Base material paste, dental alginate impression material, and method of preparing dental alginate impression material

By adding a liquid oily or lipid component to the alginate impression material paste, the viscosity decrease is mitigated, ensuring stable storage and improved kneading properties, thus reducing impression damage and enhancing accuracy.

JP2024163653APending Publication Date: 2024-11-22GC CORP
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
JP2023079446
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Conventional alginate impression materials suffer from decreased viscosity over time, leading to storage stability issues.

Method used

Incorporation of an oily component or lipid component that is liquid at room temperature into the main material paste, along with alginate and water, to maintain viscosity and improve storage stability.

Benefits of technology

The inclusion of a liquid oily or lipid component in the main material paste suppresses viscosity reduction, ensuring high storage stability and improved kneading properties, thereby reducing the likelihood of impression damage and enhancing accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163653000001
    Figure 2024163653000001
  • Figure 2024163653000002
    Figure 2024163653000002
Patent Text Reader

Abstract

To provide a base material paste with superior storage stability.SOLUTION: A base material paste used for a dental alginate impression material is provided. The base material paste contains an alginate, water, and an oily component that is liquid at a normal temperature and / or a lipid component that is liquid at the normal temperature.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a base paste, a dental alginate impression material, and a method for preparing the dental alginate impression material. [Background technology]

[0002] In dental treatment, when preparing a prosthesis, an alginate impression material is widely used as an impression material for taking an impression of the oral cavity. Known alginate impression materials include a base paste containing alginate and water, and a hardener paste containing a gelling agent and a poorly water-soluble liquid compound (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2012 / 063618 [Patent Document 2] International Publication No. 2014 / 050028 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in conventional alginate impression materials, the viscosity of the base paste is prone to decrease over time, posing a problem with the storage stability of the base paste.

[0005] An object of the present invention is to provide a base paste having excellent storage stability. [Means for solving the problem]

[0006] A base paste according to one embodiment of the present invention is a base paste used in dental alginate impression materials, and contains alginate, water, and an oily component that is liquid at room temperature and / or a lipid component that is liquid at room temperature. Effect of the Invention

[0007] According to one aspect of the present invention, a base paste having excellent storage stability can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, an embodiment of the present invention will be described in detail.

[0009] [Main paste] The base paste of this embodiment is used for dental alginate impression materials.

[0010] In this specification, the dental alginate impression material is a dental preparation for taking an impression that utilizes the reaction between a water-soluble alginate and gypsum to produce and harden insoluble calcium alginate, and the base paste is a paste-like material that constitutes the base material of the dental alginate impression material.

[0011] The base paste contains an alginate, water, and an oily component that is liquid at room temperature and / or a lipid component that is liquid at room temperature.

[0012] Examples of alginates include alkali metal salts of alginic acid such as sodium alginate and potassium alginate, and ammonium salts of alginic acid such as ammonium alginate and triethanolamine alginate. Among these, from the viewpoints of availability, ease of handling, and physical properties of the hardened body of the dental alginate impression material of the present embodiment described below, alkali metal salts of alginic acid are preferred, and potassium alginate is more preferred.

[0013] The alginate may be used alone or in combination of two or more kinds.

[0014] Furthermore, the viscosity of a 1% by mass aqueous solution of alginate at 20° C. is preferably 0.001 Pa·s or more and 0.5 Pa·s or less, and more preferably 0.1 Pa·s or more and 0.4 Pa·s or less. When a 1% by mass aqueous solution of alginate has a viscosity of 0.001 Pa·s or more at 20° C., the impression is less likely to be damaged when a dental impression material using the base paste of this embodiment is used in combination with a conventional alginate impression material.

[0015] Furthermore, when the viscosity of a 1% by mass aqueous solution of alginate at 20°C is 0.5 Pa·s or less, the fluidity of the mixture of the base paste and the hardener paste increases, and the accuracy of the impression is improved when the base paste of this embodiment is used in combination with an alginate impression material.

[0016] The content of alginate in the base paste is not particularly limited, and is, for example, 0.5% by mass or more and 30% by mass or less, preferably 1% by mass or more and 20% by mass or less, and more preferably 3% by mass or more and 15% by mass or less.

[0017] When the alginate content in the main paste is 0.5% by mass or more, the impression is less likely to be damaged when an alginate impression material (hereinafter sometimes referred to as a dental impression material) using the main paste of this embodiment is used in combination with a conventional alginate impression material, and when the alginate content is 30% by mass or less, the accuracy of the impression is improved when a dental impression material using the main paste of this embodiment is used in combination with a conventional alginate impression material.

[0018] As the water, for example, ion-exchanged water, distilled water, etc. can be used, and water that has been sterilized with sodium hypochlorite or the like can also be used.

[0019] The water content in the base paste is not particularly limited, and is, for example, 75% by mass or more and 99% by mass or less, preferably 80% by mass or more and 97% by mass or less, and more preferably 85% by mass or more and 95% by mass or less.

[0020] An oily component that is liquid at room temperature (hereinafter, sometimes referred to as an oily component) is an oily liquid within the room temperature range (for example, within the range of 20°C ± 15°C). A lipid component that is liquid at room temperature (hereinafter, sometimes referred to as a lipid component) is a liquid that contains lipids within the room temperature range (for example, within the range of 20°C ± 15°C).

[0021] The melting point of the oil component and / or lipid component is not particularly limited, but is preferably 25° C. or lower, more preferably 21° C. or lower, and even more preferably 15° C. or lower. When the melting point of the oil component and / or lipid component is 25° C. or lower, the oil component and / or lipid component can maintain a liquid state at room temperature.

[0022] Examples of oily components that are liquid at room temperature include hydrocarbon compounds, fatty acids, oils and fats, etc. Examples of lipid components that are liquid at room temperature include phospholipids, etc. These oily components and / or lipid components may be used alone or in combination of two or more.

[0023] The hydrocarbon compound may, for example, be liquid paraffin.

[0024] Examples of fatty acids include oleic acid, linoleic acid, and linolenic acid.

[0025] The fats and oils include vegetable oils, such as linseed oil, soybean oil, cottonseed oil, olive oil, castor oil, and corn oil.

[0026] Examples of phospholipids include soybean-derived lecithin (soybean lecithin).

[0027] The content of the oily component and / or lipid component in the base paste is not particularly limited, but is preferably 0.5% by mass or more and 3.5% by mass or less, more preferably 1% by mass or more and 3% by mass or less, and even more preferably 1.5% by mass or more and 2.5% by mass or less. When the content of the oily component and / or lipid component in the base paste is 0.5% by mass or more, the viscosity reduction suppression effect is easily obtained, and when it is 3.5% by mass or less, separation of the paste is unlikely to occur.

[0028] The base paste may contain other components as long as the purpose of the present invention is not impaired. The other components contained in the base paste may further include a filler, a colorant, a preservative, a disinfectant, a fragrance, a pH adjuster, a surfactant, a hardening retarder, etc.

[0029] Examples of materials constituting the filler include clay minerals such as diatomaceous earth, talc, and smectite, and inorganic oxides such as silica and alumina. These fillers may be used alone or in combination of two or more.

[0030] Examples of the surfactant include polyoxyethylene alkyl ether, etc. These surfactants may be used alone or in combination of two or more.

[0031] Examples of the hardening retarder include phosphates such as trisodium phosphate and tripotassium phosphate, and condensed phosphates such as sodium pyrophosphate and potassium pyrophosphate. These hardening retarders may be used alone or in combination of two or more.

[0032] The viscosity of the main paste at 20° C. is preferably 50,000 mPa·s or more and 110,000 mPa·s or less, more preferably 75,000 mPa·s or more and 105,000 mPa·s or less, and even more preferably 80,000 mPa·s or more and 100,000 mPa·s or less.

[0033] When the viscosity of the base paste at 20°C is 50,000 mPa·s or more, the kneading property of the base paste after storage is improved, and when it is 110,000 mPa·s or less, the strength of the hardened dental impression material is improved, even in the base paste after storage.

[0034] Furthermore, the base paste of the present embodiment has a lower viscosity than conventional paste-like alginate impression materials and can be used in the combined impression technique.

[0035] As described above, the base paste of this embodiment contains alginate, water, and an oily component that is liquid at room temperature and / or a lipid component that is liquid at room temperature, which makes it possible to suppress the decrease in viscosity of the base paste due to changes over time, and to obtain a base paste with high storage stability.

[0036] In addition, the base paste of the present embodiment can be made to have a lower viscosity than conventional paste-like alginate impression materials, and can suppress a decrease in viscosity while maintaining the low viscosity. Therefore, the base paste of the present embodiment can be used in the combined impression method (a method in which two uncured materials are layered on top of each other).

[0037] [Dental alginate impression material] The dental alginate impression material of this embodiment includes a base paste and a hardener paste.

[0038] As the base paste, the base paste of this embodiment (base paste containing alginate, water, and an oily component that is liquid at room temperature and / or a lipid component that is liquid at room temperature) is used.

[0039] As the hardener paste, the above-mentioned hardener paste (hardener paste containing a gelling agent and a poorly water-soluble liquid compound) is used.

[0040] The content of alginate in the dental alginate impression material is not particularly limited, and is, for example, 0.3% by mass or more and 20% by mass or less, preferably 0.6% by mass or more and 13% by mass or less, and more preferably 2% by mass or more and 10% by mass or less.

[0041] When the dental alginate impression material of this embodiment contains 0.3% by mass or more of alginate, the impression is less likely to be damaged when the dental alginate impression material of this embodiment is used in combination with a conventional alginate impression material. On the other hand, when the dental alginate impression material of this embodiment contains 20% by mass or less of alginate, the accuracy of the impression is improved when the dental alginate impression material of this embodiment is used in combination with a conventional alginate impression material.

[0042] The water content in the dental alginate impression material of this embodiment is not particularly limited, and is, for example, 40% by mass or more and 75% by mass or less, preferably 45% by mass or more and 70% by mass or less, and more preferably 50% by mass or more and 65% by mass or less.

[0043] The content of oily components and / or lipid components in the dental alginate impression material of this embodiment is not particularly limited, and is, for example, 0.3 mass% or more and 2.5 mass% or less, preferably 0.6 mass% or more and 2 mass% or less, and more preferably 1 mass% or more and 1.5 mass% or less.

[0044] When the content of the oily component and / or lipid component in the dental alginate impression material is 0.3% by mass or more, the viscosity decrease of the base paste is suppressed even after the storage period has elapsed, and the storage stability of the base paste can be improved.When the content of the oily component and / or lipid component in the base paste is 2.5% by mass or less, the viscosity of the base paste can be kept low while suppressing the decrease in the viscosity.

[0045] [Hardening paste] The hardener paste is a material that is mixed into the base paste and hardens the dental alginate impression material.

[0046] The hardener paste contains a gelling agent and a poorly water-soluble liquid compound.

[0047] As the gelling agent, a compound of a divalent or higher metal can be used.

[0048] The compound of a divalent or higher metal is not particularly limited, and examples thereof include divalent or higher metals and their salts, oxides, hydroxides, etc. These may be used alone or in combination of two or more kinds.

[0049] Examples of divalent or higher metals include calcium, magnesium, zinc, aluminum, iron, titanium, zirconium, and tin.

[0050] Examples of salts of divalent or higher metals include calcium sulfate dihydrate (CaSO 4 2H 2 O), calcium sulfate hemihydrate (CaSO 4 1 / 2H 2 O), anhydrous calcium sulfate (CaSO 4 ) etc.

[0051] Examples of the oxides of divalent or higher metals include calcium oxide, magnesium oxide, zinc oxide, titanium oxide, zirconium oxide, and tin oxide.

[0052] Examples of the hydroxides of divalent or higher metals include calcium hydroxide, magnesium hydroxide, zinc hydroxide, aluminum hydroxide, and iron hydroxide.

[0053] The content of the gelling reactant in the hardener paste is not particularly limited, but is preferably 10% by mass or more and 60% by mass or less. When the content of the gelling reactant in the hardener paste is 10% by mass or more, the strength of the hardened body of the dental alginate impression material using the hardener paste is improved, and when it is 60% by mass or less, the operation time of the dental impression material is extended.

[0054] The poorly water-soluble liquid compound is not particularly limited as long as it can make the gelling reactant into a paste, and examples thereof include hydrocarbon compounds, aliphatic alcohols, aromatic alcohols, fatty acids, fatty acid esters, silicone oils, etc. These may be used alone or in combination of two or more. The poorly water-soluble liquid compound may be the same as the oily component and / or lipid component used in the above-mentioned base paste.

[0055] In this specification, poor water solubility means that the solubility in 100 g of water at 20° C. is 5 g or less.

[0056] Examples of the hydrocarbon compound include aliphatic chain hydrocarbon compounds such as hexane, heptane, octane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, kerosene, 2,7-dimethyloctane, and 1-octene; alicyclic hydrocarbon compounds such as cycloheptane and cyclononane; and liquid paraffin.

[0057] Examples of the aliphatic alcohol include saturated aliphatic alcohols such as 1-hexanol and 1-octanol, and unsaturated aliphatic alcohols such as citronellol and oleyl alcohol.

[0058] Examples of aromatic alcohols include benzyl alcohol and m-cresol.

[0059] Examples of fatty acids include saturated fatty acids such as hexanoic acid and octanoic acid, and unsaturated fatty acids such as oleic acid and linoleic acid.

[0060] Examples of fatty acid esters include ethyl octanoate, butyl phthalate, oleic acid glyceride, olive oil, sesame oil, cod liver oil, and whale oil.

[0061] Examples of silicone oils include polydimethylsiloxane, polymethylphenylsiloxane, polymethylhydrogensiloxane, and polyphenylhydrogensiloxane.

[0062] The content of the poorly water-soluble liquid compound in the hardener paste is not particularly limited, but is preferably 10% by mass or more and 50% by mass or less, and more preferably 15% by mass or more and 30% by mass or less. When the content of the poorly water-soluble liquid compound in the hardener paste is 10% by mass or more, the operability of the dental alginate impression material of the present embodiment using the hardener paste is improved, and when it is 50% by mass or less, the strength of the hardened body of the dental alginate impression material is improved.

[0063] The hardener paste preferably further contains polybutene, which improves the hardening property of the dental alginate impression material of the present embodiment and extends the operation time of the dental alginate impression material.

[0064] The polybutene is preferably liquid. The polybutene can be synthesized by copolymerizing isobutene and 1-butene. The number average molecular weight of the polybutene is preferably 300 to 4,000.

[0065] The content of polybutene in the hardener paste is preferably 0.5% by mass or more and 30% by mass or less, more preferably 1% by mass or more and 20% by mass or less. When the content of polybutene in the hardener paste is 0.5% by mass or more and 30% by mass or less, the operability of the dental alginate impression material of this embodiment is improved.

[0066] The hardener paste may further contain a filler, a hardening retarder, a hardening regulator, a surfactant, a colorant, a preservative, a disinfectant, a fragrance, a pH adjuster, and the like.

[0067] Examples of materials constituting the filler include clay minerals such as diatomaceous earth, talc, and smectite, and inorganic oxides such as silica and alumina. These fillers may be used alone or in combination of two or more.

[0068] Examples of the hardening retarder include phosphates such as trisodium phosphate and tripotassium phosphate, and condensed phosphates such as sodium pyrophosphate and potassium pyrophosphate. These hardening retarders may be used alone or in combination of two or more.

[0069] Examples of the hardening regulator include potassium titanium fluoride, potassium silicofluoride, etc. These hardening regulators may be used alone or in combination of two or more.

[0070] Examples of the surfactant include polyoxyethylene alkyl ether, etc. These surfactants may be used alone or in combination of two or more.

[0071] The consistency of the hardener paste is not particularly limited, but is preferably 30 mm or more. When the consistency of the hardener paste is 30 mm or more, the fluidity of the kneaded product of the main paste and the hardener paste is high. Therefore, when the dental alginate impression material of this embodiment is used in combination with a conventional alginate impression material, the accuracy of the impression is improved.

[0072] As described above, the dental alginate impression material of this embodiment has the main paste and hardener paste of this embodiment, and thus the effect of the main paste of this embodiment can be obtained. That is, in the dental alginate impression material of this embodiment, the viscosity reduction due to the change over time of the main paste contained therein is suppressed, so that the storage stability of the main paste is high, and therefore the decrease in the kneadability of the dental alginate impression material can be suppressed when the main paste is used. Therefore, in the dental alginate impression material of this embodiment, the impression is less likely to be damaged, and the accuracy of the impression is improved.

[0073] In addition, the main paste contained in the dental alginate impression material of this embodiment has a lower viscosity than conventional paste-like alginate impression materials, and the viscosity is prevented from decreasing while maintaining the low viscosity, so that the dental alginate impression material of this embodiment can be used in the combined impression method.

[0074] [Method for preparing dental alginate impression material] The method for preparing a dental alginate impression material of this embodiment is a method for preparing a dental alginate impression material by kneading the above-mentioned main material paste and hardener paste.

[0075] As a method for preparing the dental alginate impression material, for example, a manual or electric extrusion device is used to extrude the base paste and the hardener paste filled in a separated packaging container, and the mixture is passed through a nozzle to prepare a kneaded mixture. The obtained kneaded mixture can be applied to teeth as a dental alginate impression material.

[0076] Examples of packaging containers include molded resin or metal products, and resin or metal bags.

[0077] The mass ratio of the base paste to the hardener paste when the base paste and the hardener paste are kneaded is not particularly limited and is, for example, 1-5, preferably 1-4, and more preferably 1-3.

[0078] In the method for preparing a dental alginate impression material according to this embodiment, the above-mentioned base paste and hardener paste are mixed to obtain the above-mentioned dental alginate impression material, thereby obtaining the effects of the base paste according to this embodiment.

[0079] Specifically, the method for preparing a dental alginate impression material according to the present embodiment suppresses a decrease in viscosity due to changes over time in the main paste contained in the obtained dental alginate impression material, thereby improving the storage stability of the main paste, and therefore suppresses a decrease in the kneadability of the dental alginate impression material when the main paste is used. Therefore, by using the method for preparing a dental alginate impression material according to the present embodiment, the impression of the obtained dental alginate impression material is less likely to be damaged, improving the accuracy of the impression.

[0080] Furthermore, the dental alginate impression material obtained by the method for preparing a dental alginate impression material according to the present embodiment contains a main paste that has a lower viscosity than conventional paste-like alginate impression materials, and the viscosity is prevented from decreasing while maintaining the low viscosity. Therefore, by using the method for preparing a dental alginate impression material according to the present embodiment, the obtained dental alginate impression material can be used for the combined impression method.

[0081] [Combined impression material] The dental alginate impression material of the present embodiment can be used as the combined impression material of the present embodiment. In this specification, the combined impression material is a material for making an impression by the combined impression method (a method of overlapping two uncured materials).

[0082] The combination impression material of the present embodiment is used in combination with another alginate impression material. Specifically, the combination impression material of the present embodiment is applied to an object to be taken an impression of, for example, teeth, and then the other alginate impression material is applied.

[0083] The other alginate impression material is not particularly limited, but for example, an alginate impression material used in the agar-alginate combined impression technique can be used.

[0084] Other alginate impression materials may be of powder type or of paste type having a base paste containing alginate and water, a gelling agent, and a hardener paste containing a poorly water-soluble liquid compound.

[0085] The mass ratio of the association impression material of the present embodiment to the other alginate impression material is not particularly limited.

[0086] When a paste-type alginate impression material is used as the other alginate impression material, the alginate impression material is similar to the dental alginate impression material of this embodiment, except that the consistency of the kneaded product of the main material paste and the hardener paste is less than 36 mm.

[0087] As described above, the combined impression material of the present embodiment can obtain the effects of the dental alginate impression material of the present embodiment by using the dental alginate impression material of the present embodiment. That is, in the combined impression material of the present embodiment, the main material paste contained therein has high storage stability (is not easily deteriorated even after a storage period has elapsed), so that when the main material paste is used, the decrease in the kneadability of the dental alginate impression material can be suppressed, and the obtained impression is less likely to be damaged.

[0088] In addition, in the combined impression material of the present embodiment, the main paste contained in the dental alginate impression material has a lower viscosity than that of conventional alginate impression materials in paste form, and the viscosity is kept low while suppressing a decrease in viscosity, thereby improving the accuracy of impressions made using the combined impression method. EXAMPLES

[0089] The present invention will be further described below with reference to examples. In the following, numbers without units, "parts" or "%" are based on mass unless otherwise specified. The examples and comparative examples were evaluated by the following tests.

[0090] [Example 1] <Preparation of main paste> The main paste was prepared by mixing 7 parts of potassium alginate and 3 parts of sodium alginate as alginates, and 2 parts of linseed oil as an oil component that is liquid at room temperature, and adding distilled water to make the total 100 parts. The composition of the main paste is shown in Table 1.

[0091] <Preparation of hardener paste> A hardener paste was prepared by mixing 45 parts of anhydrous calcium sulfate, 23 parts of liquid paraffin, 12.5 parts of silica, 6 parts of magnesium hydroxide, 4 parts of polybutene, 3 parts of potassium titanium fluoride, 3 parts of polyoxyethylene alkyl ether, 2 parts of zinc oxide, and 1.5 parts of tripotassium phosphate. The composition of the hardener paste is shown in Table 2.

[0092] [Example 2] In preparing the base paste, 2 parts of liquid paraffin was mixed as an oil component that is liquid at room temperature, and the other components were prepared in the same manner as in Example 1. The composition of the base paste is shown in Table 1.

[0093] [Example 3] In preparing the base paste, 2 parts of oleic acid was mixed as an oil component that is liquid at room temperature, and the base paste and hardener paste were prepared in the same manner as in Example 1. The composition of the base paste is shown in Table 1.

[0094] [Example 4] In preparing the base paste, 2 parts of soybean lecithin was mixed as a lipid component that is liquid at room temperature, and the other components were prepared in the same manner as in Example 1. The composition of the base paste is shown in Table 1.

[0095] [Comparative Example 1] In preparing the main paste, the main paste and the hardening paste were prepared in the same manner as in Example 1, except that neither the oily component that is liquid at room temperature nor the lipid component that is liquid at room temperature was mixed. The composition of the main paste is shown in Table 1.

[0096] [Comparative Example 2] In preparing the base paste, 2 parts of coconut oil was mixed as an oil component that is solid at room temperature, and the base paste and hardener paste were prepared in the same manner as in Example 1. The composition of the base paste is shown in Table 1.

[0097] [Comparative Example 3] In preparing the base paste, 2 parts of Vaseline was mixed as an oily component that is solid at room temperature, and the other components were prepared in the same manner as in Example 1. The composition of the base paste is shown in Table 1.

[0098] [Comparative Example 4] In preparing the main paste, 2 parts of palmitic acid was mixed as an oil component that is solid at room temperature, and the other components were prepared in the same manner as in Example 1. The composition of the main paste is shown in Table 1.

[0099] [Comparative Example 5] In preparing the base paste, 2 parts of hydrogenated lecithin was mixed as a lipid component that is solid at room temperature, and the base paste and hardener paste were prepared in the same manner as in Example 1. The composition of the base paste is shown in Table 1.

[0100] <Storage stability> Using a viscometer (E-type viscometer RE-85, manufactured by Toki Sangyo Co., Ltd.), the viscosity of the prepared base paste at 23°C was measured under conditions of a cone angle of 3° and a shear rate of 2 (1 / sec). The base paste was then filled into a 50 mL transparent glass bottle and sealed, and stored in a constant temperature bath at 45°C for 7 days. After storage, the base paste was kept in a constant temperature bath at 23°C for 1 hour, and the viscosity was measured again. Using the viscosity values ​​before and after storage, the viscosity reduction rate was calculated according to the following formula. The evaluation criteria were as follows. The viscosity reduction rates of each example and comparative example are shown in Table 1. Viscosity decrease rate (%) = 100 - (viscosity after storage / viscosity before storage) x 100 [Evaluation Criteria] Good: Viscosity reduction rate was less than 45% Poor: Viscosity reduction rate was 45% or more.

[0101] <Mixability after storage> The base paste and the hardener paste stored for 1 hour under the above storage stability were filled into a kneading cartridge in a mass ratio of 2:1, and the paste was extruded and kneaded. The kneading property after storage was evaluated from the appearance of the paste (dental alginate impression material) discharged from the nozzle. The evaluation criteria are as follows. Table 1 shows the kneading property after storage of each example and comparative example. [Evaluation Criteria] Good: The base paste and hardener paste were discharged in a uniformly mixed state. Bad: The base paste was discharged earlier than the hardener paste, and mixing was uneven.

[0102] [Table 1]

[0103] [Table 2]

[0104] As can be seen from Table 1, the base pastes containing alginate, water, and an oily component that is liquid at room temperature or a lipid component that is liquid at room temperature had good storage stability and kneadability after storage (Examples 1 to 4).

[0105] In contrast, the base pastes that did not contain either an oily component that was liquid at room temperature or a lipid component that was liquid at room temperature had poor (or unacceptable) storage stability and kneadability after storage (Comparative Examples 1 to 5).

[0106] These results show that the base paste containing alginate, water, and an oily component that is liquid at room temperature or a lipid component that is liquid at room temperature has excellent storage stability, and the dental alginate impression material prepared by kneading the base paste and hardener paste after storage has good kneadability.

[0107] Although an embodiment of the present invention has been described above, the present invention is not limited to a specific embodiment, and various modifications and changes are possible within the scope of the invention described in the claims.

Claims

1. A base paste used in dental alginate impression materials, Contains alginate, water, and an oily component that is liquid at room temperature and / or a lipid component that is liquid at room temperature. Main paste.

2. The base paste according to claim 1 ; A hardener paste containing a gelling agent and a poorly water-soluble liquid compound; Dental alginate impression material.

3. The base paste according to claim 1 is mixed with a hardener paste containing a gelling agent and a poorly water-soluble liquid compound. A method for preparing a dental alginate impression material.

Citation Information

Patent Citations

  • Polyacrylamide-containing settable arginate composition and manufacture

    JP1984204113A

  • Impression material

    JP1985048912A

  • Forming material and manufacture

    JP1986018707A

  • Germicide-containing alginic acid impression material

    JP1989100110A

  • Dustless impression material of alginic acid salt for dentistry

    JP1991255012A