Method for evaluating all-solid-state battery, all-solid-state battery and manufacturing method thereof
The method for evaluating all-solid-state batteries with oxide-type electrolytes by using external reference electrodes addresses integration challenges, enabling accurate charge-discharge curve and impedance measurement without affecting battery operation, thus improving productivity and avoiding adverse reactions.
Patent Information
- Application Number
- JP2023199428
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2023-11-24
- Publication Date
- 2024-11-28
AI Technical Summary
Existing all-solid-state batteries using oxide-type electrolytes face challenges in integrating a reference electrode due to high-temperature sintering requirements, which complicates the formation of an interface and can affect battery operation.
A method for evaluating all-solid-state batteries using oxide-type electrolytes by providing a first and second reference electrode outside the solid electrolyte layer, allowing them to function as pseudo reference electrodes without affecting battery operation, and measuring charge-discharge curves and electrochemical impedance individually.
Enables accurate evaluation of charge-discharge characteristics and electrochemical impedance of positive and negative electrodes without interfering with battery operation, improving productivity and preventing adverse reactions during high-temperature sintering.
Smart Images

Figure 2024166041000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an evaluation method for each electrode of an all-solid-state battery having an oxide-type solid electrolyte, using a reference electrode, an all-solid-state battery, and a method for manufacturing the same. [Background technology]
[0002] An all-solid-state battery has a positive electrode, a negative electrode, and an electrolyte in a solid state. The solid electrolytes used in all-solid-state batteries include sulfide type, polymer type, oxide type, and the like, and are used according to their respective advantages.
[0003] For example, sulfide-type and polymer-type electrolytes are relatively soft, and therefore have the advantage that an interface between the electrolyte and the electrode is easily formed, but have the disadvantage that their safety is relatively low.
[0004] Oxide-type electrolytes are relatively hard, and therefore have the disadvantage that it is difficult to form an interface between the electrolyte and the electrodes, but have the advantage of being relatively safe.
[0005] Some of such all-solid-state batteries are provided with a reference electrode to observe the charge / discharge curves of the positive electrode and the negative electrode individually (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2022-07408 [Patent Document 2] Patent Publication No. 2021-64579 Summary of the Invention [Problem to be solved by the invention]
[0007] However, since neither Patent Document 1 nor Patent Document 2 uses an oxide-type electrolyte, it is relatively easy to introduce a reference electrode into the electrolyte. In contrast, in the case of an oxide-type electrolyte, it is necessary to sinter the electrolyte at high temperatures, which makes it difficult to introduce a reference electrode into the electrolyte. Furthermore, in the case of a configuration in which a reference electrode is inserted between a positive electrode and a negative electrode as in Patent Document 1, there is a problem in that the reference electrode affects the operation of the battery consisting of positive and negative electrodes.
[0008] In view of the above circumstances, an object of the present invention is to provide an evaluation method for an all-solid-state battery capable of evaluating an all-solid-state battery with high accuracy without a reference electrode affecting the operation of the battery, an all-solid-state battery in which a reference electrode does not affect the operation of the battery, and a manufacturing method thereof. [Means for solving the problem]
[0009] An aspect of the present invention for solving the above-mentioned problems is a method for evaluating an all-solid-state battery including a positive electrode layer, a negative electrode layer, and a solid electrolyte layer containing an oxide solid electrolyte therebetween, a positive electrode-side wiring connected to the positive electrode layer, and a negative electrode-side wiring connected to the negative electrode layer, the method comprising: forming a positive electrode-side solid electrolyte layer containing an oxide solid electrolyte and a first reference electrode on the opposite side of the positive electrode layer from the solid electrolyte layer; forming a negative electrode-side solid electrolyte layer containing an oxide solid electrolyte and a second reference electrode on the opposite side of the negative electrode layer from the solid electrolyte layer; short-circuiting the first reference electrode and the second reference electrode; and performing evaluation between the short-circuited first reference electrode and the short-circuited second reference electrode and the positive electrode layer and the negative electrode layer, respectively.
[0010] In this embodiment, without providing a reference electrode in the solid electrolyte layer that needs to be sintered, a positive electrode-side solid electrolyte layer and a first reference electrode are provided on the outside of the positive electrode layer, and a negative electrode-side solid electrolyte layer and a second reference electrode are provided on the outside of the negative electrode layer, and the first reference electrode and the second reference electrode function as pseudo reference electrodes. This makes it possible to individually measure the charge / discharge characteristics of the positive electrode layer and the negative electrode layer, i.e., the charge / discharge curves, and to individually measure and evaluate the electrochemical impedances of the positive electrode layer and the negative electrode layer in any charging state during charging and discharging, without the reference electrode affecting the operation of the battery, while the all-solid-state battery is being operated as a battery.
[0011] It is also preferable to form a first electrode layer having two or more potentials at which a redox reaction occurs on one side of the solid electrolyte layer, and then to form the positive electrode layer by electrochemically adjusting the redox state by transferring metal ions contained in the first reference electrode to the first electrode layer. This makes it possible to easily form a stable first electrode layer, and by electrochemically adjusting the redox state of the first electrode layer, it is possible to form and evaluate a positive electrode layer that is excellent as an electrode.
[0012] It is also preferable to form a second electrode layer having two or more potentials at which a redox reaction occurs on the other surface of the solid electrolyte layer, and then to form the negative electrode layer by electrochemically adjusting the redox state by transferring metal ions contained in the second reference electrode to the second electrode layer. This makes it possible to easily form a stable second electrode layer, and by electrochemically adjusting the redox state of the second electrode layer, it is possible to form and evaluate a negative electrode layer that is excellent as an electrode.
[0013] It is preferable that the positive electrode layer, the negative electrode layer, the first reference electrode, the second reference electrode, the positive electrode-side solid electrolyte layer, and the negative electrode-side solid electrolyte layer contain sodium.
[0014] This makes it possible to evaluate an all-solid-state battery made of a sodium ion secondary battery. It is also preferable to measure the charge / discharge characteristics of the positive electrode layer and the negative electrode layer individually. According to this, without providing a reference electrode in the solid electrolyte layer that needs to be sintered, a positive electrode-side solid electrolyte layer and a first reference electrode are provided on the outside of the positive electrode layer, and a negative electrode-side solid electrolyte layer and a second reference electrode are provided on the outside of the negative electrode layer, and the first reference electrode and the second reference electrode are short-circuited to function as a pseudo reference electrode, so that while the all-solid-state battery is operating as a battery, the charge / discharge characteristics of the positive electrode layer and the negative electrode layer, i.e., the charge / discharge curves, can be measured and evaluated individually without the reference electrode affecting the operation of the battery.
[0015] In addition, it is preferable to measure the electrochemical impedance of the working electrode in any charging state during charging and discharging by using one of the positive electrode layer and the negative electrode layer as a working electrode and the other as a counter electrode, and the first reference electrode and the second reference electrode shorted together as reference electrodes. In this way, the all-solid-state battery can be evaluated by measuring the electrochemical impedance of each of the positive electrode layer and the negative electrode layer in any charging state during charging and discharging without the reference electrode affecting the operation of the battery, and a more accurate evaluation can be performed.
[0016] Another aspect of the present invention is an all-solid-state battery comprising a solid electrolyte layer including a positive electrode layer, a negative electrode layer, and an oxide solid electrolyte therebetween, a positive electrode-side wiring connected to the positive electrode layer, and a negative electrode-side wiring connected to the negative electrode layer, the all-solid-state battery comprising a positive electrode-side solid electrolyte layer containing an oxide solid electrolyte and a first reference electrode on the opposite side of the positive electrode layer from the solid electrolyte layer, and a negative electrode-side solid electrolyte layer containing an oxide solid electrolyte and a second reference electrode on the opposite side of the negative electrode layer from the solid electrolyte layer.
[0017] In this embodiment, without providing a reference electrode in the solid electrolyte layer that needs to be sintered, while the all-solid-state battery is being operated as a battery, the first reference electrode and the second reference electrode function as pseudo reference electrodes without affecting the operation of the battery, and the charge / discharge curves of the positive electrode layer and the negative electrode layer can be measured and evaluated.
[0018] In addition, it is preferable that a portion of the positive electrode side wiring is embedded in the positive electrode layer, and a portion of the negative electrode side wiring is embedded in the negative electrode layer. In this way, the positive electrode side wiring embedded in the positive electrode layer and the negative electrode side wiring embedded in the negative electrode layer can be utilized to operate as an all-solid-state battery.
[0019] Another aspect of the present invention is a method for manufacturing an all-solid-state battery having a solid electrolyte layer including a positive electrode layer, a negative electrode layer, and an oxide solid electrolyte therebetween, a positive electrode side wiring connected to the positive electrode layer, and an anode side wiring connected to the anode layer, the method comprising: laminating a positive electrode electrode mix that becomes the positive electrode layer, a negative electrode electrode mix that becomes the anode layer, and a solid electrolyte material that becomes the solid electrolyte layer between the positive electrode electrode mix and the negative electrode electrode mix; laminating a positive electrode side solid electrolyte material containing an oxide solid electrolyte on the side opposite to the solid electrolyte material of the positive electrode electrode mix; laminating a negative electrode side solid electrolyte material containing an oxide solid electrolyte on the side opposite to the solid electrolyte material of the anode electrode mix; a sintering step of forming a sintered laminate in which a first electrode layer is formed from the positive electrode mixture, a second electrode layer is formed from the negative electrode mixture, the solid electrolyte layer is formed from the solid electrolyte material, the positive electrode-side solid electrolyte layer is formed from the positive electrode-side solid electrolyte material, and the negative electrode-side solid electrolyte layer is formed from the negative electrode-side solid electrolyte material; and a reference electrode forming step of providing a first reference electrode on the side of the positive electrode-side solid electrolyte layer opposite to the first electrode layer, and providing a second reference electrode on the side of the negative electrode-side solid electrolyte layer opposite to the second electrode layer.
[0020] In this embodiment, the first and second reference electrodes are not exposed to high temperatures during sintering, so the first and second reference electrodes do not become inoperable due to high temperatures. In addition, since there is no need to provide a reference electrode in the solid electrolyte layer, it is possible to prevent a problem that would occur when the reference electrode is provided in the solid electrolyte layer and the surrounding solid electrolyte material is changed into a different composition or substance due to an unexpected reaction with the reference electrode, which would adversely affect the operation of the battery. Therefore, it is possible to easily manufacture an all-solid-state battery that has the first and second reference electrodes and that can measure the charge / discharge curves of the positive electrode layer and the negative electrode layer individually and measure and evaluate the electrochemical impedances of the positive electrode layer and the negative electrode layer individually in any charging state during charging / discharging without affecting the operation of the battery.
[0021] Another aspect of the present invention is a method for producing an all-solid-state battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer therebetween, the solid electrolyte layer including an oxide solid electrolyte, a positive electrode side wiring connected to the positive electrode layer, and a negative electrode side wiring connected to the negative electrode layer, the method comprising the steps of: laminating a positive electrode electrode mix that becomes the positive electrode layer, a negative electrode electrode mix that becomes the negative electrode layer, and a solid electrolyte material that becomes the solid electrolyte layer between the positive electrode electrode mix and the negative electrode electrode mix; laminating a positive electrode side solid electrolyte material including an oxide solid electrolyte on the side opposite to the solid electrolyte material of the positive electrode electrode mix; laminating a negative electrode side solid electrolyte material including an oxide solid electrolyte on the side opposite to the solid electrolyte material of the negative electrode electrode mix; a lamination step of laminating a first reference electrode mixture on the side opposite to the positive electrode mixture of the positive electrode material and a second reference electrode mixture on the side opposite to the negative electrode mixture of the negative electrode material to form a laminate; and a sintering step of firing the laminate to form a sintered laminate in which a first electrode layer is formed from the positive electrode mixture, a second electrode layer is formed from the negative electrode mixture, the solid electrolyte layer is formed from the solid electrolyte material, a positive electrode side solid electrolyte layer is formed from the positive electrode side solid electrolyte material, a negative electrode side solid electrolyte layer is formed from the negative electrode side solid electrolyte material, a first reference electrode layer is formed from the first reference electrode mixture, and a second reference electrode layer is formed from the second reference electrode mixture.
[0022] In this embodiment, the first and second reference electrodes can be formed by sintering outside the solid electrolyte layer without providing a reference electrode inside the solid electrolyte layer, and therefore it is possible to prevent the reference electrode from reacting unexpectedly with the surrounding solid electrolyte material, etc., to change into a different composition or substance, thereby causing a problem that adversely affects the operation of the battery, by providing the reference electrode in the solid electrolyte layer. Therefore, it is possible to easily manufacture an all-solid-state battery that has the first and second reference electrodes and that can measure the charge / discharge curves of the positive electrode layer and the negative electrode layer individually without affecting the operation of the battery during operation as a battery, and can measure and evaluate the electrochemical impedances of the positive electrode layer and the negative electrode layer individually at any charging state during charging and discharging.
[0023] Here, it is preferable that the first electrode layer has two or more types of oxidation-reduction reactions, the first reference electrode contains a metal contained in the electrode mixture for the positive electrode, and the method further includes a positive electrode formation step of applying a voltage between the first reference electrode and the first electrode layer of the sintered laminate to transfer metal ions contained in the first reference electrode to the first electrode layer, thereby forming the positive electrode layer.
[0024] According to this method, a stable first electrode layer is formed by the sintering process, and then the redox state of the first electrode layer is electrochemically adjusted by the positive electrode formation process after the sintering process, thereby forming a positive electrode layer that is excellent as an electrode. In addition, since a stable first electrode layer is formed in the sintering process, there is no need to control the sintering conditions with high precision, and productivity can be improved.
[0025] It is also preferable that the first electrode layer has two or more types of oxidation-reduction reactions, the first reference electrode layer contains a metal contained in the electrode mixture for the positive electrode, and the method further includes a positive electrode and first reference electrode formation step of applying a voltage between the first reference electrode layer and the first electrode layer of the sintered laminate to move metal ions contained in the first reference electrode layer to the first electrode layer to form the positive electrode layer from the first electrode layer and form a first reference electrode from the first reference electrode layer.
[0026] According to this, after forming stable first electrode layer and first reference electrode layer by the sintering step, the redox state of the first electrode layer and first reference electrode layer is electrochemically adjusted by the positive electrode and first reference electrode forming step after the sintering step, thereby forming a positive electrode layer and a first reference electrode that are excellent as electrodes. Furthermore, since the stable first electrode layer and first reference electrode layer are formed in the sintering step, there is no need to control the sintering conditions with high precision, and productivity can be improved.
[0027] In addition, it is preferable that the metal is sodium, whereby the sodium ions of the first reference electrode are transferred to the first electrode layer, and the redox state of the first electrode layer is electrochemically adjusted to form the positive electrode layer.
[0028] It is also preferable that the second electrode layer has two or more types of oxidation-reduction reactions, the second reference electrode contains a metal contained in the electrode mixture for the negative electrode, and the method further includes a negative electrode formation step of applying a voltage between the second reference electrode and the second electrode layer of the sintered laminate to transfer metal ions contained in the second reference electrode to the second electrode layer to form the negative electrode layer.
[0029] According to this method, a stable second electrode layer is formed by the sintering process, and then the redox state of the second electrode layer is electrochemically adjusted by the negative electrode formation process after the sintering process, thereby forming a negative electrode layer that is excellent as an electrode. In addition, since a stable second electrode layer is formed in the sintering process, there is no need to control the sintering conditions with high precision, and productivity can be improved.
[0030] It is also preferable that the second electrode layer has two or more types of oxidation-reduction reactions, the second reference electrode layer contains a metal contained in the negative electrode electrode mixture, and the method further includes a negative electrode and second reference electrode formation step of applying a voltage between the second reference electrode layer and the second electrode layer of the sintered laminate to move metal ions contained in the second reference electrode layer to the second electrode layer to form the negative electrode layer from the second electrode layer and form a second reference electrode from the second reference electrode layer.
[0031] According to this, after stable second electrode layer and second reference electrode layer are formed by the sintering process, the redox state of the second electrode layer and second reference electrode layer is electrochemically adjusted by the negative electrode and second reference electrode forming process after the sintering process, thereby forming a negative electrode layer and a second reference electrode that are excellent as electrodes. Furthermore, since the stable second electrode layer and second reference electrode layer are formed in the sintering process, there is no need to control the sintering conditions with high precision, and productivity can be improved.
[0032] In addition, it is preferable that the metal is sodium, whereby the sodium ions of the second reference electrode are transferred to the second electrode layer, and the redox state of the second electrode layer is electrochemically adjusted to form the negative electrode layer.
[0033] In addition, the lamination step preferably includes a wiring embedding step of embedding a part of the positive electrode wiring in the positive electrode electrode mixture and a part of the negative electrode wiring in the negative electrode electrode mixture, whereby the positive electrode wiring can be reliably connected to the positive electrode layer and the negative electrode wiring can be reliably connected to the negative electrode layer. Effect of the Invention
[0034] According to the present invention, there are provided a method for evaluating an all-solid-state battery, which can measure the charge / discharge curves of the positive electrode layer and the negative electrode layer individually without the reference electrode affecting the operation of the battery while the all-solid-state battery is being operated as a battery, and can evaluate the state of the all-solid-state battery by individually measuring the electrochemical impedance of the positive electrode layer and the negative electrode layer in any charging state during charging / discharging, as well as an all-solid-state battery and a method for manufacturing the same. [Brief description of the drawings]
[0035] [Figure 1] FIG. 1 is an exploded perspective view of an all-solid-state battery according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view of an all-solid-state battery according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a side view illustrating a method for manufacturing an all-solid-state battery according to an embodiment of the present invention. [Figure 4] FIG. 2 is a side view illustrating a method for manufacturing an all-solid-state battery according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a cross-sectional view illustrating a method for evaluating an all-solid-state battery according to one embodiment of the present invention. [Figure 6] 1 is a graph showing the results of charge / discharge measurement of an all-solid-state battery according to one embodiment of the present invention. [Figure 7] 1 is a graph showing evaluation results of an all-solid-state battery according to one embodiment of the present invention. [Figure 8]FIG. 11 is a side view illustrating another method for manufacturing an all-solid-state battery according to an embodiment of the present invention. [Figure 9] 1 is a graph showing the measurement results of electrochemical impedance of an all-solid-state battery according to one embodiment of the present invention. [Figure 10] 1 is a graph showing the measurement results of electrochemical impedance of an all-solid-state battery according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] The present invention will be described in detail below based on embodiments.
[0037] (Embodiment) Fig. 1 is an exploded perspective view of an all-solid-state battery according to one embodiment of the present invention, and Fig. 2 is a cross-sectional view of the all-solid-state battery.
[0038] The all-solid-state battery 1 of this embodiment is a sodium ion secondary battery that uses a compound containing sodium in the electrodes and performs charging and discharging by the movement of sodium ions.
[0039] Specifically, as shown in FIG. 1 , the all-solid-state battery 1 includes a solid electrolyte layer 2, a positive electrode layer 10 provided on one surface of the solid electrolyte layer 2, a negative electrode layer 20 provided on the other surface of the solid electrolyte layer 2 opposite to the positive electrode layer 10, a positive electrode side wiring 14 connected to the positive electrode layer 10, and a negative electrode side wiring 24 connected to the negative electrode layer 20.
[0040] On the side of the positive electrode layer 10 opposite to the solid electrolyte layer 2, a positive electrode side solid electrolyte layer 11, a first reference electrode 12, and a positive electrode side tab 13 are laminated.
[0041] Moreover, on the side of the negative electrode layer 20 opposite to the solid electrolyte layer 2, a negative electrode solid electrolyte layer 21, a second reference electrode 22, and a negative electrode tab 23 are laminated.
[0042] That is, the all-solid-state battery 1 of this embodiment has a positive electrode side tab 13, a first reference electrode 12, a positive electrode side solid electrolyte layer 11, a positive electrode layer 10, a solid electrolyte layer 2, a negative electrode layer 20, a negative electrode side solid electrolyte layer 21, a second reference electrode 22, and a negative electrode side tab 23 stacked in this order.
[0043] The solid electrolyte layer 2 is a layer containing a solid electrolyte, and may further contain a binder. The solid electrolyte is made of an oxide solid electrolyte formed by sintering. Examples of the oxide solid electrolyte include solid electrolytes containing Li element, Y element (Y is at least one of Na, Nb, B, Al, Si, P, Ti, Zr, Mo, W, S, K, Ca, and Mg), and O element. Examples of the binder used in the solid electrolyte layer 2 include rubber-based binders such as butylene rubber (BR) and styrene butadiene rubber (SBR), and fluoride-based binders such as polyvinylidene fluoride (PVdF). In this embodiment, for example, an NZSP ceramic electrolyte of Nasicon type Na3Zr2(SiO4)2(PO4) (NZSP) containing sodium and zirconium is used as the solid electrolyte of the solid electrolyte layer 2. Of course, the solid electrolyte layer 2 is not limited to the NZSP ceramic electrolyte, and may be, for example, Na 3.1 Zr 1.95 Mg 0.05 SiPO 12 (NZMSP) may also be used.
[0044] The positive electrode layer 10 and the negative electrode layer 20 are in contact with the solid electrolyte layer 2. The positive electrode layer 10 and the negative electrode layer 20 include at least an active material and a solid electrolyte. The positive electrode layer 10 and the negative electrode layer 20 may include a conductive assistant such as conductive carbon. In this embodiment, the positive electrode layer 10 and the negative electrode layer 20 are made of an active material having two or more potentials at which an oxidation-reduction reaction occurs. As the active material of the positive electrode layer 10 and the negative electrode layer 20, a Nasicon-type Na3Ti2(PO4)3 NTP electrode active material containing sodium and titanium having the same crystal structure as the solid electrolyte layer 2 and a similar chemical composition is used. In this way, by using a Nasicon-type NTP electrode active material having the same crystal structure as the solid electrolyte layer 2 and a similar chemical composition as the positive electrode layer 10 and the negative electrode layer 20, high battery performance can be obtained. In addition, by using the NTP electrode active material as the active material of the positive electrode layer 10 and the negative electrode layer 20, the redox state can be adjusted and the layer can be used as both the positive electrode and the negative electrode of the all-solid-state battery 1, as will be described in detail later. Of course, the active material of the positive electrode layer 10 and the negative electrode layer 20 is not limited to the above-mentioned materials, and may be, for example, Na3V2(PO4)3(NVP), Na4Ni3(PO4)2P2O7(NNPP), Na 0.66 Ni 0.33 Mn 0.67 O2, etc. may be used. The active materials of the positive electrode layer 10 and the negative electrode layer 20 are not limited to the same material, and different materials may be used. For example, the active material of the positive electrode layer 10 may be Na4Ni3(PO4)2P2O7 (NNPP), and the active material of the negative electrode layer 20 may be NaTi2(PO4)3 (NTP).
[0045] The positive electrode side solid electrolyte layer 11 and the negative electrode side solid electrolyte layer 21 are made of an oxide solid electrolyte. The positive electrode side solid electrolyte layer 11 and the negative electrode side solid electrolyte layer 21 may be sodium conductors containing the same material (composition) and the same sodium as the solid electrolyte layer 2. In this embodiment, the positive electrode side solid electrolyte layer 11 and the negative electrode side solid electrolyte layer 21 use the same material as the solid electrolyte layer 2, that is, a Nasicon type NZSP ceramic electrolyte containing sodium and zirconium. In addition, the positive electrode side solid electrolyte layer 11 and the negative electrode side solid electrolyte layer 21 need to have the same amount. Of course, the positive electrode side solid electrolyte layer 11 and the negative electrode side solid electrolyte layer 21 may be materials of different compositions from the solid electrolyte layer 2 as long as they are the same material and ion conductors of metal ions contained in the first reference electrode 12 and the second reference electrode 22.
[0046] The first reference electrode 12 and the second reference electrode 22 are made of flat plates formed of a metal having electrical conductivity. In addition, when the first reference electrode 12 and the second reference electrode 22 are heated simultaneously when the positive electrode side solid electrolyte layer 11 and the negative electrode side solid electrolyte layer 21 are sintered, it is necessary to use a material that can withstand the sintering temperature. In addition, the first reference electrode 12 preferably contains a metal element contained in the positive electrode layer 10. In addition, the second reference electrode 22 preferably contains a metal element contained in the negative electrode layer 20. That is, as the first reference electrode 12 and the second reference electrode 22, a flat plate of sodium metal, an alloy containing sodium, or the like can be used. In this embodiment, the first reference electrode 12 and the second reference electrode 22 are made of a flat plate of sodium metal. The first reference electrode 12 and the second reference electrode 22 need to use the same material.
[0047] Moreover, the first reference electrode 12 and the second reference electrode 22 are not limited to flat plates formed of metal. The first reference electrode 12 and the second reference electrode 22 may be formed of a material containing an active material and a solid electrolyte. The first reference electrode 12 and the second reference electrode 22 may be formed of a material containing only an active material without containing a solid electrolyte. That is, the first reference electrode 11 and the second reference electrode 22 may be formed of a material containing at least an active material. The first reference electrode 12 and the second reference electrode 22 may contain a conductive assistant such as conductive carbon. That is, the first reference electrode 12 may be formed simultaneously with the positive electrode side solid electrolyte layer 11 by stacking a first reference electrode mixture containing a metal element contained in the positive electrode layer 10, for example, an active material that causes an intercalation / deintercalation reaction of sodium, on a positive electrode side solid electrolyte material before sintering to become the positive electrode side solid electrolyte layer 11, and sintering the first reference electrode mixture together with the positive electrode side solid electrolyte material. Similarly, the second reference electrode 22 may be formed simultaneously with the negative electrode-side solid electrolyte layer 21 by stacking a second reference electrode mixture containing an active material that causes a metal element contained in the negative electrode layer 20, for example, an active material that causes an intercalation / deintercalation reaction of sodium, on the negative electrode-side solid electrolyte material before sintering that becomes the negative electrode-side solid electrolyte layer 21, and sintering the second reference electrode mixture together with the negative electrode-side solid electrolyte material. Of course, the first reference electrode 12 and the second reference electrode 22 can be formed simultaneously by simultaneously sintering the positive electrode-side solid electrolyte layer 11 and the negative electrode-side solid electrolyte layer 21. As a material for such a first reference electrode 12 and the second reference electrode 22, for example, Na3V2(PO4)3(NVP) or the like can be used. Note that the first reference electrode 12 and the second reference electrode 22 need to be made of the same material. In addition, it is preferable that the first reference electrode 12 and the second reference electrode 22 use an electrode mixture containing an active material whose reaction potential is constant with respect to the capacity. This can improve the reliability of the measured potential when the first reference electrode 12 and the second reference electrode 22 are used as reference electrodes. In addition, it is preferable that the first reference electrode mixture that becomes the first reference electrode 12 and the second reference electrode mixture that becomes the second reference electrode 22 are the same in amount.
[0048] The positive electrode side tab 13 and the negative electrode side tab 23 are formed of a conductive material, such as aluminum foil, nickel foil, sheet-like carbon, etc. It is preferable that the positive electrode side tab 13 and the negative electrode side tab 23 are made of the same material.
[0049] In addition, the positive electrode layer 10 and the negative electrode layer 20 are electrically connected to a positive electrode side wiring 14 and a negative electrode side wiring 24, respectively. In this embodiment, the positive electrode side wiring 14 has its tip portion embedded in the positive electrode layer 10, and the negative electrode side wiring 24 has its tip portion embedded in the negative electrode layer 20. Here, the positive electrode side wiring 14 is preferably provided in the center part of the positive electrode layer 10 in the thickness of the positive electrode layer 10, i.e., in the stacking direction of the positive electrode layer 10, the solid electrolyte layer 2, and the negative electrode layer 20. This allows the positive electrode side wiring 14 to be connected to the positive electrode layer 10 without being electrically biased. The position of the negative electrode side wiring 24 relative to the negative electrode layer 20 is also the same as that of the positive electrode side wiring 14. Here, charging and discharging of the all-solid-state battery 1 is carried out via the positive electrode side wiring 14 and the negative electrode side wiring 24.
[0050] In such an all-solid-state battery 1, the positive electrode layer 10 and the negative electrode layer 20 can be used as counter electrodes as shown in FIG. 5(a). In addition, as shown in FIG. 5(b), while the all-solid-state battery 1 is operated as a battery, the first reference electrode 12 and the second reference electrode 22 are short-circuited to use them as reference electrodes, so that the charge / discharge characteristics of the positive electrode layer 10 and the negative electrode layer 20, that is, the charge / discharge curves, can be measured and evaluated individually. That is, in the all-solid-state battery 1 of this embodiment, it is not necessary to embed a reference electrode in the solid electrolyte layer 2, and the reference electrode embedded in the solid electrolyte layer 2 does not adversely affect the operation of the battery. Therefore, an all-solid-state battery 1 in which the reference electrode does not affect the operation of the battery can be realized. The evaluation results of the positive electrode layer 10 and the negative electrode layer 20 will be described in detail later.
[0051] The method for manufacturing such an all-solid-state battery 1 includes a lamination step, a sintering step, a reference electrode forming step, a positive electrode forming step, and a negative electrode forming step. 3 and 4 are cross-sectional views illustrating the method for manufacturing the all-solid-state battery 1 of this embodiment.
[0052] 3(a), in the lamination step, a powder of the solid electrolyte material 102 which becomes the solid electrolyte layer 2, a positive electrode mixture 210 which becomes the positive electrode layer 10 and contains at least an active material and a solid electrolyte, a negative electrode mixture 220 which becomes the negative electrode layer 20 and contains at least an active material and a solid electrolyte, a powder of the positive electrode side solid electrolyte material 211 which becomes the positive electrode side solid electrolyte layer 11, and a powder of the negative electrode side solid electrolyte material 221 which becomes the negative electrode side solid electrolyte layer 21 are laminated to form a laminate 30. In the lamination step, the laminate 30 is formed by pressure molding.
[0053] The lamination process of this embodiment also includes a wiring embedding process of embedding a part of the positive electrode side wiring 14 in the positive electrode electrode mixture 210 and embedding a part of the negative electrode side wiring 24 in the negative electrode electrode mixture 220. In this embodiment, one end of the positive electrode side wiring 14 is embedded in the positive electrode electrode mixture 210, and the tip of the negative electrode side wiring 24 is embedded in the negative electrode electrode mixture 220. Of course, the part where the positive electrode side wiring 14 is embedded in the positive electrode electrode mixture 210 is not limited to the tip, and may be the center. In other words, two ends of the positive electrode side wiring 14 may be led out from the positive electrode electrode mixture 210. The same applies to the negative electrode side wiring 24. As described above, the positive electrode wiring 14 is preferably provided at the center in the stacking direction of the positive electrode mixture 210. The negative electrode wiring 24 is preferably provided at the center in the stacking direction of the negative electrode mixture 220.
[0054] In the sintering step, as shown in FIG. 3(b), the laminate 30 is fired to form a sintered laminate 31. In this embodiment, the laminate 30 is sintered by a spark plasma sintering (SPS) method. As a result, the solid electrolyte material 102 of the laminate 30 is sintered to form the solid electrolyte layer 2. Similarly, the positive electrode solid electrolyte material 211 and the negative electrode solid electrolyte material 221 are sintered to form the positive electrode solid electrolyte layer 11 and the negative electrode solid electrolyte layer 21, respectively. The positive electrode electrode mixture 210 is sintered to form the first electrode layer 10A, and the negative electrode electrode mixture 220 is sintered to form the second electrode layer 20A.
[0055] In this way, the first electrode layer 10A and the second electrode layer 20A formed by sintering the positive electrode mixture 210 and the negative electrode mixture 220 through the sintering process can be formed as layers containing stable NTP, i.e., NaTi2(PO4)3. Hereinafter, NTP is expressed as N[X]TP according to the number [X] of Na. Therefore, the first electrode layer 10A and the second electrode layer 20A formed through the sintering process are expressed as N1TP.
[0056] 3(c), the reference electrode formation step includes forming a first reference electrode 12 on the side of the positive electrode-side solid electrolyte layer 11 opposite to the first electrode layer 10A, and forming a second reference electrode 22 on the side of the negative electrode-side solid electrolyte layer 21 opposite to the second electrode layer 20A. The first reference electrode 12 and the second reference electrode 22 are formed by pressing metal plates together.
[0057] In the positive electrode formation process, as shown in FIG. 4(a), a constant current is applied between the first reference electrode 12 and the first electrode layer 10A, causing metal ions contained in the first reference electrode 12, in this embodiment sodium ions, to migrate to the first electrode layer 10A via the positive electrode-side solid electrolyte layer 11, and forming the positive electrode layer 10 of N3TP from the first electrode layer 10A of N1TP as shown in FIG. 4(b).
[0058] In the negative electrode formation process, as shown in FIG. 4(a), a constant current is applied between the second reference electrode 22 and the second electrode layer 20A, so that metal ions contained in the second reference electrode 22, in this embodiment, sodium ions, are transferred to the second electrode layer 20A via the negative electrode-side solid electrolyte layer 21, and as shown in FIG. 4(b), the negative electrode layer 20 of N3TP is formed from the second electrode layer 20A of N1TP. That is, after the first electrode layer 10A and the second electrode layer 20A of N1TP are formed stable by the sintering process, the redox states of the first electrode layer 10A and the second electrode layer 20A are electrochemically adjusted in the positive electrode formation process and the negative electrode formation process after the sintering process, thereby forming the positive electrode layer 10 and the negative electrode layer 20 of N3TP. It is preferable that the current applied when forming the positive electrode layer 10 and the negative electrode layer 20 is as small as possible. This is because if a large current is applied, a sufficient amount of sodium ions cannot be transferred, and there is a possibility that the positive electrode layer 10 and the negative electrode layer 20 of N3TP cannot be formed.
[0059] The positive electrode layer 10 and the negative electrode layer 20 thus formed are in the initial state of a symmetrical battery with N3TP as the initial state, and therefore can be a high-performance battery utilizing the oxidation-reduction reaction of titanium ions in the positive electrode layer 10 and the negative electrode layer 20 by the conduction of sodium ions. That is, as shown in FIG. 5(a), in the initial state of the all-solid-state battery 1, the positive electrode layer 10 and the negative electrode layer 20 are N3TP, and by charging the all-solid-state battery 1, sodium ions are conducted, and the positive electrode layer 10 becomes N1TP, and the negative electrode layer 20 becomes N4TP. In addition, by discharging the charged all-solid-state battery 1 shown in FIG. 5(b), the state shown in FIG. 5(a), that is, the positive electrode layer 10 and the negative electrode layer 20 become N3TP.
[0060] Incidentally, it is possible to directly form the positive electrode layer 10 and the negative electrode layer 20 of N3TP by the sintering process, but it is difficult to manufacture because it is necessary to control the sintering conditions such as the atmosphere during sintering with high precision. In contrast, as in this embodiment, the first electrode layer 10A and the second electrode layer 20A of N1TP are formed stably by the sintering process, and then the redox state of the first electrode layer 10A and the second electrode layer 20A is electrochemically adjusted by the positive and negative electrode forming process, so that the positive electrode layer 10 and the negative electrode layer 20 of N3TP can be formed relatively easily. In other words, in this embodiment, the sintering process can be easily performed to improve productivity.
[0061] In the all-solid-state battery 1 manufactured in this manner, a charge-discharge measurement was carried out between the positive electrode layer 10 and the negative electrode layer 20. The charge-discharge measurement was carried out at a voltage range of 2.0 V to 0.0 V and a current density of 0.02 mA / cm 2 The results are shown in Fig. 6. From the obtained results, it was confirmed that the potential difference between the positive electrode layer 10 and the negative electrode layer 20 was approximately 1.7 V. In addition, since a plateau was observed near 1.7 V, the all-solid-state battery 1 can be used as a secondary battery.
[0062] In addition, as shown in FIG. 5, the first reference electrode 12 and the second reference electrode 22 of the all-solid-state battery 1 were short-circuited to form pseudo reference electrodes, and the potentials of the positive electrode layer 10 and the negative electrode layer 20 during charging and discharging, i.e., the charge and discharge curves, were measured separately. The results are shown in FIG. 7. In FIG. 7, the measurement results of the positive electrode layer 10 are shown by a solid line, and the measurement results of the negative electrode layer 20 are shown by a dotted line. As can be seen from the results obtained, while the electrode pair of the positive electrode layer 10 and the negative electrode layer 20 is being operated as a battery, the charge and discharge characteristics of the positive electrode layer 10 and the negative electrode layer 20, i.e., the charge and discharge curves, can be measured and evaluated individually, and the all-solid-state battery 1 can be evaluated.
[0063] Here, another manufacturing method using reference electrodes containing Na3V2(PO4)3 (NVP) as an active material and a solid electrolyte as the first reference electrode 12 and the second reference electrode 22 of the all-solid-state battery 1 will be described with reference to Fig. 8. Fig. 8 is a side view for explaining another manufacturing method of the all-solid-state battery 1. Also, duplicated descriptions of steps similar to those in the manufacturing method of the all-solid-state battery 1 described above will be omitted.
[0064] The method for manufacturing the all-solid-state battery 1 includes a lamination step, a firing step, a positive electrode and a first reference electrode forming step, and a negative electrode and a second reference electrode forming step.
[0065] As shown in FIG. 8(a), the lamination step is performed by laminating a powder of the solid electrolyte material 102 to be the solid electrolyte layer 2, a cathode electrode mixture 210 containing at least an active material and a solid electrolyte to be the cathode layer 10, a cathode electrode mixture 220 containing at least an active material and a solid electrolyte to be the anode layer 20, a powder of the cathode side solid electrolyte material 211 to be the cathode side solid electrolyte layer 11, a powder of the anode side solid electrolyte material 221 to be the anode side solid electrolyte layer 21, a first reference electrode mixture 212 to be the first reference electrode 12, and a second reference electrode mixture 222 to be the second reference electrode 22 to form a laminate 30A. In addition, in the lamination step, the laminate 30A is formed by pressure molding. In addition, the first reference electrode mixture 212 and the second reference electrode mixture 222 are formed of a material containing at least an active material as described above. Moreover, the lamination step includes a wiring embedding step, similarly to the above-mentioned manufacturing method.
[0066] In the firing step, as shown in FIG. 8(b), the laminate 30A is fired in the same manner as in the above-mentioned manufacturing method to form a sintered laminate 31A. As a result, the solid electrolyte material 102 of the laminate 30A is sintered to form the solid electrolyte layer 2. Similarly, the positive electrode side solid electrolyte material 211 and the negative electrode side solid electrolyte material 221 are sintered to form the positive electrode side solid electrolyte layer 11 and the negative electrode side solid electrolyte layer 21, respectively. The positive electrode electrode mixture 210 is sintered to form the first electrode layer 10A, and the negative electrode electrode mixture 220 is sintered to form the second electrode layer 20A. The first reference electrode mixture 212 and the second reference electrode mixture 222 are sintered to form the first reference electrode layer 12A and the second reference electrode layer 22A, respectively. After the firing step, the positive electrode side tab 13 is fixed to the first reference electrode layer 12A, and the negative electrode side tab 23 is fixed to the second reference electrode layer 22A.
[0067] In this way, the first electrode layer 10A and the second electrode layer 20A obtained by sintering the positive electrode mixture 210 and the negative electrode mixture 220 by the sintering process can be formed as a layer containing stable NTP, i.e., NaTi2(PO4)3. Hereinafter, NTP is expressed as N[X]TP according to the number [X] of Na. Therefore, the active material of the first electrode layer 10A and the second electrode layer 20A formed by the sintering process is expressed as N1TP. Similarly, the first reference electrode layer 12A and the second reference electrode layer 22A obtained by sintering the first reference electrode mixture 212 and the second reference electrode mixture 222 by the sintering process can be formed as a layer containing stable NVP, i.e., Na3V2(PO4)3. Hereinafter, NVP is expressed as N[X]VP according to the number [X] of Na. Therefore, the first reference electrode layer 12A and the second reference electrode layer 22A formed by the sintering process are expressed as N3VP.
[0068] In the positive electrode and first reference electrode forming step, as shown in FIG. 8(c), a constant current is applied between the first reference electrode layer 12A and the first electrode layer 10A in the same manner as in the above-mentioned positive electrode forming step, so that metal ions contained in the first reference electrode layer 12A, in this embodiment, sodium ions, are transferred to the first electrode layer 10A via the positive electrode-side solid electrolyte layer 11, and as shown in FIG. 8(d), a positive electrode layer 10 of N3TP is formed from the first electrode layer of N1TP. Note that the amount of active material contained in the first reference electrode layer 12A (first reference electrode mixture 212) must be sufficiently larger than the amount of active material contained in the first electrode layer 10A (positive electrode mixture 210). As a result, by transferring sodium ions from the first reference electrode layer 12A to the first electrode layer 10A, a first reference electrode 12 in which N3VP and N1VP are mixed can be formed from the first reference electrode layer 12A containing N3VP. In this manner, the first reference electrode 12 exhibits a constant potential due to the mixture of N1VP and N3VP.
[0069] In the negative and second electrode forming process, a constant current is applied between the second reference electrode layer 22A and the second electrode layer 20A, and metal ions, in this embodiment, sodium ions, contained in the second reference electrode layer 22A are transferred to the second electrode layer 20A through the negative electrode-side solid electrolyte layer 21, to form the negative electrode layer 20 of N3TP from the second electrode layer 20A of N1TP. The amount of active material contained in the second reference electrode layer 22A (second reference electrode mixture 222) must be sufficiently larger than the amount of active material contained in the second electrode layer 20A (negative electrode mixture 220). This allows the second reference electrode 22 in which N3VP and N1VP are mixed to be formed from the second reference electrode layer 22A containing N3VP by transferring sodium ions from the second reference electrode layer 22A to the second electrode layer 20A. In this way, the second reference electrode 22 is in a mixed state of N1VP and N3VP, and the second reference electrode 12 shows a constant potential.
[0070] That is, after forming the stable first electrode layer 10A and second electrode layer 20A of N1TP and the stable first reference electrode layer 12A and second reference electrode layer 22A of N3VP by the sintering process, the redox states of the first electrode layer 10A and the second electrode layer 20A are electrochemically adjusted in the positive electrode and first reference electrode forming process and the negative electrode and second reference electrode forming process after the sintering process to form the positive electrode layer 10 and the negative electrode layer 20 of N3TP. Also, the redox states of the first reference electrode layer 12A and the second reference electrode layer 22A are electrochemically adjusted to form the first reference electrode 12 and the second reference electrode 22 in a mixed state of N1VP and N3VP. It is preferable that the current applied when forming the positive electrode layer 10 and the negative electrode layer 20 and the first reference electrode 12 and the second reference electrode 22 is as small as possible. This is because when a large current is applied, a sufficient amount of sodium ions cannot migrate, making it impossible to form the positive electrode layer 10 and negative electrode layer 20 of N3TP, and it may not be possible to form the first reference electrode 12 and second reference electrode 22 in a mixed state of N1VP and N3VP.
[0071] The positive electrode layer 10 and the negative electrode layer 20 thus formed form a symmetric battery with N3TP as the initial state, and therefore can be a high-performance battery that utilizes the oxidation-reduction reaction of titanium ions in the positive electrode layer 10 and the negative electrode layer 20 through the conduction of sodium ions.
[0072] In addition, as in the present manufacturing method, after forming the first electrode layer 10A and the second electrode layer 20A of N1TP stable by the sintering process, the redox state of the first electrode layer 10A and the second electrode layer 20A is electrochemically adjusted by the positive / negative electrode and the first and second reference electrode forming process, so that the positive electrode layer 10 and the negative electrode layer 20 of N3TP can be formed relatively easily. Similarly, after forming the first reference electrode layer 12A and the second reference electrode layer 22A of N3VP stable by the sintering process, the redox state of the first reference electrode layer 12A and the second reference electrode layer 22A is electrochemically adjusted by the positive / negative electrode and the first and second reference electrode forming process, so that the first reference electrode 12 and the second reference electrode 22 in a mixed state of N1VP and N3VP can be formed relatively easily. In other words, in the present manufacturing method, the sintering process can be easily performed to improve productivity.
[0073] As described above, according to the evaluation method of the all-solid-state battery 1 of this embodiment, while the all-solid-state battery 1 having an oxide-type solid electrolyte is operated as a battery, the charge / discharge characteristics of the positive electrode layer 10 and the negative electrode layer 20, i.e., the charge / discharge curves are measured, and the all-solid-state battery 1 can be evaluated. That is, in the case of an all-solid-state battery having a solid electrolyte layer using an oxide-type solid electrolyte, since the solid electrolyte layer is formed by sintering at a high temperature, it is difficult to provide a reference electrode inside the solid electrolyte layer. That is, when a reference electrode is embedded inside the solid electrolyte layer 2, when the solid electrolyte layer 2 is sintered, the reference electrode may melt and become inoperable due to the high temperature during sintering, or the reference electrode may undergo an unexpected reaction with the surrounding solid electrolyte material, etc., due to the high temperature during sintering, and may change into a different composition or substance. In contrast, with the configuration of the all-solid-state battery 1 of this embodiment, it is not necessary to embed a reference electrode inside the solid electrolyte layer 2 formed by sintering, and the first reference electrode 12 and the second reference electrode 22 can be provided after the solid electrolyte layer 2 is sintered. Therefore, the first reference electrode 12 and the second reference electrode 22 can be prevented from melting and becoming non-functional due to the high temperature during sintering, and from reacting with the surrounding solid electrolyte material and the like.
[0074] Moreover, the evaluated all-solid-state battery 1 can be used as a secondary battery. That is, even if the first reference electrode 12 and the second reference electrode 22 are provided, there is no problem in the function of the all-solid-state battery 1. Furthermore, according to the manufacturing method of the all-solid-state battery 1 of this embodiment, the oxidation-reduction state of the positive electrode layer 10 and the negative electrode layer 20 can be electrochemically adjusted to relatively easily form the positive electrode layer 10 and the negative electrode layer 20 that are optimal as electrodes of a secondary battery. That is, the positive electrode layer 10 and the negative electrode layer 20 can be formed of stable materials when they are formed by sintering, and therefore productivity can be improved.
[0075] Moreover, as with the positive electrode layer 10 and the negative electrode layer 20, the first reference electrode 12 and the second reference electrode 22 can be formed relatively easily as optimal reference electrodes for secondary batteries by electrochemically adjusting the redox states of the first reference electrode 12 and the second reference electrode 22. In other words, the first reference electrode 12 and the second reference electrode 22 can be formed of a stable material when formed by sintering, thereby improving productivity.
[0076] As another method for evaluating the all-solid-state battery 1, the electrochemical impedance of each of the positive electrode layer 10 and the negative electrode layer 20 can be measured at any state of charge (SOC) during charging and discharging. That is, as shown in FIG. 5, the first reference electrode 12 and the second reference electrode 22 of the all-solid-state battery 1 are short-circuited to form a pseudo reference electrode, and either one of the positive electrode layer 10 and the negative electrode layer 20 is used as a working electrode and the other is used as a counter electrode, and the electrochemical impedance of the working electrode can be measured at any state of charge (SOC) during charging and discharging. The results are shown in FIG. 9 and FIG. 10. FIG. 9 is a graph showing the measurement results of the electrochemical impedance measured with the positive electrode layer 10 as the working electrode and the electrochemical impedance measured with the negative electrode layer 20 as the working electrode in an environment of SOC 50% and temperature 20°C. Moreover, the full cell in Fig. 10 shows the results of measuring the electrochemical impedance between the two electrodes, the positive electrode layer 10 and the negative electrode layer 20, at SOC 50% and temperature 20°C, and the positive electrode + negative electrode shows the results of adding up the data of the positive electrode and the negative electrode in Fig. 9 for each frequency (1 MHz to 20 mHz). In Figs. 9 and 10, Na3V2(PO4)3 (NVP) was used as the first reference electrode 12 and the second reference electrode 22. That is, the all-solid-state battery 1 was manufactured by the other manufacturing method described above.
[0077] As shown in FIG. 10, the impedance spectrum of the full cell and the impedance spectrum of the positive electrode and the negative electrode are very similar, and it is understood that the impedance spectra of the positive electrode and the negative electrode can be measured separately. That is, according to the all-solid-state battery 1 of this embodiment, in any charge / discharge state of the all-solid-state battery 1 having an oxide-type solid electrolyte, the electrochemical impedance of each of the positive electrode layer 10 and the negative electrode layer 20 can be measured separately to evaluate the all-solid-state battery 1 without the first reference electrode 12 and the second reference electrode 22 affecting the operation of the battery. That is, with the configuration of the all-solid-state battery 1 of this embodiment, it is not necessary to embed a reference electrode inside the solid electrolyte layer 2 formed by sintering, and the first reference electrode 12 and the second reference electrode 22 can be provided outside the solid electrolyte layer 2 by sintering the reference electrode mixture together with other materials. Therefore, it is possible to prevent the first reference electrode 12 and the second reference electrode 22 from melting and becoming inoperable due to the high temperature during sintering, or from reacting with the surrounding solid electrolyte material, etc.
[0078] (Other embodiments) Although one embodiment of the present invention has been described above, the basic configuration of the present invention is not limited to the above.
[0079] For example, in the above-described embodiment, the positive electrode side wiring 14 and the negative electrode side wiring 24 are embedded inside the positive electrode layer 10 and the negative electrode layer 20, respectively, but are not particularly limited thereto. For example, metal tabs may be crimped onto the respective side surfaces of the positive electrode layer 10 and the negative electrode layer 20, and the positive electrode side wiring and the negative electrode side wiring may be connected to the respective metal tabs. In other words, the lamination process does not have to include the wiring embedding process.
[0080] In the all-solid-state battery 1 according to the embodiment described above, the positive electrode layer 10 and the negative electrode layer 20 are each made of a material having two or more potentials at which an oxidation-reduction reaction occurs, but the present invention is not limited thereto, and only one of the positive electrode layer 10 and the negative electrode layer 20 may be made of a material having two or more potentials at which an oxidation-reduction reaction occurs. In other words, in the manufacturing method of the all-solid-state battery 1, only one of the positive electrode forming step and the negative electrode forming step may be performed. In addition, both the positive electrode forming step and the negative electrode forming step may use a material that does not have two or more potentials at which an oxidation-reduction reaction occurs. In other words, the manufacturing method may be such that neither the positive electrode forming step nor the negative electrode forming step is performed.
[0081] In the above-described embodiment, the positive electrode side tab 13 and the negative electrode side tab 23 are provided in the all-solid-state battery 1, but this is not particularly limited, and either or both of the positive electrode side tab 13 and the negative electrode side tab 23 may be omitted. For example, when performing the above-described evaluation method, the evaluation can be performed by temporarily contacting the probe pin with the first reference electrode 12 and the second reference electrode 22.
[0082] Further, for example, in the above-described embodiment, a sodium ion secondary battery is exemplified as the all-solid-state battery 1, but the present invention is not particularly limited thereto, and even if it is a lithium ion secondary battery, the same effects can be obtained with the same configuration as in the above-described embodiment. [Explanation of symbols]
[0083] Reference Signs List 1... all-solid-state battery, 2... solid electrolyte layer, 10... positive electrode layer, 11... positive electrode side solid electrolyte layer, 12... first reference electrode, 12A... first reference electrode layer, 13... positive electrode side tab, 14... positive electrode side wiring, 20... negative electrode layer, 21... negative electrode side solid electrolyte layer, 22... second reference electrode, 22A... second reference electrode layer, 23... negative electrode side tab, 24... negative electrode side wiring, 10A... first electrode layer, 20A... second electrode layer, 30... laminate, 31... sintered laminate, 102... solid electrolyte material, 210... positive electrode electrode mixture, 211... positive electrode side solid electrolyte material, 220... negative electrode electrode mixture, 221... negative electrode side solid electrolyte material, 212... first reference electrode mixture, 222... second reference electrode mixture
Claims
1. A method for evaluating an all-solid-state battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer therebetween, the solid electrolyte layer including an oxide solid electrolyte, a positive electrode side wiring connected to the positive electrode layer, and a negative electrode side wiring connected to the negative electrode layer, the method comprising the steps of: a cathode-side solid electrolyte layer including an oxide solid electrolyte and a first reference electrode are formed on the opposite side of the cathode layer from the solid electrolyte layer; a negative electrode-side solid electrolyte layer including an oxide solid electrolyte and a second reference electrode are formed on the opposite side of the negative electrode layer from the solid electrolyte layer; The first reference electrode and the second reference electrode are short-circuited, and an evaluation is performed between the short-circuited first reference electrode and the short-circuited second reference electrode and between the positive electrode layer and the negative electrode layer, respectively. A method for evaluating an all-solid-state battery.
2. the positive electrode layer, the negative electrode layer, the first reference electrode, the second reference electrode, the positive electrode-side solid electrolyte layer, and the negative electrode-side solid electrolyte layer contain sodium, The method for evaluating an all-solid-state battery according to claim 1 .
3. The charge / discharge characteristics of the positive electrode layer and the negative electrode layer are measured individually. The method for evaluating an all-solid-state battery according to claim 1 .
4. one of the positive electrode layer and the negative electrode layer is used as a working electrode, the other as a counter electrode, and the first reference electrode and the second reference electrode, which are short-circuited, are used as reference electrodes, and the electrochemical impedance of the working electrode is measured in an arbitrary charging state during charging and discharging. A method for evaluating an all-solid-state battery.
5. An all-solid-state battery comprising: a positive electrode layer, a negative electrode layer, and a solid electrolyte layer therebetween, the solid electrolyte layer including an oxide solid electrolyte; a positive electrode side wiring connected to the positive electrode layer; and a negative electrode side wiring connected to the negative electrode layer, A cathode-side solid electrolyte layer including an oxide solid electrolyte and a first reference electrode are provided on the opposite side of the cathode layer from the solid electrolyte layer, The negative electrode layer is provided on the opposite side to the solid electrolyte layer with an anode-side solid electrolyte layer containing an oxide solid electrolyte and a second reference electrode. An all-solid-state battery characterized by:
6. The positive electrode side wiring is partially embedded in the positive electrode layer, The negative electrode side wiring is partially embedded in the negative electrode layer. The all-solid-state battery according to claim 5 .
7. A method for producing an all-solid-state battery comprising: a positive electrode layer, a negative electrode layer, and a solid electrolyte layer therebetween, the solid electrolyte layer including an oxide solid electrolyte; a positive electrode side wiring connected to the positive electrode layer; and a negative electrode side wiring connected to the negative electrode layer, the method comprising the steps of: A positive electrode mixture that will become the positive electrode layer and a negative electrode mixture that will become the negative electrode layer are laminated, and a solid electrolyte material that will become the solid electrolyte layer is laminated between the positive electrode mixture and the negative electrode mixture; A positive electrode side solid electrolyte material containing an oxide solid electrolyte is laminated on the opposite side of the positive electrode mixture from the solid electrolyte material; a lamination step of laminating an anode-side solid electrolyte material containing an oxide solid electrolyte on the side opposite to the solid electrolyte material of the anode electrode mixture to form a laminate; a sintering step of forming a sintered laminate by firing the laminate, the sintered laminate including a first electrode layer formed from the positive electrode mixture, a second electrode layer formed from the negative electrode mixture, the solid electrolyte layer formed from the solid electrolyte material, a positive electrode-side solid electrolyte layer formed from the positive electrode-side solid electrolyte material, and a negative electrode-side solid electrolyte layer formed from the negative electrode-side solid electrolyte material; a reference electrode forming step of providing a first reference electrode on the side of the positive electrode-side solid electrolyte layer opposite to the first electrode layer and providing a second reference electrode on the side of the negative electrode-side solid electrolyte layer opposite to the second electrode layer; Equipped with A method for producing an all-solid-state battery comprising the steps of:
8. A method for producing an all-solid-state battery comprising: a positive electrode layer, a negative electrode layer, and a solid electrolyte layer therebetween, the solid electrolyte layer including an oxide solid electrolyte; a positive electrode side wiring connected to the positive electrode layer; and a negative electrode side wiring connected to the negative electrode layer, the method comprising the steps of: A positive electrode mixture that will become the positive electrode layer and a negative electrode mixture that will become the negative electrode layer are laminated, and a solid electrolyte material that will become the solid electrolyte layer is laminated between the positive electrode mixture and the negative electrode mixture; A positive electrode side solid electrolyte material containing an oxide solid electrolyte is laminated on the opposite side of the positive electrode mixture from the solid electrolyte material; a negative electrode side solid electrolyte material containing an oxide solid electrolyte is laminated on the opposite side of the negative electrode electrode mixture from the solid electrolyte material; A first reference electrode mixture is laminated on the side of the positive electrode electrolyte material opposite to the positive electrode mixture; a lamination step of laminating a second reference electrode mixture on the negative electrode-side electrolyte material on a side opposite to the negative electrode-side electrode mixture to form a laminate; a sintering step of firing the laminate to form a sintered laminate in which a first electrode layer is formed from the positive electrode mixture, a second electrode layer is formed from the negative electrode mixture, the solid electrolyte layer is formed from the solid electrolyte material, a positive electrode-side solid electrolyte layer is formed from the positive electrode-side solid electrolyte material, a negative electrode-side solid electrolyte layer is formed from the negative electrode-side solid electrolyte material, a first reference electrode layer is formed from the first reference electrode mixture, and a second reference electrode layer is formed from the second reference electrode mixture; Equipped with A method for producing an all-solid-state battery comprising the steps of:
9. The first electrode layer has two or more types of oxidation-reduction reactions, The first reference electrode contains a metal contained in the electrode mixture for the positive electrode, The method further includes a positive electrode forming step of applying a voltage between the first reference electrode and the first electrode layer of the sintered laminate to move metal ions contained in the first reference electrode to the first electrode layer, thereby forming the positive electrode layer. The method for producing an all-solid-state battery according to claim 8 .
10. The first electrode layer has two or more types of oxidation-reduction reactions, the first reference electrode layer contains a metal contained in the positive electrode mixture, The method further includes a positive electrode and first reference electrode forming step of applying a voltage between the first reference electrode layer and the first electrode layer of the sintered laminate to move metal ions contained in the first reference electrode layer to the first electrode layer, thereby forming the positive electrode layer from the first electrode layer and forming a first reference electrode from the first reference electrode layer. The method for producing an all-solid-state battery according to claim 8 .
11. the metal is sodium; The method for producing an all-solid-state battery according to claim 9 or 10.
12. The second electrode layer has two or more types of oxidation-reduction reactions, The second reference electrode contains a metal contained in the electrode mixture for the negative electrode, a negative electrode forming step of applying a voltage between the second reference electrode and the second electrode layer of the sintered laminate to move metal ions contained in the second reference electrode to the second electrode layer, thereby forming the negative electrode layer. The method for producing an all-solid-state battery according to claim 7 .
13. The second electrode layer has two or more types of oxidation-reduction reactions, the second reference electrode layer contains a metal contained in the negative electrode mixture, The method further includes a negative electrode and second reference electrode forming step of applying a voltage between the second reference electrode layer and the second electrode layer of the sintered laminate to move metal ions contained in the second reference electrode layer to the second electrode layer, thereby forming the negative electrode layer from the second electrode layer and forming a second reference electrode from the second reference electrode layer. The method for producing an all-solid-state battery according to claim 8 .
14. the metal is sodium; The method for producing an all-solid-state battery according to claim 12 or 13.
15. the lamination step includes a wiring embedding step of embedding a portion of the positive electrode side wiring in the positive electrode electrode mixture and embedding a portion of the negative electrode side wiring in the negative electrode electrode mixture, The method for producing an all-solid-state battery according to claim 7 or 8.
Citation Information
Patent Citations
All-solid battery
JP2021064579A
All-solid battery
JP2022007408A