Resin composition
The resin composition, combining epoxy resin, an active ester curing agent, and an inorganic filler with a silane compound, addresses the need for low dielectric insulating layers while preventing haloing, enhancing reliability in printed wiring boards and semiconductor devices.
Patent Information
- Application Number
- JP2023083437
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-19
AI Technical Summary
There is a demand for resin compositions that can form insulating layers with low dielectric constants and low dielectric loss tangents, but existing materials cause a haloing phenomenon, leading to delamination around via holes due to deterioration during roughening treatments.
A resin composition comprising epoxy resin, an active ester curing agent, an inorganic filler, and a silane compound with a silicon atom as a ring constituent atom, which together form a cured product with low dielectric properties and suppress the haloing phenomenon.
The composition achieves a cured product with low dielectric properties and prevents delamination, ensuring continuity reliability in printed wiring boards and semiconductor devices.
Smart Images

Figure 2024166975000004 
Figure 2024166975000005 
Figure 2024166975000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition. The present invention further relates to an adhesive film, a printed wiring board, and a semiconductor device obtained by using the resin composition. [Background technology]
[0002] 2. Description of the Related Art A known manufacturing technique for printed wiring boards is a build-up method in which insulating layers and conductor layers are alternately stacked.
[0003] As an insulating material for a printed wiring board used in such an insulating layer, for example, Patent Document 1 discloses a resin composition. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2022 / 038893 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, there has been an increasing demand for resin compositions capable of forming insulating layers having low dielectric constants and dielectric loss tangents. The dielectric constant and dielectric loss tangent are sometimes collectively referred to as dielectric properties.
[0006] In order to lower the dielectric properties of the insulating layer, it is possible to include a material that lowers the dielectric properties, such as an active ester-based curing agent. However, it has been found that the cured product of the resin composition containing the material that lowers the dielectric properties causes a haloing phenomenon that reduces the reliability of electrical continuity. Here, the haloing phenomenon refers to the occurrence of delamination between the insulating layer and the inner layer substrate around the via hole. This haloing phenomenon usually occurs when the resin around the via hole is deteriorated during the formation of the via hole, and the deteriorated part is eroded during the roughening treatment. The deteriorated part is usually observed as a discolored part.
[0007] The present invention has been devised in view of the above problems, and aims to provide a resin composition capable of giving a cured product having low dielectric properties and capable of suppressing the haloing phenomenon, an adhesive film containing the resin composition, a printed wiring board having an insulating layer formed using the resin composition, and a semiconductor device. [Means for solving the problem]
[0008] As a result of intensive research into the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by incorporating a combination of (A) an epoxy resin, (B) an active ester-based curing agent, (C) an inorganic filler, and (D) a silane compound having a silicon atom as a ring-constituting atom, and have thus completed the present invention.
[0009] That is, the present invention includes the following. [1] (A) epoxy resin, (B) an active ester curing agent, (C) an inorganic filler, and (D) A resin composition containing a silane compound having a silicon atom as a ring-constituting atom. [2] The resin composition according to [1], wherein the component (C) contains either a hollow inorganic filler (C-1) or a solid inorganic filler (C-2). [3] The resin composition according to [1] or [2], wherein the component (C) contains a hollow inorganic filler (C-1). [4] The resin composition according to any one of [1] to [3], wherein the component (C) is surface-treated with the component (D). [5] The resin composition according to any one of [1] to [4], wherein the content of component (C) is 50 mass% or more, relative to 100 mass% of the non-volatile components in the resin composition. [6] The resin composition according to any one of [1] to [5], wherein the content of the (D) component is 0.1% by mass or more and 5% by mass or less, when the resin components in the resin composition are taken as 100% by mass. [7] An adhesive film comprising a support and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of [1] to [6]. [8] A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of [1] to [6]. [9] A semiconductor device comprising the printed wiring board according to [8]. Effect of the Invention
[0010] According to the present invention, it is possible to provide a resin composition capable of giving a cured product having low dielectric properties and capable of suppressing the haloing phenomenon, an adhesive film containing the resin composition, a printed wiring board having an insulating layer formed using the resin composition, and a semiconductor device. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic diagram of an insulating layer obtained by curing a resin composition according to a first embodiment of the present invention into a sheet shape, together with an inner layer substrate. [Diagram 2] FIG. 2 is a plan view showing a schematic view of the surface of an insulating layer obtained by curing the resin composition according to the first embodiment of the present invention into a sheet shape, the surface being opposite to the conductive layer. [Diagram 3] FIG. 3 is a cross-sectional view showing a roughening-treated insulating layer obtained by curing the resin composition according to the first embodiment of the present invention into a sheet shape, together with an inner layer substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0013] [Resin composition] The resin composition of the present invention contains (A) an epoxy resin, (B) an active ester-based curing agent, (C) an inorganic filler, and (D) a silane compound having a silicon atom as a ring-constituting atom. In the present invention, by containing the components (A), (B), (C), and (D) in combination, a cured product having low dielectric properties and capable of suppressing the haloing phenomenon can be obtained. In addition, a cured product having excellent elongation at break can usually be obtained.
[0014] The resin composition may further contain optional components in combination with the components (A) to (D). Examples of the optional components include a curing agent (E) (excluding those corresponding to the component (B)), a curing accelerator (F), a thermoplastic resin (G), other additives (H), and a solvent (I). Each component contained in the resin composition will be described in detail below.
[0015] <(A) Epoxy resin> The resin composition contains an epoxy resin (A) as component (A). By including the epoxy resin (A) in the resin composition, a cured product exhibiting good mechanical strength and insulation reliability can be obtained. The epoxy resin (A) may be used alone or in combination of two or more kinds.
[0016] Examples of the epoxy resin (A) include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type Examples of the epoxy resin include epoxy resins, glycidyl cyclohexane type epoxy resins, alkyl diglycidyl ether type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, phenolphthalimidine type epoxy resins, etc. The epoxy resins may be used alone or in combination of two or more.
[0017] The resin composition preferably contains, as component (A), an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the epoxy resin (A) is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.
[0018] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition may contain only a liquid epoxy resin as component (A), may contain only a solid epoxy resin, or may contain a combination of a liquid epoxy resin and a solid epoxy resin. Of these, from the viewpoint of achieving the effects of the present invention significantly, it is preferable to contain a combination of a liquid epoxy resin and a solid epoxy resin.
[0019] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0020] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, glycidyl amine type epoxy resin, and epoxy resin having a butadiene structure, glycidyl cyclohexane type epoxy resin, phenolphthalimidine type epoxy resin, and alkyl diglycidyl ether type epoxy resin are preferred, bisphenol A type epoxy resin, bisphenol F type epoxy resin, and alkyl diglycidyl ether type epoxy resin are more preferred, and bisphenol A type epoxy resin is even more preferred.
[0021] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; and "ZX1" manufactured by Nippon Steel Chemical & Material Co., Ltd. Examples of epoxy resins include "EX-721" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nagase ChemteX Corporation, "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation, "PB-3600" (epoxy resin having a butadiene structure) manufactured by Daicel Corporation, "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical & Material Corporation, and "YED216D" (alkyl diglycidyl ether type epoxy resin) manufactured by Mitsubishi Chemical Corporation. These may be used alone or in combination of two or more types.
[0022] As the solid epoxy resin, a solid epoxy resin having two or more epoxy groups in one molecule is preferable, a solid epoxy resin having three or more epoxy groups in one molecule is more preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is even more preferable.
[0023] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, and biphenyl type epoxy resin is more preferred.
[0024] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin), "HP-4700", "HP-4710" (naphthalene type tetrafunctional epoxy resin), "N-690" (cresol novolac type epoxy resin), "N-695" (cresol novolac type epoxy resin), "HP-7200", "HP-7200HH", "HP-7200H" (dicyclopentadiene type epoxy resin), "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000", "HP6000L" (naphthylene ether type epoxy resin), and "EPPN-502H" (trisphenol type epoxy resin), "NC7000L" (naphthol novolac type epoxy resin), "NC3000H", "NC3000", "NC3000L" manufactured by Nippon Kayaku Co., Ltd. Examples of epoxy resins include "NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthalene type epoxy resin) and "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YL6121" (biphenyl type epoxy resin), "YX4000HK" (bixylenol type epoxy resin), and "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd.; "YL7760" (bisphenol AF type epoxy resin), "YL7800" (fluorene type epoxy resin), "jER1010" (solid bisphenol A type epoxy resin), and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; and "WHR-991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. These may be used alone or in combination of two or more.
[0025] When a liquid epoxy resin and a solid epoxy resin are used in combination as component (A), the ratio by mass (liquid epoxy resin:solid epoxy resin) is preferably 1:0.1 to 1:20, more preferably 1:0.15 to 1:10, and particularly preferably 1:0.2 to 1:5. When the ratio by mass of the liquid epoxy resin and the solid epoxy resin is within this range, the desired effects of the present invention can be significantly obtained.
[0026] The epoxy equivalent of the (A) component is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. Within this range, a cured product of the resin composition can be obtained with sufficient crosslink density. The epoxy equivalent is the mass of an epoxy resin containing one equivalent of epoxy groups. This epoxy equivalent can be measured according to JIS K7236.
[0027] From the viewpoint of significantly obtaining the desired effects of the present invention, the weight average molecular weight (Mw) of the component (A) is preferably 100 to 5000, more preferably 150 to 3000, and even more preferably 200 to 1500. The weight average molecular weight of the epoxy resin is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).
[0028] From the viewpoint of obtaining a cured product exhibiting good mechanical strength and insulation reliability, the content of the (A) component is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 55% by mass or less, more preferably 50% by mass or less, and particularly preferably 45% by mass or less.
[0029] In the present invention, unless otherwise specified, the content of each component in the resin composition is a value when the non-volatile components in the resin composition are 100 mass %, and the non-volatile components mean all non-volatile components in the resin composition excluding the solvent.
[0030] From the viewpoint of obtaining a cured product exhibiting good mechanical strength and insulation reliability, the content of the (A) component, relative to 100 mass% of the resin component in the resin composition, is preferably 30 mass% or more, more preferably 40 mass% or more, even more preferably 50 mass% or more, and is preferably 70 mass% or less, more preferably 65 mass% or less, even more preferably 60 mass% or less.
[0031] In the present invention, the resin component in the resin composition refers to the non-volatile components of the resin composition excluding the inorganic filler (C).
[0032] <(B) Active ester curing agent> The resin composition contains an active ester curing agent (B) as the component (B). The active ester curing agent (B) as the component (B) does not include those corresponding to the above-mentioned component (A). The active ester curing agent (B) can usually form a bond by reacting with the epoxy resin (A) to cure the resin composition. By incorporating a combination of the component (A) and the active ester curing agent (B) in the resin composition, a cured product with low dielectric properties can be obtained. The component (B) may be used alone or in combination of two or more.
[0033] As the (B) active ester curing agent, generally, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferably used. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.
[0034] Specifically, the (B) component may include dicyclopentadiene-type active ester curing agents, naphthalene-type active ester curing agents containing a naphthalene structure, active ester curing agents containing an acetylated product of phenol novolac, active ester curing agents containing a benzoylation product of phenol novolac, active ester curing agents which are acetylated products of phenol novolac, active ester curing agents containing a styryl group and a naphthalene structure, and the like, and dicyclopentadiene-type active ester curing agents are preferred. As the dicyclopentadiene-type active ester curing agent, active ester curing agents containing a dicyclopentadiene-type diphenol structure are preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.
[0035] Commercially available products of component (B) include active ester curing agents containing a dicyclopentadiene-type diphenol structure, such as "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "EXB-8000L-65TM" (manufactured by DIC Corporation); naphthalene-type active ester curing agents containing a naphthalene structure, such as "HP-B-8151-62T", "EXB9416-70BK", "EXB-8100L-65T", "EXB-8150L-65T", "EXB-8150-65T", "HPC-8150-60T", "HPC-8150-62T" (manufactured by DIC Corporation), and "PC1300-02-65T" (manufactured by Air Water Corporation); and a phosphorus-containing active ester compound, such as "EXB9401" (manufactured by DIC Corporation). "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester-based hardener containing an acetylated product of phenol novolac; "YLH1026" (manufactured by Mitsubishi Chemical Corporation) as an active ester-based hardener containing a benzoylated product of phenol novolac; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester-based hardener which is an acetylated product of phenol novolac; "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester-based hardeners which are benzoylated products of phenol novolac; "EXB-8500-65T" (manufactured by DIC Corporation); and "PC1300-02-65MA" (manufactured by Air Water Corporation) as an active ester-based hardener containing a styryl group and a naphthalene structure.
[0036] From the viewpoint of being able to reduce the dielectric tangent and obtaining a cured product with excellent peel strength, the active ester group equivalent of the component (B) is preferably 50 g / eq. to 500 g / eq., more preferably 50 g / eq. to 400 g / eq., and even more preferably 100 g / eq. to 300 g / eq. The active ester group equivalent is the mass of an active ester-based curing agent containing one equivalent of an active ester group.
[0037] The ratio of the amount of the epoxy resin (A) to the active ester curing agent (B) is preferably 0.01 or more, more preferably 0.3 or more, and even more preferably 0.5 or more, and is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less, in terms of the ratio of [total number of active groups of the active ester curing agent] / [total number of epoxy groups of the epoxy resin]. Here, the "number of epoxy groups of the epoxy resin" refers to the total value of all values obtained by dividing the mass of the non-volatile components of the epoxy resin present in the resin composition by the epoxy equivalent. In addition, the "number of active groups of the active ester curing agent" refers to the total value of all values obtained by dividing the mass of the non-volatile components of the active ester curing agent present in the resin composition by the active ester group equivalent. By setting the ratio of the amount of the epoxy resin to the active ester curing agent within this range, it is possible to obtain the effects of the present invention remarkably.
[0038] From the viewpoint of obtaining a cured product having excellent dielectric properties, the content of the (B) component is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, based on 100% by mass of the non-volatile components in the resin composition, and the upper limit is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less.
[0039] From the viewpoint of obtaining a cured product with excellent dielectric properties, the content of the (B) component, relative to 100 mass% of the resin component in the resin composition, is preferably 10 mass% or more, more preferably 15 mass% or more, even more preferably 20 mass% or more, and is preferably 40 mass% or less, more preferably 35 mass% or less, even more preferably 30 mass% or less.
[0040] <(C) Inorganic filler> The resin composition contains an inorganic filler (C) as the component (C). By including the inorganic filler (C) in the resin composition, a cured product with low dielectric properties can be obtained. The inorganic filler (C) is usually included in the resin composition in the form of particles. The component (C) may be used alone or in combination of two or more types.
[0041] (C) An inorganic compound is used as the material of the inorganic filler. (C) Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferable as the silica.
[0042] (C) Inorganic fillers can be classified into (C-1) hollow inorganic fillers having internal voids and (C-2) solid inorganic fillers having no internal voids. (C) Inorganic fillers preferably contain either (C-1) hollow inorganic fillers or (C-2) solid inorganic fillers, and more preferably contain (C-1) hollow inorganic fillers from the viewpoint of obtaining a cured product with low dielectric properties.
[0043] The (C-1) hollow inorganic filler may be a monohollow particle having only one hole inside the particle, a multihollow particle having two or more holes inside the particle, or a combination of a monohollow particle and other hollow particles.
[0044] Since the hollow inorganic filler (C-1) has pores, it usually has a porosity of more than 0 volume%. The porosity of the hollow inorganic filler (C-1) is preferably 10 volume% or more, more preferably 15 volume% or more, and particularly preferably 20 volume% or more. In addition, from the viewpoint of the mechanical strength of the cured product of the resin composition, the porosity of the hollow inorganic filler (C-1) is preferably 80 volume% or less, more preferably 75 volume% or less, and particularly preferably 70 volume% or less.
[0045] The porosity P (volume %) of an inorganic filler is defined as the volume ratio of the total volume of one or more voids present inside the particle to the total volume of the particle based on the outer surface of the particle (total volume of voids / volume of particle). For example, the measured value of the actual density of the inorganic filler D M (g / cm 3 ), and the theoretical value of the material density of the material forming the inorganic filler D T (g / cm 3 ) is used to calculate the following formula (1):
number
[0046] (C-1) Hollow inorganic filler generally has voids formed within the particle and an outer shell formed of an inorganic material surrounding the voids. Usually, the voids are separated from the outside of the particle by the outer shell. In this case, it is preferable that the voids do not communicate with the outside of the particle. Therefore, it is preferable that the outer shell is a non-porous shell that does not have holes that communicate the voids with the outside of the particle. The fact that the outer shell is non-porous can be confirmed by observation with a transmission electron microscope (TEM).
[0047] From the viewpoint of obtaining the effects of the present invention remarkably, the average particle size of the hollow inorganic filler (C-1) is preferably 0.01 μm or more, more preferably 0.1 μm or more, particularly preferably 0.3 μm or more, and is preferably 5 μm or less, more preferably 4 μm or less, particularly preferably 3 μm or less.
[0048] The average particle size of particles can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, a particle size distribution of particles is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample of the inorganic filler can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the inorganic filler by ultrasonic waves for 10 minutes. The measurement sample is measured using a laser diffraction particle size distribution measuring device with blue and red light wavelengths as the light source, and the volume-based particle size distribution of the inorganic filler is measured using a flow cell method, and the average particle size can be calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.
[0049] From the viewpoint of obtaining the effects of the present invention remarkably, the BET specific surface area of the hollow inorganic filler (C-1) is preferably 1 m 2 / g or more, more preferably 2m 2 / g or more, particularly preferably 5m 2 / g or more, preferably 100m 2 / g or less, more preferably 50m 2 / g or less, particularly preferably 30m 2 The BET specific surface area of the particles can be measured by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.
[0050] The hollow inorganic filler (C-1) may be a commercially available product. Examples of commercially available hollow inorganic filler (C-1) include "MG-005" manufactured by Taiheiyo Cement Corporation and "LHP-208" manufactured by Ube Exsymo Co., Ltd.
[0051] In addition, the hollow inorganic filler (C-1) may be produced, for example, by the method described in Japanese Patent No. 5940188 or a method equivalent thereto. To give a specific example, hollow silica particles as one example of the hollow inorganic filler (C-1) can be produced by a method including the steps of: preparing an aqueous solution containing a substance capable of forming pores and a basic compound; mixing and stirring the aqueous solution with an alkoxysilane to precipitate silica particles; removing the substance capable of forming pores from the silica particles to obtain a hollow silica precursor; and calcining the hollow silica precursor.
[0052] In addition, the hollow inorganic filler (C-1) may be produced by, for example, the method described in Japanese Patent No. 5864299 or a method equivalent thereto. To give a specific example, hollow silica particles as one example of the hollow inorganic filler (C-1) can be produced by a method including: (a) a step of preparing an aqueous solution containing a substance capable of forming hollow spaces and a basic compound; (b) a step of adding an alkoxysilane to the aqueous solution and stirring at 0°C to 100°C to precipitate silica particles; (c) a step of removing the substance capable of forming hollow spaces from the silica particles obtained by the step (b) to obtain a hollow silica precursor; and (c) a step of calcining the hollow silica precursor obtained by the step (c) at a temperature exceeding 900°C to obtain hollow silica.
[0053] From the viewpoint of improving moisture resistance and dispersibility, the hollow inorganic filler (C-1) may be treated with a surface treatment agent other than the component (D) described below. Examples of the surface treatment agent other than the component (D) include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, titanate coupling agents, etc. The surface treatment agent may be used alone or in any combination of two or more.
[0054] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).
[0055] From the viewpoint of improving dispersibility, the degree of surface treatment with a surface treatment agent other than component (D) is preferably within a specific range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 8% by mass of a surface treatment agent other than component (D), more preferably with 0.2% to 5% by mass of a surface treatment agent other than component (D), and even more preferably with 0.3% to 3% by mass of a surface treatment agent other than component (D).
[0056] The degree of surface treatment with a surface treatment agent other than component (D) can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition, it is more preferable that the content is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:
[0057] The amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of the inorganic filler can be measured using a carbon analyzer. The carbon analyzer that can be used is the "EMIA-320V" manufactured by Horiba, Ltd.
[0058] From the viewpoint of obtaining the effects of the present invention prominently, the content (mass %) of the hollow inorganic filler (C-1) is preferably 0 mass % or more, more preferably 15 mass % or more, and even more preferably 20 mass % or more, and is preferably 70 mass % or less, more preferably 65 mass % or less, and even more preferably 60 mass % or less, when the non-volatile components in the resin composition are taken as 100 mass %.
[0059] From the viewpoint of obtaining the effects of the present invention prominently, the content (volume %) of the hollow inorganic filler (C-1) is preferably 1 vol% or more, more preferably 3 vol% or more, and even more preferably 5 vol% or more, and is preferably 70 vol% or less, more preferably 60 vol% or less, and even more preferably 50 vol% or less, when the non-volatile components in the resin composition are taken as 100 vol%.
[0060] From the viewpoint of obtaining the effects of the present invention remarkably, the specific gravity of the component (C-1) is preferably 3.50 g / cm 3 Less than or equal to 3.00 g / cm 3 More preferably, 2.50 g / cm 3 or less, preferably 0.05 g / cm 3 More preferably, 0.5 g / cm 3 More preferably, 1.0 g / cm 3 The specific gravity can be measured by the method described in the Examples below.
[0061] The (C-2) solid inorganic filler is an inorganic filler with a porosity of 0% by volume. The (C-2) solid inorganic filler may be a commercially available product. Examples of commercially available (C-2) solid inorganic fillers include "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "Cellspheres" and "MGH-005" manufactured by Pacific Cement Corporation; and "Spherique" and "BA-1" manufactured by JGC Catalysts and Chemicals Co., Ltd.
[0062] The average particle size of the solid inorganic filler (C-2) is preferably 0.01 μm or more, more preferably 0.1 μm or more, and even more preferably 0.3 μm or more, and is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less. The average particle size of the component (C-2) can be measured by the same method as that for the average particle size of the hollow inorganic filler (C-1).
[0063] The BET specific surface area of the solid inorganic filler (C-2) is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, preferably 100m 2 / g or less, more preferably 70m 2 / g or less, more preferably 40m 2 The BET specific surface area of the component (C-2) can be measured in the same manner as for the BET specific surface area of the component (C-2).
[0064] The (C-2) solid inorganic filler may be treated with a surface treatment agent other than the (D) component, like the (C-1) hollow inorganic filler. The surface treatment agent other than the (D) component, the degree of the surface treatment, the amount of carbon, etc. are as described above.
[0065] The content (mass %) of the (C-2) solid inorganic filler, assuming that the non-volatile components in the resin composition are 100 mass %, may be 0 mass % or more, and is preferably 10 mass % or more, more preferably 20 mass % or more, and particularly preferably 30 mass % or more, and is preferably 85 mass % or less, more preferably 80 mass % or less, and particularly preferably 75 mass % or less.
[0066] The content (volume %) of the (C-2) solid inorganic filler may be 0 volume % or more than 0 volume %, and is preferably 5 volume % or more, more preferably 10 volume % or more, and even more preferably 20 volume % or more, and is preferably 50 volume % or less, more preferably 40 volume % or less, and even more preferably 30 volume % or less, assuming that the non-volatile components in the resin composition are 100 volume %.
[0067] The ratio of pores contained in the whole (C) inorganic filler including both the (C-1) hollow inorganic filler and the (C-2) solid inorganic filler is determined as the porosity (volume %) of the (C) inorganic filler. The porosity (volume %) of the (C) inorganic filler is a representative value representing the ratio of pores to the volume of the (C) inorganic filler on a volume basis, and is expressed as "total volume of pores / total volume of the (C) inorganic filler". The specific range of the porosity of the (C) inorganic filler is preferably 10 volume % or more, more preferably 15 volume % or more, and even more preferably 20 volume % or more, and is preferably 80 volume % or less, more preferably 70 volume % or less, and even more preferably 60 volume % or less.
[0068] The average particle size of the entire inorganic filler (C) including both the hollow inorganic filler (C-1) and the solid inorganic filler (C-2) is, from the viewpoint of obtaining the effects of the present invention significantly, preferably 0.01 μm or more, more preferably 0.1 μm or more, even more preferably 0.3 μm or more, and is preferably 5 μm or less, more preferably 4 μm or less, even more preferably 3 μm or less.
[0069] The BET specific surface area of the entire inorganic filler (B) including both the hollow inorganic filler (C-1) and the solid inorganic filler (C-2) is preferably 1 m 2 / g or more, more preferably 2m 2 / g or more, more preferably 5m 2 / g or more, preferably 100m 2 / g or less, more preferably 50m 2 / g or less, more preferably 30m 2 / g or less.
[0070] When the (C) component includes both a (C-1) hollow inorganic filler and a (C-2) solid inorganic filler, the content (volume %) of the (C-1) hollow inorganic filler in the total inorganic fillers is, from the viewpoint of significantly obtaining the effects of the present invention, preferably 0 volume %, more preferably 0 volume % or more, and even more preferably 30 volume % or more, when the content of the total inorganic fillers is 100 volume %, and is preferably 100 volume %, more preferably 100 volume % or less, and even more preferably 75 volume % or less.
[0071] From the viewpoint of obtaining the effects of the present invention prominently, the content (mass %) of the (C) inorganic filler, when the non-volatile components in the resin composition are taken as 100 mass %, is preferably 50 mass % or more, more preferably 55 mass % or more, even more preferably 60 mass % or more, and is preferably 85 mass % or less, more preferably 80 mass % or less, and particularly preferably 75 mass % or less.
[0072] From the viewpoint of achieving a remarkable effect of the present invention, the content (volume %) of the (C) inorganic filler is preferably 20 vol% or more, more preferably 30 vol% or more, and even more preferably 40 vol% or more, and is preferably 80 vol% or less, more preferably 75 vol% or less, and particularly preferably 70 vol% or less, when the non-volatile components in the resin composition are taken as 100 vol%.
[0073] <(D) Silane compound having silicon atom as ring constituent atom> The resin composition contains, as the component (D), a silane compound having a silicon atom as a constituent atom of the (D) ring. The silane compound having a silicon atom as a constituent atom of the (D) ring as the component (D) does not include those corresponding to the above-mentioned components (A) to (C). By including the component (D) in the resin composition, the haloing phenomenon can be suppressed. The component (D) may be used alone or in combination of two or more kinds.
[0074] As the component (D), a compound having a cyclic structure and containing a silicon atom as a ring-constituting atom constituting the cyclic structure can be used. The cyclic structure may be a monocyclic, polycyclic, or condensed ring, but from the viewpoint of obtaining the effects of the present invention more significantly, a monocyclic structure is preferable. In addition, the cyclic structure may be a saturated cyclic structure or an unsaturated cyclic structure, but from the viewpoint of obtaining the effects of the present invention more significantly, a saturated cyclic structure is preferable. The cyclic structure is preferably a 3- to 10-membered ring, more preferably a 4- to 6-membered ring, further preferably a 5- or 6-membered ring, and particularly preferably a 5-membered ring.
[0075] The cyclic structure has a carbon atom in addition to a silicon atom as a ring-constituting atom. The ring-constituting atom may also have a heteroatom such as a nitrogen atom, an oxygen atom, or a sulfur atom. From the viewpoint of obtaining the effects of the present invention more significantly, the (D) component preferably has a silicon atom, a carbon atom, and a nitrogen atom as ring-constituting atoms, and the (D) component is preferably a cyclic silazane compound.
[0076] The number of silicon atoms as ring-constituting atoms is preferably 1 to 5, more preferably 1 or 2, and even more preferably 1. When a heteroatom is contained as a ring-constituting atom, the number of the heteroatom is preferably 1 to 3, more preferably 1 or 2, and even more preferably 1.
[0077] The component (D) preferably has 1 to 3 cyclic structures, more preferably 1 or 2 cyclic structures, and even more preferably 1 cyclic structure, in one molecule.
[0078] In the (D) component, the silicon atom as a ring-constituting atom is preferably bonded to an alkoxy group. Examples of the alkoxy group include a methoxy group, an ethoxy group, a propyloxy group, an isopropyloxy group, a butyloxy group, a pentyloxy group, and a hexyloxy group. Among them, the alkoxy group is preferably a methoxy group from the viewpoint of obtaining the effects of the present invention more prominently.
[0079] The component (D) is preferably a compound represented by formula (D-1). [ka] In the formula, R 1 and R 2 each independently represents a monovalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, A represents a heteroatom, and n represents an integer of 1 to 4.
[0080] R 1 and R 2each independently represents a monovalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. The monovalent hydrocarbon group having 1 to 20 carbon atoms is preferably a monovalent hydrocarbon group having 1 to 15 carbon atoms, more preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms, and even more preferably a monovalent hydrocarbon group having 1 to 6 carbon atoms. This number of carbon atoms does not include the number of carbon atoms of the substituent. Examples of the monovalent hydrocarbon group include an alkyl group, an alkenyl group, and an aryl group. The alkyl group may be linear, branched, or cyclic, and the preferred number of carbon atoms is as described above. Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, sec-butyl, n-pentyl, isopentyl, neopentyl, cyclopentyl, n-hexyl, isohexyl, cyclohexyl, n-heptyl, isoheptyl, n-octyl, isooctyl, tert-octyl, n-nonyl, isononyl, n-decyl, and isodecyl. The alkenyl group may be linear, branched, or cyclic, and the preferred number of carbon atoms is as described above. Examples of the alkenyl group include vinyl, allyl, butenyl, and methallyl groups. Examples of the aryl group include aryl groups such as phenyl, tolyl, and xylyl. An aryl group is preferred, and R 1 From the viewpoint of obtaining the effects of the present invention remarkably, R is preferably an aryl group, and more preferably a phenyl group. 2 From the viewpoint of obtaining the effects of the present invention remarkably, is preferably an alkyl group, and more preferably a methyl group.
[0081] R 1 and R 2 The monovalent hydrocarbon group represented by may have a substituent. The substituent is not particularly limited, and examples thereof include a halogen atom, -OH, -OC 1-6 Alkyl group, -N(C 1-10 (alkyl group) 2 , C 1-20 Alkyl group, C 2-30 Alkenyl group, C 2-30 Alkynyl group, C 6-10An aryl group, -NH 2 , -CN, -C(O)O-C 1-10 An alkyl group, -COOH, -C(O)H, -NO 2 etc. may be mentioned. Here, the term "C p-q " (where p and q are positive integers and p < q) represents that the number of carbon atoms of the organic group described immediately after this term is p to q. For example, the expression "C 1-10 alkyl group" indicates an alkyl group having 1 to 10 carbon atoms. These substituents may be bonded to each other to form a ring, and the ring structure includes spiro rings and fused rings.
[0082] A represents a heteroatom, and the heteroatom is as described above.
[0083] n represents an integer from 1 to 4, preferably 2 or 3, more preferably 3.
[0084] Examples of the component (D) include 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-methyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-methyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-butyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-butyl-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-butyl-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-butyl-1-aza-2-silacyclopentane, 2-Ethoxy-2-Methyl-1-butyl-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1-cyclohexyl-1-aza-2-silacyclopentane, 2-Methoxy-2-Methyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-Diethoxy-1 -Cyclohexyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-phenyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-phenyl-1-aza-2-silacyclopentane 2,2-dimethoxy-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2-Methoxy-2-methyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2-Ethoxy-2-methyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane 2,2-Dimethoxy-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-Methoxy-2-methyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-Ethoxy-2-methyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane , 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-Methoxy-2-methyl-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-Ethoxy-2-methyl-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1 -(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane , 2,2-dimethoxy-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2- Silacyclopentane, 2,2-dimethoxy-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-Methoxy-2-methyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-Ethoxy-2-methyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2 -Silacyclopentane, 2,2-dimethoxy-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-dimethylmethoxysilylbutyl) -1-aza-2-silacyclopentane, 2,2-dimethoxy-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2- Dimethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Dimethoxy-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-Methoxy-2-Methyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-Ethoxy-2-Methyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Dimethyl 2-methoxy-2-methyl-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-methyl) 2-Methoxy-2-methyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-Ethoxy-2-methyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Dimethyoxy 2-methoxy-2-methyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-dimethylethoxysilylpropyl, )-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-dimethylethoxysilylbutyl)-1 -Aza-2-silacyclopentane, 2,2-diethoxy-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-methyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-methyl-1-aza-2-silacyclopentane, 2 -ethoxy-2-methyl-1-methyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-butyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-butyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-butyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-butyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-cyclohexyl-1-aza-2-silacyclopentane, 2-methoxy-2 -Methyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-cyclohexyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-cyclohexyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-phenyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-phenyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane 2-ethoxy-2-methyl-1-(2-methoxycarbonyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2, 2-diethoxy-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(2-methoxycarbonyl-2-methyl)ethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane , 2,2-diethoxy-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-trimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2- Diethoxy-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-trimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-methyldimethoxysilylmethylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1 -Methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-methyldimethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy- 1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-methyldimethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-methyldimethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-di Ethoxy-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-dimethylmethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2, 2-diethoxy-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-dimethylmethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane Cyclopentane, 2,2-diethoxy-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-dimethylmethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-triethoxysilylmethyl-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-triethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2- Diethoxy-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-triethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethyl-1-methyldiethoxysilylmethylmethyl-1-aza-2-silacyclopentane, 2,2-diethoxy 2-ethoxy-2-methyl-1-methyldiethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-diethoxy-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-methyldiethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane 2,2-Dimethyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-Ethoxy-2-methyl-1-(4-methyldiethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-Di, Methoxy-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2-Methoxy-2-methyl-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-dimethylethoxysilylmethyl-1-aza-2-silacyclopentane, 2-Ethoxy-2-methyl-1-dimethylethoxysilylmethyl- 2,2-Dimethoxy-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2-Methoxy-2-Methyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Dimethyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-Diethoxy-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane -Aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(3-dimethylethoxysilylpropyl)-1-aza-2-silacyclopentane, 2,2-dimethoxy-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-methoxy-2-methyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2,2-dimethyl-1-(4-dimethylethoxysilylbutyl)-1-aza -2-silacyclopentane, 2,2-diethoxy-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, 2-ethoxy-2-methyl-1-(4-dimethylethoxysilylbutyl)-1-aza-2-silacyclopentane, tetrakis(3,4-epoxycyclohexylethyl)-tetramethylcyclotetrasiloxane, bis(3-glycidyloxypropyl)-hexaalkylcyclotetrasiloxane, and the like.
[0085] Component (D) may be a commercially available product, such as "X-88-398" (2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane) manufactured by Shin-Etsu Chemical Co., Ltd., or "KR-470," "X-40-2678," or "X-40-2728" manufactured by Shin-Etsu Silicones Co., Ltd.
[0086] The form of the (D) component contained in the resin composition of the present invention is not particularly limited, but it is preferably contained in the resin composition in any one of the following forms (i) to (iii), more preferably in the resin composition in any one of forms (ii) and (iii), and even more preferably in the resin composition in form (iii). (i) The component (D) is contained alone in the resin composition. (ii) Component (D) is contained as a surface treatment agent for inorganic filler (C). (iii) The resin composition contains the component (D) as a surface treatment agent for the inorganic filler (C) and also contains the component (D) alone in the resin composition.
[0087] "Containing component (D) as a surface treatment agent for inorganic filler (C)" means that inorganic filler (C) is surface-treated with component (D). In this case, component (D) is usually present on the surface of inorganic filler (C). Also, "containing component (D) alone in resin composition" means that component (D) is not contained as a surface treatment agent for inorganic filler (C). When component (D) is not contained as a surface treatment agent for inorganic filler (C), component (D) is free in the resin composition. In the present invention, component (D) can uniformly treat the surface of inorganic filler (C), so that the haloing phenomenon can be effectively suppressed.
[0088] When the (D) component is contained as a surface treatment agent for the (C) component, from the viewpoint of suppressing the haloing phenomenon, the content of the (D) component, relative to 100 mass% of the non-volatile components in the resin composition, is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, even more preferably 0.5 mass% or more, and is preferably 3 mass% or less, more preferably 2.5 mass% or less, even more preferably 2 mass% or less.
[0089] When the (D) component is contained as a surface treatment agent for the (C) component, from the viewpoint of suppressing the haloing phenomenon, the content of the (D) component, relative to 100 mass% of the resin component in the resin composition, is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, even more preferably 0.8 mass% or more, 1 mass% or more, or 1.5 mass% or more, and is preferably 5 mass% or less, more preferably 4 mass% or less, and even more preferably 3 mass% or less.
[0090] When the component (D) is contained as a surface treatment agent for the component (C), the degree of surface treatment with the component (D) (the content of the component (D)), from the viewpoint of suppressing the haloing phenomenon, is preferably 0.1 mass% or more, more preferably 0.2 mass% or more, even more preferably 0.3 mass% or more, or 0.6 mass% or more, relative to 100 mass% of the inorganic filler (C), and is preferably 8 mass% or less, more preferably 5 mass% or less, and even more preferably 4 mass% or less.
[0091] When the content (mass%) of the (B) component when the nonvolatile components in the resin composition are taken as 100% by mass is b, and the content (mass%) of the (D) component when the nonvolatile components in the resin composition are taken as 100% by mass is d, b / d is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more, and is preferably 50 or less, more preferably 40 or less, and even more preferably 30 or less, 20 or less, 15 or less, or 10 or less. By adjusting the contents of the (B) component and the (D) component so that b / d falls within the above range, a cured product with low dielectric properties can be obtained, and the haloing phenomenon can also be suppressed.
[0092] <(E) Hardener> The resin composition may further contain a (E) curing agent as an optional component in addition to the above-mentioned components. The (E) curing agent as the (E) component does not include those corresponding to the above-mentioned (A) to (D) components. As the (E) curing agent, a compound having a function of reacting with the (A) component to cure the resin composition can be used, and examples thereof include phenol-based curing agents, naphthol-based curing agents, carbodiimide-based curing agents, benzoxazine-based curing agents, and cyanate ester-based curing agents. Among them, the (E) curing agent preferably contains a phenol-based curing agent from the viewpoint of obtaining the effects of the present invention significantly. The (E) curing agent may be used alone or in combination of two or more kinds.
[0093] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferable. Also, from the viewpoint of adhesion to the conductor layer, a nitrogen-containing phenol-based curing agent is preferable, and a triazine skeleton-containing phenol-based curing agent is more preferable.
[0094] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN-495V", "SN375", and "SN395" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA3018-50P", "EXB-9500", and "KA-1163" manufactured by DIC Corporation.
[0095] The carbodiimide curing agent is a compound having one or more carbodiimide groups (-N=C=N-) in one molecule, and the carbodiimide curing agent is preferably a compound having two or more carbodiimide groups in one molecule.
[0096] Specific examples of the carbodiimide-based curing agent include commercially available carbodiimide-based curing agents such as Carbodilite V-03 (carbodiimide group equivalent: 216 g / eq., V-05 (carbodiimide group equivalent: 262 g / eq.), V-07 (carbodiimide group equivalent: 200 g / eq.), V-09 (carbodiimide group equivalent: 200 g / eq.), and Stavaxol P (carbodiimide group equivalent: 302 g / eq.), all manufactured by Nisshinbo Chemical Co., Ltd.
[0097] Specific examples of benzoxazine-based curing agents include "HFB2006M" manufactured by Showa Polymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.
[0098] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230", and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.
[0099] The ratio of the amount of the (A) component to the (E) component is the ratio of [total number of epoxy groups in the (A) component]:[total number of active groups in the (E) component], and is preferably in the range of 1:0.01 to 1:10, more preferably 1:0.05 to 1:8, and even more preferably 1:0.08 to 1:5. Here, the "total number of epoxy groups in the epoxy resin" refers to the total value obtained by dividing the mass of the non-volatile components of the (A) component present in the resin composition by the epoxy equivalent. In addition, the "total number of active groups in the (E) component" refers to the total value obtained by dividing the mass of the non-volatile components of the (E) component present in the resin composition by the active group equivalent. By setting the ratio of the amount of the (E) component to the (A) component within this range, the effects of the present invention can be obtained significantly.
[0100] The ratio of the amount of the (A) component to the (B) and (E) components is preferably 1:0.01 to 1:10, more preferably 1:0.3 to 1:5, and even more preferably 1:0.4 to 1:4, in terms of the ratio of [total number of epoxy groups in the (A) component] to [total number of active groups in the (B) and (E) components]. Here, the "total number of active groups in the (B) and (E) components" refers to the total value of the mass of the non-volatile components of the (B) and (E) components present in the resin composition divided by the active group equivalent. By setting the ratio of the amount of the (A) component to the (B) and (E) components within this range, the effects of the present invention can be obtained significantly.
[0101] From the viewpoint of obtaining the desired effect of the present invention remarkably, the content of the (E) component is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 8% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.
[0102] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (E) component, relative to 100 mass% of the resin component in the resin composition, is preferably 1 mass% or more, more preferably 3 mass% or more, and even more preferably 5 mass% or more, and is preferably 20 mass% or less, more preferably 15 mass% or less, and even more preferably 10 mass% or less.
[0103] <(F) Curing accelerator> In addition to the above-mentioned components, the resin composition may further contain a curing accelerator as an optional component (F). The curing accelerator (F) as the component (F) does not include those corresponding to the above-mentioned components (A) to (E). By including the component (F), it becomes possible to further accelerate the curing of the component (A). The component (F) may be used alone or in combination of two or more kinds.
[0104] Examples of the component (F) include phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, metal-based curing accelerators, amine-based curing accelerators, etc. Among these, curing accelerators selected from amine-based curing accelerators and metal-based curing accelerators are preferred, and amine-based curing accelerators are particularly preferred.
[0105] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutyl phosphonium bromide, tetrabutyl phosphonium chloride, tetrabutyl phosphonium acetate, tetrabutyl phosphonium decanoate, tetrabutyl phosphonium laurate, bis(tetrabutyl phosphonium)pyromellitate, tetrabutyl phosphonium hydrogenhexahydrophthalate, tetrabutyl phosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butyldimethylphosphonium tetraphenylborate; methyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium bromide, propyl triphenyl phosphonium bromide, butyl triphenyl phosphonium bromide, benzyl triphenyl phosphonium chloride, tetraphenyl phosphonium bromide, p-tolyl triphenyl phosphonium tetra-p-tolylborate, tetraphenyl phosphonium bromide, and the like. aromatic phosphonium salts such as tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine Examples of aromatic phosphines include tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.
[0106] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. aromatic dimethylureas such as butylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bisdimethylurea].
[0107] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.
[0108] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct imidazole compounds such as 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins.
[0109] As the imidazole-based curing accelerator, commercially available products may be used, for example, "1B2PZ", "2MZA-PW", "2PHZ-PW", and "C11Z-A" manufactured by Shikoku Chemical Industry Co., Ltd., and "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0110] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0111] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene.
[0112] As the amine-based curing accelerator, a commercially available product may be used, for example, "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0113] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (F) component, relative to 100 mass% of the non-volatile components in the resin composition, is preferably 0.01 mass% or more, more preferably 0.03 mass% or more, even more preferably 0.05 mass% or more, and is preferably 1 mass% or less, more preferably 0.8 mass% or less, even more preferably 0.5 mass% or less.
[0114] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (F) component, relative to 100 mass% of the resin component in the resin composition, is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, and is preferably 1.5 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less.
[0115] <(G)Thermoplastic resin> The resin composition may further contain a thermoplastic resin (G) as an optional component in addition to the above-mentioned components. The thermoplastic resin (G) as the component (G) does not include those corresponding to the above-mentioned components (A) to (F).
[0116] Examples of the (G) thermoplastic resin include polyimide resin, phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, etc. In one embodiment, the (G) thermoplastic resin preferably contains a thermoplastic resin selected from the group consisting of polyimide resin and phenoxy resin, and more preferably contains a phenoxy resin. The thermoplastic resin may be used alone or in combination of two or more kinds.
[0117] Specific examples of polyimide resins include "SLK-6100" manufactured by Shin-Etsu Chemical Co., Ltd., and "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd.
[0118] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group.
[0119] Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both of which are phenoxy resins containing a bisphenol A skeleton); "YX8100" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol S skeleton); "YX6954" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol acetophenone skeleton); "FX280" and "FX293" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", "YL7482", and "YL7891BH30" manufactured by Mitsubishi Chemical Corporation.
[0120] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd.; S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.
[0121] Examples of polyolefin resins include ethylene-based copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin polymers such as polypropylene and ethylene-propylene block copolymer.
[0122] Examples of polybutadiene resins include hydrogenated polybutadiene skeleton-containing resins, hydroxy group-containing polybutadiene resins, phenolic hydroxy group-containing polybutadiene resins, carboxy group-containing polybutadiene resins, acid anhydride group-containing polybutadiene resins, epoxy group-containing polybutadiene resins, isocyanate group-containing polybutadiene resins, urethane group-containing polybutadiene resins, polyphenylene ether-polybutadiene resins, and the like.
[0123] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.
[0124] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.
[0125] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.
[0126] A specific example of the polyphenylene ether resin is NORYL SA90 manufactured by SABIC, etc. A specific example of the polyetherimide resin is ULTEM manufactured by GE, etc.
[0127] Examples of polycarbonate resins include hydroxyl group-containing carbonate resins, phenolic hydroxyl group-containing carbonate resins, carboxyl group-containing carbonate resins, acid anhydride group-containing carbonate resins, isocyanate group-containing carbonate resins, and urethane group-containing carbonate resins. Specific examples of polycarbonate resins include Mitsubishi Gas Chemical's "FPC0220," Asahi Kasei Chemical's "T6002" and "T6001" (polycarbonate diols), and Kuraray's "C-1090," "C-2090," and "C-3090" (polycarbonate diols). Specific examples of polyether ether ketone resins include Sumitomo Chemical's "Sumiploy K."
[0128] Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, and polycyclohexane dimethyl terephthalate resin.
[0129] The weight average molecular weight (Mw) of the thermoplastic resin (G) is, from the viewpoint of significantly obtaining the effects of the present invention, preferably 5,000 or more, more preferably 8,000 or more, even more preferably 10,000 or more, particularly preferably 20,000 or more, and is preferably 100,000 or less, more preferably 70,000 or less, even more preferably 60,000 or less, particularly preferably 50,000 or less.
[0130] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (G) thermoplastic resin, when the non-volatile components in the resin composition are taken as 100 mass%, is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, even more preferably 1 mass% or more, and is preferably 5 mass% or less, more preferably 3 mass% or less, even more preferably 2 mass% or less.
[0131] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (G) thermoplastic resin, when the resin component in the resin composition is taken as 100 mass%, is preferably 1 mass% or more, more preferably 1.5 mass% or more, even more preferably 2 mass% or more, and is preferably 10 mass% or less, more preferably 8 mass% or less, even more preferably 5 mass% or less.
[0132] <(H) Other Additives> The resin composition may further contain other additives as optional components in addition to the above-mentioned components. (H) Other additives include, for example, radical polymerizable compounds; elastomers; polymerization initiators; organometallic compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentone and montmorillonite; defoamers such as silicone-based defoamers, acrylic defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion improvers such as urea silane; adhesion imparting agents such as triazole-based adhesion imparters, tetrazole-based adhesion imparters, and triazine-based adhesion imparters; hindered forms. antioxidants such as phenol-based antioxidants; fluorescent brightening agents such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers; photopolymerization initiation assistants such as tertiary amines; and photosensitizers such as pyrarizones, anthracenes, coumarins, xanthones, and thioxanthones. (H) Other additives may be used alone or in combination of two or more.
[0133] <(I) Solvent> The resin composition may further contain an arbitrary solvent as a volatile component in addition to the non-volatile components described above. (I) As the solvent, a known solvent can be appropriately used, and the type is not particularly limited, and an organic solvent is preferable. (I) As the solvent, for example, ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, etc.; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, anisole, etc.; alcohol-based solvents such as methanol, ethanol, propanol, butanol, ethylene glycol, etc.; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, methyl methoxypropionate, etc. Examples of the solvent include ether ester solvents such as ethyl acetate, ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate, ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butylcarbitol), amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, sulfoxide solvents such as dimethyl sulfoxide, nitrile solvents such as acetonitrile and propionitrile, aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. (I) The solvent may be used alone or in combination of two or more in any ratio.
[0134] From the viewpoint of obtaining the effect of the present invention significantly, the resin composition preferably contains 0.5% by mass or more and 6% by mass or less of the (I) solvent, based on 100% by mass of all the components of the resin composition. Specifically, the (I) solvent is preferably contained in an amount of 5% by mass or less, more preferably 4% by mass or less, and more preferably 0.5% by mass or more, more preferably 0.8% by mass or more, and even more preferably 1% by mass or more, based on 100% by mass of all the components of the resin composition.
[0135] The method for preparing the resin composition of the present invention is not particularly limited, and examples thereof include a method in which the blending components are mixed and dispersed using a rotary mixer or the like, with the addition of a solvent or the like as necessary.
[0136] <Physical properties and applications of resin compositions> By curing the resin composition of the present invention, an insulating layer formed of a cured product of the resin composition can be obtained. When a via hole is formed in this insulating layer and a roughening treatment is performed, the haloing phenomenon can be suppressed. These effects will be described below with reference to the drawings.
[0137] 1 is a cross-sectional view showing an insulating layer 100 obtained by curing a resin composition according to a first embodiment of the present invention into a sheet shape, together with an inner layer substrate 200. In this figure, a cross section of the insulating layer 100 is shown cut along a plane that passes through a center 120C of a bottom 120 of a via hole 110 and is parallel to the thickness direction of the insulating layer 100.
[0138] As shown in FIG. 1, the insulating layer 100 according to the first embodiment of the present invention is a layer obtained by curing a resin composition layer formed on an inner layer substrate 200 including a conductor layer 210, and is made of a cured product of the resin composition layer. In addition, a via hole 110 is formed in the insulating layer 100. The via hole 110 is generally formed in a forward tapered shape in which the diameter is larger toward the surface 100U of the insulating layer 100 opposite the conductor layer 210 and the diameter is smaller toward the conductor layer 210, and is ideally formed in a columnar shape having a constant diameter in the thickness direction of the insulating layer 100. This via hole 110 is usually formed by irradiating the surface 100U of the insulating layer 100 opposite the conductor layer 210 with laser light to remove a part of the insulating layer 100.
[0139] The bottom of the via hole 110 on the conductor layer 210 side is appropriately called "via bottom" and indicated by the reference symbol 120. The diameter of the via bottom 120 is called bottom diameter Lb. The opening formed on the opposite side of the via hole 110 from the conductor layer 210 is appropriately called "via top" and indicated by the reference symbol 130. The diameter of the via top 130 is called top diameter Lt. Usually, the via bottom 120 and the via top 130 are formed so that their planar shape is circular when viewed from the thickness direction of the insulating layer 100, but they may be elliptical. When the planar shape of the via bottom 120 and the via top 130 is elliptical, the bottom diameter Lb and the top diameter Lt respectively represent the major axis of the elliptical shape.
[0140] In this case, the closer to 100% the taper ratio Lb / Lt (%) obtained by dividing the bottom diameter Lb by the top diameter Lt, the better the shape of the via hole 110. By using the resin composition layer of the present invention, it is possible to easily control the shape of the via hole 110, and therefore it is possible to realize a via hole 110 with a taper ratio Lb / Lt close to 100%.
[0141] For example, the resin composition is heated at 100° C. for 30 minutes, and then heated at 180° C. for 30 minutes to harden the resin composition, to obtain an insulating layer 100. The insulating layer 100 is then irradiated with CO under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, energy of 0.2 mJ / shot, number of shots of 2, and burst mode (10 kHz). 2When a via hole 110 with a top diameter Lt of about 70 μm is formed by irradiating a laser beam, the taper ratio Lb / Lt of the via hole 110 can be set to preferably 75% to 100%, more preferably 80% to 100%, and particularly preferably 85% to 100%.
[0142] The taper ratio Lb / Lt of the via hole 110 can be calculated from the bottom diameter Lb and the top diameter Lt of the via hole 110. The bottom diameter Lb and the top diameter Lt of the via hole 110 can be measured by cutting out the insulating layer 100 using a FIB (focused ion beam) so as to reveal a cross section that is parallel to the thickness direction of the insulating layer 100 and passes through the center 120C of the via bottom 120, and then observing the cross section with an electron microscope.
[0143] FIG. 2 is a plan view showing a schematic view of a surface 100U of an insulating layer 100 obtained by curing a resin composition according to a first embodiment of the present invention into a sheet shape, the surface 100U being opposite to a conductor layer 210 (not shown in FIG. 2).
[0144] 2, when looking at the insulating layer 100 with a via hole 110 formed therein, a discolored area 140 where the insulating layer 100 has changed color may be observed around the via hole 110. The discolored area 140 may be formed by deterioration of the resin when the via hole 110 is formed, and is usually formed continuously from the via hole 110. In many cases, the discolored area 140 is a whitened area.
[0145] 3 is a cross-sectional view showing a roughening-treated insulating layer 100 obtained by curing the resin composition according to the first embodiment of the present invention into a sheet shape, together with an inner layer substrate 200. In FIG. 3, a cross section of the insulating layer 100 is shown cut along a plane passing through the center 120C of the via bottom 120 of the via hole 110 and parallel to the thickness direction of the insulating layer 100.
[0146] 3, when the insulating layer 100 in which the via hole 110 is formed is subjected to a roughening treatment, a haloing phenomenon occurs, and the insulating layer 100 in the discolored portion 140 peels off from the conductor layer 210, and a gap portion 160 continuing from the edge 150 of the via bottom 120 may be formed. This gap portion 160 is usually formed by erosion of the discolored portion 140 during the roughening treatment.
[0147] By using the resin composition of the present invention, the above-mentioned haloing phenomenon can be suppressed, and therefore, peeling of the insulating layer 100 from the conductor layer 210 can be suppressed, so that the size of the gap 160 can be reduced.
[0148] The edge 150 of the via bottom 120 corresponds to the edge on the inner circumference side of the gap 160. Therefore, the distance Wb from the edge 150 of the via bottom 120 to the end 170 on the outer circumference side of the gap 160 (i.e., the end farther from the center 120C of the via bottom 120) corresponds to the size of the gap 160 in the in-plane direction. Here, the in-plane direction refers to the direction perpendicular to the thickness direction of the insulating layer 100. In the following description, the distance Wb may be referred to as the halo distance Wb of the via hole 110 from the edge 150 of the via bottom 120. The degree of suppression of the halo phenomenon can be evaluated by the halo distance Wb from the edge 150 of the via bottom 120. Specifically, it can be evaluated that the halo distance Wb from the edge 150 of the via bottom 120 is smaller, the more effectively the halo phenomenon can be suppressed.
[0149] For example, a resin composition layer containing a resin composition is heated at 100° C. for 30 minutes, and then heated at 180° C. for 30 minutes to harden the resin composition to obtain an insulating layer 100. The insulating layer 100 is then irradiated with CO under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, energy of 0.2 mJ / shot, number of shots of 2, and burst mode (10 kHz). 2 A laser beam is applied to form a via hole 110 with a top diameter Lt of about 70 μm. The substrate is then immersed in a swelling liquid at 60° C. for 5 minutes, then in an oxidizing agent solution at 80° C. for 10 minutes, then in a neutralizing liquid at 40° C. for 5 minutes, and then dried at 80° C. for 15 minutes.
[0150] The halo distance Wb from the edge 150 of the via bottom 120 can be measured by using a FIB (focused ion beam) to remove the insulating layer 100 so as to reveal a cross section that is parallel to the thickness direction of the insulating layer 100 and passes through the center 120C of the via bottom 120, and then observing the cross section with an electron microscope.
[0151] Furthermore, by using the resin composition of the present invention, the shape of the via hole 110 in the insulating layer 100 before the roughening treatment can be easily controlled, and therefore, it is usually possible to easily control the shape of the via hole 110 in the insulating layer 100 after the roughening treatment. Therefore, even after the roughening treatment, the shape of the via hole 110 can be made good, just like before the roughening treatment. Therefore, by using the resin composition of the present invention, it is possible to realize a via hole 110 with a taper ratio Lb / Lt close to 100% in the insulating layer after the roughening treatment.
[0152] For example, the resin composition layer is heated at 100° C. for 30 minutes, and then heated at 180° C. for 30 minutes to harden the resin composition layer, to obtain an insulating layer 100. The insulating layer 100 is then irradiated with CO under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, energy of 0.2 mJ / shot, number of shots of 2, and burst mode (10 kHz). 2 A laser beam is irradiated to form a via hole 110 with a top diameter Lt of about 70 μm. The via hole 110 is then immersed in a swelling solution at 60° C. for 5 minutes, then immersed in an oxidizing agent solution at 80° C. for 10 minutes, then immersed in a neutralizing solution at 40° C. for 5 minutes, and then dried at 80° C. for 15 minutes. By using the resin composition of the present invention, the taper ratio Lb / Lt of the via hole 110 formed in the insulating layer 100 thus obtained can be set to preferably 76% to 100%, more preferably 80% to 100%, and particularly preferably 85% to 100%.
[0153] The taper ratio Lb / Lt of the via hole 110 can be calculated from the bottom diameter Lb and the top diameter Lt of the via hole 110. The bottom diameter Lb and the top diameter Lt of the via hole 110 can be measured by cutting out the insulating layer 100 using a FIB (focused ion beam) so as to reveal a cross section that is parallel to the thickness direction of the insulating layer 100 and passes through the center 120C of the via bottom 120, and then observing the cross section with an electron microscope.
[0154] Furthermore, according to the study of the present inventor, it has been found that, in general, the larger the diameter of the via hole 110, the larger the size of the discolored portion 140 tends to be, and therefore the size of the gap portion 160 also tends to be larger. Therefore, the degree of suppression of the halo phenomenon can be evaluated by the ratio of the size of the gap portion 160 to the diameter of the via hole 110. For example, the evaluation can be performed by the halo ratio Hb to the bottom radius Lb / 2 of the via hole 110. Here, the bottom radius Lb / 2 of the via hole 110 refers to the radius of the via bottom 120 of the via hole 110. In addition, the halo ratio Hb to the bottom radius Lb / 2 of the via hole 110 is a ratio obtained by dividing the halo distance Wb from the edge 150 of the via bottom 120 by the bottom radius Lb / 2 of the via hole 110. The smaller the halo ratio Hb to the bottom radius Lb / 2 of the via hole 110, the more effectively the halo phenomenon can be suppressed.
[0155] For example, the resin composition is heated at 100° C. for 30 minutes, and then heated at 180° C. for 30 minutes to harden the resin composition, to obtain an insulating layer 100. The insulating layer 100 is then irradiated with CO under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, energy of 0.2 mJ / shot, number of shots of 2, and burst mode (10 kHz). 2A laser beam is irradiated to form a via hole 110 having a top diameter Lt of 30 μm±2 μm. The via hole 110 is then immersed in a swelling solution at 60° C. for 5 minutes, then immersed in an oxidizing agent solution at 80° C. for 10 minutes, then immersed in a neutralizing solution at 40° C. for 5 minutes, and then dried at 80° C. for 15 minutes. By using the resin composition of the present invention, the haloing ratio Hb of the via hole 110 formed in the insulating layer 100 thus obtained to the bottom radius Lb / 2 can be preferably 35% or less, more preferably 30% or less, and even more preferably 25% or less.
[0156] The halo ratio Hb of the via hole 110 to the bottom radius Lb / 2 can be calculated from the bottom diameter Lb of the via hole 110 and the halo distance Wb from the edge 150 of the via bottom 120 of the via hole 110.
[0157] Furthermore, by using the resin composition of the present invention, it is usually possible to suppress the formation of discolored portion 140 during the formation of via hole 110. Therefore, as shown in Fig. 2, the size of discolored portion 140 can be reduced, and ideally, discolored portion 140 can be eliminated. The size of discolored portion 140 can be evaluated by the haloing distance Wt from edge 180 of via top 130 of via hole 110.
[0158] The edge 180 of the via top 130 corresponds to the edge on the inner circumference side of the discolored portion 140. The halo distance Wt from the edge 180 of the via top 130 represents the distance from the edge 180 of the via top 130 to the edge 190 on the outer circumference side of the discolored portion 140. It can be evaluated that the smaller the halo distance Wt from the edge 180 of the via top 130, the more effectively the formation of the discolored portion 140 can be suppressed.
[0159] The halo distance Wt from the edge 180 of the via top 130 can be measured by observation with an optical microscope.
[0160] Moreover, according to the study of the present inventor, it has been found that, in general, the larger the diameter of the via hole 110, the larger the size of the discolored portion 140 tends to be. Therefore, the degree of suppression of the formation of the discolored portion 140 can be evaluated by the ratio of the size of the discolored portion 140 to the diameter of the via hole 110. For example, the evaluation can be performed by the halo ratio Ht to the top radius Lt / 2 of the via hole 110. Here, the top radius Lt / 2 of the via hole 110 refers to the radius of the via top 130 of the via hole 110. Also, the halo ratio Ht to the top radius Lt / 2 of the via hole 110 is a ratio obtained by dividing the halo distance Wt from the edge 180 of the via top 130 by the top radius Lt / 2 of the via hole 110. The smaller the halo ratio Ht to the top radius Lt / 2 of the via hole 110, the more effectively the formation of the discolored portion 140 can be suppressed.
[0161] For example, the resin composition layer is heated at 100° C. for 30 minutes, and then heated at 180° C. for 30 minutes to harden the resin composition layer, to obtain an insulating layer 100. The insulating layer 100 is then irradiated with CO under the conditions of a mask diameter of 1 mm, a pulse width of 16 μs, energy of 0.2 mJ / shot, number of shots of 2, and burst mode (10 kHz). 2 When a via hole 110 with a top diameter Lt of approximately 70 μm is formed by irradiating laser light, the haloing ratio Ht of the via hole 110 to the top radius Lt / 2 can be preferably 45% or less, more preferably 40% or less, and even more preferably 35% or less.
[0162] The halo ratio Ht of the via hole 110 to the top radius Lt / 2 can be calculated from the top diameter Lt of the via hole 110 and the halo distance Wt from the edge 180 of the via top 130 of the via hole 110.
[0163] In the manufacturing process of the printed wiring board, the via hole 110 is usually formed without another conductor layer (not shown) being provided on the surface 100U of the insulating layer 100 opposite the conductor layer 210. Therefore, if the manufacturing process of the printed wiring board is understood, it is possible to clearly recognize the structure in which the via bottom 120 is on the conductor layer 210 side and the via top 130 is open on the opposite side of the conductor layer 210. However, in the completed printed wiring board, there may be cases where conductor layers are provided on both sides of the insulating layer 100. In this case, it may be difficult to distinguish the via bottom 120 and the via top 130 depending on the positional relationship with the conductor layer. However, usually, the top diameter Lt of the via top 130 is equal to or larger than the bottom diameter Lb of the via bottom 120. Therefore, in the above case, it is possible to distinguish the via bottom 120 and the via top 130 depending on the diameter size.
[0164] In addition to suppressing the haloing phenomenon, the resin composition of the present invention can provide a cured product having low dielectric properties. Furthermore, by curing the resin composition of the present invention, an insulating layer having excellent elongation at break is usually obtained.
[0165] The cured product obtained by thermally curing the resin composition at 200°C for 90 minutes exhibits the characteristic of a low dielectric loss tangent. Thus, the cured product provides an insulating layer with a low dielectric loss tangent. The dielectric loss tangent is preferably 0.008 or less, more preferably 0.005 or less, and even more preferably 0.004 or less. The lower limit of the dielectric loss tangent may be 0.0001 or more. The dielectric loss tangent can be measured according to the method described in the examples below.
[0166] The cured product obtained by thermally curing the resin composition at 200°C for 90 minutes exhibits the characteristic of a low relative dielectric constant. Thus, the cured product provides an insulating layer with a low relative dielectric constant. The relative dielectric constant is preferably 4 or less, more preferably 3.5 or less, and even more preferably 3 or less. The lower limit of the relative dielectric constant may be 1 or more. The relative dielectric constant can be measured according to the method described in the examples below.
[0167] A cured product obtained by thermally curing a resin composition at 200°C for 90 minutes usually exhibits the property of high elongation at break. Thus, the cured product provides an insulating layer with high elongation at break. The elongation at break is measured by a tensile test in accordance with JIS K7127. The elongation at break is preferably 1% or more, more preferably 1.3% or more, and even more preferably 1.7% or more. The upper limit of the elongation at break may be 10% or less. The elongation at break can be measured according to the method described in the examples below.
[0168] The resin composition of the present invention can provide a cured product having low dielectric properties and capable of suppressing the haloing phenomenon. Furthermore, it can provide a cured product having excellent elongation at break. Therefore, the resin composition of the present invention can be suitably used as a resin composition for insulating purposes. Specifically, it can be suitably used as a resin composition for forming an insulating layer (resin composition for forming an insulating layer) for forming a conductor layer (including a rewiring layer) formed on an insulating layer.
[0169] Furthermore, in the multilayer printed wiring board described below, the resin composition can be suitably used as a resin composition for forming an insulating layer of a multilayer printed wiring board (resin composition for forming an insulating layer of a multilayer printed wiring board) and a resin composition for forming an interlayer insulating layer of a printed wiring board (resin composition for forming an interlayer insulating layer of a printed wiring board).
[0170] In addition, for example, when a semiconductor chip package is manufactured through the following steps (1) to (6), the resin composition of the present invention can be suitably used as a resin composition for a rewiring formation layer (resin composition for forming a rewiring formation layer) as an insulating layer for forming a rewiring layer, and as a resin composition for sealing a semiconductor chip (resin composition for sealing a semiconductor chip). When a semiconductor chip package is manufactured, a rewiring layer may be further formed on the sealing layer. (1) A step of laminating a temporary fixing film onto a substrate; (2) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (3) forming an encapsulation layer on the semiconductor chip; (4) peeling the substrate and the temporary fixing film from the semiconductor chip; (5) forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; and (6) A process of forming a rewiring layer as a conductor layer on the rewiring formation layer.
[0171] [Adhesive film] The adhesive film of the present invention comprises a support and a resin composition layer formed from the resin composition of the present invention provided on the support.
[0172] The thickness of the resin composition layer is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less, from the viewpoint of making the printed wiring board thinner and being able to provide a cured product with excellent insulation even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 5 μm or more.
[0173] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.
[0174] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0175] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0176] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.
[0177] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.
[0178] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.
[0179] In one embodiment, the adhesive film may further include other layers as necessary. Examples of such other layers include a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.
[0180] The adhesive film can be produced, for example, by preparing a resin varnish by dissolving the resin composition in a solvent, applying the resin varnish onto a support using a die coater or the like, and then drying the varnish to form a resin composition layer. The solvent is as described above.
[0181] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the solvent in the resin varnish, for example, when a resin varnish containing 30 mass % to 60 mass % of the solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.
[0182] The adhesive film can be stored in a rolled form. When the adhesive film has a protective film, it can be used by peeling off the protective film.
[0183] [Printed wiring board] The printed wiring board of the present invention includes an insulating layer formed from a cured product of the resin composition of the present invention.
[0184] The printed wiring board can be produced, for example, by using the above-mentioned adhesive film by a method including the following steps (I) and (II). (I) A step of laminating the adhesive film on the inner layer substrate so that the resin composition layer of the adhesive film is bonded to the inner layer substrate. (II) A step of thermally curing the resin composition layer to form an insulating layer
[0185] The "inner layer substrate" used in step (I) is a member that becomes the substrate of a printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed during the manufacture of a printed wiring board is also included in the "inner layer substrate" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.
[0186] The lamination of the inner layer substrate and the adhesive film can be carried out, for example, by thermocompression bonding the adhesive film to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the adhesive film to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression member not directly onto the adhesive film but via an elastic material such as heat-resistant rubber so that the adhesive film can sufficiently follow the surface irregularities of the inner layer substrate.
[0187] The lamination of the inner layer substrate and the adhesive film may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.
[0188] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.
[0189] After lamination, the laminated adhesive film may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.
[0190] The support may be removed between step (I) and step (II) or after step (II).
[0191] In step (II), the resin composition layer is thermally cured to form an insulating layer. The conditions for thermally curing the resin composition layer are not particularly limited, and conditions that are usually employed when forming an insulating layer for a printed wiring board may be used.
[0192] For example, the thermal curing conditions for the resin composition layer vary depending on the type of resin composition, etc., but the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.
[0193] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. or more and less than 120° C. (preferably 60° C. or more and 115° C. or less, more preferably 70° C. or more and 110° C. or less) for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes).
[0194] In manufacturing a printed wiring board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art for use in manufacturing printed wiring boards. When the support is removed after step (II), the support may be removed between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, the formation of the insulating layer and the conductor layer in steps (II) to (V) may be repeated to form a multilayer wiring board, as necessary.
[0195] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.
[0196] Step (IV) is a step of roughening the insulating layer. Usually, in this step (IV), smears are also removed. The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by performing a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order. The swelling liquid used in the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, and the like, and is preferably an alkaline solution, and as the alkaline solution, a sodium hydroxide solution and a potassium hydroxide solution are more preferable. Examples of commercially available swelling liquids include "Swelling Dip Securigans P", "Swelling Dip Securigans SBU", and "Swelling Dip Securigant P" manufactured by Atotech Japan. The swelling treatment using a swelling liquid is not particularly limited, but can be performed, for example, by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes. The oxidizing agent used in the roughening treatment is not particularly limited, but examples thereof include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 to 30 minutes. In addition, the concentration of the permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securiganth P" manufactured by Atotech Japan. The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product is, for example, "Reduction Solution Securiganth P" manufactured by Atotech Japan. Treatment with a neutralizing solution can be performed by immersing the surface that has been roughened with an oxidizing agent in the neutralizing solution at 30°C to 80°C for 1 to 30 minutes.From the viewpoint of workability etc., a method in which the object that has been subjected to roughening treatment with an oxidizing agent is immersed in a neutralizing solution at 40° C. to 70° C. for 5 minutes to 20 minutes is preferred.
[0197] In one embodiment, the arithmetic mean roughness (Ra) of the insulating layer surface after the roughening treatment is preferably 300 nm or less, more preferably 250 nm or less, and even more preferably 200 nm or less. There is no particular limit to the lower limit, but it is preferably 30 nm or more, more preferably 40 nm or more, and even more preferably 50 nm or more. The arithmetic mean roughness (Ra) of the insulating layer surface can be measured using a non-contact surface roughness meter.
[0198] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.
[0199] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0200] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.
[0201] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.
[0202] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.
[0203] [Semiconductor Devices] The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the printed wiring board of the present invention.
[0204] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft).
[0205] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) on a conductive portion of a printed wiring board. The "conductive portion" refers to a portion of a printed wiring board that transmits an electric signal, and the portion may be either on the surface or embedded. The semiconductor chip is not particularly limited as long as it is an electric circuit element made of semiconductor material.
[0206] The method of mounting a semiconductor chip when manufacturing a semiconductor device is not particularly limited as long as the semiconductor chip functions effectively, but specific examples include a wire bonding mounting method, a flip chip mounting method, a bumpless buildup layer (BBUL) mounting method, an anisotropic conductive film (ACF) mounting method, a non-conductive film (NCF) mounting method, etc. Here, the "bumpless buildup layer (BBUL) mounting method" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess in a printed wiring board and the semiconductor chip is connected to the wiring on the printed wiring board." EXAMPLES
[0207] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" mean "parts by mass" and "% by mass", respectively.
[0208] <Measurement of the average particle size of inorganic fillers> 100 mg of inorganic filler and 10 g of methyl ethyl ketone were weighed into a vial and dispersed by ultrasonic waves for 10 minutes. Using a laser diffraction particle size distribution measuring device (HORIBA, Ltd.'s "LA-960"), the particle size distribution of the inorganic filler was measured on a volume basis using a flow cell method with blue and red light source wavelengths. From the particle size distribution obtained, the average particle size of the inorganic filler was calculated as the median diameter.
[0209] <Measurement of average porosity of inorganic filler> The density of the inorganic filler was measured using a true density measuring device (QUANTACHROME's "ULTRAPYCNOMETER 1000"). In this measurement, nitrogen was used as the measurement gas. The measured density (measured value) D M (g / cm 3 ) and the material density (theoretical value) D of the inorganic material (silica) that forms the inorganic filler T (g / cm 3) was used to measure the average porosity of the inorganic filler according to the above formula (I). In the above formula (I), the material density (theoretical value) of silica as the inorganic material is 2.2 g / cm 3 It was decided.
[0210] <Synthesis Example 1: Production of Hollow Silica Particles 1> Hollow silica particles 1 were synthesized according to the description in Japanese Patent No. 5864299. The average particle size of the obtained hollow silica particles 1 was 2.0 μm, and the porosity was 50% by volume.
[0211] <Example 1> 280 parts of solid silica (average particle size 0.5 μm, Admatechs' "SO-C2") and 1.68 parts of aminosilane coupling agent (Shin-Etsu Chemical's "X-88-398") were mixed with 100 parts of MEK and 20 parts of solvent naphtha, heated and stirred at 60°C for 2 hours, and then cooled to room temperature. This produced a stirred liquid containing solid silica surface-treated with an aminosilane coupling agent. The mixture was mixed with 30 parts of bisphenol A epoxy resin (Mitsubishi Chemical's "828US", epoxy equivalent approx. 180 g / eq.), 30 parts of biphenyl epoxy resin (Nippon Kayaku's "NC3000H", epoxy equivalent approx. 269 g / eq.), 14 parts of triazine skeleton-containing phenolic hardener (DIC's "LA-3018-50P", hydroxyl equivalent approx. 151 g / eq., 2-methoxypropanol solution with 50% non-volatile components), and 10 parts of active ester compound. A resin varnish was prepared by mixing 40 parts of a resin (DIC Corporation's "HPC-8000-65T," active group equivalent weight approximately 223 g / eq., toluene solution with 65% nonvolatile content), 10 parts of a phenoxy resin (Mitsubishi Chemical Corporation's "YX6954BH30," a 1:1 solution of MEK and cyclohexanone with 30% nonvolatile content), and 6 parts of a curing accelerator ("DMAP," 4-dimethylaminopyridine, MEK solution with 5% solid content by mass) and dispersing the mixture uniformly using a high-speed rotating mixer.
[0212] A PET film (Toray Industries, Inc., "Lumirror R80", thickness 38 μm) that had been treated with an alkyd resin-based release agent (Lintec Corporation, "AL-5") was prepared as a support. A resin varnish was uniformly applied onto the release layer of the support using a die coater so that the thickness of the resin composition layer after drying was 40 μm, and the resin varnish was dried at 80 to 120°C (average 100°C) for 4 minutes to produce an adhesive film.
[0213] <Example 2> In Example 1, the stirring liquid containing the solid silica surface-treated with aminosilane coupling agent is changed to the stirring liquid containing the solid silica surface-treated with aminosilane coupling agent and the hollow silica surface-treated with aminosilane coupling agent. Except for the above, the same procedure as in Example 1 is followed to prepare a resin varnish and an adhesive film.
[0214] A stirred liquid containing solid silica surface-treated with an aminosilane coupling agent and hollow silica surface-treated with an aminosilane coupling agent was obtained by the following method. 140 parts of solid silica (average particle size 0.5 μm, Admatechs' "SO-C2"), 70 parts of hollow silica (average particle size 0.5 μm, porosity 50 volume%, Ube Exsymo's "LHP-208"), and 2.24 parts of aminosilane coupling agent (Shin-Etsu Chemical's "X-88-398") were mixed with 100 parts of MEK and 20 parts of solvent naphtha, heated and stirred at 60°C for 2 hours, and then cooled to room temperature. As a result, a stirred liquid containing solid silica surface-treated with an aminosilane coupling agent and hollow silica surface-treated with an aminosilane coupling agent was obtained.
[0215] <Example 3> In Example 2, 1) 70 parts of hollow silica (average particle size 0.5 μm, porosity 50 vol%, Ube Exsymo's "LHP-208") was replaced with 70 parts of hollow silica particles 1 (average particle size 2.0 μm, porosity 50 vol%). 2) The amount of silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 2.24 parts to 3.08 parts. Except for the above, the resin varnish and adhesive film were prepared in the same manner as in Example 2.
[0216] <Example 4> In Example 1, 1) 280 parts of solid silica (average particle size 0.5 μm, Admatechs' "SO-C2") was replaced with 140 parts of hollow silica particles 1 (average particle size 2.0 μm, porosity 50% by volume), 2) The amount of silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 1.68 parts to 4.48 parts. A resin varnish and an adhesive film were prepared in the same manner as in Example 1 except for the above.
[0217] <Example 5> The amount of the silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 1.68 parts to 0.84 parts in Example 1. A resin varnish and an adhesive film were prepared in the same manner as in Example 1 except for the above.
[0218] <Example 6> In Example 4, the amount of the silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed from 4.48 parts to 2.24 parts. A resin varnish and an adhesive film were prepared in the same manner as in Example 4 except for the above.
[0219] <Comparative Example 1> In Example 1, 1.68 parts of the silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was replaced with 1.68 parts of an aminosilane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.). A resin varnish and an adhesive film were prepared in the same manner as in Example 1 except for the above.
[0220] <Comparative Example 2> In Example 4, 4.88 parts of the silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was replaced with 4.48 parts of an aminosilane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.). A resin varnish and an adhesive film were prepared in the same manner as in Example 4 except for the above.
[0221] <Comparative Example 3> In Example 4, 4.88 parts of the silane coupling agent ("X-88-398" manufactured by Shin-Etsu Chemical Co., Ltd.) was changed to 8.96 parts of an aminosilane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.). A resin varnish and an adhesive film were prepared in the same manner as in Example 4 except for the above.
[0222] <Comparative Example 4> The silane coupling agent (X-88-398 manufactured by Shin-Etsu Chemical Co., Ltd.) (4.88 parts) was not used in Example 1. A resin varnish and an adhesive film were prepared in the same manner as in Example 1 except for the above points.
[0223] <Preparation of cured product for evaluation> The adhesive films having a thickness of 40 μm produced in the examples and comparative examples were heated at 200° C. for 90 minutes to thermally cure the resin composition layers, and then the support was peeled off. The resulting cured products are referred to as “cured products for evaluation.”
[0224] <Measurement of relative permittivity and dielectric loss tangent> The cured product for evaluation was cut into a test piece having a width of 2 mm and a length of 80 mm. The relative dielectric constant and dielectric loss tangent of the test piece were measured by the cavity resonance perturbation method at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C using an "HP8362B" manufactured by Agilent Technologies. Measurements were performed on two test pieces, and the average value was calculated.
[0225] <Measurement of elongation at break> The cured product for evaluation was subjected to a tensile test in accordance with Japanese Industrial Standards (JIS K7127) using a Tensilon universal testing machine ("RTC-1250A" manufactured by Orientec Co., Ltd.) to measure the elongation at break.
[0226] <Preparation of a sample for evaluating haloing> (1) Surface preparation for inner layer circuit boards Both sides of a glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.4 mm, Panasonic R1515A) with an inner layer circuit formed were etched 1 μm with a microetching agent (Mec CZ8101) to roughen the copper surface.
[0227] (2) Lamination of adhesive film with support Using a batch-type vacuum pressure laminator (MVLP-500, manufactured by Meiki Co., Ltd.), each adhesive film prepared was laminated on both sides of the inner layer circuit board. Lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing for 30 seconds at 100°C and a pressure of 0.74 MPa.
[0228] (3) Curing of the resin composition layer The laminated adhesive film was cured at 130° C. for 30 minutes, and then at 170° C. for 30 minutes to cure the resin composition layer, thereby forming an insulating layer.
[0229] (4) Via hole formation CO 2 Using a laser processing machine (Hitachi Via Mechanics, LC-2E21B / 1C), the insulating layer was drilled under the conditions of a mask diameter of 1.60 mm, a focus offset value of 0.050, a pulse width of 25 μs, a power of 0.66 W, an aperture of 13, a shot number of 2, and a burst mode (10 kHz), forming multiple via holes so that the top diameter (diameter) of the via holes on the insulating layer surface was approximately 50 μm. Then, the support was peeled off.
[0230] (5) Roughening treatment The inner layer circuit board on which the insulating layer was formed was immersed in a swelling liquid, Swelling Dip Securigant P (aqueous solution of glycol ethers and sodium hydroxide) containing diethylene glycol monobutyl ether manufactured by Atotech Japan, at 60°C for 10 minutes, and then Concentrate Compact P (KMnO 4The substrate was immersed in a neutralizing solution (aqueous solution of sulfuric acid, manufactured by Atotech Japan) at 40°C for 5 minutes, and then dried at 80°C for 30 minutes. This substrate is called the evaluation substrate.
[0231] <Measurement of via hole dimensions, halo distance, and halo ratio after roughening treatment> The cross-section of the evaluation substrate was observed using a FIB-SEM composite device ("SMI3050SE" manufactured by SII Nano Technology Co., Ltd.). In detail, the insulating layer was cut out using a FIB (focused ion beam) so that a cross-section parallel to the thickness direction of the insulating layer and passing through the center of the via bottom of the via hole appeared. This cross-section was observed by SEM. The bottom diameter and top diameter of the via hole were measured from the observed image.
[0232] In addition, in the image observed by SEM, a gap was observed that was formed by the insulating layer peeling off from the copper foil layer of the inner layer substrate, continuing from the edge of the via bottom. Therefore, from the observed image, the distance r1 from the center of the via bottom to the edge of the via bottom (corresponding to the inner radius of the gap) and the distance r2 from the center of the via bottom to the far end of the gap (corresponding to the outer radius of the gap) were measured, and the difference between these distances r1 and r2 (r2-r1) was calculated as the halo distance from the edge of the via bottom at that measurement point.
[0233] The above measurement was performed on five randomly selected via holes. The average of the top diameters of the five measured via holes was adopted as the top diameter Lt of the sample after the roughening treatment. The average of the bottom diameters of the five measured via holes was adopted as the bottom diameter Lb of the sample after the roughening treatment. Furthermore, the average of the halo distances of the five measured via holes was adopted as the halo distance Wb from the edge of the via bottom of the sample.
[0234] From the measurement results, the taper ratio (the ratio of the top diameter Lt of the via hole after the roughening treatment to the bottom diameter Lb, “Lb / Lt”) and the halo ratio Hb (the ratio of the halo distance Wb from the edge of the via bottom after the roughening treatment to the radius (Lb / 2) of the via bottom of the via hole after the roughening treatment, “Wb / (Lb / 2)”) were calculated and evaluated according to the following criteria. ○: Haloing ratio Hb is 35% or less. △: Haloing ratio Hb is greater than 35% and less than 50%. ×: Haloing ratio Hb is greater than 50%.
[0235] [Table 1] *In the table, the content (mass%) of component (C) represents the content when the nonvolatile components in the resin composition are taken as 100 mass%, the content (volume%) of component (C) represents the content when the nonvolatile components in the resin composition are taken as 100 volume%, and the content of component (D) represents the content when the resin components in the resin composition are taken as 100 mass%.
[0236] In Examples 1 to 6, it was confirmed that even when components (E) to (G) were not contained, the results were similar to those of the above Examples, although to different degrees. [Explanation of symbols]
[0237] 100 Insulating layer 100U The surface of the insulating layer opposite the conductive layer 110 Beer Hall 120 Beer Bottom 120C Center of via bottom 130 Beer Top 140 Discolored area 150 Edge of via bottom 160 Gap 170 End 180 Via top edge 190 Outer edge 200 Inner layer board 210 Conductive layer (first conductive layer) Lb Bottom diameter of via hole Lt Top diameter of via hole Wt Halo distance from the edge of the via top Wb Halo distance from the edge of the via bottom
Claims
1. (A) an epoxy resin, (B) an active ester-based curing agent, (C) an inorganic filler, and (D) a resin composition containing a silane compound having a silicon atom as a ring-constituting atom.
2. The resin composition according to claim 1, wherein the component (C) comprises either a hollow inorganic filler (C-1) or a solid inorganic filler (C-2).
3. The resin composition according to claim 1, wherein the component (C) comprises a hollow inorganic filler (C-1).
4. The resin composition according to claim 1 , wherein the component (C) has been surface-treated with the component (D).
5. The resin composition according to claim 1, wherein the content of the component (C) is 50% by mass or more, based on 100% by mass of non-volatile components in the resin composition.
6. The resin composition according to claim 1 , wherein the content of the component (D) is 0.1% by mass or more and 5% by mass or less, when the resin component in the resin composition is 100% by mass.
7. An adhesive film comprising a support and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of claims 1 to 6.
8. A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of claims 1 to 6.
9. A semiconductor device comprising the printed wiring board according to claim 8.
Citation Information
Patent Citations
Resin composition
JP2013173841A
Resin composition
JP2015034300A
Resin composition for semiconductor sealing, and semiconductor device
JP2019077840A
Curable resin composition
JP2020164699A
Thermosetting resin composition and semiconductor device
JP2022029527A