Silicone rubber composition for acoustic lens and method for producing the same
A silicone rubber composition with nano-silica particles addresses ultrasonic wave attenuation and impedance issues in acoustic lenses by using a specific manufacturing process, resulting in improved sensitivity and reduced reflection.
Patent Information
- Application Number
- JP2023083819
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
AI Technical Summary
Existing acoustic lenses for ultrasound diagnostic apparatuses face challenges in minimizing ultrasonic wave attenuation and achieving acoustic impedance close to that of living tissue, leading to suboptimal detection sensitivity and reflection issues.
A silicone rubber composition containing 82 to 86 parts by mass of nano-silica particles with an average diameter of 50 to 70 nm, combined with silicone rubber, is used to manufacture acoustic lenses through a process involving kneading, molding, and heat-treating at 150 to 170°C for 18 to 30 hours without a vulcanizing agent, resulting in a sheet with reduced acoustic attenuation and suitable impedance.
The composition achieves ultrasonic wave attenuation of 7 dB/mm or less and acoustic impedance of 1.45±0.05 MRayl, enhancing detection sensitivity and reducing measurement variations.
Smart Images

Figure 2024167618000002 
Figure 2024167618000003 
Figure 2024167618000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a silicone rubber composition for acoustic lenses and a method for producing the same. [Background technology]
[0002] Ultrasound diagnostic devices used for health checkups and the like can image the subject's organs and the like by transmitting ultrasound to the subject and receiving the reflected waves. Such ultrasound diagnostic devices are equipped with an ultrasound probe, and an acoustic lens is provided at a portion that transmits and receives ultrasound and is in close contact with the subject (e.g., Patent Document 1). From the viewpoint of suppressing reflection of ultrasound between the acoustic lens and the body surface of the subject, it is desirable for the acoustic lens to exhibit an acoustic impedance close to that of a living body. Furthermore, from the viewpoint of increasing the detection sensitivity of ultrasound received from the subject, it is required that the acoustic lens have a small amount of ultrasound attenuation. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-95178 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention provides a silicone rubber composition for acoustic lenses suitable for producing acoustic lenses with low ultrasonic attenuation, and a method for producing the same. [Means for solving the problem]
[0005] [1] A silicone rubber composition for acoustic lenses, comprising silicone rubber and nanosilica particles, the nanosilica particles being contained in an amount of 82 to 86 parts by mass out of a total mass of 100 parts by mass of the entire composition. [2] The silicone rubber composition for acoustic lenses according to [1], wherein the average particle size of the nanosilica particles is 50 to 70 nm. [3] A method for producing a silicone rubber composition for acoustic lenses, comprising the steps of: obtaining a mixture by kneading uncured silicone rubber with nanosilica particles; molding the mixture into a desired shape to obtain an uncured molded body; and heat-treating the uncured molded body at a specified temperature for a specified time to obtain a cured molded body. [4] The method for producing a silicone rubber composition for acoustic lenses according to [3], wherein the desired shape is a sheet having a thickness of 3 to 7 mm, and the predetermined temperature and time are 150 to 170°C and 18 to 30 hours. [5] The method for producing a silicone rubber composition for acoustic lenses according to [3] or [4], wherein no vulcanizing agent for curing is mixed into the kneaded mixture. Effect of the Invention
[0006] According to the silicone rubber composition for acoustic lenses and the manufacturing method thereof of the present invention, the attenuation of ultrasonic waves can be reduced, for example, to 7 dB / mm or less. Also, the acoustic impedance can be set in the range of 1.45±0.05 MRayl. Furthermore, by using an aqueous solution containing a surfactant during measurement, the variation in the measured values can be suppressed. [Brief description of the drawings]
[0007] [Figure 1] 1 shows the results of investigating the acoustic characteristics of the compositions prepared in Test Examples 1 to 3. [Diagram 2] 1 shows the results of investigating the rate of weight change before and after heat curing of the composition prepared in Test Example 2. [Diagram 3] This shows the results of investigating the change in acoustic characteristics due to the presence or absence of a surfactant in Test Example 4. [Figure 4] 4 shows the results of investigating the variation in measurement values due to the presence or absence of a surfactant in Test Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <Silicone rubber composition for acoustic lenses> A first aspect of the present invention is a silicone rubber composition for an acoustic lens, which comprises a silicone rubber and nanosilica particles.
[0009] Examples of silicone rubbers include those having an organopolysiloxane skeleton, and preferably those containing a methyl group or a vinyl group (e.g., silicone rubber having a dimethylpolysiloxane structure), but are not limited thereto. The silicone rubber may include modified silicone rubbers such as alkyd silicone and epoxy silicone.
[0010] Nanosilica particles are aggregates of nano-level silica particles with a particle diameter of less than 1 μm. Those manufactured and sold as so-called fumed silica are suitable. Nanosilica particles may be aggregated to form submicron-sized aggregates. The content of silica (SiO2) in the total mass of the nanosilica particles is preferably 99% or more. The average particle size of the nanosilica particles is preferably 50 to 70 nm, which is determined by observing the surface or cross section of the silicone rubber composition of this embodiment with an electron microscope and averaging the longest diameters (longest diameters) of 10 or more nanosilica particles randomly selected from the nanosilica particles contained within the observation field. The specific surface area of nanosilica particles is, for example, 50 to 380 m 2 / g range is preferred. It is preferable that silanol groups are present on the surface of the nanosilica particles. The true specific gravity of the nanosilica particles is preferably in the range of, for example, 2.0 to 2.4. Nanosilica particles having the above-mentioned preferable properties are commercially available and can be purchased, for example, from Nippon Aerosil Co., Ltd.
[0011] In the silicone rubber composition for acoustic lenses of this embodiment, the nanosilica particles are preferably contained in a proportion of 82 to 86 parts by mass out of a total mass of 100 parts by mass of the entire composition, and the remainder is preferably silicone rubber. The above preferred content ratio can sufficiently reduce the amount of acoustic attenuation.
[0012] The silicone rubber composition for acoustic lenses of this embodiment may contain any optional components other than the silicone rubber and the nanosilica particles. Examples of optional components include moisture that can be unavoidably mixed in during production, vulcanizing agents used in curing silicone rubber, dyes, pigments, and the like. However, in a preferred production method described below, the heat curing treatment is carried out without the inclusion of a vulcanizing agent, making it possible to thoroughly remove moisture from within the silicone rubber composition for acoustic lenses. From the viewpoint of reducing the amount of ultrasonic attenuation while maintaining the acoustic impedance of the acoustic lens formed from the present composition within a suitable range, the content of optional components contained in the present composition is preferably 0 to 10 mass %, more preferably 0 to 5 mass %, and even more preferably 0 to 1 mass %, relative to the total mass of the present composition.
[0013] The water content in the silicone rubber composition for acoustic lenses of this embodiment is preferably 100 ppm or less, more preferably 80 ppm or less, and even more preferably 50 ppm or less, relative to the total mass of the composition. When the content is within the above preferred range, the effect of reducing the amount of ultrasonic attenuation can be further achieved while keeping the acoustic impedance within the above preferred range. The water content of the present composition is a value measured by the Karl Fischer method.
[0014] As the vulcanizing agent, a general vulcanizing agent for silicone rubber can be used, and examples thereof include 2,5-dimethyl-2,5-ditertiarybutylperoxycyclohexane, p-methylbenzoyl peroxide, and ditertiarybutyl peroxide. It is optional whether or not a vulcanizing agent is blended in the present composition. When a vulcanizing agent is blended, the blending amount can be, for example, 0.1 to 1 part by mass per 100 parts by mass of the silicone rubber.
[0015] The silicone rubber composition for acoustic lenses of this embodiment can be produced by a conventional method in the same manner as known silicone rubber compositions, but the production method of the second embodiment described below is preferred. The silicone rubber composition for acoustic lenses of this embodiment can be molded by ordinary methods in the same manner as known silicone rubber compositions, and is suitable as a material for acoustic lenses of desired shapes.
[0016] When the silicone rubber composition for acoustic lenses of this embodiment is molded into a sheet of the desired thickness (for example, 5 mm±0.2 mm) and irradiated with longitudinal ultrasonic waves of 10.0 MHz at 25°C in the thickness direction, the attenuation is preferably 7.0 dB / mm or less, more preferably 6.5 dB / mm or less, and even more preferably 6.0 dB / mm or less. The sheet is a test specimen that resembles a simple acoustic lens. The smaller the attenuation in the acoustic lens, the more efficient and sensitive the ultrasonic measurement can be.
[0017] The acoustic properties of a molded article made of the silicone rubber composition for acoustic lenses of this embodiment are evaluated and measured as follows. All of the acoustic properties are measured when the molded article is at 25° C. and 1 atmospheric pressure.
[0018] <Sound speed> The sound speed (unit: m / s) in the molded body is preferably 900 to 1600 m / s, which is close to the sound speed in living tissue, and can be, for example, 950 to 1050 m / s (approximately 1000 m / s). The sound speed in the molded body is determined by measuring the time (propagation time) required for ultrasonic waves (longitudinal waves with a frequency of 1.0 to 10.0 MHz) emitted from a surface (one surface) of a sheet-like test piece and reflected by the back surface (the other surface) to reach the surface, and calculating the propagation distance / propagation time. For measuring the sound velocity, for example, an ultrasonic thickness gauge "Echometer 1060" (manufactured by Nihon Matec Co., Ltd.) can be used.
[0019] <Acoustic impedance> The acoustic impedance of the molded article is preferably in the range of 1.40 to 1.60 MRayl, which is close to the acoustic impedance of a living body. The density ρ (g / cm 3 The density ρ can be calculated from the mass (g) of the molded body and the sound speed v (m / s) by the formula: ρ × v. Here, the sound speed v can be calculated by the above-mentioned measuring method, and the density ρ can be calculated by multiplying the mass (g) of the molded body by its volume (cm 3 ) to find the answer.
[0020] <Acoustic attenuation> The acoustic attenuation of the molded article (also simply referred to as attenuation) is preferably small for longitudinal waves of ultrasonic waves having a frequency of 1.0 to 10.0 MHz, in order to enable ultrasonic waves to be transmitted and received with high efficiency and high sensitivity and to obtain high-quality images. Specifically, the attenuation of the ultrasonic waves is preferably 8.0 dB / mm or less, more preferably 7.0 dB / mm or less, and even more preferably 6.0 dB / mm or less. The amount of attenuation is calculated using the following formula: Formula: 20×log 10 [(Intensity B1 / Intensity B2)] / (Propagation distance) The intensity B1 in the above formula is calculated as the intensity value of ultrasonic waves received on the front surface after ultrasonic waves are emitted from the front surface (one surface) of a sheet-like test piece and reflected by the back surface (the other surface). Here, intensity B1 is the intensity of the ultrasonic waves after they have made one round trip through the test piece, and intensity B2 is the intensity of the ultrasonic waves after they have made two round trips through the test piece, with the propagation distance being twice the thickness of the test piece. The attenuation can be measured, for example, by using an ultrasonic thickness gauge "Echometer 1060" (manufactured by Nihon Matec Co., Ltd.).
[0021] <<Method for producing silicone rubber composition for acoustic lenses>> A second aspect of the present invention is a method for producing a silicone rubber composition for acoustic lenses, comprising the steps of: obtaining a kneaded product by kneading uncured silicone rubber with nanosilica particles (kneading step); molding the kneaded product into a desired shape to obtain an uncured molded body (molding step); and heat-treating the uncured molded body at a prescribed temperature for a prescribed time to obtain a cured molded body (curing step). It is preferable to produce the silicone rubber composition for acoustic lenses of the first embodiment by the production method of this embodiment.
[0022] In the kneading step, the above-mentioned materials are kneaded to obtain a kneaded product. The blending ratio of the kneading materials is preferably within the above-mentioned preferred range. As the kneading method, a known resin composition kneading method using a kneader or multiple rolls can be applied. From the viewpoint of facilitating molding in the next step, the obtained kneaded product preferably has a viscosity and hardness equivalent to those of commonly known materials that can be molded into a desired shape, such as clay, paste, gel, etc.
[0023] In the molding step, the kneaded material obtained in the previous step is molded into a desired shape to obtain an uncured molded body. The uncured molded body may be in a so-called semi-cured state. The desired shape may be, for example, a sheet having a thickness of 3 to 7 mm. The sheet shape is preferable because moisture in the sheet is easily removed during heat curing in the next step. There is no particular limitation on the method for forming the irregular lump kneaded material into a sheet, and a known device for forming a resin composition (for example, a roll molding machine) can be used.
[0024] In the curing step, the uncured molded body obtained in the previous step is heated and cured to obtain the desired molded body. The heat curing temperature and time are preferably 150 to 170° C. and 18 to 30 hours. This range is preferable because it is easy to remove moisture from within the uncured molded body during the heat curing treatment and to obtain the desired molded body with reduced acoustic attenuation. EXAMPLES
[0025] [Test Example 1] Silicone rubber (manufactured by Shin-Etsu Silicones, a general-purpose SR lens material with hardness 70°Hs and specific gravity 1.4), silicone rubber (manufactured by Shin-Etsu Silicones, hardness 17°Hs, specific gravity 0.98, raw rubber), nanosilica particles (40 nm nanosilica), and 0.5 parts by mass of a vulcanizing agent (manufactured by Shin-Etsu Silicones, vulcanizing agent A) were thoroughly kneaded in a kneader to obtain a silicone rubber composition (kneaded product) for acoustic lenses. The obtained kneaded product was formed into a sheet with a thickness of about 1 to 2 mm, and heat cured at 180° C. for 10 minutes. The obtained sheet sample was used as an acoustic lens, and the acoustic impedance (unit: MRayl) and acoustic attenuation (10 MHz conversion value; unit: dB / mm) were measured at 25°C using the method described above. The results are shown in Figure 1.
[0026] [Test Example 2] Silicone rubber (manufactured by Shin-Etsu Silicone Co., Ltd.), silicone rubber (manufactured by Shin-Etsu Silicone Co., Ltd.), and nanosilica particles were thoroughly kneaded in a kneader to obtain a silicone rubber composition for acoustic lenses (kneaded material). Here, no commonly used vulcanizing agent was added, and the kneaded material obtained was molded into a sheet with a thickness of 5 mm and heat-treated at 160°C for 24 hours. After heat treatment, a vulcanizing agent was added. The obtained sheet sample was used as an acoustic lens, and the acoustic characteristics were measured in the same manner as in Test Example 1. The results are shown in FIG.
[0027] [Test Example 3] The same materials as in Test Example 2 were mixed and kneaded 30 times with a three-roll mill. The obtained silicone rubber composition for acoustic lenses was molded into a sheet having a thickness of 5 mm and was heat treated at 160° C. for 24 hours. The obtained sheet sample was used as an acoustic lens, and the acoustic characteristics were measured in the same manner as in Test Example 1. The results are shown in FIG.
[0028] (Preliminary Examination) A silicone rubber composition for acoustic lenses containing no vulcanizing agent was obtained in the same manner as in Test Example 2. This was molded into a sheet with a thickness of 5 mm and heated at 180°C for 16 hours. The weight was measured before and after heating, and the rate of change was calculated. This test was performed three times and the weight change rates were plotted, the results of which are shown in Figure 2. The results in FIG. 2 show that the moisture in the composition is removed during heat curing.
[0029] [Test Example 4] Using sheet samples (thickness: 1 to 2 mm) obtained in the same manner as in Test Example 3, the acoustic attenuation was measured at 25°C. In the measurements, a comparison was made between the case where water was applied between the measurement probe and the sheet sample and the case where an aqueous surfactant solution was applied. This test was performed on five sheet samples. The results are shown in Figure 3. The average of these five results is shown in Figure 4.
[0030] When the same sheet was measured, the difference in noise level was up to 0.9 dB / mm depending on whether or not a surfactant was used. When comparing the measurements of the five sheets, the differences were small, ranging from -0.1 to 0.5 dB / mm, when surfactant was present. From the results shown in FIGS. 3 and 4, it is clear that the use of an aqueous surfactant solution can reduce the variability in acoustic measurements.
[0031] [Test Example 5] The kneaded product obtained in the same manner as in Test Example 1 was formed into a sheet having a thickness of 1 to 2 mm and heat cured at 180° C. for 10 minutes. The obtained sheet sample was used as an acoustic lens, and the acoustic characteristics were measured at 25° C. in the same manner as in Test Example 1. The results are shown in Table 1. Incidentally, the 40 nm nanosilica (represented as nanosilica A in the table) has silanol groups on its surface, and is known to be hydrophilic.
[0032] [Test Example 6] The kneaded product obtained in the same manner as in Test Example 2 was molded into a sheet with a thickness of 5 mm and heat-treated at 160° C. for 24 hours. A vulcanizing agent was added to the obtained sheet sample, which was used as an acoustic lens and the acoustic properties were measured in the same manner as in Test Example 5. The results are shown in Table 1.
[0033] [Test Example 7] The surface of the 40 nm silica was treated with a commercially available silane coupling agent to obtain silica nanoparticles with hydrophobic surfaces. Except for using this, a sheet sample was obtained in the same manner as in Test Example 1, and the acoustic properties were measured. The results are shown in Table 1.
[0034] [Test Example 8] A sheet sample was obtained and its acoustic properties were measured in the same manner as in Test Example 1, except that nanosilica particles (surface-treated 40 nm silica) (referred to as Nanosilica B in the table) were used. The results are shown in Table 1. The surface of Nanosilica B was treated with trimethylsilane to make it hydrophobic.
[0035] [Table 1]
[0036] The results of Test Examples 5 to 8 show that an acoustic lens with reduced acoustic attenuation can be obtained by subjecting an uncured silicone rubber composition that does not contain a vulcanizing agent to a heat curing treatment at 150 to 170°C for 18 to 30 hours.
[0037] <Acoustic lens molding> An acoustic lens can be molded by charging the silicone rubber composition according to the present invention into a concave mold and pressing it. Depending on the shape of the mold used, for example, an acoustic lens with a flange can also be molded. Although detailed test results are not shown, the inventors have found through their investigation that the less the charged silicone rubber composition flows or deforms within the mold during pressing, the more the acoustic properties, particularly the attenuation, of the resulting acoustic lens are reduced.
Claims
1. A silicone rubber composition for acoustic lenses comprising silicone rubber and nanosilica particles, wherein the nanosilica particles are contained in an amount of 82 to 86 parts by mass per 100 parts by mass of the total mass of the entire composition.
2. 2. The silicone rubber composition for acoustic lenses according to claim 1, wherein the average particle size of the nanosilica particles is 50 to 70 nm.
3. a step of obtaining a kneaded product by kneading uncured silicone rubber and nanosilica particles; a step of forming the kneaded product into a desired shape to obtain an uncured molded body; a step of heat-treating the uncured molded body at a predetermined temperature for a predetermined time to obtain a cured molded body; A method for producing a silicone rubber composition for acoustic lenses, comprising:
4. The desired shape is a sheet having a thickness of 3 to 7 mm, The predetermined temperature and time are 150 to 170°C and 18 to 30 hours. A method for producing the silicone rubber composition for acoustic lenses according to claim 3.
5. No vulcanizing agent for curing is blended into the kneaded product. A method for producing the silicone rubber composition for acoustic lenses according to claim 3.
Citation Information
Patent Citations
Curable organosiloxane composition
JP1990102264A
Multi-layer laminate and manufacturing method therefor
JP2001322199A
Resin composition
JP2006036915A
Composite composition of inorganic oxide particle and silicone resin, transparent composite material, and method for producing the same
JP2013064163A
Condensed curable resin composition, cured article, molded body, and semiconductor device