation method is a method for producing a toner by carrying out a step of preparing a binder resin particle dispersion liquid, a step of preparing a release agent particle dispersion liquid as required, and a step of preparing a colorant particle dispersion liquid, mixing the obtained dispersion liquids, and aggregating the particles to a predetermined particle size. The method for producing a toner by the emulsion polymerization aggregation method will be described below.

[0086] (Step of Preparing Binder Resin Particle Dispersion) In this step, a dispersion of binder resin particles containing the above-mentioned first polymer is prepared. Specifically, a monomer represented by general formula (1a) is prepared, and the prepared monomer, and if necessary, a monomer represented by general formula (2a) and other monomers are added to an aqueous medium containing a polymerization initiator, and a polymerization reaction is carried out under heating and stirring to prepare a dispersion of binder resin particles. In this specification, the term "aqueous medium" refers to a solvent containing at least 50% by mass of water. Examples of components other than water in the aqueous medium include methanol, ethanol, isopropanol, acetone, dimethylformamide, methyl cellosolve, and tetrahydrofuran.

[0087] Examples of the polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate, azobisaminodipropane acetate, azobiscyanovaleric acid and its salts, hydrogen peroxide, and the like.

[0088] In order to improve the dispersibility of the oil droplets, a surfactant may be added to the aqueous medium in advance. Examples of the surfactant include anionic surfactants such as polyoxyethylene (2) dodecyl ether sodium sulfate, sodium dodecyl sulfate, and sodium dodecylbenzenesulfonate.

[0089] When the monomer is added to the aqueous medium, a chain transfer agent may be added to the aqueous medium, if necessary. Examples of the chain transfer agent include n-octyl mercaptan and n-octyl-3-mercaptopropionate.

[0090] The polymerization temperature is preferably within the range of 50° C. to 100° C., and more preferably 55° C. to 90° C. The polymerization time is preferably 1 hour to 12 hours.

[0091] The volume-based median diameter of the binder resin particles in the binder resin particle dispersion obtained in this step is preferably 30 nm or more and 300 nm or less, more preferably 50 nm or more and 250 nm or less, and even more preferably 100 nm or more and 200 nm or less. The above median diameter can be measured using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).

[0092] In this step, a release agent may be added to the aqueous medium together with the monomer.

[0093] (Step of Preparing Release Agent Particle Dispersion) In this step, a release agent is added to an aqueous medium and dispersed in the form of particles to prepare a release agent particle dispersion.

[0094] The method for dispersing the release agent in a particulate form is not particularly limited, but for example, the release agent can be dispersed using a homogenizer.

[0095] The volume-based median diameter of the release agent particles in the release agent particle dispersion liquid obtained in this step is preferably 100 nm or more and 1000 nm or less, and more preferably 200 nm or more and 700 nm or less. The median diameter of the release agent particles can be measured using a laser diffraction particle size distribution analyzer (LA-750, manufactured by Horiba, Ltd.).

[0096] (Step of Preparing Colorant Particle Dispersion) In this step, a colorant is added to an aqueous medium and dispersed in the form of particles to prepare a colorant particle dispersion.

[0097] The method for dispersing the colorant in a particulate form is not particularly limited, but for example, the colorant can be dispersed using a homogenizer.

[0098] The volume-based median diameter of the release agent particles in the colorant particle dispersion liquid obtained in this step is preferably 100 nm or more and 300 nm or less, and more preferably 50 nm or more and 200 nm or less. The median diameter of the colorant particles can be measured using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).

[0099] (Process for agglomerating resin particles) In this process, an aggregating agent is added to a binder resin particle dispersion (a mixed liquid to which a release agent particle dispersion and a colorant particle dispersion are further added as necessary), and the particles are aggregated and fused together while being heated and stirred.

[0100] Examples of the flocculant include sodium chloride, potassium chloride, lithium chloride, calcium chloride, magnesium chloride, zinc chloride, polyaluminum chloride, copper sulfate, magnesium sulfate, manganese sulfate, aluminum sulfate, etc. These flocculants can be used alone or in combination of two or more kinds.

[0101] The amount of the coagulant used is not particularly limited, but from the viewpoint of toner particle size controllability, it is preferably from 2% by mass to 30% by mass, and more preferably from 5% by mass to 20% by mass, based on the solid content of the binder resin that constitutes the toner particles.

[0102] In this step, after the addition of the flocculant, it is preferable to quickly raise the temperature by heating, and the heating rate is preferably 0.05° C. / min or more. The upper limit of the heating rate is not particularly limited, but it is preferably 15° C. / min or less from the viewpoint of suppressing the generation of coarse particles due to the rapid progress of fusion. Furthermore, after the dispersion for aggregation reaches a desired temperature, it is preferable to maintain the temperature of the dispersion for aggregation for a certain period of time, preferably until the volume-based median diameter is 4.5 μm or more and 7.0 μm or less, to continue the fusion.

[0103] After this step, the associated particles obtained in this step are aged as necessary, and then subjected to a washing / filtering step, a drying step, and an external additive addition step as necessary, to obtain a toner.

[0104] (ripening process) In this step, the dispersion liquid in which the associated particles are dispersed is heated and stirred, and an aging treatment is performed by adjusting the heating temperature, stirring speed, heating time, etc. until the shape of the associated particles has a desired circularity. The aging treatment is performed as necessary.

[0105] (Washing and filtration process) In this process, the toner particles are separated from the toner particle dispersion liquid, and the toner cake (a mass of toner particles in a wet state aggregated into a cake-like mass) obtained by solid-liquid separation is washed to remove any attached substances such as surfactants and coagulants.

[0106] The method for solid-liquid separation is not particularly limited, but examples thereof include centrifugal separation, reduced pressure filtration using a Nutsche filter or the like, and filtration using a filter press or the like.

[0107] (drying process) In this step, the washed toner cake is dried. The drying method is not particularly limited, but examples thereof include a flash jet dryer, a spray dryer, a vacuum freeze dryer, and a reduced pressure dryer.

[0108] (g) Addition of external additives This step is carried out as necessary when an external additive is added to the toner particles.

[0109] As a mixer for the external additives, a mechanical mixer such as a Henschel mixer, a coffee mill, or a sample mill can be used.

[0110] 1-4.Career The carrier is mixed with the above-mentioned toner base particles to form a two-component magnetic toner. The carrier may be any known magnetic particle that can be contained in a toner.

[0111] Examples of the magnetic particles include particles containing magnetic materials such as iron, steel, nickel, cobalt, ferrite, and magnetite, as well as alloys of these with aluminum and lead. The carrier may be a coated carrier in which the surface of a particle made of the magnetic material is coated with a resin or the like, or a resin-dispersed carrier in which the magnetic material is dispersed in a binder resin. Examples of the resin for coating include olefin resin, styrene resin, styrene-acrylic resin, silicone resin, polyester resin, and fluororesin. Examples of the binder resin include acrylic resin, styrene-acrylic resin, polyester resin, fluororesin, and phenol resin.

[0112] The average particle size of the carrier is preferably 20 μm or more and 100 μm or less, more preferably 25 μm or more and 80 μm or less, on a volume basis. The average particle size of the carrier can be measured by a laser diffraction type particle size distribution measuring device equipped with a wet disperser, such as HELOS manufactured by SYMPATEC.

[0113] The content of the carrier is preferably 2% by mass or more and 10% by mass or less with respect to the total mass of the toner base particles and the carrier.

[0114] 2. Image forming method and image forming apparatus Another embodiment of the present invention relates to an image forming apparatus including a toner image forming section that develops an electrostatic latent image with a toner to form a toner image, and a fixing device that transfers the toner image to a recording medium and fixes the toner image to the recording medium, and an image forming method using the image forming apparatus. In this embodiment, the fixing device fixes the toner to the recording medium.

[0115] The image forming apparatus may be a four-cycle type image forming apparatus consisting of four types of color developing devices, namely, yellow, magenta, cyan, and black, and one electrophotographic photosensitive member, or may be a tandem type image forming apparatus consisting of four types of color developing devices, namely, yellow, magenta, cyan, and black, and four electrophotographic photosensitive members, one for each color.

[0116] 1 is a schematic diagram showing an example of an image forming apparatus 1 according to the present embodiment. The image forming apparatus 1 shown in FIG. 1 includes an image processing section 30, an image forming section 40, a paper transport section 50, a fixing device 60, and an image reading section 70.

[0117] Image forming section 40 has image forming units 41Y, 41M, 41C, and 41K that form images using toners of the respective colors Y (yellow), M (magenta), C (cyan), and K (black). Since these have the same configuration except for the toners contained therein, hereinafter, the symbols representing the colors may be omitted. Image forming section 40 further has an intermediate transfer unit 42 and a secondary transfer unit 43. These correspond to transfer devices.

[0118] The image forming unit 41 includes an exposure device 411, a development device 412, an electrophotographic photoconductor (image carrier) 413, a charging device 414, and a drum cleaning device 415. The charging device 414 is, for example, a corona charger. The charging device 414 may be a contact charging device that charges the electrophotographic photoconductor 413 by contacting a contact charging member such as a charging roller, a charging brush, or a charging blade with the electrophotographic photoconductor 413. The exposure device 411 includes, for example, a semiconductor laser as a light source, and a light deflection device (polygon motor) that irradiates the electrophotographic photoconductor 413 with laser light according to an image to be formed. The electrophotographic photoconductor 413 is a negatively charged organic photoconductor having photoconductivity. The electrophotographic photoconductor 413 is charged by the charging device 414.

[0119] The developing device 412 is a two-component developing device. The developing device 412 has, for example, a developing container that contains a two-component developer, a developing roller (magnetic roller) that is rotatably arranged at the opening of the developing container, a partition that divides the inside of the developing container so that the two-component developer can communicate with each other, a transport roller for transporting the two-component developer on the opening side of the developing container toward the developing roller, and a stirring roller for stirring the two-component developer in the developing container. The developing container contains, for example, a two-component developer.

[0120] Intermediate transfer unit 42 has intermediate transfer belt (intermediate transfer body) 421, primary transfer roller 422 that presses intermediate transfer belt 421 against electrophotographic photosensitive body 413, multiple support rollers 423 including backup roller 423A, and belt cleaning device 426. Intermediate transfer belt 421 is stretched in a loop shape around multiple support rollers 423. Intermediate transfer belt 421 runs at a constant speed in the direction of arrow A as at least one drive roller among multiple support rollers 423 rotates.

[0121] The belt cleaning device 426 has an elastic member 426a. The elastic member 426a comes into contact with the intermediate transfer belt 421 after the secondary transfer, and removes deposits on the surface of the intermediate transfer belt 421. The elastic member 426a is made of an elastic body, and includes a cleaning blade, a brush, and the like.

[0122] The secondary transfer unit 43 has an endless secondary transfer belt 432 and a plurality of support rollers 431 including a secondary transfer roller 431A. The secondary transfer belt 432 is stretched by the secondary transfer roller 431A and the support rollers 431 in a loop shape.

[0123] The fixing device 60 has, for example, a fixing roller 62, an endless heating belt 10 that covers the outer peripheral surface of the fixing roller 62 and heats and melts the toner that constitutes the toner image on the paper S, and a pressure roller 63 that presses the paper S against the fixing roller 62 and the heating belt 10. The paper S corresponds to a recording medium.

[0124] Image forming apparatus 1 further includes an image reading section 70, an image processing section 30, and a paper transport section 50. Image reading section 70 includes a paper feeder 71 and a scanner 72. Paper transport section 50 includes a paper feed section 51, a paper discharge section 52, and a transport path section 53. Three paper feed tray units 51a to 51c that make up paper feed section 51 store paper S (standard paper, special paper) identified based on basis weight, size, etc., by preset type. Transport path section 53 includes a plurality of transport roller pairs, such as registration roller pair 53a.

[0125] The formation of an image by the image forming apparatus 1 will be described. The scanner 72 optically scans and reads the document D on the contact glass. The reflected light from the document D is read by the CCD sensor 72a and becomes input image data. The input image data is subjected to predetermined image processing in the image processing unit 30 and sent to the exposure device 411.

[0126] Electrophotographic photoreceptor 413 rotates at a constant peripheral speed. Charging device 414 uniformly charges the surface of electrophotographic photoreceptor 413 to negative polarity. In exposure device 411, a polygon mirror of a polygon motor rotates at high speed, and laser light corresponding to input image data of each color component is developed along the axial direction of electrophotographic photoreceptor 413 and irradiated onto the outer circumferential surface of electrophotographic photoreceptor 413 along the axial direction. In this way, an electrostatic latent image is formed on the surface of electrophotographic photoreceptor 413.

[0127] In the developing device 412, the toner base particles are charged by stirring and transporting the two-component developer in the developing container, and the two-component developer is transported to the developing roller, which forms a magnetic brush on the surface of the developing roller. The charged toner base particles electrostatically adhere from the magnetic brush to the electrostatic latent image on the electrophotographic photoreceptor 413. In this way, the electrostatic latent image on the surface of the electrophotographic photoreceptor 413 is visualized, and a toner image corresponding to the electrostatic latent image is formed on the surface of the electrophotographic photoreceptor 413. The term "toner image" refers to the state in which toner is gathered in the form of an image.

[0128] The toner image on the surface of the electrophotographic photoreceptor 413 is transferred to an intermediate transfer belt 421 by an intermediate transfer unit 42. Residual toner remaining on the surface of the electrophotographic photoreceptor 413 after the transfer is removed by a drum cleaning device 415 having a drum cleaning blade that is in sliding contact with the surface of the electrophotographic photoreceptor 413.

[0129] The intermediate transfer belt 421 is pressed against the electrophotographic photoreceptor 413 by the primary transfer roller 422, whereby a primary transfer nip is formed for each electrophotographic photoreceptor by the electrophotographic photoreceptor 413 and the intermediate transfer belt 421. In the primary transfer nip, toner images of each color are transferred to the intermediate transfer belt 421 in order, superimposed thereon.

[0130] Meanwhile, secondary transfer roller 431A is pressed against backup roller 423A via intermediate transfer belt 421 and secondary transfer belt 432. As a result, a secondary transfer nip is formed by intermediate transfer belt 421 and secondary transfer belt 432. Paper S passes through the secondary transfer nip. Paper S is transported to the secondary transfer nip by paper transport unit 50. Correction of the skew of paper S and adjustment of the transport timing are performed by a registration roller unit in which registration roller pair 53a is arranged.

[0131] When the paper S is transported to the secondary transfer nip, a transfer bias is applied to the secondary transfer roller 431A. By applying this transfer bias, the toner image carried on the intermediate transfer belt 421 is transferred to the paper S (a process of adhering the toner for developing an electrostatic image to a recording medium). The paper S to which the toner image has been transferred is transported by the secondary transfer belt 432 toward the fixing device 60.

[0132] Any deposits such as residual toner remaining on the surface of intermediate transfer belt 421 after the secondary transfer are removed by a belt cleaning device 426 having a cleaning blade that is in sliding contact with the surface of intermediate transfer belt 421. At this time, since the above-mentioned intermediate transfer body is used as the intermediate transfer belt, it is possible to reduce dynamic frictional force over time.

[0133] The fixing device 60 sandwiches the heating belt 10 between a rotating fixing roller 62 and a pressure roller 63 to form a fixing nip, and heats and presses the conveyed paper S in the fixing nip. In this way, the toner image is fixed to the paper S (a process of fixing the toner for developing an electrostatic image to a recording medium). The paper S with the fixed toner image is discharged outside the machine by a paper discharge section 52 equipped with a paper discharge roller 52a. EXAMPLES

[0134] The present invention will now be described with reference to examples, which should not be construed as limiting the scope of the present invention.

[0135] 1. Preparation of Resin Particle Dispersion (Binder resin particle dispersion 1) Isobutyl methacrylate (iBuMA) 42g Styrene (St) 530g n-Butyl acrylate (nBA) 217g Methacrylic acid (MAA) 46g n-Octyl-3-mercaptopropionate 5.5g A surfactant solution prepared by dissolving 8 g of sodium dodecyl sulfate in 3 L of ion-exchanged water was charged into a 5 L reaction vessel (SUS kettle) equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and the liquid temperature was raised to 80°C while stirring at a stirring speed of 230 rpm under a nitrogen stream.

[0136] After the temperature was raised, a solution of 10 g of potassium persulfate dissolved in 200 g of ion-exchanged water was added, and the liquid temperature was again raised to 80°C, and the above-mentioned monomer mixture was added dropwise over 100 minutes. After the dropwise addition, the liquid temperature was raised to 80°C, and polymerization was carried out by stirring for 2 hours, thereby preparing a binder resin particle dispersion. The volume-based median diameter of the binder resin particles in the obtained binder resin particle dispersion was 115 nm. The molecular weight of the polymer contained in the binder resin was 22,300.

[0137] The above median diameter is a value measured by dynamic light scattering using a particle size measuring device (Microtrac UPA-150, manufactured by Nikkiso Co., Ltd.).

[0138] The above molecular weight is a value measured by the following procedure. (1) Using a gel permeation chromatograph (HLC-8220, manufactured by Tosoh Corporation) and a column (TSKguard column + TSKgel Super HZM-M triple column, manufactured by Tosoh Corporation), the column temperature was maintained at 40°C, and tetrahydrofuran (THF) was passed as a carrier solvent at a flow rate of 0.2 ml / min. The measurement sample was dissolved in tetrahydrofuran to a concentration of 1 mg / ml under dissolution conditions in which the sample was treated for 5 minutes at room temperature (25°C) using an ultrasonic disperser. (2) Next, the sample solution was obtained by processing it through a membrane filter with a pore size of 0.2 μm, and 10 μl of this sample solution was injected into the device together with the above-mentioned carrier solvent and detected using a refractive index detector (RI detector). The peak value was determined from the molecular weight distribution of the measured sample.

[0139] (Colorant particle dispersion) Carbon black (Mogul (registered trademark) L manufactured by Cabot Corporation) 10 parts by weight Sodium dodecylbenzenesulfonate aqueous solution (concentration 20% by mass) 1.5 parts by mass Ion-exchanged water 90 parts by weight The above components were mixed and dispersed in an SC mill (SC100 / 32-XZ, Nippon Coke and Engineering Co., Ltd.) to obtain a colorant particle dispersion. The volume-based median diameter of the colorant particles in the dispersion (measured using a particle size measuring device (Microtrac UPA-150, Nikkiso Co., Ltd.)) was 155 nm.

[0140] (Release agent particle dispersion) Behenyl behenate 100 parts by weight Sodium dodecyl sulfate 5 parts by mass Ion-exchanged water 240 parts by weight The above components were dispersed in a round stainless steel flask using a homogenizer (Ultra Turrax (registered trademark) T50, manufactured by IKA) for 10 minutes, and then dispersed using a pressure discharge homogenizer to obtain a release agent particle dispersion. The volume-based median diameter of the release agent particles in the dispersion (measured using a laser diffraction particle size distribution analyzer (LA-750, manufactured by Horiba, Ltd.)) was 530 nm.

[0141] 2. Preparation of toner base particles (Toner base particles 1) Binder resin particle dispersion 237 parts by weight Colorant particle dispersion 42 parts by weight Release agent particle dispersion 18 parts by weight Polyaluminum chloride 1.8 parts by mass Ion-exchanged water 600 parts by weight The above components were mixed and dispersed in a round stainless steel flask using a homogenizer (Ultra-Turrax (registered trademark) T50, manufactured by IKA), and the liquid temperature was then raised to 55°C while stirring the contents of the flask in a heating oil bath. After the liquid temperature was kept at 55°C for 30 minutes, it was confirmed that aggregated particles with a volumetric median diameter (measured using a particle size measuring device (Microtrac UPA-150, manufactured by Nikkiso Co., Ltd.)) of 4.8 μm were generated in the solution. The temperature of the heating oil bath was then further increased to 56°C and the liquid was kept for 2 hours, confirming that the volumetric median diameter of the aggregated particles had become 5.9 μm.

[0142] Then, 1 mol / L of sodium hydroxide was added to the flask to adjust the pH of the solution to 5.0 at a liquid temperature of 56°C. The round stainless steel flask was then sealed using a magnetic seal, and the liquid temperature was raised to 98°C while continuing stirring. Stirring was continued for 6 hours to complete fusion (fusion) between the binder resin particles, thereby preparing toner base particle dispersion liquid 1. The volume-based median diameter of the toner base particles in toner base particle dispersion liquid 1 (measured using a particle size measuring device (Microtrac UPA-150, manufactured by Nikkiso Co., Ltd.)) was 6.1 μm.

[0143] The toner base particle dispersion 1 was subjected to solid-liquid separation using a basket centrifuge (MARKIII model number 60×40, manufactured by Matsumoto Machinery Works, Ltd.) to form a wet cake of toner base particles. The wet cake was washed with ion-exchanged water at 45° C. until the electrical conductivity of the filtrate from the basket centrifuge reached 5 μS / cm, and then transferred to a dryer (flash jet dryer, manufactured by Seishin Enterprise Co., Ltd.) and dried until the moisture content reached 0.5% by mass, to obtain toner base particles 1.

[0144] (Toner base particles 2-12) A binder resin particle dispersion was separately prepared so that the composition and composition ratio of the monomers in the binder resin were the values ​​shown in Table 1, and toner base particles 2 to 12 were obtained in the same manner as toner base particle 1, except that each prepared binder resin particle dispersion was used (for toner base particle 11, a hydrocarbon wax (HNP-0910, paraffin wax, manufactured by Nippon Seiro Co., Ltd.) was used instead of behenyl behenate in the release agent dispersion). In Table 1, iBuA stands for isobutyl acrylate, MeOSt stands for methoxystyrene, and 2EHA stands for 2-ethylhexyl acrylate, respectively.

[0145] (Toner base particles 13) Toner base particles 12 were obtained in the same manner as toner base particles 4, except that the release agent particle dispersion liquid was not used.

[0146] 3. Toner Preparation (Toner 1) To 100 parts by mass of toner base particles, 1 part by mass of hydrophobic silica (number average primary particle diameter = 12 nm) and 0.3 parts by mass of hydrophobic titania (number average primary particle diameter = 20 nm) were added, and mixed using a Henschel Mixer (registered trademark) to perform external additive treatment, thereby producing Toner 1.

[0147] (Toner 2-13) Toners 2 to 13 were obtained in the same manner as Toner 1, except that the toner base particles used were changed to Toner base particles 2 to 13.

[0148] The ratio X of the content of the first structural unit to the total content of the first structural unit and the second structural unit in each toner is shown in Table 1. The ratio X was calculated from the charge ratio of isobutyl methacrylate (or isobutyl acrylate) and styrene (or methoxystyrene).

[0149] 3. Evaluation 3-1. Folding Fixation Toners 1 to 13 were loaded in order into a multifunction printer (bizhub PRO (registered trademark) C6500, manufactured by Konica Minolta, Inc.). The surface temperature of the fixing and heating member of the thermal roll fixing method was set to 150° C., and the recording medium was a 350 g / m2 toner with a basis weight of 150 g / m2 under an environment of normal temperature and normal humidity (temperature 20° C., relative humidity 50% RH). 2 The image was formed on thick paper of 6 g / m 3 A solid image with the toner fixed thereon was obtained as a visible image.

[0150] The obtained solid image was then folded using a folding machine, and air was blown onto it at a pressure of 0.35 MPa to observe the state of the fold and evaluate the fold fixability according to the following criteria: In this evaluation, a rank of 3 or higher was deemed to be acceptable. Rank 5: No peeling was observed near the folds Rank 4: Slight peeling along the creases was observed Rank 3: Partial peeling along the crease was observed. Rank 2: Thin linear peeling along the creases was observed. Rank 1: Thick linear peeling along the crease was observed

[0151] 3-2. Heat resistant storage properties 0.5 g of Toner 1 was placed in a 10 mL glass bottle with an inner diameter of 21 mm, the lid was closed, and the bottle was shaken 600 times at room temperature using a Tap Denser KYT-2000 (manufactured by Seishin Enterprise Co., Ltd.). After that, the bottle was left with the lid removed in an environment of 55°C and 35% RH for 2 hours.

[0152] Next, the toner 1 after standing was placed on a 48 mesh (350 μm mesh size) sieve while being careful not to break up the toner aggregates. The toner was then set in a powder tester (manufactured by Hosokawa Micron Corporation), fixed with a presser bar and a knob nut, and vibration intensity was adjusted to a feed width of 1 mm, and vibration was applied for 10 seconds. The amount of toner remaining on the sieve was then measured, and the measured amount of toner was divided by the initial weight of the toner (0.5 g) to calculate the toner aggregation rate. The toner aggregation rate was evaluated for heat-resistant storage stability according to the following evaluation criteria. The heat-resistant storage stability of toners 2 to 13 was also evaluated in the same manner. ◎: Toner coagulation rate is less than 15% by mass (developer has excellent heat-resistant storage properties) ○: Toner cohesion rate is 15% by mass or more and less than 20% by mass (developer has good heat-resistant storage properties) △: Toner cohesion rate is 20% by mass or more and less than 25% by mass (heat resistance storage property of developer is slightly poor) ×: Toner cohesion rate is 25% by mass or more (developer has poor heat resistance for storage and cannot be used)

[0153] Table 1 shows the evaluation results for each toner.

[0154] [Table 1]

[0155] In Examples 1 to 11 in which the binder resin had a polymer having a first structural unit represented by general formula (1) and the toner contained a release agent, it was possible to improve low-temperature fixability while suppressing an extreme decrease in heat-resistant storage stability.

[0156] It was also found that the higher the content of the first structural unit, the higher the low-temperature fixability. On the other hand, by appropriately reducing the content of the first structural unit, the deterioration of heat-resistant storage stability could be further suppressed. [Industrial Applicability]

[0157] The toner for developing electrostatic images of the present invention can sufficiently improve low-temperature fixing ability and can suppress an extreme decrease in heat-resistant storage stability, and therefore the present invention is useful in the field of image formation. [Explanation of symbols]

[0158] 1. Image forming device 10 Heating belt 30 Image processing section 40 Image forming section 41Y, 41M, 41C, 41K Image forming unit 42 Intermediate transfer unit 43 Secondary transfer unit 50 Paper transport section 51 Paper feed section 51a, 51b, 51c Paper feed tray unit 52 Paper output section 52a Paper ejection roller 53 Conveying path section 53a Registration roller pair 60 Fixing device 62 Fixing roller 63 Pressure Roller 70 Image reading unit 71 Paper feeder 72 Scanner 72a CCD sensor 411 Exposure equipment 412 Developing device 413 Electrophotographic photoreceptor 414 Charging device 415 Drum cleaning device 421 Intermediate transfer belt 422 Primary transfer roller 423, 431 Support roller 423A Backup roller 426 Belt cleaning device 426a Elastic members 431A Secondary transfer roller 432 Secondary transfer belt D Manuscript S paper

Claims

1. A toner for developing an electrostatic image, the toner comprising a binder resin and a release agent in a toner base particle, The binder resin contains a first polymer having a first structural unit represented by general formula (1), Toner for developing electrostatic images. 【Chemistry 1】 (In the general formula (1), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; R 2 is a branched alkyl group having 3 to 5 carbon atoms.

2. In the general formula (1), R 2 2. The toner for developing electrostatic images according to claim 1, wherein is an isobutyl group.

3. In the general formula (1), R 1 2. The toner for developing electrostatic images according to claim 1, wherein is a methyl group.

4. 2. The toner for developing electrostatic images according to claim 1, wherein the release agent is a hydrocarbon wax or a fatty acid ester wax.

5. The first polymer is a copolymer further having a second structural unit represented by general formula (2), or The binder resin further contains a second polymer having a second structural unit represented by general formula (2) and not having the first structural unit. The toner for developing electrostatic images according to claim 1. 【Chemistry 2】 (In the general formula (2), R 3 is a hydrogen atom or an alkoxy group having 1 to 3 carbon atoms.

6. In the general formula (2), R 3 6. The toner for developing electrostatic images according to claim 5, wherein is a hydrogen atom or a methoxy group.

7. 6. The toner for developing electrostatic images according to claim 5, wherein in the binder resin, a content of the first structural unit is 10% by mass or more and 90% by mass or less with respect to a total mass of a content of the first structural unit and a content of the second structural unit.

8. 6. The toner for developing electrostatic images according to claim 5, wherein in the binder resin, a content of the first structural unit is 25% by mass or more and 80% by mass or less with respect to a total mass of a content of the first structural unit and a content of the second structural unit.

9. 6. The toner for developing electrostatic images according to claim 5, wherein the first polymer is a copolymer further having a second structural unit represented by general formula (2).

10. 10. The toner for developing an electrostatic image according to claim 9, wherein the first polymer is a copolymer further having a third structural unit different from the first structural unit and the second structural unit.

11. The toner for developing electrostatic images according to claim 10, wherein the third structural unit is a structural unit derived from (meth)acrylic acid or a (meth)acrylic acid ester.

12. 11. The toner for developing electrostatic images according to claim 10, wherein the third structural unit is at least one structural unit derived from a compound selected from the group consisting of (meth)acrylic acid, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.

13. A method for producing a toner for developing an electrostatic image, the toner base particles containing a binder resin and a release agent, comprising the steps of: preparing a monomer represented by general formula (1a); and polymerizing the prepared monomer in an aqueous medium to prepare a particle dispersion liquid of the binder resin containing a first polymer having a first structural unit. A method for producing a toner for developing electrostatic images. 【Chemistry 3】 (In the general formula (1a), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; R 2 is a branched alkyl group having 3 to 5 carbon atoms.

14. A step of adhering the toner for developing an electrostatic image according to any one of claims 1 to 12 to a recording medium; a step of fixing the electrostatic image developing toner adhered to the recording medium; The image forming method according to claim 1,

Citation Information

Patent Citations

  • Toner for electrostatic charge image development, method for manufacturing the same, image forming method, and image forming apparatus

    JP2007279714A

  • Toner binder and toner

    JP2008287229A

  • Method for production of binder resin for toner, binder resin for toner, and toner

    JP2010015159A