Tool for shaving steel wire
A skin shaving tool for ferritic stainless steel wire rods with tailored rake and relief angles, along with C-chamfered surfaces, addresses tool wear and machinability issues, improving tool life and cutting efficiency.
Patent Information
- Application Number
- JP2023079527
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing skin cutting tools for ferritic stainless steel wire rods, such as SUS430, suffer from shortened tool life, cutter marks, and black scale residue due to high loads and poor machinability, primarily because of the differences in machinability between the ferritic and austenite phases.
A skin shaving tool designed for ferritic stainless steel wire rods with specific rake angle (5° to 15°), relief angle (1° to 10°), and C-chamfered surface, featuring a rake chamfer angle (45° to 70°) and chamfer width (0.3 to 0.8 mm), which suppresses workpiece adhesion and improves machining properties.
The tool design enhances tool life and machining properties by stabilizing cutting behavior, reducing friction and heat generation, and preventing tool wear, resulting in more stable and efficient cutting performance.
Smart Images

Figure 2024163696000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a tool for scraping a surface of a drawn steel wire, and more particularly to a tool for scraping a surface of a ferritic stainless steel wire. [Background technology]
[0002] In the manufacturing process of metal wires such as steel, copper, and aluminum, a thin layer of the outer skin is removed to remove scratches, oxide films, foreign matter, etc. on the wire surface. The skinning device for this purpose is equipped with a skinning tool with a hole diameter slightly smaller than the diameter of the wire, and the wire is passed through the tool to remove the skin. For optimal skinning, it is necessary to change the shape of the skinning tool to match the properties of the metal wire.
[0003] For example, Patent Document 1 discloses a shaving tool for manufacturing a wire made of two-phase stainless steel. In general, in stainless steel, the ferrite phase is likely to adhere to a shaving die as a shaving tool, while the austenite phase is tough and hard, which accelerates tool wear and is poor in chip cutting ability. In addition, in two-phase stainless steel, even if annealing is performed so that the grain size becomes large in general stainless steel, the grain size remains small, and the steel is hard and poor in machinability. In view of such properties, the shape of the shaving die is set to a rake face land angle (rake chamfer angle) of 10 to 30°, a rake angle of 10 to 25°, a relief angle of 3 to 10°, a rake face land width (chamfer width) of 0.1 to 0.5 mm, and a cutting edge radius of 0.02 to 0.08 mm, thereby significantly reducing surface defects of the wire (wire product) after shaving, and as a result, improving fatigue resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-83704 A Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, there is a large difference in machinability between the ferrite phase and the austenite phase in stainless steel, and when using austenitic stainless steel wire or duplex stainless steel wire skin scraping tools in the skin scraping process of ferritic stainless steel wire such as SUS430, problems such as shortened tool life, cutter marks and black scale remaining due to tool chipping, rough surface skin due to high load, etc. were prominent. Therefore, a skin scraping tool for ferritic stainless steel wire was required.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a scraping tool suitable for producing ferritic stainless steel wire such as SUS430. [Means for solving the problem]
[0007] The present invention is a skin scraping tool for scraping the surface of a ferritic stainless steel wire, characterized in that the rake angle γ is in the range of 5° to 15°, the clearance angle α is in the range of 1° to 10°, the rake chamfer angle η at the tip formed by C-chamfering is in the range of 45° to 70°, and the chamfer width ω is in the range of 0.3 to 0.8 mm.
[0008] According to this feature, adhesion of the work material to the tip of the tool can be suppressed, thereby extending the tool life and improving the machining properties of the product.
[0009] In the above-mentioned invention, the rake angle γ may be in the range of 5° to 10°. With this feature, the tool life can be further extended and the machining properties of the product can be improved. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a cross-sectional view of a wire and a scraping tool during drawing. [Diagram 2]FIG. 2 is a side cross-sectional view of a leather scraping tool. [Diagram 3] FIG. 2 is an enlarged cross-sectional side view of the cutting edge of the leather scraping tool. [Figure 4] FIG. 1 is a cross-sectional view showing a model shape of a skin scraping tool used in a numerical analysis. [Diagram 5] 13 is a graph showing the results of a numerical analysis regarding the maximum temperature. [Figure 6] 13 is a graph showing the results of a numerical analysis on maximum stress. [Figure 7] 13 is a graph showing the results of a numerical analysis of the principal force. [Figure 8] 6 is a graph showing voltage changes in the chip breaker drive motor of (a) the embodiment and (b) the comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] A wire steel material peeling tool will be described as one embodiment of the present invention.
[0012] As shown in Figure 1, the skin scraping tool 1 has a hole 2 with a diameter slightly smaller than the diameter of the wire 10 to be skin scraped, and by pulling the wire 10 through the hole 2, the surface of the wire 10 can be scraped off as chips 11. By pulling the wire 10 to the right on the page, the skin scraping tool 1 is relatively given a cutting direction to the left on the page.
[0013] As shown in FIG. 2, the leather scraping tool 1 is a circular shaving die having a cutting edge 3 on the cutting direction tip side (left side of the drawing) of its inner periphery.
[0014] 3, the cross-sectional shape of the cutting edge 3 is determined by the rake angle γ, which is the angle between the rake face on the cutting direction side and the plane perpendicular to the cutting direction, the clearance angle α, which is the angle between the clearance face on the inner diameter side and the cutting direction, and the chamfer shape. In the case of C-chamfering, the chamfer shape is determined by the rake chamfer angle η, which is the angle with respect to the plane perpendicular to the cutting direction, and the chamfer width ω, which is the width of the chamfer.
[0015] Here, the wire 10 to be scraped is made of ferritic stainless steel, and has different cutting properties from other austenitic stainless steels and duplex stainless steels. For example, Patent Document 1 states that in duplex stainless steels, the ferritic phase is prone to adhesion to the scraping tool, whereas the austenitic phase has poor chip cutting properties. Therefore, the scraping tool 1 is designed to be compatible with ferritic stainless steel wires, and is capable of suppressing adhesion of the workpiece to the tool, that is, seizure, caused by temperature rise.
[0016] Therefore, the rake angle γ is in the range of 5° to 15°, the clearance angle α is in the range of 1° to 10°, and the chamfer is a C-chamfer, with the rake chamfer angle η of the tip formed thereby in the range of 45° to 70° and the chamfer width ω in the range of 0.3 to 0.8 mm.
[0017] A larger rake angle γ makes it easier to cut chips and reduces the cutting force and shear stress involved in cutting. On the other hand, it makes the behavior during cutting unstable and makes the tool more likely to wear. Taking these factors into consideration, the rake angle γ is set in the above-mentioned range. In addition, it is also preferable to set the rake angle γ in the range of 5° to 10°, since this stabilizes the behavior during cutting and increases the tool life.
[0018] The clearance angle α particularly affects the friction with the scraped wire 10, and increasing the clearance angle reduces the contact pressure that causes the friction and suppresses heat generation. On the other hand, the clearance angle α of the tool has a shape that accelerates wear of the cutting edge 3. Taking these factors into consideration, the clearance angle α is set to the above range.
[0019] The chamfer shape was C chamfer, which can reduce the temperature during cutting compared to R chamfer.
[0020] In addition, by increasing the chamfer angle η, the behavior during cutting can be stabilized and the wear of the cutting edge can be reduced. On the other hand, the chip cutting ability is reduced, and the cutting force and shear stress accompanying cutting are increased, leading to an increase in temperature. On the other hand, it has been found by the numerical analysis described below that the temperature can be reduced even if the chamfer angle η is increased. In ferritic stainless steels, even if the chip cutting ability, which is a problem in austenitic stainless steels, is reduced, if the temperature can be reduced, it is believed that the adhesion of the workpiece material can be suppressed and the tool life can be improved. Taking these factors into consideration, the chamfer angle η is set to the above range.
[0021] By increasing the chamfer width ω, the cutting edge 3 can be made sturdy. On the other hand, it reduces the chip cutting ability, increases the cutting force and shear stress involved in cutting, and leads to an increase in temperature. Taking these factors into consideration, the chamfer width ω is set to the above range.
[0022] In addition, the results of the following numerical analysis were also used in selecting these numerical ranges.
[0023] A model as shown in Fig. 4(a) and (b) was set as a skin scraping tool, and the cutting temperature, maximum stress, and principal component of cutting resistance were numerically analyzed. The analysis conditions were as follows: the rake angle was 10°, the clearance angle was 6°, the chamfering amount on the rake face side was set to four values: 0.1mm, 0.15mm, 0.2mm, and 0.3mm, and the chamfering angle was set to five values: 15°, 30°, 45°, 60°, and 75°. The chamfering was a C-chamfer. For example, if the chamfering amount on the rake face side is 0.3mm and the chamfering angle is 60°, the chamfering width ω is 0.452mm. The cutting speed was 90m / min, the cutting depth was 0.1mm, and the processing length was 10m. Assuming that the wire material to be cut is SUS430 and the material of the scraping tool is cemented carbide UTi20T, the friction coefficient due to shear friction is 1.0 and the heat transfer coefficient is 10000kw / m 2 It was assumed that K.
[0024] As a result, as shown in FIG. 5(a), it was found that the maximum cutting temperature tends to be the lowest when the chamfer angle is 60°. As mentioned above, generally, increasing the chamfer angle leads to an increase in temperature, but it is considered that the temperature may be reduced even if the chamfer angle is increased by combining with other factors. FIG. 5(b) shows the analysis results of a comparative example in which the chamfer amount in the case of R chamfering is set to four values from 0.1 to 0.4 mm, and the temperature tends to be higher than that in the case of C chamfering. When the cutting temperature increases, the wear rate of the skin scraping tool increases, so it is preferable to lower the cutting temperature in consideration of the tool life. In other words, although it depends on the chamfer amount and other shapes, it was inferred that the most preferable chamfering is C chamfering and the chamfer angle is 60°.
[0025] Next, as shown in Figure 6(a), it was found that the maximum stress tends to increase sharply when the rake chamfer angle is set to 75°. An increase in the maximum stress makes the cutting edge more susceptible to chipping. For this reason, it was inferred that a rake chamfer angle of 70° or less is preferable. Note that Figure 6(b) shows the analysis results of a comparative example with R chamfering, but no significant difference was observed from the case of C chamfering in the embodiment.
[0026] As shown in Fig. 7(a), the principal force is the wire drawing load (winding load), and the larger the chamfer angle, the larger the increase in the principal force tends to be. In particular, the principal force increases sharply when the chamfer angle is set to 75°. It was therefore presumed that the chamfer angle should be set to 70° or less. Fig. 7(b) shows the analysis results of a comparative example in which the chamfer is R, and it was found that the principal force increases sharply as the chamfer amount increases. It was also found that the principal force tends to be lower in the example in which the chamfer is C when the chamfer angle is 60° or less.
[0027] [Prototype testing] Two prototypes of the above-mentioned skin scraping tools were manufactured, and the results of skin scraping processing will be described.
[0028] The shape of the cutting edge of the prototype skin scraping tool as an example was a rake angle γ of 7°, a clearance angle α of 5°, a chamfer shape of C chamfer, a chamfer angle η of 60°, and a chamfer amount (the length of the line segment projected onto a plane perpendicular to the cutting direction, which is the distance from the cutting edge before chamfering to the end of the chamfered part on the chamfered side after chamfering) of 0.27 mm. The chamfer width ω was calculated after measuring the shape of the manufactured skin scraping tool, and was 0.464 mm and 0.447 mm, respectively. The inner diameter of the skin scraping tool was 17.21 mm. As a comparative example, a conventional skin scraping tool having an R chamfer with a chamfer amount of 0.55 mm and a clearance chamfer amount of 0.33 mm was also used.
[0029] Using this kind of skin scraping tool, we performed skin scraping by drawing a φ17.60 mm wire rod made of SUS430 with black skin remaining on its surface. The cutting speed (winding speed) was 100 mm / min.
[0030] During the surface scraping process, a rotating body is provided upstream of the surface scraping tool as a chip breaker that cuts the chips, and the cutting ability of the chips can be evaluated from the load acting on the rotating body. The cutting ability is converted into a voltage value and output, for example.
[0031] As shown in Figures 8(a) and (b), the above-mentioned fluctuations in voltage value tended to be smaller in both the average value and the variation in the example (a) than in the comparative example (b). In detail, the average value of the voltage in the example was 2.63V, and the standard deviation σ was 0.67V. On the other hand, the average value of the voltage in the comparative example was 2.76V, and the standard deviation σ was 0.91V. In other words, it can be inferred that the example obtained a more stable cutting performance in the skin scraping process than the comparative example. The figure also shows the measurement results of the voltage values of the drive motors of the supply stand on the wire supply side and the winding drum on the winding side. Such fluctuations in the voltage value also correspond to the fluctuations in the respective rotation loads, but no significant difference was found between the example and the comparative example.
[0032] As described above, according to the above-mentioned embodiment, a scraping tool suitable for manufacturing ferritic stainless steel wire including SUS430 can be obtained.
[0033] Although the representative embodiments of the present invention and modified examples based thereon have been described above, the present invention is not necessarily limited to these, and a person skilled in the art will be able to find various alternative embodiments and modified examples without departing from the spirit of the present invention or the scope of the appended claims. [Explanation of symbols]
[0034] 1. Skin scraping tool 2 holes 10 wire rod 11 Chips α Clearance angle γ Rake angle η Rake chamfer angle ω Chamfer width
Claims
1. A scraping tool for scraping off the surface of a ferritic stainless steel wire, The rake angle γ is in the range of 5° to 15°, the clearance angle α is in the range of 1° to 10°, A steel wire scraping tool characterized in that the rake chamfer angle η of the tip formed by C-chamfering is in the range of 45° to 70°, and the chamfer width ω is in the range of 0.3 to 0.8 mm.
2. 2. The tool for scraping steel wire rods according to claim 1, wherein the rake angle γ is in the range of 5° to 10°.
Citation Information