Glaze composition

A glaze composition with crystalline alumina and zircon forms a single layer with subdued color and low gloss, addressing the need for aesthetically pleasing and durable ceramic products for exterior use.

JP2024162940AActive Publication Date: 2024-11-21HAKUSUI CHEM IND +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023100080
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2023-06-19
Publication Date
2024-11-21
Estimated Expiration
2043-06-19

AI Technical Summary

Technical Problem

Existing glaze compositions fail to provide a glaze layer with suppressed gloss and subdued color tone suitable for ceramic products used in exterior construction and wall materials, which are aesthetically preferred and require durability against weathering.

Method used

A glaze composition containing crystalline alumina and crystalline zircon in specific ratios, along with other components like feldspar, silica, clay, and a solvent, is applied to form a single glaze layer with a red color tone and low gloss.

Benefits of technology

The glaze layer achieves a calm color tone with low gloss, making ceramic products suitable for exterior applications, enhancing their aesthetic appeal and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162940000001
    Figure 2024162940000001
  • Figure 2024162940000002
    Figure 2024162940000002
  • Figure 2024162940000003
    Figure 2024162940000003
Patent Text Reader

Abstract

To provide a glaze composition that can form a glazed layer with the glossiness restrained and capable of imparting an inconspicuous color tone onto a ceramic product, and a production method of the ceramic product used with the glaze composition.SOLUTION: A glaze composition according to the present invention contains crystalline alumina and crystalline zircon. The glaze composition has a ratio of the crystalline zircon of 50 mass% or more and 70 mass% or less on the basis of the total amount of the crystalline alumina and the crystalline zircon.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glaze composition capable of forming a glaze layer having a suppressed gloss and capable of imparting a subdued color tone to a ceramic product, and a method for manufacturing a ceramic product using the glaze composition. [Background technology]

[0002] A glaze layer is a glassy film that covers the surface of a ceramic product, and it not only gives the ceramic product a variety of colors and textures, but also prevents water and dirt from penetrating the base material, and increases its strength to make it durable and easy to handle. A glaze composition generally contains an alkali component that increases the solubility of the glaze components, feldspar or silica containing glass components, and clay that increases adhesion to the base material. In addition, the color and texture of the glaze layer can be adjusted by adjusting the composition of the components.

[0003] For example, Patent Document 1 discloses a glaze layer having high diffuse reflectivity, which has a first glaze layer containing Al and / or Zr and a glassy component, and a second glaze layer containing zirconium silicate particles, white inorganic oxide particles, and a glassy component. Patent Document 2 discloses a glaze composition that includes a frit containing zirconium element and zirconium silicate particles, and can realize a glaze layer that is high diffuse reflectivity and also has stain resistance.

[0004] Patent Document 3 discloses a clay tile having a first glaze layer disposed on the back surface of a base layer and a second glaze layer disposed on the front surface of the base layer, in which the glaze constituting the first glaze layer contains one or more materials selected from the group consisting of α-alumina, zircon, spodumene, petalite, and cordierite, and which has high bending fracture strength and small mass.

[0005] Patent Document 4 discloses a glaze that contains a basic glaze, a borosilicate frit which is a frit whose main components are boric acid and silicic acid, and aluminum phosphate and / or an aluminum phosphate compound, and that can form a glaze layer that is difficult to separate from a base layer.

[0006] Patent Document 5 discloses a glaze that may contain zircon and the like in addition to a lithium-containing material. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2014-193803 A [Patent Document 2] JP 2014-166925 A [Patent Document 3] JP 2017-190645 A [Patent Document 4] JP 2004-210612 A [Patent Document 5] JP 2003-238238 A Summary of the Invention [Problem to be solved by the invention]

[0008] As described above, various techniques for forming a glaze layer having various properties have been developed. For example, Patent Documents 1 and 2 disclose glaze compositions for forming a glaze layer having high diffuse reflectance. It is true that materials for tiles and toilets used in bathrooms and other places tend to be blue, which gives a refreshing feeling, and have a high gloss. On the other hand, for exteriors and walls, ceramic products with a muted red color and low gloss are preferred. If the glaze layer is not formed, a ceramic product with a low gloss will be obtained, but from the standpoint of aesthetics and durability against rain and temperature changes, it is better to use a glaze. It is preferable to provide a layer. Therefore, an object of the present invention is to provide a glaze composition capable of forming a glaze layer having a suppressed gloss and capable of imparting a subdued color tone to a ceramic product, and a method for manufacturing a ceramic product using the glaze composition. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that a glaze layer capable of imparting a reddish color tone with suppressed gloss can be formed using a glaze composition containing crystalline alumina and crystalline zircon in a specific ratio, and have completed the present invention. The present invention will now be described.

[0010] [1] It contains crystalline alumina and crystalline zircon. A glaze composition, characterized in that the proportion of the crystalline zircon with respect to the total of the crystalline alumina and the crystalline zircon is 50 mass % or more and 70 mass % or less. [2] The glaze composition according to [1], wherein the total ratio of the crystalline alumina and the crystalline zircon in the glaze layer forming components is 2% by mass or more and 25% by mass or less. [3] The glaze composition according to [1], wherein the mixture of the crystalline alumina and the crystalline zircon has a volume-based average particle size of 0.5 μm or more and 2 μm or less. [4] The glaze composition according to [1] above, further comprising water. [5] The glaze composition according to [1] above, further comprising feldspar and / or silica. [6] The glaze composition according to [1] above, further comprising a thickener. [7] The glaze composition according to [1] above, further comprising clay. [8] The glaze composition according to [1] above, further comprising an alkaline component. [9] A step of applying the glaze composition according to any one of [1] to [8] to a base material; and A method for producing a ceramic product, comprising the step of firing the base material. Effect of the Invention

[0011] The glaze layer formed on the base material by the glaze composition according to the present invention is reddish in color and has a muted color tone with low gloss. Therefore, the ceramic product having the glaze layer formed by the glaze composition according to the present invention is very useful industrially as a building material that requires a muted color tone, such as an exterior construction material or an exterior wall material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The glaze composition according to the present invention contains crystalline alumina (Al2O3) and crystalline zircon (ZrSiO4).

[0013] Crystalline alumina is a particle of alumina having a crystalline structure, and is different from a composite oxide that forms a crystalline structure with other metal oxides. It is also different from amorphous and non-crystalline glass or frit formed by mixing with other components. That is, general glass contains silica (SiO2), and while silica can be vitrified by itself, alumina cannot be vitrified by itself, but when mixed with silica, etc., it becomes amorphous and non-crystalline glass. Frit is used to suppress the absorption of water-soluble components such as sodium carbonate and potassium carbonate into the base material, and is a vitreous particle manufactured by mixing water-soluble components with silica, alumina, etc. in advance and heating them. Although the melting point of alumina is over 2000°C, it can be melted at less than 1000°C by mixing it with other components and heating it, and becomes amorphous and non-crystalline glass. Glass and frit are generally transparent and are distinguished from white crystalline alumina.

[0014] Crystalline zircon is not a simple mixture of zirconia (ZrO2) and silica (SiO2), but a composite oxide of zirconia and silica, and is used as a white pigment like crystalline alumina. Note that crystalline zircon is not a composite oxide that forms crystals with metal oxides other than zirconium and silicon, like crystalline alumina.

[0015] In the glaze composition according to the present invention, the ratio of crystalline zircon to the total of crystalline alumina and crystalline zircon is adjusted to 50% by mass or more and 70% by mass or less. By adjusting the ratio within the range, the color tone of the glaze layer formed from the glaze composition according to the present invention becomes warm, that is, the a* value in the L*a*b* color system becomes a positive value, and the gloss level becomes sufficiently low. The ratio is preferably 65% ​​by mass or less, more preferably 60% by mass or less.

[0016] The ratio of crystalline zircon to the total of crystalline alumina and crystalline zircon may be determined from the amounts of crystalline alumina and crystalline zircon blended when the glaze composition according to the present invention is prepared, but when the amounts of each are unknown after preparation, it can be determined by combining X-ray fluorescence analysis and quantification of zirconia based on Test Example 1 described below. X-ray fluorescence analysis can identify the types and relative ratios of elements contained in a sample, but cannot distinguish between the zirconium oxide and silicon oxide components contained in zircon, which is a composite oxide, and zirconia and silica present alone. Therefore, by referring to "Quantitative Determination of Unreacted Zirconia in the Reaction of Zirconia and Silica to Form Zircon," Analytical Chemistry, Vol. 27, pp. 362-365 (1978) by Minoru Hashiba, Eiji Miura, Yukio Nurishi, and Yasuzo Hibino, the ratio of zirconium oxide contained in zircon in zirconium oxide measured by X-ray fluorescence analysis to zirconia present alone can be determined, and the ratio of alumina and zircon in the sample can be determined. Specifically, 10 times the amount of ammonium sulfate is added as a flux to the zirconia in the sample determined by X-ray fluorescence analysis, and the sample is heated at 400-450°C for 1-2 hours, after which the zirconia present alone is selectively dissolved and extracted in 4N sulfuric acid, filtered, and the solids are washed with warm water. The filtrate and washing water are combined, and ammonia water is gradually added until a gel-like precipitate is formed, filtered, and thoroughly washed with 2% warm ammonium nitrate aqueous solution. The solid obtained is heated to 1000°C and weighed, so that the amount of zirconia present independently can be measured, and the ratio of zircon to zirconia present independently in the sample can be calculated.

[0017] The crystalline alumina and crystalline zircon according to the present invention do not include, for example, amorphous vitreous alumina contained in frit, etc. Since white crystalline alumina and crystalline zircon can be distinguished from vitreous frit, etc., by microscopic observation, for example, the frit in a predetermined amount of sample is removed under microscopic observation, and the ratio of crystalline zircon to the total of crystalline alumina and crystalline zircon in the remaining sample is obtained by the above-mentioned method.

[0018] In the glaze composition according to the present invention, the amount of crystalline alumina and crystalline zircon is preferably adjusted appropriately within a range in which the color tone of the glaze layer can be adjusted. For example, the total ratio of crystalline alumina and crystalline zircon in the glaze layer forming components is preferably 2% by mass or more and 25% by mass or less. If the ratio is 2% by mass or more, the color tone of the glaze layer can be more reliably adjusted. If the ratio is 25% by mass or less, the blending of general components of the glaze composition can be more reliably performed. The ratio is preferably 5% by mass or more, more preferably 10% by mass or more, and more preferably 22% by mass or less, more preferably 20% by mass or less. The glaze layer forming components are components that form the glaze layer, and refer to solid components other than those that are decomposed by firing and substantially removed from the glaze layer, such as solvents and thickeners, and mainly refer to metal oxides.

[0019] The total amount of crystalline alumina and crystalline zircon relative to the entire glaze composition according to the present invention, including the solvent, may be appropriately adjusted, but is preferably, for example, 1 mass % or more and 20 mass % or less.

[0020] The glaze composition according to the present invention preferably contains a solvent. A glaze composition containing a solvent has the advantage of being easily applied to a substrate. Examples of the solvent include water, glycerin, polyethylene glycol, monoethylene glycol, and a mixed solvent of two or more of these. Organic solvents other than water are used to dissolve or disperse each component, as well as to adjust the viscosity.

[0021] The amount of the solvent in the glaze composition may be appropriately adjusted, but may be, for example, 5% by mass or more and 60% by mass or less with respect to the entire glaze composition. The proportion is preferably 10% by mass or more, more preferably 20% by mass or more, and is preferably 50% by mass or less.

[0022] Glaze compositions generally contain an alkaline component that improves the solubility and decomposition of each component, a component that improves the adhesion between the glaze layer and the base, and a component that melts upon firing to form a transparent glaze layer.

[0023] A typical glaze composition includes feldspar, silica, and clay. Feldspar generally has the chemical formula (K,Na,Ca,Ba)(Al,Si)4O8, which is the Si content in SiO4. 4+ Part of the material is Al. 3+ The SiO4 tetrahedrons are filled with K to neutralize the charge change. + ,Na + ,Ca 2+ ,Ba 2+ It has a crystal structure containing Al, etc. Naturally occurring feldspar is mainly classified into a ternary system with end members KAlSiO8 (potassium feldspar), NaAlSiO8 (sodium feldspar), and CaAlSiO8 (calcium feldspar), and KAlSiO8-NaAlSiO8 and NaAlSiO8-CaAlSiO8 form continuous solid solutions, and each series is collectively called alkali feldspar and plagioclase. Thus, although feldspar contains Al, it forms a composite oxide and does not contain crystalline alumina alone, so in this disclosure, crystalline alumina and the Al contained in feldspar are considered to be the same. 3+ and aluminum composite oxides are to be distinguished.

[0024] Silica is mainly composed of silica, and melts during firing to form a transparent glaze layer. Note that zircon contains silicon (Si), but is a composite oxide with zirconium, so in this disclosure, silica and silica are distinguished from crystalline zircon.

[0025] The proportion of feldspar and / or silica in the glaze composition according to the present invention may be appropriately adjusted within a range that provides a glaze layer that has high adhesion to the base and is aesthetically pleasing. For example, it is preferably 10% by mass or more and 50% by mass or less. The proportion of feldspar and / or silica in the glaze layer forming components is preferably 20% by mass or more and 95% by mass or less.

[0026] Clay is a mineral particle of less than 2μm in size according to international law, and is mainly composed of aluminum silicate crystals. By adding clay to the glaze, the adhesion between the base and the glaze layer is improved.

[0027] The proportion of clay in the glaze composition according to the present invention may be appropriately adjusted within a range that provides high adhesion to the base. For example, it is preferably 1% by mass or more and 30% by mass or less. The proportion of clay in the glaze layer forming components is preferably 2% by mass or more and 60% by mass or less.

[0028] The glaze composition may contain a thickener. The thickener increases the viscosity of the glaze composition, and can suppress dripping even when the composition is applied thickly to a base material. Examples of the thickener include carboxymethylcellulose (CMC), dextrin, gum arabic, glaze bond, etc.

[0029] The proportion of the thickener in the glaze composition according to the present invention may be appropriately adjusted so that the viscosity of the glaze composition falls within an appropriate range, for example, preferably from 0.01% by mass to 5% by mass.

[0030] The glaze composition may contain an alkaline component. The alkaline component has the effect of increasing the solubility and decomposition of insoluble or poorly soluble components in a solvent. The alkaline component itself remains as an oxide to form the glaze layer. Examples of the alkaline component include calcium compounds such as calcium oxide, calcium carbonate, limestone, marble, ash, wollastonite, and calcium phosphate; strontium carbonate; barium compounds such as barium carbonate and barium sulfate; lithium carbonate; and zinc oxide. Potassium and sodium are also contained in feldspar, lithium is contained in petalite and spodumene, and magnesium is contained in talc and dolomite, but these are generally contained as complex oxides, and therefore, in the present disclosure, they are distinguished from the alkaline component. Frits containing potassium, sodium, lithium, and the like are also distinguished from the alkaline component.

[0031] The proportion of the alkaline component in the glaze composition according to the present invention may be appropriately adjusted within a range that improves the solubility and decomposition of insoluble or poorly soluble components in a solvent. For example, the alkaline component may not be blended. When the alkaline component is blended, the proportion of the alkaline component is preferably more than 0% by mass and 15% by mass or less. In addition, the proportion of the alkaline component in the glaze layer forming components is preferably 0% by mass or more and 30% by mass or less.

[0032] In the glaze composition, it is preferable to finely grind the particles. For example, the average particle diameter of the glaze composition is preferably 1 μm or more and 50 μm or less. If the average particle diameter is 50 μm or less, a glaze layer with a sufficiently smooth texture can be formed. If the average particle diameter is 1 μm or more, excessive energy is not required for grinding. The average particle diameter is more preferably 5 μm or more, more preferably 10 μm or more, more preferably 30 μm or less, and even more preferably 20 μm or less. In the present disclosure, the average particle diameter is measured by a laser diffraction type particle size distribution measuring device, and the standard of the average particle diameter includes volume standard, weight standard, number standard, etc., and the volume standard is preferable.

[0033] The volumetric average particle size of the mixture of the crystalline alumina and the crystalline zircon in the glaze composition is preferably 0.5 μm or more and 2 μm or less. If the average particle size is 0.5 μm or more, excessive energy is not required for crushing the particles, and the possibility of excessively reducing productivity is relatively low, and if it is 2 μm or less, the brightness of the glaze layer can be sufficiently increased.

[0034] The glaze composition according to the present invention is preferably used to form a single glaze layer. In some cases, two or more glaze layers are laminated, but in such cases, the glaze composition must be repeatedly applied to the base material and dried, which reduces production efficiency. In contrast, the glaze composition according to the present invention can form a single glaze layer with a low gloss and a subdued color tone.

[0035] A method for producing a ceramic product by forming a glaze layer on a base material using the glaze composition according to the present invention will be described below.

[0036] 1. Coating process In this step, the glaze composition according to the present invention is applied to the base material. In the present disclosure, the base material refers to the stage before the application of the glaze in the ceramic industry. For example, it refers to a product that has been molded and fired. The firing conditions for the base material may be such that the base material is completely fired, or the firing temperature may be lower than the firing temperature of the glaze composition.

[0037] The coating amount of the glaze composition may be appropriately adjusted according to the desired glaze layer. For example, it is 0.02 g / cm per unit area of ​​the base material. 2 More than 0.2g / cm 2 It can be as follows:

[0038] 2. Firing process In this step, the base coated with the glaze composition is fired to form a glaze layer on the base. The firing temperature may be adjusted as appropriate depending on the composition of the base, but it is preferable to finally fire the base at a temperature of 800°C or higher and 1300°C or lower. It is also preferable to increase the firing temperature stepwise or continuously from about 100°C, taking into account the distillation of the solvent and the decomposition of the thickener.

[0039] The glaze layer formed by the glaze composition according to the present invention has a chromaticity of a * Since the glaze layer is reddish in color with a positive value of γ and has a subdued color tone with low gloss, the ceramic product having the glaze layer is useful as a building material where a subdued color tone is required, such as an exterior construction material or exterior wall material. EXAMPLES

[0040] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and it is possible to carry out the present invention by making appropriate modifications within the scope of the above and below-mentioned aims, and all of these modifications are included in the technical scope of the present invention.

[0041] Examples 1 and 2 (1) Preparation of glazed samples The composition shown in Table 1 and 10 mm alumina balls (400 g) were placed in a ball mill (Marugama Seitosho Co., Ltd., internal volume: 400 mL) and were ground and mixed for 1 hour.

[0042] [Table 1]

[0043] Separately, a clay pot ("G-99" manufactured by Sabri) was molded into a 5cm x 5cm x 0.5cm square shape, and the temperature was raised from room temperature to 1000°C over 3 hours, then from 1000°C to 1215°C over 4 hours, and the temperature was maintained at 1215°C for 4 hours to obtain the green body. The temperature of the Referthermo was 1240°C. The glaze composition (2.5 g) was sprayed onto the base using a spray gun, and the temperature was raised from room temperature to 200°C in 1 hour, from 200°C to 400°C in 1 hour, from 400°C to 600°C in 1 hour, from 600°C to 800°C in 1 hour, from 800°C to 1000°C in 1 hour, and from 1000°C to 1160°C in 1 hour, and then fired at 1160°C for 4 hours to obtain a glazed sample. The temperature of the Refer Thermo was 1187°C.

[0044] (2) Measurement of color difference Using a spectrophotometer ("CM-5" manufactured by Konica Minolta), the lightness L * , chromaticity a * and b * The light source used was D65, the field of view was set at 10°C, and the measurement diameter was set at 8 mm. Each item was measured at five points on one sample, and the average value was calculated. The results are shown in Table 2.

[0045] (3) Gloss measurement The gloss of the glazed samples obtained above was measured using a gloss checker ("IG-320" manufactured by Horiba, Ltd.). The incident angle of the irradiation light was set to 60°. Measurements were taken at two points for each sample, and the average value was calculated. The results are shown in Table 2. In Table 2, alumina and zircon are both crystalline.

[0046] [Table 2]

[0047] As shown in Table 2, the brightness of the sample glazed with the glaze composition of the present invention is high and bright, while the chromaticity a * is a positive value leaning towards magenta, and the low gloss level in particular demonstrates that the color tone is subdued.

[0048] Test Example 1: Measurement of alumina / zircon ratio (1) Preparation of calibration curve by X-ray fluorescence analysis Zirconium oxide (Kishida Chemical Co., Ltd., purity 99.9%), silicon oxide (Kojundo Chemical Laboratory Co., Ltd., purity 99.9%), and alumina (Kishida Chemical Co., Ltd., special grade, purity 99.0%) were mixed thoroughly in a mortar in the composition shown in Table 3 to prepare a sample for the calibration curve. Note that "%" below indicates "% by mass."

[0049] [Table 3]

[0050] 0.4 g of each calibration curve sample and 4 g of anhydrous lithium tetraborate (Kishida Chemical Co., Ltd., purity 98.0%) for fluorescent X-ray analysis were weighed and mixed, and glass beads were prepared using a benchtop high-frequency bead sampler. Using the five glass beads thus obtained, calibration curves showing the relationship between the fluorescent X-ray intensity of zirconium oxide, silicon oxide, and alumina and their concentrations in each sample were created using an X-ray fluorescence analyzer.

[0051] (2) Measurement of analytical samples A reference sample with a mass ratio of alumina:zircon = 45:55 was subjected to fluorescent X-ray analysis, and the concentrations of zirconium oxide, silicon oxide, and alumina in the reference sample were determined using a calibration curve. The results are shown in Table 4.

[0052] [Table 4]

[0053] (3) Quantitative analysis of zirconia X-ray fluorescence analysis cannot distinguish between the zirconium oxide and silicon oxide components contained in zircon, which is a composite oxide, and zirconia and silica that exist independently. Therefore, the amount of zirconia in the reference sample was quantified with reference to Minoru Hashiba, Eiji Miura, Yukio Nurishi, and Yasuzo Hibino, "Quantitative Determination of Unreacted Zircon in the Reaction of Zircon and Silica to Form Zircon," Analytical Chemistry, Vol. 27, pp. 362-365 (1978). 0.2g of the reference sample and 2g of ammonium sulfate (Kishida Chemical, special grade, purity 99.5%) as a flux were weighed out and mixed thoroughly in a mortar. The mixed sample was calcined at 450°C for 2 hours, after which 4N sulfuric acid was added and the mixture was filtered to separate the filtrate from the residue, which was then washed with warm water. The filtrate and washings were combined, and ammonia water was added to check for any cloudy matter, but none was detected. This confirmed that the reference sample did not contain zirconia, and all of the zirconium oxide detected by X-ray fluorescence analysis was a component contained in zircon. Since the molecular weight of silicon oxide is 60.09 and that of zirconium oxide is 123.22, the molar ratio of silicon oxide to zirconium oxide in the reference sample was calculated to be 17.74 / 60.09:36.21 / 123.22 = 29.5:29.4, and it was believed that the reference material contained a small amount of silica. By subtracting the free silica from the silicon oxide in the X-ray fluorescence analysis, the calculation was 17.74-60.09 x 0.001 = 17.68%. Therefore, the ratio of zircon to the total of alumina and zircon in the reference sample can be calculated as [(36.21+17.68) / (36.21+17.68+45.52)]×100=54.21%, and the alumina:zircon ratio in the reference sample was calculated as 45.79:54.21. This result is almost identical to the mixture ratio of the reference sample, 45:55, and the difference is due to experimental error.

Claims

1. Contains crystalline alumina and crystalline zircon, A glaze composition, characterized in that the ratio of the crystalline zircon to the total of the crystalline alumina and the crystalline zircon is 50 mass % or more and 70 mass % or less.

2. 2. The glaze composition according to claim 1, wherein the total ratio of the crystalline alumina and the crystalline zircon in the glaze layer forming components is 2% by mass or more and 25% by mass or less.

3. 2. The glaze composition according to claim 1, wherein the mixture of the crystalline alumina and the crystalline zircon has a volume-based average particle size of 0.5 μm or more and 2 μm or less.

4. The glaze composition according to claim 1, further comprising water.

5. The glaze composition according to claim 1, further comprising feldspar and / or silica.

6. The glaze composition according to claim 1, further comprising a thickener.

7. The glaze composition of claim 1 further comprising clay.

8. The glaze composition according to claim 1, further comprising an alkali component.

9. A step of applying the glaze composition according to any one of claims 1 to 8 to a base material; and A method for producing a ceramic product, comprising the step of firing the base material.

Citation Information

Patent Citations

  • Ceramics sintered compact, glaze, and manufacturing method for ceramics sintered compact

    JP2003238238A

  • Glaze and ceramic product

    JP2004210612A

  • Glaze composition capable of forming glaze layer having high diffuse reflection property and stain resistance, and member having glaze layer formed thereby

    JP2014166925A

  • Member having high-diffuse-reflectance enamel layer and production method thereof

    JP2014193803A

  • Clay roof tile

    JP2017190645A