Toner
The toner with controlled tetrahydrofuran-insoluble components and optimized particle size achieves both low-temperature fixability and heat-resistant storage stability, enhancing color development in image formation.
Patent Information
- Application Number
- JP2023078077
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Existing toners struggle to achieve excellent low-temperature fixability and heat-resistant storage stability while maintaining excellent color development.
The toner comprises pulverized toner base particles with a specific volume median diameter and a binder resin containing a controlled amount of tetrahydrofuran-insoluble components, which are ultrasonically treated to maintain elasticity and chargeability, along with an external additive to enhance image formation.
The toner exhibits excellent low-temperature fixability, heat-resistant storage stability, and superior color development, ensuring effective image formation.
Smart Images

Figure 2024162513000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner. [Background technology]
[0002] In an electrophotographic image forming apparatus, for example, a toner containing positively charged toner particles is used. The toner is required to have, for example, excellent low-temperature fixing property and heat-resistant storage stability, and to be able to form an image with excellent color development. In response to such requirements, for example, a developing toner having toner particles with a certain range of tetrahydrofuran (THF) insoluble component has been proposed (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-220569 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, even with the toner described in Patent Document 1, it is difficult to form an image having excellent color development while exhibiting excellent low-temperature fixability and heat-resistant storage stability.
[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide a toner which is excellent in low-temperature fixing property and heat-resistant storage stability, and is capable of forming an image with excellent color development. [Means for solving the problem]
[0006] The toner according to the present invention includes toner particles. The toner particles include toner base particles and an external additive attached to the surface of the toner base particles. The toner base particles are pulverized toner base particles. The volume median diameter of the toner base particles is 5.20 μm or more and 6.50 μm or less. The toner base particles contain a binder resin. The binder resin has a content of tetrahydrofuran insoluble components of 4.50 mass % or more and 16.00 mass % or less. The binder resin has a content of tetrahydrofuran insoluble components of 2.20 mass % or less after one minute of ultrasonic treatment at an output of 200 W and a frequency of 28 kHz. In an infrared absorption spectrum of the toner particles obtained by infrared spectroscopy, -1 The height of the peak that appears above is 0.0070A or more and 0.0300A or less. Effect of the Invention
[0007] The toner according to the present invention is excellent in low-temperature fixing property and heat-resistant storage stability, and can form images with excellent color development. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a diagram illustrating an example of a toner particle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] A preferred embodiment of the present invention will be described below. The toner is an aggregate (e.g., powder) of toner particles. The external additive is an aggregate (e.g., powder) of external additive particles. Unless otherwise specified, the evaluation results (values indicating shape, physical properties, etc.) of the powder (more specifically, the powder of toner particles, the powder of external additive particles, magnetic powder, etc.) are the number average values measured for each of a considerable number of particles selected from the powder.
[0010] Volume median diameter of powder (D 50) is a value measured using a laser diffraction / scattering particle size distribution analyzer (e.g., HORIBA, Ltd.'s "LA-920V2" or Beckman Coulter, Inc.'s "Coulter Counter Multisizer 3" unless otherwise specified.
[0011] Unless otherwise specified, the number average primary particle diameter of a powder is the number average value of the circle equivalent diameters of primary particles (Heywood diameter: diameter of a circle having the same area as the projected area of a primary particle) measured using a scanning electron microscope. The number average primary particle diameter of a powder is, for example, the number average value of the circle equivalent diameters of 100 primary particles. The number average primary particle diameter of particles refers to the number average primary particle diameter of particles in the powder unless otherwise specified.
[0012] Unless otherwise specified, the chargeability refers to the chargeability in triboelectric charging. For example, a standard carrier (standard carrier for negatively charged toner: N-01, standard carrier for positively charged toner: P-01) provided by the Imaging Society of Japan is mixed with the measurement target (e.g., toner) and stirred to triboelectrically charge the measurement target. The charge amount of the measurement target is measured before and after triboelectric charging, for example, with a small suction-type charge amount measuring device (Trek's "MODEL 212HS"), and the greater the change in charge amount before and after triboelectric charging, the stronger the chargeability of the measurement target.
[0013] Unless otherwise specified, the softening point (Tm) is a value measured using a high-speed flow tester (Shimadzu Corporation's "CFT-500D"). In the S-shaped curve (horizontal axis: temperature, vertical axis: stroke) measured using the high-speed flow tester, the temperature at which "(baseline stroke value + maximum stroke value) / 2" is obtained corresponds to Tm (softening point).
[0014] Unless otherwise specified, the measured value of the melting point (Mp) is the temperature of the maximum endothermic peak in an endothermic curve (vertical axis: heat flow (DSC signal), horizontal axis: temperature) measured using a differential scanning calorimeter ("DSC-6220" manufactured by Seiko Instruments Inc.) This endothermic peak appears due to melting of the crystallized site.
[0015] Unless otherwise specified, the glass transition point (Tg) is a value measured according to JIS (Japanese Industrial Standards) K7121-2012 using a differential scanning calorimeter (DSC-6220 manufactured by Seiko Instruments Inc.). In the endothermic curve measured by the differential scanning calorimeter (vertical axis: heat flow (DSC signal), horizontal axis: temperature), the temperature of the inflection point due to the glass transition (specifically, the temperature of the intersection between the extrapolated line of the baseline and the extrapolated line of the falling line) corresponds to Tg (glass transition point).
[0016] Unless otherwise specified, the measured values of the acid value and the hydroxyl value are values measured in accordance with "JIS (Japanese Industrial Standards) K0070-1992".
[0017] Unless otherwise specified, the "major component" of a material means the component that is contained in the largest amount in the material on a mass basis.
[0018] Hereinafter, the compound and its derivatives may be collectively referred to by adding "based" after the compound name. When the compound name is followed by "based" to represent the name of a polymer, it means that the repeating unit of the polymer is derived from the compound or its derivative.
[0019] <Toner> The toner according to the embodiment of the present invention will be described below. The toner of the present invention includes toner particles. The toner particles include toner base particles and an external additive attached to the surface of the toner base particles. The toner base particles are pulverized toner base particles. The volume median diameter of the toner base particles is 5.20 μm or more and 6.50 μm or less. The toner base particles contain a binder resin. The binder resin has a content of tetrahydrofuran insoluble components of 4.50 mass % or more and 16.00 mass % or less. The binder resin has a content of tetrahydrofuran insoluble components of 2.20 mass % or less after ultrasonic treatment at an output of 200 W and a frequency of 28 kHz for 1 minute. In the infrared absorption spectrum of the toner particles obtained by infrared spectroscopy, -1 The height of the peak that appears above is 0.0070A or more and 0.0300A or less.
[0020] The toner of the present invention can be suitably used for developing electrostatic latent images. The toner of the present invention may be used as a one-component developer. The toner of the present invention may be mixed with a carrier using a mixing device (e.g., a bowl mill) and used as a two-component developer. When used as a one-component developer, the toner of the present invention is charged (e.g., positively charged) by friction with a developing sleeve or a toner charging member in a developing device. An example of a toner charging member is a doctor blade. When used as a two-component developer, the toner of the present invention is charged (e.g., positively charged) by friction with a carrier in a developing device.
[0021] [Toner particles] Fig. 1 shows an example of a toner particle 1 contained in the toner of the present invention. The toner particle 1 shown in Fig. 1 includes a toner base particle 2 and an external additive 3 attached to the surface of the toner base particle 2. The external additive 3 includes silica particles 4 and external additive particles 5 other than the silica particles 4.
[0022] Toner particle 1, which is an example of toner particles, has been described above with reference to FIG. 1. However, the toner particles contained in the toner of the present invention may have a structure different from that of toner particle 1 shown in FIG. 1. Specifically, in the toner of the present invention, the external additive may contain only silica particles 4, or may contain only other external additive particles 5. The toner particles may also be toner particles having a shell layer (hereinafter, sometimes referred to as capsule toner particles). In capsule toner particles, the toner mother particles have, for example, a toner core containing a binder resin, and a shell layer covering the surface of the toner core.
[0023] The toner of the present invention, having the above-mentioned configuration, is excellent in low-temperature fixing property and heat-resistant storage stability, and can form images with excellent color development. The reason why the toner of the present invention can exhibit the above-mentioned effects is presumed to be as follows. The toner of the present invention contains a certain amount of tetrahydrofuran-insoluble components in the binder resin. This tetrahydrofuran-insoluble component is a resin that has an extremely high molecular weight and an intramolecular entangled structure. The tetrahydrofuran-insoluble components impart appropriate elasticity to the toner particles and suppress the aggregation of the toner particles. As a result, the tetrahydrofuran-insoluble components impart heat-resistant storage stability to the toner of the present invention.
[0024] On the other hand, known toners containing toner particles with high elasticity tend to have insufficient low-temperature fixability because the toner particles do not melt sufficiently during fixing. In addition, such known toners tend to be unable to sufficiently cover (conceal) the surface of a recording medium with the melted toner particles during the fixing process, resulting in insufficient color development of the formed image. In contrast, at least a part of the tetrahydrofuran-insoluble components contained in the toner of the present invention is soluble in tetrahydrofuran and loses elasticity when energy (for example, heat or ultrasonic treatment) is applied from the outside. This is due to the fact that the tetrahydrofuran-insoluble components are relatively simply entangled in the molecules. In other words, the structure of a resin that is intricately entangled in the molecules is hardly changed even when ultrasonic treatment is performed, and the solubility and elasticity in tetrahydrofuran are not changed. In contrast, a resin that is relatively simply entangled in the molecules is disentangled when energy is applied from the outside, and is soluble in tetrahydrofuran and loses elasticity. Therefore, in the toner of the present invention, the content of the tetrahydrofuran insoluble component in the binder resin is 4.50% by mass or more under normal conditions (before ultrasonic treatment), but is reduced to 2.20% by mass or less after ultrasonic treatment. In actual image formation, the fixing process (heating process) for fixing the toner particles causes the tetrahydrofuran insoluble component to be solubilized and the elasticity to be reduced. Thus, in the toner of the present invention, the elasticity of the toner particles is high due to the presence of a large amount of tetrahydrofuran insoluble components under normal conditions (storage), but the tetrahydrofuran insoluble components are reduced during fixing, causing the elasticity of the toner particles to be reduced. As a result, the toner of the present invention can satisfy heat-resistant storage stability, low-temperature fixability, and color development of the formed image.
[0025] In addition, the toner of the present invention has an optimized volume median diameter of the toner base particles, and therefore the toner particles can sufficiently cover the surface of a recording medium, forming an image with excellent color development. -1The height of the peak appearing above is 0.0070 A or more and 0.0300 A or less. Since the height of the peak of the toner of the present invention is in an appropriate range (0.0070 A or more and 0.0300 A or less), the toner of the present invention can provide the toner particles with an appropriate chargeability while suppressing the deterioration of the heat-resistant storage stability. As a result, the toner of the present invention can form an image that is excellent in low-temperature fixing property and heat-resistant storage stability as well as in color development.
[0026] The toner of the present invention will be described in further detail below. Each of the components described below may be used alone or in combination of two or more, unless otherwise specified.
[0027] [Toner particles] The toner particles include toner base particles and an external additive attached to the surface of the toner base particles. In the infrared absorption spectrum of the toner particles obtained by infrared spectroscopy, -1 The height of the peak appearing above is 0.0070A or more and 0.0300A or less, preferably 0.0110A or more and 0.0200A or less, and more preferably 0.0150A or more and 0.0200A or less. By making the height of the above peak 0.0070A or more, the toner of the present invention is given good developability, and as a result, an image with excellent color development can be formed. By making the height of the above peak 0.0300A or less, the heat-resistant storage stability of the toner of the present invention is optimized. The infrared spectroscopy analysis can be performed at a temperature of 25°C by the method described in the Examples or a method based thereon.
[0028] Here, the wave number is 701 cm -1 The height of the peak that appears above indicates, for example, the amount of aromatic ring structures (particularly structures derived from styrene). The aromatic ring structures tend to impart appropriate chargeability to toner particles. On the other hand, toner particles that contain an excessive amount of aromatic ring structures tend to have poor heat-resistant storage stability.
[0029] The mass average molecular weight of the resin contained in the toner particles is preferably 85,000 to 130,000, more preferably 95,000 to 115,000, and even more preferably 100,000 to 111,000. By making the mass average molecular weight of the resin contained in the toner particles 85,000 or more, the heat-resistant storage stability of the toner of the present invention can be further optimized. By making the mass average molecular weight of the resin contained in the toner particles 130,000 or less, the low-temperature fixing property of the toner of the present invention can be further optimized. The resin contained in the toner particles is usually the same as the binder resin contained in the toner mother particles. The mass average molecular weight of the resin contained in the toner particles can be measured by the method described in the Examples or a method based thereon.
[0030] (Toner base particles) The toner base particles contain, for example, a binder resin as a main component. The toner base particles may further contain an internal additive (for example, at least one of a colorant, a release agent, a charge control agent, and a magnetic powder) as necessary. The toner base particles are pulverized toner base particles obtained by a pulverization method. The pulverization method can easily prepare toner base particles containing a certain amount of tetrahydroinsoluble components.
[0031] Volume median diameter of toner particles (D 50 ) is 5.20 μm or more and 6.50 μm or less, preferably 5.50 μm or more and 6.20 μm or less, and more preferably 5.70 μm or more and 6.00 μm or less. By making the volume median diameter of the toner base particles 5.20 μm or more, the heat-resistant storage stability of the toner of the present invention is optimized. In addition, by making the volume median diameter of the toner base particles 5.20 μm or more and 6.50 μm or less, the toner of the present invention can sufficiently cover (conceal) the surface of the recording medium with the molten toner particles in the fixing process. As a result, the toner of the present invention can form an image with excellent color development.
[0032] (Binding resin) From the viewpoint of providing a toner having excellent low-temperature fixing properties, the toner base particles preferably contain a thermoplastic resin as a binder resin, and more preferably contain a thermoplastic resin at a ratio of 85% by mass or more of the total binder resin. Examples of the thermoplastic resin include styrene resin, (meth)acrylic acid ester resin, olefin resin (e.g., polyethylene resin and polypropylene resin), vinyl resin (e.g., vinyl chloride resin, polyvinyl alcohol, vinyl ether resin, and N-vinyl resin), polyester resin, polyamide resin, and urethane resin. Copolymers of these resins, that is, copolymers in which any repeating unit is introduced into the above resin (e.g., styrene-(meth)acrylic acid ester resin, and styrene-butadiene resin), can also be used as the binder resin.
[0033] The content of the binder resin in the toner base particles is preferably from 60% by mass to 97% by mass, and more preferably from 85% by mass to 92% by mass.
[0034] The content of the tetrahydrofuran insoluble component in the binder resin is 4.50% by mass or more and 16.00% by mass or less, preferably 7.00% by mass or more and 15.00% by mass or less, and more preferably 8.00% by mass or more and 10.00% by mass or less. By making the content of the tetrahydrofuran insoluble component in the binder resin 4.50% by mass or more, the heat-resistant storage stability of the toner of the present invention can be optimized. By making the content of the tetrahydrofuran insoluble component in the binder resin 16.00% by mass or less, the low-temperature fixability of the toner of the present invention and the color development of the formed image can be optimized.
[0035] The content of the tetrahydrofuran insoluble component in the binder resin after one minute of ultrasonic treatment at an output of 200 W and a frequency of 28 kHz is 2.20% by mass or less, preferably 0.20% by mass or more and 2.20% by mass or less, more preferably 0.40% by mass or more and 2.00% by mass or less, and even more preferably 0.80% by mass or more and 1.50% by mass or less. By making the content of the tetrahydrofuran insoluble component in the binder resin after ultrasonic treatment 2.20% by mass or less, the low-temperature fixability of the toner of the present invention and the color development of the formed image can be optimized. By making the content of the tetrahydrofuran insoluble component in the binder resin after ultrasonic treatment 0.20% by mass or more, it becomes easy to adjust the content of the tetrahydrofuran insoluble component in the binder resin described above to the above range.
[0036] From the viewpoint of further optimizing the low-temperature fixability of the toner of the present invention, the binder resin is preferably a polyester resin. The polyester resin is obtained by polycondensation of one or more polyhydric alcohols and one or more polycarboxylic acids. Examples of the polyhydric alcohols for synthesizing the polyester resin include dihydric alcohols (e.g., diol compounds and bisphenol compounds) and trivalent or higher alcohols. Examples of the polycarboxylic acids for synthesizing the polyester resin include divalent carboxylic acids and trivalent or higher carboxylic acids. Instead of the polycarboxylic acids, polycarboxylic acid derivatives capable of forming ester bonds by polycondensation (e.g., polycarboxylic acid anhydrides and polycarboxylic acid halides) may be used.
[0037] Examples of diol compounds include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 2-butene-1,4-diol, 1,5-pentanediol, 2-pentene-1,5-diol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, 1,4-benzenediol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.
[0038] Examples of bisphenol compounds include bisphenol A, hydrogenated bisphenol A, ethylene oxide adducts of bisphenol A (eg, polyoxyethylene(2,2)-2,2-bis(4-hydroxyphenyl)propane), and propylene oxide adducts of bisphenol A.
[0039] Examples of trihydric or higher alcohols include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, diglycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene.
[0040] Examples of divalent carboxylic acids include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, cyclohexanedicarboxylic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, succinic acid, alkylsuccinic acids (more specifically, n-butylsuccinic acid, isobutylsuccinic acid, n-octylsuccinic acid, n-dodecylsuccinic acid, isododecylsuccinic acid), and alkenylsuccinic acids (more specifically, n-butenylsuccinic acid, isobutenylsuccinic acid, n-octenylsuccinic acid, n-dodecenylsuccinic acid, isododecenylsuccinic acid).
[0041] Examples of trivalent or higher carboxylic acids include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxylpropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, and empol trimer acid.
[0042] The polyester resin may further have a repeating unit derived from a vinyl compound. Examples of the vinyl compound include olefin compounds (e.g., ethylene, propylene, and butylene), styrene compounds, (meth)acrylic acid, and (meth)acrylic acid alkyl esters. The vinyl compound is preferably a styrene compound or a (meth)acrylic acid alkyl ester.
[0043] Examples of styrene compounds include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene.
[0044] Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, and lauryl (meth)acrylate.
[0045] The binder resin is preferably an amorphous polyester resin. On the other hand, when the binder resin contains a small amount of crystalline polyester resin, the sharp melting property of the toner particles can be optimized. From the above, the binder resin preferably contains both crystalline polyester resin and amorphous polyester resin. In the binder resin, the total content of the crystalline polyester resin and the amorphous polyester resin is preferably 90% by mass or more, more preferably 99% by mass or more, and even more preferably 100% by mass.
[0046] In addition, in many cases, it is not possible to clearly measure the Mp of an amorphous polyester resin. Therefore, a polyester resin in which no clear endothermic peak can be determined in an endothermic curve measured using a differential scanning calorimeter may be determined to be an amorphous polyester resin.
[0047] (Amorphous polyester resin) When the binder resin contains an amorphous polyester resin, the amorphous polyester resin preferably has a first repeating unit derived from a trivalent or higher carboxylic acid. The first repeating unit introduces a crosslinking structure into the amorphous polyester resin. As a result, the molecular weight of the amorphous polyester resin increases and the molecules become moderately entangled. By having an appropriate amount of the first repeating unit, the amorphous polyester resin is insoluble in tetrahydrofuran (i.e., high elasticity) under normal conditions, but becomes soluble in tetrahydrofuran (i.e., low elasticity) when energy (e.g., heat or ultrasonic treatment) is applied from the outside. As the trivalent or higher carboxylic acid, trimellitic acid is preferable, and trimellitic anhydride is more preferable.
[0048] In the total repeating units contained in the amorphous polyester resin, the content of the first repeating unit is preferably 1.5% by mass to 7.5% by mass, more preferably 3.0% by mass to 4.5% by mass. By setting the content of the first repeating unit in the amorphous polyester resin to 1.5% by mass to 7.5% by mass, it becomes easier to adjust the solubility (i.e., elasticity) of the amorphous polyester resin in tetrahydrofuran.
[0049] The amorphous polyester resin preferably further comprises a second repeating unit derived from a bisphenol compound and a third repeating unit derived from a dicarboxylic acid. The bisphenol compound is preferably an ethylene oxide adduct of bisphenol A or a propylene oxide adduct of bisphenol A. The dicarboxylic acid is preferably n-dodecenyl succinic anhydride or terephthalic acid.
[0050] The content of the second repeating unit in all repeating units contained in the amorphous polyester resin is preferably from 60.0% by mass to 90.0% by mass, and more preferably from 70.0% by mass to 80.0% by mass.
[0051] The content of the third repeating unit in all repeating units contained in the amorphous polyester resin is preferably from 10.0% by mass to 35.0% by mass, and more preferably from 15.0% by mass to 25.0% by mass.
[0052] The content of the amorphous polyester resin in the toner base particles is preferably from 50.0% by mass to 95.0% by mass, and more preferably from 70.0% by mass to 90.0% by mass.
[0053] The softening point of the amorphous polyester resin is preferably 100.0°C or more and 150.0°C or less, and more preferably 110.0°C or more and 130.0°C or less. The glass transition point of the amorphous polyester resin is preferably 45.0°C or more and 70.0°C or less, and more preferably 55.0°C or more and 65.0°C or less. The acid value of the amorphous polyester resin is preferably 3.0mgKOH / g or more and 25.0mgKOH / g or less, and more preferably 5.0mgKOH / g or more and 15.0mgKOH / g or less. The hydroxyl value of the amorphous polyester resin is preferably 5.0mgKOH / g or more and 50.0mgKOH / g or less, and more preferably 10.0mgKOH / g or more and 20.0mgKOH / g or less. The mass average molecular weight of the amorphous polyester resin is preferably 90000 or more and 150000 or less, and more preferably 105000 or more and 125000 or less. The number average molecular weight of the amorphous polyester resin is preferably 2,000 or more and 5,000 or less, and more preferably 3,200 or more and 4,000 or less.
[0054] (Crystalline polyester resin) When the binder resin contains a crystalline polyester resin, the crystalline polyester resin preferably has a fourth repeating unit derived from a styrene compound. The fourth repeating unit imparts the above-mentioned structure derived from styrene to the toner particles. As the styrene compound, styrene is preferable.
[0055] The content ratio of the fourth repeating unit in all repeating units of the crystalline polyester resin is preferably 0.5% by mass to 8.0% by mass, more preferably 1.5% by mass to 3.0% by mass. By setting the content ratio of the fourth repeating unit in the crystalline polyester resin to 0.5% by mass to 8.0% by mass, the infrared absorption spectrum of the toner particles obtained by infrared spectroscopy has a wave number of 701 cm. -1 This makes it easier to adjust the height of the peak that appears above to between 0.0070A and 0.0300A.
[0056] The crystalline polyester resin preferably has a fifth repeating unit derived from a diol compound, a sixth repeating unit derived from a dicarboxylic acid, and a seventh repeating unit derived from an alkyl (meth)acrylate ester. The diol compound is preferably 1,4-butanediol or 1,6-hexanediol. The dicarboxylic acid is preferably fumaric acid. The alkyl (meth)acrylate is preferably n-butyl (meth)acrylate.
[0057] The content of the fifth repeating unit in all repeating units contained in the crystalline polyester resin is preferably from 30.0% by mass to 55.0% by mass, and more preferably from 42.0% by mass to 48.0% by mass.
[0058] In all repeating units contained in the crystalline polyester resin, the content of the sixth repeating unit is preferably from 40.0% by mass to 65.0% by mass, and more preferably from 50.0% by mass to 55.0% by mass.
[0059] The content of the seventh repeating unit in all repeating units contained in the crystalline polyester resin is preferably from 0.5% by mass to 5.0% by mass, and more preferably from 0.8% by mass to 2.0% by mass.
[0060] The content of the crystalline polyester resin in the toner base particles is preferably from 5.0% by mass to 40.0% by mass, and more preferably from 8.0% by mass to 12.0% by mass.
[0061] The softening point of the crystalline polyester resin is preferably 70.0°C or more and 1000.0°C or less, and more preferably 85.0°C or more and 90.0°C or less. The melting point of the crystalline polyester resin is preferably 70.0°C or more and 90.0°C or less, and more preferably 75.0°C or more and 85.0°C or less. The acid value of the crystalline polyester resin is preferably 2.0mgKOH / g or more and 3.7mgKOH / g or less, and more preferably 2.8mgKOH / g or more and 3.4mgKOH / g or less. The hydroxyl value of the crystalline polyester resin is preferably 5.0mgKOH / g or more and 25.0mgKOH / g or less, and more preferably 10.0mgKOH / g or more and 20.0mgKOH / g or less. The mass average molecular weight of the crystalline polyester resin is preferably 20000 or more and 60000 or less, and more preferably 25000 or more and 40000 or less. The number average molecular weight of the crystalline polyester resin is preferably 2,000 or more and 5,000 or less, and more preferably 3,200 or more and 4,000 or less.
[0062] (Coloring agent) The toner base particles may contain a colorant. As the colorant, a known pigment or dye can be used according to the color of the toner of the present invention. From the viewpoint of forming a high-quality image using the toner of the present invention, the content of the colorant is preferably 1.0 parts by mass or more and 20.0 parts by mass or less, more preferably 2.0 parts by mass or more and 5.0 parts by mass or less, based on 100 parts by mass of the binder resin.
[0063] The toner base particles may contain a black colorant. An example of the black colorant is carbon black. The black colorant may be a colorant toned to black using a yellow colorant, a magenta colorant, and a cyan colorant.
[0064] The toner base particles may contain color colorants, including yellow, magenta, and cyan colorants.
[0065] As the yellow colorant, for example, one or more compounds selected from the group consisting of condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and arylamide compounds can be used. As the yellow colorant, for example, CI Pigment Yellow (3, 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 191, and 194), Naphthol Yellow S, Hansa Yellow G, and CI Vat Yellow can be mentioned.
[0066] As the magenta colorant, for example, one or more compounds selected from the group consisting of condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds can be used. As the magenta colorant, for example, CI Pigment Red (2, 3, 5, 6, 7, 19, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, and 254) can be used.
[0067] As the cyan colorant, for example, one or more compounds selected from the group consisting of copper phthalocyanine compounds, anthraquinone compounds, and basic dye lake compounds can be used. As the cyan colorant, for example, CI Pigment Blue (1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, and 66), phthalocyanine blue, CI Vat Blue, and CI Acid Blue can be used.
[0068] (Charge control agent) The toner base particles may contain a charge control agent. The charge control agent is used, for example, for the purpose of providing a toner having excellent charge stability or charge rise characteristics. The charge rise characteristics of a toner are an index of whether or not the toner can be charged to a predetermined charge level in a short period of time. By incorporating a positively chargeable charge control agent in the toner base particles, the cationic nature of the toner base particles can be enhanced.
[0069] Examples of the positively charged charge control agent include azine compounds, direct dyes, acid dyes, alkoxylated amines, alkylamides, quaternary ammonium salt compounds, and resins containing quaternary ammonium cationic groups. The charge control agent is preferably a quaternary ammonium salt compound.
[0070] Examples of the azine compound include pyridazine, pyrimidine, pyrazine, 1,2-oxazine, 1,3-oxazine, 1,4-oxazine, 1,2-thiazine, 1,3-thiazine, 1,4-thiazine, 1,2,3-triazine, 1,2,4-triazine, 1,3,5-triazine, 1,2,4-oxadiazine, 1,3,4-oxadiazine, 1,2,6-oxadiazine, 1,3,4-thiadiazine, 1,3,5-thiadiazine, 1,2,3,4-tetrazine, 1,2,4,5-tetrazine, 1,2,3,5-tetrazine, 1,2,4,6-oxatriazine, 1,3,4,5-oxatriazine, phthalazine, quinazoline, and quinoxaline.
[0071] Examples of direct dyes include Azin Fast Red FC, Azin Fast Red 12BK, Azin Violet BO, Azin Brown 3G, Azin Light Brown GR, Azin Dark Green BH / C, Azin Deep Black EW, and Azin Deep Black 3RL.
[0072] Acid dyes include, for example, Nigrosine BK, Nigrosine NB, and Nigrosine Z.
[0073] Examples of quaternary ammonium salt compounds include benzyldecylhexylmethylammonium chloride, decyltrimethylammonium chloride, 2-(methacryloyloxy)ethyltrimethylammonium chloride, and dimethylaminopropylacrylamide methyl chloride quaternary salt.
[0074] From the viewpoint of providing a toner having excellent charging stability, the content of the charge control agent is preferably 0.1 parts by mass to 5.0 parts by mass, more preferably 0.5 parts by mass to 3.0 parts by mass, per 100 parts by mass of the binder resin.
[0075] (Release agent) The toner base particles may contain a release agent. The release agent is used, for example, for the purpose of imparting offset resistance to the toner of the present invention. From the viewpoint of imparting sufficient offset resistance to the toner of the present invention, the content of the release agent is preferably 1.0 parts by mass or more and 20.0 parts by mass or less, more preferably 3.0 parts by mass or more and 8.0 parts by mass or less, relative to 100 parts by mass of the binder resin.
[0076] Examples of the release agent include aliphatic hydrocarbon waxes, oxides of aliphatic hydrocarbon waxes, vegetable waxes, animal waxes, mineral waxes, ester waxes mainly composed of fatty acid esters, and waxes in which a part or all of the fatty acid esters are deoxidized. Examples of the aliphatic hydrocarbon waxes include low molecular weight polyethylene, low molecular weight polypropylene, polyolefin copolymers, polyolefin waxes, microcrystalline waxes, paraffin waxes, and Fischer-Tropsch waxes. Examples of the oxides of aliphatic hydrocarbon waxes include oxidized polyethylene waxes and block copolymers of oxidized polyethylene waxes. Examples of the vegetable waxes include candelilla wax, carnauba wax, Japan wax, jojoba wax, and rice wax. Examples of the animal waxes include beeswax, lanolin, and spermaceti. Examples of the mineral waxes include ozokerite, ceresin, and petrolatum. Examples of the ester waxes mainly composed of fatty acid esters include montan acid ester wax and castor wax. An example of the wax in which the fatty acid ester is partially or completely deoxidized is deoxidized carnauba wax. As the release agent, an ester wax is preferable.
[0077] When the toner base particles contain a release agent, a compatibilizer may be added to the toner base particles in order to improve the compatibility between the binder resin and the release agent.
[0078] (External additives) As the external additive, inorganic particles are preferred. As the inorganic particles, silica particles or metal oxide particles (more specifically, alumina, titanium oxide, magnesium oxide, zinc oxide, strontium titanate, barium titanate, etc.) are preferred, and silica particles or titanium oxide particles are more preferred. The number average primary particle diameter of the silica particles is preferably 5 nm or more and 200 nm or less, more preferably 10 nm or more and 40 nm or less. The number average primary particle diameter of the titanium oxide particles is preferably 50 nm or more and 600 nm or less, more preferably 300 nm or more and 450 nm or less.
[0079] The content of the external additive in the toner particles is preferably from 0.1 parts by mass to 15.0 parts by mass, and more preferably from 1.0 parts by mass to 4.0 parts by mass, relative to 100 parts by mass of the toner base particles, from the viewpoint of suppressing detachment from the toner base particles while fully exerting its function.
[0080] [Toner manufacturing method] The toner of the present invention can be produced, for example, by a production method including a step of preparing toner base particles and a step of adding an external agent.
[0081] (Toner Base Particle Preparation Process) In the toner base particle preparation process, the toner base particles are prepared by a pulverization method. The toner base particle preparation process includes, for example, a melt-kneading process and a pulverization process. The toner base particle preparation process may further include a mixing process before the melt-kneading process. In addition, the toner base particle preparation process may further include at least one of a fine pulverization process and a classification process after the pulverization process.
[0082] In the mixing step, the binder resin and the internal additives added as necessary are mixed to obtain a mixture. In the melting and kneading step, the toner materials are melted and kneaded to obtain a molten and kneaded product. For example, the mixture obtained in the mixing step is used as the toner material. In the pulverizing step, the obtained molten and kneaded product is cooled, for example, to room temperature (25°C), and then pulverized to obtain a pulverized product. If it is necessary to reduce the diameter of the pulverized product obtained in the pulverizing step, a step of further pulverizing the pulverized product (fine pulverizing step) may be performed. In addition, if the particle size of the pulverized product is to be uniform, a step of classifying the obtained pulverized product (classifying step) may be performed. Through the above steps, the pulverized product, that is, toner base particles, is obtained.
[0083] (External addition process) In the external addition step, the above-mentioned toner base particles and the external additive are mixed using a mixer, and the external additive is attached to the surface of the toner base particles. This results in the toner of the present invention. The external additive includes specific external additive particles and other external additive particles that are used as necessary. As an example of the mixer, an FM mixer (manufactured by Nippon Coke & Engineering Co., Ltd.) can be mentioned. EXAMPLES
[0084] The present invention will be described in more detail below using examples, but the present invention is not limited to the scope of the examples.
[0085] [Volume median diameter measurement] Volume median diameter of toner particles (D 50 ) was measured using a particle size meter (Beckman Coulter, Inc., Coulter Counter Multisizer 3).
[0086] [Infrared spectroscopy] In the infrared spectroscopic analysis, a Fourier transform infrared spectrometer ("Frontier" manufactured by PerkinElmer) was used as the measuring device. The measuring mode was ATR (attenuated total reflection) mode. Diamond (refractive index 2.4) was used as the ATR crystal.
[0087] The ATR crystal was attached to the measuring device, and 1 mg of the measurement target (toner of each of the Examples and Comparative Examples described below) was placed on the ATR crystal. Then, the sample was pressed with a load of 60 N to 80 N using the pressure arm of the measuring device. Then, the FT-IR spectrum of the sample (horizontal axis: wave number of the irradiated infrared light, vertical axis: absorbance) was measured under the condition of an infrared light incidence angle of 45°. From the obtained FT-IR spectrum, it was found that the wave number of 701 cm -1 The height of the peak that appeared (a peak indicating a structure derived from styrene) was read.
[0088] [Measurement of mass average molecular weight and number average molecular weight] The mass average molecular weight and number average molecular weight were measured by the following method. First, 10 mg of the measurement object (polyester resin or toner particles) was mixed with 5 mL of tetrahydrofuran (THF) to obtain a mixture. The obtained mixture was left to stand at room temperature for 2 hours. Next, the mixture was further stirred to thoroughly mix the measurement object and THF. Next, the mixture was passed through a sample treatment filter (Tomsic Corporation, "TITAN2-30PTFE 0.45 μm Eco Pack"), and the mixture that passed through was used as a GPC sample. The mass average molecular weight and number average molecular weight of the resin contained in the GPC sample were measured by gel filtration chromatography (GPC) under the following conditions.
[0089] (GPC conditions) Measuring device: Tosoh Corporation "HLC-8220GPC" Column: Ultra-high performance semi-micro SEC column ("TSKgel SuperMultipore HZ-H" manufactured by Tosoh Corporation, packing material: styrene-divinylbenzene resin, column size: inner diameter 4.6 mm x length 15 cm, packing material particle size: 6 μm) Number of columns: 3 Eluent: Tetrahydrofuran Eluent flow rate: 1.0mL / min Sample solution volume: 150μL Column temperature: 40℃ Detector: RI (refractive index) detector Calibration curve: A calibration curve created using monodisperse polystyrene standard samples (F-40, F-20, F-4, F-1, A-5000, A-2500 and A-1000) manufactured by Tosoh Corporation and n-propylbenzene.
[0090] [Synthesis of amorphous polyester resin] Amorphous polyester resins A to H were prepared by the following method. The softening point (Tm), glass transition point (Tg), acid value, hydroxyl value, mass average molecular weight (Mw) and number average molecular weight (Mn) of the amorphous polyester resins A to H are shown in Table 1 below.
[0091] (Amorphous polyester resin A) A four-neck flask equipped with a thermometer (thermocouple), a dehydration tube, a nitrogen introduction tube, and a stirrer was used as a reaction vessel. 1700 parts by mass of BPA-PO (bisphenol A propylene oxide adduct) and 650 parts by mass of BPA-EO (bisphenol A ethylene oxide adduct) as polyhydric alcohols, 200 parts by mass of dodecenyl succinic anhydride, 400 parts by mass of terephthalic acid, and 100 parts by mass of trimellitic anhydride as polycarboxylic acids, and 4 parts by mass of dibutyltin oxide as a catalyst were added to the reaction vessel. The contents of the reaction vessel were then reacted for 9 hours at a temperature of 220°C and atmospheric pressure while removing water produced by the reaction (first reaction). Thereafter, the contents of the reaction vessel were further reacted at a temperature of 220°C and under reduced pressure (pressure 8.0 kPa) (second reaction). At this time, the reaction time was adjusted to a time at which the softening point of the product (amorphous polyester resin A) reached the temperature shown in Table 1 below. After the reaction was completed, the content of the reaction vessel was removed and cooled, thereby obtaining amorphous polyester resin A (softening point: 124.8° C.).
[0092] (Amorphous polyester resins B to H) Amorphous polyester resins B to H were prepared in the same manner as in the preparation of amorphous polyester resin A, except for the following changes. In the preparation of amorphous polyester resins B to H, the amounts of raw materials used were changed as shown in Table 1 below. In addition, in the preparation of amorphous polyester resins B to H, the reaction time in the second reaction was adjusted so that the softening point of the obtained product was as shown in Table 1 below.
[0093] In the following Table 1, "DDSA" refers to dodecenyl succinic anhydride. "TPA" refers to trimellitic anhydride. "TMA" refers to trimellitic anhydride. "Parts" refers to parts by mass.
[0094] [Table 1]
[0095] [Synthesis of crystalline polyester resin] Crystalline polyester resins a to e were prepared by the following method. The softening point (Tm), melting point (Mp), acid value, hydroxyl value, mass average molecular weight (Mw) and number average molecular weight (Mn) of the crystalline polyester resins a to e are shown in Table 2 below.
[0096] (Crystalline polyester resin a) A four-neck flask equipped with a thermometer (thermocouple), a dehydration tube, a nitrogen introduction tube, and a stirrer was used as a reaction vessel. 995 parts by mass of 1,4-butanediol and 260 parts by mass of 1,6-hexanediol as polyhydric alcohols, 1500 parts by mass of fumaric acid as polycarboxylic acid, and 2.5 parts by mass of hydroquinone were added to the reaction vessel. The contents of the reaction vessel were reacted for 5 hours at a temperature of 170°C and atmospheric pressure while removing water produced by the reaction (first reaction). Next, the contents of the reaction vessel were reacted for another 1.5 hours at a temperature of 210°C and atmospheric pressure (second reaction). Next, the contents of the reaction vessel were reacted for another 1.0 hour at a temperature of 210°C and under a reduced pressure atmosphere (pressure 8.0 kPa) (third reaction). Next, 70 parts by mass of styrene and 50 parts by mass of butyl methacrylate were added to the reaction vessel as vinyl compounds. Next, the contents of the reaction vessel were reacted for an additional 1.5 hours at a temperature of 210°C and atmospheric pressure (fourth reaction). Next, the contents of the reaction vessel were reacted for an additional hour at a temperature of 210°C and in a reduced pressure atmosphere (pressure 8.0 kPa) (fifth reaction). After the fifth reaction was completed, the contents of the reaction vessel were removed and cooled. As a result, crystalline polyester resin a was obtained.
[0097] (Crystalline polyester resins b to e) Crystalline polyester resins b to e were prepared in the same manner as for preparing crystalline polyester resin a, except for the following changes. In preparing crystalline polyester resins b to e, the amounts of raw materials used were changed as shown in Table 2 below. In Table 2 below, "parts" refers to parts by mass.
[0098] [Table 2]
[0099] <Toner Preparation> The toners of Examples 1 to 13 and Comparative Examples 1 to 7 were prepared by the following method.
[0100] [Example 1] Using an FM mixer ("FM-20B" manufactured by Nippon Coke & Engineering Co., Ltd.), 80.0 parts by mass of amorphous polyester resin A and 10.0 parts by mass of crystalline polyester resin a as binder resins, 4.0 parts by mass of carbon black ("MA-100" manufactured by Mitsubishi Chemical Corporation, number average primary particle diameter 24 nm) as a colorant, 5.0 parts by mass of ester wax ("Nissan Electol (registered trademark) WEP-3" manufactured by NOF Corporation, melting point: 73°C) as a release agent, and 1.0 part by mass of a quaternary ammonium salt compound ("BONTRON (registered trademark) P-51" manufactured by Orient Chemical Industry Co., Ltd.) as a charge control agent were mixed at a rotation speed of 200 rpm for 4 minutes.
[0101] The mixture was then melt-kneaded using a twin-screw extruder (Ikegai Corporation, "PCM-30") at a material supply rate of 6 kg / hour, an axis rotation speed of 160 rpm, and a cylinder temperature of 120°C. The kneaded product was then cooled. The kneaded product was coarsely pulverized using a Rotoplex mill (Toa Machinery Manufacturing Co., Ltd., "8 / 16 type"), and then finely pulverized using a mechanical pulverizer (Freund-Turbo Corporation, "Turbo Mill RS"). The finely pulverized product was classified using a classifier (Nitetsu Mining Co., Ltd., "EJ-LABO Model EJ-L-3"). As a result, powdered toner base particles with a volume median diameter of 5.82 μm were obtained.
[0102] 100.0 parts by mass of the above-mentioned toner base particles, 1.2 parts by mass of hydrophobic silica particles ("AEROSIL (registered trademark) RA-200H" manufactured by Nippon Aerosil Co., Ltd., number average primary particle diameter: 12 nm) as an external additive, and 0.8 parts by mass of titanium oxide particles ("EC-100" manufactured by Titanium Kogyo Co., Ltd.) were mixed using an FM mixer ("FM-10" manufactured by Nippon Coke and Engineering Co., Ltd.) at a rotation speed of 3000 rpm and a jacket control temperature of 20° C. for 2 minutes. This produced a black toner of Example 1.
[0103] Except for changing the type of colorant as shown below, the cyan toner of Example 1, the magenta toner of Example 1, and the yellow toner of Example 1 were prepared in the same manner as the preparation of the black toner of Example 1. Hereinafter, the black toner, cyan toner, magenta toner, and yellow toner of Example 1 will be collectively referred to as the "toner of Example 1." Magenta toner colorant: "CI Pigment Red 269" manufactured by Sanyo Pigment Co., Ltd. Cyan toner colorant: "CI Pigment Blue 15:3" manufactured by Sanyo Pigment Co., Ltd. Yellow toner colorant: "CI Pigment Yellow 74" manufactured by Dainichiseika Color & Chemicals Co., Ltd.
[0104] [Examples 2 to 13 and Comparative Examples 1 to 7] The type and amount of the amorphous polyester resin and the crystalline polyester resin used in the preparation of the toner base particles, and the volume median diameter (D 50 ) were changed as shown in Table 3 below, the toners of Examples 2 to 13 and Comparative Examples 1 to 7 were prepared in the same manner as in the preparation of the toner of Example 1. In the measurement of the physical properties and evaluation of the performance of the toners of each Example and Comparative Example, for those not affected by the colorant, the measurement or evaluation was performed using a black toner as a representative example.
[0105] [Table 3]
[0106] [Infrared spectroscopy] The black toners of Examples 1 to 13 and Comparative Examples 1 to 7 were subjected to infrared spectroscopy (FT-IR) by the above-mentioned method to obtain the infrared absorption spectrum of the toner particles. -1 The height of the peak that appeared above was measured. The measurement results are shown in Table 4 below.
[0107] [Measurement of tetrahydrofuran insoluble matter] The content ratio of the tetrahydrofuran insoluble component in the binder resin was measured for the black toners of Examples 1 to 13 and Comparative Examples 1 to 7 by the following method. First, 40 mL of THF (tetrahydrofuran) and 0.05 g of the measurement target were put into a sample bottle. As the measurement target, a mixture of the same composition as the binder resin contained in each toner (for example, in the case of the black toner of Example 1, a mixture of 0.044 g of amorphous polyester resin A and 0.006 g of crystalline polyester resin a) was used. After stirring the contents of the sample bottle for 3 hours using a rotary mixer, the sample bottle was left to stand for 24 hours. Then, 5 mL of the supernatant was collected from the sample bottle with a syringe. The collected 5 mL of the supernatant was transferred to a metal dish and allowed to dry naturally. After drying, the component remaining on the metal dish was taken as the tetrahydrofuran insoluble component of the binder resin before ultrasonic treatment.
[0108] The mass m of the tetrahydrofuran insoluble component in the binder resin before ultrasonic treatment on the metal dish was measured. The value obtained by multiplying the mass m by 8 corresponds to the mass M of the component soluble in 40 mL of THF in 0.05 g of the measurement object. The content ratio of the tetrahydrofuran insoluble component in the binder resin before ultrasonic treatment in the measurement object was calculated by applying the measured mass M to the following formula. The measurement results are shown in Table 4 below. Content of tetrahydrofuran insoluble matter = 100 × [0.05 g - (mass M [g])] / 0.05 g
[0109] Next, the content ratio of the THF insoluble component in the binder resin after ultrasonic treatment was measured for the black toners in Examples 1 to 13 and Comparative Examples 1 to 7. 40 mL of THF (tetrahydrofuran) and 0.05 g of the above-mentioned measurement target (a mixture having the same composition as the binder resin contained in each toner) were put into a sample bottle. The contents of the above-mentioned sample bottle were subjected to ultrasonic treatment at an output of 200 W and a frequency of 28 kHz for 1 minute. Next, the contents of the sample bottle were stirred for 3 hours using a rotary mixer, and the sample bottle was left to stand for 24 hours. Then, 5 mL of the supernatant was collected from the sample bottle with a syringe. The collected 5 mL of the supernatant was transferred to a metal dish and allowed to dry naturally. After drying, the components remaining on the metal dish were taken as the tetrahydrofuran insoluble components of the binder resin after ultrasonic treatment. Then, the content ratio of the tetrahydrofuran insoluble components of the binder resin after ultrasonic treatment was calculated by the same method as that for measuring the content ratio of the tetrahydrofuran insoluble components of the binder resin before ultrasonic treatment. The measurement results are shown in Table 4 below.
[0110] [Mass average molecular weight of resin contained in toner particles] The mass average molecular weight of the resin contained in the toner particles was measured by the above-mentioned method for the black toners of Examples 1 to 13 and Comparative Examples 1 to 7. The measurement results are shown in Table 4 below.
[0111] [Table 4]
[0112] <Evaluation> The toners of Examples 1 to 13 and Comparative Examples 1 to 7 were evaluated for color development, low-temperature fixability, and heat-resistant storage stability of the images formed by the toners. The evaluations were performed at a temperature of 23° C. and a humidity of 50%, unless otherwise specified. The evaluation results are shown in Table 5 below.
[0113] [Preparation of developer] Using a powder mixer (Aichi Electric Co., Ltd.'s "Rocking Mixer (registered trademark)", mixing method: container rotation rocking method), 8 parts by mass of the toner to be evaluated (any of the toners in Examples 1 to 13 and Comparative Examples 1 to 7) and 100 parts by mass of the carrier (Kyocera Document Solutions Co., Ltd.'s "TASKalfa 7054ci" carrier) were mixed for 30 minutes. As a result, evaluation initial developers (specifically, evaluation black initial developer, evaluation magenta initial developer, evaluation cyan initial developer, and evaluation yellow initial developer) containing the toner to be evaluated (toner concentration about 7% by mass) were obtained.
[0114] In addition, 100 parts by mass of toner (any of the toners in Examples 1 to 13 and Comparative Examples 1 to 7) and 10 parts by mass of carrier (carrier for "TASKalfa 7054ci" manufactured by Kyocera Document Solutions Co., Ltd.) were mixed for 30 minutes using the above-mentioned powder mixer. As a result, refill developers (specifically, refill black developer for evaluation, refill magenta developer for evaluation, refill cyan developer for evaluation, and refill yellow developer for evaluation) containing the toner to be evaluated (toner concentration about 91% by mass) were obtained.
[0115] [Evaluation machine] A color multifunction printer (TASKalfa 7054ci manufactured by Kyocera Document Solutions Inc., photoconductor drum: amorphous silicon drum) was used as the evaluation machine. This evaluation machine was equipped with a photoconductor, a developing device that develops an electrostatic latent image formed on the photoconductor with a developer (specifically, a toner contained in the developer), a developer discharge section that discharges the developer in the developing device, a replenishment developer supply section that replenishes the replenishment developer into the developing device, and a fixing device that fixes the toner to a recording medium. That is, this evaluation machine adopted a trickle development method. An initial developer for evaluation (specifically, any of the black initial developer for evaluation, the magenta initial developer for evaluation, the cyan initial developer for evaluation, and the yellow initial developer for evaluation) was put into the developing device of the evaluation machine (specifically, any of the black initial developer for evaluation, the magenta initial developer for evaluation, the cyan initial developer for evaluation, and the yellow initial developer for evaluation). In addition, a refill developer (specifically, any one of a refill black developer for evaluation, a refill magenta developer for evaluation, a refill cyan developer for evaluation, and a refill yellow developer for evaluation) was added to the refill black developer supplying section of the evaluation machine. The evaluation machine had a linear speed of 322 mm / sec and a toner loading amount of 0.37 mg / cm. 3 The evaluation machine was modified so that the fixing temperature of the fixing device could be set as desired. A4-sized plain paper ("C" paper by Fujifilm Business Innovation Co., Ltd.) was used as the recording medium. 2 ") was used.
[0116] [Color development] Using the evaluation machine, solid images (specifically, black solid image, cyan solid image, magenta solid image, and yellow solid image) were formed on the recording medium. The fixing temperature of the fixing device was set to 170°C. Using a fluorescent spectrodensitometer ("FD-5" manufactured by Konica Minolta, Inc.), the lightness (L*) of the black solid image and the chroma (C*) of the cyan solid image, magenta solid image, and yellow solid image were measured. The L* of the black solid image is judged to be less than 18.0 as pass, and 18.0 or more as fail. The C* of the cyan solid image is judged to be 60.0 or more as pass, and less than 60.0 as fail. The C* of the magenta solid image is judged to be 72.0 or more as pass, and less than 72.0 as fail. The C* of the yellow solid image is judged to be 97.0 or more as pass, and less than 97.0 as fail. The color development was evaluated according to the following criteria. In Table 5 below, "C / M / Y / K" in color development indicates the chroma (C*) of the cyan solid image, magenta solid image, and yellow solid image, and the lightness (L*) of the black solid image. For example, "62.2 / 74.1 / 99.3 / 16.2" in "C / M / Y / K" in Example 1 indicates that the C* of the cyan solid image is 62.2, the C* of the magenta solid image is 74.1, the C* of the yellow solid image is 99.3, and the L* of the black solid image is 16.2.
[0117] (Color development criteria) A (good): All of L* of the black solid image, C* of the cyan solid image, C* of the magenta solid image, and C* of the yellow solid image passed. B (poor): At least one of L* of a black solid image, C* of a cyan solid image, C* of a magenta solid image, and C* of a yellow solid image was unacceptable.
[0118] [Low temperature fixability] Using the evaluation machine, a black solid image (specifically, an unfixed toner image before passing through the fixing device) measuring 25 mm x 25 mm was formed on the recording medium. The recording medium (evaluation paper) on which the black solid image was formed was then passed through the fixing device of the evaluation machine. At this time, the fixing temperature of the fixing device was increased by 5°C from 120°C to 220°C, and the possibility of fixing was judged for each fixing temperature, and the minimum temperature (minimum fixing temperature) at which the black solid image (toner image) could be fixed to the evaluation paper was measured.
[0119] Whether the toner could be fixed was evaluated by the folding and rubbing test shown below. In the folding and rubbing test, the evaluation paper was folded so that the surface on which the black solid image was formed was on the inside and the crease passed through the center of the black solid image. Next, the folded evaluation paper was rubbed back and forth five times on the crease while applying a load of 1 kg using a brass weight (1 kg) covered with cotton cloth. Next, the evaluation paper was unfolded, and the length of peeling of the toner (peeling length) in the part of the folded part of the evaluation paper where the black solid image was fixed was measured. If the peeling length was 1 mm or less, it was determined that the folding and rubbing test was passed and the toner was fixed to the evaluation paper. If the peeling length was more than 1 mm, it was determined that the folding and rubbing test was failed and the toner was not fixed to the evaluation paper. For each evaluation developer, the formation of the black solid image and the folding and rubbing test were repeated while changing the fixing temperature, and the minimum temperature (minimum fixing temperature) among the fixing temperatures that passed the folding and rubbing test was obtained. The low-temperature fixability was judged according to the following criteria.
[0120] (Low temperature fixability standard) A (very good): The minimum fixing temperature is 150° C. or lower. B (Good): The minimum fixing temperature is 155°C or higher and 160°C or lower. C (poor): The minimum fixing temperature is 165° C. or higher.
[0121] [Heat-resistant storage stability] 3 g of the toner to be evaluated (specifically, black toner among the toners of Examples 1 to 13 and Comparative Examples 1 to 7) was placed in a polyethylene container with a capacity of 20 mL. The above container was left standing for 3 hours in a thermostatic chamber set at 55° C. After leaving it for 3 hours, the container was removed from the thermostatic chamber. The toner was removed from the container and used as the toner for evaluation. The obtained toner for evaluation was placed on a 200 mesh (75 μm opening) sieve with a known mass. Then, the mass of the sieve containing the toner for evaluation was measured to determine the mass of the toner before sieving. Next, the sieve was set in a powder property evaluation device ("Powder Tester (registered trademark) PT-X" manufactured by Hosokawa Micron Corporation), and the sieve was vibrated for 30 seconds at an amplitude of 1.0 mm according to the manual of the powder property evaluation device to sieve the toner for evaluation. After sieving, the mass of the toner that did not pass through the sieve was measured. Then, based on the mass of the toner before sieving and the mass of the toner after sieving, the degree of cohesion [mass %] was calculated according to the following formula. In the formula, the "mass of the toner after sieving" is the mass of the toner that did not pass through the sieve (i.e., the toner that remained on the sieve after sieving). The heat-resistant storage stability was evaluated according to the following criteria. Cohesion degree [mass %] = 100 × mass of toner after sieving / mass of toner before sieving
[0122] (Standards for heat resistance storage) A (very good): The degree of aggregation is 10% by mass or less. B (Good): The degree of aggregation is more than 10% by mass and 20% by mass or less. C (poor): The degree of aggregation is more than 20% by mass.
[0123] [Table 5]
[0124] The toners of Examples 1 to 13 contained toner particles. The toner particles were provided with toner base particles and an external additive attached to the surface of the toner base particles. The toner base particles were pulverized toner base particles. The volume median diameter of the toner base particles was 5.20 μm or more and 6.50 μm or less. The toner base particles contained a binder resin. The content of tetrahydrofuran insoluble components in the binder resin was 4.50 mass % or more and 16.00 mass % or less. The content of tetrahydrofuran insoluble components in the binder resin after ultrasonic treatment at an output of 200 W and a frequency of 28 kHz for 1 minute was 2.20 mass % or less. In the infrared absorption spectrum of the toner particles obtained by infrared spectroscopy, -1 The height of the peak appearing at the top was 0.0070A or more and 0.0300A or less. The toners of Examples 1 to 13 were excellent in low-temperature fixing property and heat-resistant storage stability, and were able to form images with excellent color development. In addition, the toners of Examples 1 to 11 had a mass average molecular weight of the resin contained in the toner particles of 85,000 or more and 130,000 or less. As a result, the toners of Examples 1 to 11 had extremely good low-temperature fixing property and heat-resistant storage stability.
[0125] In contrast, the toner of Comparative Example 1 had an excessively small volume median diameter of the toner base particles. Also, the toner of Comparative Example 2 had an excessively large volume median diameter of the toner base particles. When the toner base particles are either excessively large or excessively small in size, it becomes difficult for them to adequately cover the surface of the recording medium and impart color development to the image. Therefore, the toners of Comparative Examples 1 and 2 formed images with poor color development.
[0126] The toner of Comparative Example 3 had a tetrahydrofuran insoluble component content of less than 4.50% by mass in the binder resin. The toner of Comparative Example 3 lacked the tetrahydrofuran insoluble component, which is a component that imparts elasticity to the binder resin. Therefore, the toner of Comparative Example 3 had poor heat resistance storage stability.
[0127] The toner of Comparative Example 4 had a tetrahydrofuran insoluble component content in the binder resin of more than 16.00% by mass. The toner of Comparative Example 4 contained an excessive amount of tetrahydrofuran insoluble components, which are components that inhibit the toner particles from dissolving and spreading during fixing. As a result, the toner of Comparative Example 4 had poor color development of the formed image.
[0128] The toner of Comparative Example 5 had a tetrahydrofuran insoluble component content in the binder resin after ultrasonic treatment of more than 2.20% by mass. It is considered that the components that are not solubilized in tetrahydrofuran even after ultrasonic treatment strongly inhibit the toner particles from dissolving and spreading during fixing. The toner of Comparative Example 5 had poor color development due to the excessive content of such components.
[0129] The toner of Comparative Example 6 has a wave number of 701 cm in the infrared absorption spectrum of the toner particles. -1 The height of the peak that appeared above was less than 0.0070A. The height of the above peak indicates the amount of the structure derived from styrene contained in the toner particles. The structure derived from styrene imparts charging properties to the toner. The toner of Comparative Example 6 had an insufficient amount of the structure derived from styrene, so the charging amount was insufficient and the color development of the formed image was poor.
[0130] The toner of Comparative Example 7 has a wave number of 701 cm in the infrared absorption spectrum of the toner particles. -1 The height of the peak that appeared on the top was less than 0.0070 A. The structure derived from styrene is effective in imparting chargeability to toner particles if it is present in an appropriate amount, but if it is present in excess, it reduces the heat-resistant storage stability of the toner. Therefore, the toner of Comparative Example 7 had poor heat-resistant storage stability. [Industrial Applicability]
[0131] The toner of the present invention can be used to form images in, for example, a copier, a printer, or a multifunction machine. [Explanation of symbols]
[0132] 1 Toner particles 2. Toner base particles 3. External additives 4. Silica particles 5 Other external additive particles
Claims
1. A toner comprising toner particles, The toner particles include a toner base particle and an external additive attached to a surface of the toner base particle, the toner base particles are pulverized toner base particles, The volume median diameter of the toner base particles is 5.20 μm or more and 6.50 μm or less, The toner base particles contain a binder resin, The content of the tetrahydrofuran insoluble component in the binder resin is 4.50% by mass or more and 16.00% by mass or less, the content of the tetrahydrofuran insoluble component in the binder resin after one minute of ultrasonic treatment at an output of 200 W and a frequency of 28 kHz is 2.20 mass% or less; In the infrared absorption spectrum of the toner particles obtained by infrared spectroscopy, the wave number is 701 cm -1 The height of the peak appearing on the toner is 0.0070 A or more and 0.0300 A or less.
2. 2. The toner according to claim 1, wherein the mass average molecular weight of the resin contained in the toner particles is 85,000 or more and 130,000 or less.
3. The binder resin includes an amorphous polyester resin, The amorphous polyester resin has a first repeating unit derived from a trivalent or higher carboxylic acid, 3. The toner according to claim 1, wherein a content ratio of the first repeating unit in all repeating units contained in the amorphous polyester resin is 1.5% by mass or more and 7.5% by mass or less.
4. The toner according to claim 3 , wherein the amorphous polyester resin further comprises a second repeating unit derived from a bisphenol compound and a third repeating unit derived from a divalent carboxylic acid.
5. The binder resin includes a crystalline polyester resin, The crystalline polyester resin has a fourth repeating unit derived from a styrene compound, 3. The toner according to claim 1, wherein a content ratio of the fourth repeating unit in all repeating units contained in the crystalline polyester resin is 0.5% by mass or more and 8.0% by mass or less.
6. The toner according to claim 5 , wherein the crystalline polyester resin further comprises a fifth repeating unit derived from a diol compound, a sixth repeating unit derived from a divalent carboxylic acid, and a seventh repeating unit derived from an alkyl (meth)acrylate ester.
7. The toner according to claim 5, wherein the crystalline polyester resin has a mass average molecular weight of 20,000 or more and 60,000 or less.
8. The toner according to claim 5, wherein the acid value of the crystalline polyester resin is from 2.0 mgKOH / g to 3.7 mgKOH / g.
Citation Information
Patent Citations
Toner for electrostatic charge image development and manufacturing method of the same, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2012220569A